- 2025-10-24
- Publication Date
- 2025-12-12
AI Technical Summary
Existing perovskite solar cells using organic small molecules or polymers as hole transport layer materials are expensive and have low transmission rates, which affect photoelectric conversion efficiency and long-term stability, limiting their large-area production and application.
Indolocarbazole compounds are used as hole transport layer materials. The molecular dipole moment is enhanced by the asymmetric conjugated structure system, the energy level matching is optimized, and the excessive aggregation of molecules is suppressed by benzene ring groups, so as to achieve uniform coverage and improve carrier transport efficiency.
This improved hole mobility and fill factor, enhanced the photoelectric conversion efficiency of perovskite solar cells, and reduced production costs.
Smart Images

Figure CN121108188A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the technical field of perovskite solar cells, in particular to an indolocarbazole compound, a perovskite solar cell and a preparation method. BACKGROUND
[0002] With the continuous development of new energy, perovskite solar cells, as a new type of solar cell after sensitized solar cells, have always been concerned. In the past decade, the laboratory photoelectric conversion efficiency of perovskite solar cells has been improved from 3.8% to 26.7%, which is expected to replace silicon-based solar cells and become the next generation of most potential photovoltaic products.
[0003] Perovskite solar cells generally consist of five parts: a conductive substrate, an electron transport layer, a light absorbing layer, a hole transport layer and a metal electrode. The commonly used hole transport layer material is Spiro-OMeTAD, which causes poor thermal stability of perovskite solar cells due to the presence of LiTFSI. In organic-inorganic hybrid solar cells, the hole transport layer is generally composed of organic small molecules or polymer hole transport materials. The above-mentioned organic small molecules or polymer hole transport materials are expensive and have low transmission rate, which affects the photo-thermal conversion efficiency and long-term stability of perovskite solar cells, thus limiting their large-scale production and application. SUMMARY
[0004] The present application provides an indolocarbazole compound, a perovskite solar cell and a preparation method, which effectively solves the technical problem of high cost and low transmission rate of existing organic small molecules or polymers as hole transport layer materials, resulting in poor photoelectric conversion efficiency of perovskite solar cells. At the same time, an indolocarbazole compound for the hole transport layer material of perovskite solar cells is provided, thereby effectively improving the hole mobility, fill factor and photoelectric conversion efficiency of inverted perovskite solar cells.
[0005] The first object of the present application is to provide an indolocarbazole compound, the structural general formula of which is ; wherein L1, L2 are each independently C0-C6 alkylene; R1, R2 are each independently hydrogen atom or C1-C4 alkoxy.
[0006] As a preferred embodiment, L1 is C1-C4 alkylene, L2 is C0-C2 alkylene, and R1, R2 are each independently methoxy.
[0007] As a preferred embodiment, the indolocarbazole compound is any one of the following structural formula: 、 、 、 , , , , , , , , , , , , , , .
[0008] A second objective of this invention is to provide a method for preparing the above-mentioned indolocarbazole compounds, comprising the following steps: Using compounds of Formula 1 and Formula 2 as raw materials, the compounds were dissolved in N,N-dimethylformamide at room temperature and subjected to a substitution reaction under the action of a base and a phase transfer catalyst. A brominated alkyl chain was successfully attached to the N atom of the carbazole in the asymmetric indolocarbazole molecule to obtain the compound of Formula 3.
[0009] Using compounds of formula 3 and formula 4 as raw materials, a reflux reaction is carried out at 140℃~180℃ to obtain compound 5.
[0010] Using the compound of formula 5 and trimethylbromosilane of formula 6 as starting materials, the compounds were dissolved in 1,4-dioxane and hydrolyzed at room temperature to yield the indole-carbazole compound of formula 7. The synthetic route is as follows: In this context, L1 and L2 are each independently C0 to C6 alkylene groups; R1 and R2 are each independently hydrogen atoms or C1 to C4 alkoxy groups.
[0011] In a preferred embodiment, the molar ratio of the compound of Formula 1 to the compound of Formula 2 is 1:10 to 20; the molar ratio of the compound of Formula 3 to the compound of Formula 4 is 1:10 to 30; and the molar ratio of the compound of Formula 5 to the trimethylbromosilane of Formula 6 is 1:5 to 15.
[0012] The third objective of this invention is to provide a perovskite solar cell, which comprises, from bottom to top, a bottom electrode, a hole transport layer, a perovskite light-absorbing layer, a passivation layer, an electron transport layer, and a top electrode, wherein the hole transport layer is prepared using an indole-carbazole compound as described in any one of the above-mentioned methods.
[0013] In a preferred embodiment, an indole-carbazole compound is mixed with anhydrous ethanol to obtain a coating solution with a concentration of 4 mg / mL to 12 mg / mL. The coating solution is then spin-coated onto the bottom electrode at a speed of 1000 rpm to 5000 rpm and annealed at 100°C to 150°C to obtain a hole transport layer.
[0014] In a preferred embodiment, a perovskite precursor solution is spin-coated onto the hole transport layer at a rotation speed of 500 rpm to 8000 rpm and annealed at 100°C to 300°C to obtain a perovskite light-absorbing layer; 2-phenylethylamine hydroiodate is dissolved in isopropanol to obtain a passivation solution, which is then spin-coated onto the surface of the perovskite light-absorbing layer and annealed at 100°C to obtain a passivation layer.
[0015] As a preferred embodiment, the perovskite precursor solution is prepared by dissolving PbI2, MABr, PbBr2, FAI, and CsI in a mixed solution composed of N,N-dimethylformamide and dimethyl sulfoxide, and shaking at room temperature to obtain the perovskite precursor solution.
[0016] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention provides an indole-carbazole compound, which is an organic small molecule material with an asymmetric molecular structure. Its asymmetric conjugated structure enhances the molecular dipole moment and optimizes energy level matching. Simultaneously, the benzene ring groups on the side chains of the hole transport layer molecule further suppress excessive molecular aggregation, achieving uniform coverage and efficient carrier transport, thereby significantly improving transport efficiency. Using this indole-carbazole compound as the material for the hole transport layer of perovskite solar cells effectively improves hole mobility and fill factor, thus endowing perovskite solar cells with excellent photoelectric conversion efficiency.
[0017] Furthermore, the highest occupied molecular orbital (HOMO) and lowest unoccupied molecular orbital (LUMO) energy levels of the indole-carbazole compounds provided by this invention can be precisely controlled through substituent optimization, enabling a good match between the HOMO energy level and the energy levels of the perovskite absorber layer. This excellent energy level matching significantly improves carrier collection efficiency, thereby enhancing the fill factor and photoelectric conversion efficiency.
[0018] The indole-carbazole compounds provided by this invention use inexpensive raw materials and have high synthesis yields, thereby greatly reducing the cost of perovskite solar cells. Attached Figure Description
[0019] Figure 1 This is a schematic diagram of the structure of the perovskite solar cell provided by the present invention, wherein 1 is the top electrode, 2 is the electron transport layer, 3 is the passivation layer, 4 is the perovskite light-absorbing layer, 5 is the hole transport layer, and 6 is the bottom electrode.
[0020] Figure 2 The indole-carbazole compound provided in Example 1 of this invention 1H NMR spectrum. Detailed Implementation
[0021] To enable those skilled in the art to better understand and implement the technical solutions of this invention, the invention is further described below with reference to specific embodiments. However, the embodiments are not intended to limit the invention. Unless otherwise specified, the following test methods and detection methods are conventional methods; unless otherwise specified, the reagents and raw materials are commercially available.
[0022] Existing hole transport layer materials, using small organic molecules or polymers, suffer from high costs and low transport rates, thus affecting photoelectric conversion efficiency and long-term stability, limiting their large-scale production and application. To address these technical problems, this invention provides indole-carbazole compounds, perovskite solar cells, and their preparation methods.
[0023] The technical solution of the present invention will be described in detail below.
[0024] This invention provides an indole-carbazole compound with the following general structural formula: Wherein, L1 and L2 are each independently C0-C6 alkylene groups; R1 and R2 are each independently a hydrogen atom or a C1-C4 alkoxy group. More preferably, L1 is a C1-C4 alkylene group, L2 is a C0-C2 alkylene group, and R1 and R2 are each independently a methoxy group. The specific indobenzocarbazole compounds provided in subsequent embodiments of the present invention are... , , , , , , , , , , , , , , , , or The above-mentioned indolocarbazole compounds were named Compound 1 to Compound 18, respectively.
[0025] This invention also provides a method for preparing the above-mentioned organic small molecule hole transport material, comprising the following steps: Using compounds of Formula 1 and Formula 2 as raw materials, the compounds were dissolved in N,N-dimethylformamide at room temperature and subjected to a substitution reaction under the action of a base and a phase transfer catalyst. A brominated alkyl chain was successfully attached to the N atom of the carbazole in the asymmetric indolocarbazole molecule to obtain the compound of Formula 3.
[0026] Using compounds of formula 3 and formula 4 as raw materials, a reflux reaction is carried out at 140℃~180℃ to obtain compound 5.
[0027] Using the compound of Formula 5 and trimethylbromosilane of Formula 6 as starting materials, the mixture was dissolved in 1,4-dioxane and hydrolyzed at room temperature to obtain the organic small molecule hole transport material of Formula 7. The synthetic route is as follows: .
[0028] In this context, L1 and L2 are each independently C0 to C6 alkylene groups; R1 and R2 are each independently hydrogen atoms or C1 to C4 alkoxy groups.
[0029] It should be noted that the molar ratio of the compound of Formula 1 to the compound of Formula 2 is 1:10 to 20; the molar ratio of the compound of Formula 3 to the compound of Formula 4 is 1:10 to 30; and the molar ratio of the compound of Formula 5 to the trimethylbromosilane of Formula 6 is 1:5 to 15.
[0030] This invention also provides a hole transport layer, using the indole-carbazole compound described in any one of the above claims as the material of the hole transport layer. The hole transport layer is prepared by mixing the indole-carbazole compound with anhydrous ethanol to obtain a coating solution with a concentration of 4 mg / mL to 12 mg / mL. The coating solution is then spin-coated onto the bottom electrode at a speed of 1000 rpm to 5000 rpm for 10 s to 50 s, followed by annealing at 100℃ to 150℃ for 10 min to obtain the hole transport layer.
[0031] It should be noted that, in this invention, the perovskite precursor solution is spin-coated onto the hole transport layer at a rotation speed of 500 rpm to 8000 rpm, and annealed at 100℃ to 300℃ for 20 min to 60 min to obtain the perovskite light-absorbing layer; 2-phenylethylamine hydroiodate is dissolved in isopropanol to obtain a passivation solution, which is then spin-coated onto the surface of the perovskite light-absorbing layer at a speed of 5000 rpm for 20 s to 30 s, and annealed at 100℃ for 5 min to obtain the passivation layer. The perovskite precursor solution is prepared by dissolving 1.1 mol / L PbI2, 0.2 mol / L MABr, 0.2 mol / L PbBr2, 1 mol / L FAI, and 0.06 mol / L CsI in 1250 μL of a mixed solution composed of N,N-dimethylformamide and dimethyl sulfoxide in a volume ratio of 4:1, and shaking at room temperature for 3 h.
[0032] The invention will now be described in detail through the following embodiments and comparative examples.
[0033] Example 1 An indolocarbazole compound with the following structural formula: .
[0034] The preparation method of the above-mentioned indolocarbazole compounds includes the following steps: Synthesis of S1, Intermediate 1: 0.9 mL of 1,4-dibromobutane and 0.15 g of NaH were dissolved in a flask containing 20 mL of N,N-dimethylformamide (DMF). 0.83 g (2.51 mmol) of 5-phenyl-5,7-dihydroindole[2,3-b]carbazole was dissolved in 3 mL of DMF and slowly added using a syringe. The reaction was carried out at room temperature for 24 h. After the reaction, the mixture was extracted with dichloromethane to obtain the organic phase. The organic phase was dried with anhydrous sodium sulfate, and the solvent was removed by vacuum distillation to obtain the crude product. The crude product was separated by chromatographic column chromatography using petroleum ether / ethyl acetate at a volume ratio of 10:1 to obtain 0.89 g of Intermediate 1, with a yield of 79%. The synthetic route is as follows:
[0035] .
[0036] Synthesis of S2, Intermediate 2: 0.89 g (2.0 mmol) of the above intermediate 1 was dissolved in 6 mL of triethyl phosphite, and the reaction solution was heated under reflux for 18 h. After the reaction was complete, the solvent was removed by vacuum distillation to obtain the crude product. The crude product was separated by column chromatography using petroleum ether / ethyl acetate at a volume ratio of 1:6 as the eluent to obtain 0.82 g of intermediate 2, with a yield of 76%. The synthetic route is as follows:
[0037] .
[0038] Synthesis of S3, Compound 7: 0.76 g (1.5 mmol) of the above intermediate 2 and 15 mL of 1,4-dioxane were added to a three-necked flask. Under nitrogen protection, 1.72 mL of trimethylbromosilane was added dropwise, and the reaction was carried out at 25 °C for 24 h. After the reaction was completed, the solvent was removed by vacuum distillation, and then dissolved in 10 mL of methanol. 15 mL of deionized water was added dropwise until the solution became turbid. The mixture was stirred for another 15 h, and the solid was filtered off. The solid was washed with deionized water and dried to give 0.56 g of the product, with a yield of 82%. The synthetic route is as follows: .
[0039] Example 2 An indolocarbazole compound with the following structural formula: .
[0040] The preparation method of the above-mentioned indolocarbazole compounds includes the following steps: Synthesis of S1, Intermediate 1: 3.9 mmol (1 g) of 5,7-dihydroindole[2,3-b]carbazole, 0.4 mL of 2-bromoethylbenzene, 0.195 mmol of tris(dibenzylacetone)dipalladium, 0.39 mmol of tri-tert-butylphosphine, and 7.8 mmol of sodium tert-butoxide were dissolved in a double-necked flask containing 30 mL of toluene solvent. The mixture was then heated at 135 °C for 15 h. After the reaction was complete, the mixture was extracted with dichloromethane to obtain the organic phase. The organic phase was dried with anhydrous sodium sulfate, and the solvent was removed by vacuum distillation to obtain the crude product. The crude product was separated by chromatographic column chromatography using petroleum ether / dichloromethane at a volume ratio of 1:2 as the eluent to obtain 0.6 g of Intermediate 1, with a yield of 53%. The synthetic route is as follows:
[0041] .
[0042] Synthesis of S2, Intermediate 2: 0.9 mL of 1,4-dibromobutane and 0.15 g of NaH were dissolved in a flask containing 20 mL of DMF. 2.51 mmol of the above intermediate 1 was dissolved in 3 mL of DMF and slowly added using a syringe. The reaction was carried out at room temperature for 24 h. After the reaction was complete, the mixture was extracted with dichloromethane to obtain the organic phase. The organic phase was dried with anhydrous sodium sulfate, and the solvent was removed by vacuum distillation to obtain the crude product. The crude product was separated by chromatographic column chromatography using petroleum ether / ethyl acetate at a volume ratio of 10:1 to obtain 0.85 g of intermediate 1, with a yield of 78%. The synthetic route is as follows:
[0043] .
[0044] Synthesis of S3, Intermediate 3: 0.89 g (2.0 mmol) of the above intermediate 2 was dissolved in 6 mL of triethyl phosphite, and the reaction solution was heated under reflux for 18 h. After the reaction was complete, the solvent was removed by vacuum distillation to obtain the crude product. The crude product was separated by column chromatography using petroleum ether / ethyl acetate at a volume ratio of 1:6 as the eluent to obtain 0.82 g of intermediate 3, with a yield of 76%. The synthetic route is as follows:
[0045] .
[0046] Synthesis of S4, Compound 9: 1.5 mmol of the above intermediate 3 and 15 mL of 1,4-dioxane were added to a three-necked flask. Under nitrogen protection, 1.72 mL of trimethylbromosilane was added dropwise, and the reaction was carried out at 25 °C for 24 h. After the reaction was completed, the solvent was removed by vacuum distillation, and then dissolved in 10 mL of methanol. 15 mL of deionized water was added dropwise until the solution became turbid. The mixture was stirred for another 15 h, and the solid was filtered off. The solid was washed with deionized water and dried to give 0.52 g of the product, with a yield of 81%. The synthetic route is as follows: .
[0047] Example 3 An indolocarbazole compound with the following structural formula: .
[0048] The preparation method of the above-mentioned indolocarbazole compounds includes the following steps: Synthesis of S1, Intermediate 1: 3.9 mmol (1 g) of 5,7-dihydroindole[2,3-b]carbazole, 0.4 mL of 2-bromoethylbenzene, 0.195 mmol of tris(dibenzylacetone)dipalladium, 0.39 mmol of tri-tert-butylphosphine, and 7.8 mmol of sodium tert-butoxide were dissolved in a two-necked flask containing 30 mL of toluene solvent. The mixture was then heated at 135 °C for 15 h. After the reaction was complete, the mixture was extracted with dichloromethane to obtain the organic phase. The organic phase was dried with anhydrous sodium sulfate, and the solvent was removed by vacuum distillation to obtain the crude product. The crude product was separated by chromatographic column chromatography using petroleum ether / dichloromethane at a volume ratio of 1:2 as the eluent to obtain 0.6 g of Intermediate 1, with a yield of 53%. The synthetic route is as follows:
[0049] .
[0050] Synthesis of S2, Intermediate 2: 0.9 mL of 1,4-dibromobutane and 0.15 g of NaH were dissolved in a flask containing 20 mL of DMF. 2.51 mmol of the above intermediate 1 was dissolved in 3 mL of DMF and slowly added using a syringe. The reaction was carried out at room temperature for 24 h. After the reaction was complete, the mixture was extracted with dichloromethane to obtain the organic phase. The organic phase was dried with anhydrous sodium sulfate, and the solvent was removed by vacuum distillation to obtain the crude product. The crude product was separated by chromatographic column chromatography using petroleum ether / ethyl acetate at a volume ratio of 10:1 to obtain 0.85 g of intermediate 1, with a yield of 78%. The synthetic route is as follows:
[0051] .
[0052] Synthesis of S3, Intermediate 3: 0.89 g (2.0 mmol) of the above intermediate 2 was dissolved in 6 mL of triethyl phosphite, and the reaction solution was heated under reflux for 18 h. After the reaction was complete, the solvent was removed by vacuum distillation to obtain the crude product. The crude product was separated by column chromatography using petroleum ether / ethyl acetate at a volume ratio of 1:6 as the eluent to obtain 0.82 g of intermediate 2, with a yield of 76%. The synthetic route is as follows:
[0053] .
[0054] Synthesis of S4, Compound 18: 1.5 mmol of the above intermediate 3 and 15 mL of 1,4-dioxane were added to a three-necked flask. Under nitrogen protection, 1.72 mL of trimethylbromosilane was added dropwise, and the reaction was carried out at 25 °C for 24 h. After the reaction was completed, the solvent was removed by vacuum distillation, and then dissolved in 10 mL of methanol. 15 mL of deionized water was added dropwise until the solution became turbid. The mixture was stirred for another 15 h, and the solid was filtered off. The solid was washed with deionized water and dried to give 0.52 g of the product, with a yield of 81%. The synthetic route is as follows: .
[0055] Example 4 An indole-carbazole compound, namely compound 1, has the following structural formula: .
[0056] The preparation method of the above-mentioned indolocarbazole compounds is to prepare compound 1 according to the preparation method of compound 7 in Example 1, except that 1,4-dibromobutane in S1 of Example 1 is replaced with 1,2-dibromobutane.
[0057] Example 5 An indole-carbazole compound, namely compound 4, has the following structural formula: .
[0058] The preparation method of the above-mentioned indolocarbazole compounds is the same as the preparation method of compound 7 in Example 1 to prepare compound 4, except that 1,4-dibromobutane in S1 of Example 1 is replaced with 1,3-dibromopropane.
[0059] Example 6 An indole-carbazole compound, namely compound 2, has the following structural formula: .
[0060] The preparation method of the above-mentioned indolocarbazole compounds is the same as the preparation method of compound 9 in Example 2, except that 2-bromoethylbenzene in S1 of Example 2 is replaced with bromomethylbenzene and 1,4-dibromoethane in S2 is replaced with 1,2-dibromoethane.
[0061] Example 7 An indolocarbazole compound, namely compound 3, has the following structural formula: .
[0062] The preparation method of the above-mentioned indolocarbazole compounds is the same as the preparation method of compound 9 in Example 2, except that 1,4-dibromoethane in S2 of Example 2 is replaced with 1,2-dibromoethane.
[0063] Example 8 An indolocarbazole compound, namely compound 5, has the following structural formula: .
[0064] The preparation method of the above-mentioned indolocarbazole compounds is the same as the preparation method of compound 9 in Example 2, except that 2-bromoethylbenzene in S1 of Example 2 is replaced with bromomethylbenzene and 1,4-dibromoethane in S2 is replaced with 1,3-dibromopropane.
[0065] Example 9 An indole-carbazole compound, namely compound 6, has the following structural formula: .
[0066] The preparation method of the above-mentioned indolocarbazole compounds is the same as the preparation method of compound 9 in Example 2, except that 1,4-dibromoethane in S2 of Example 2 is replaced with 1,3-dibromopropane.
[0067] Example 10 An indole-carbazole compound, namely compound 8, has the following structural formula: .
[0068] The preparation method of the above-mentioned indolocarbazole compounds is the same as the preparation method of compound 9 in Example 2, except that 2-bromoethylbenzene in S1 of Example 2 is replaced with bromomethylbenzene.
[0069] Example 11 An indole-carbazole compound, namely compound 10, has the following structural formula: .
[0070] The preparation method of the above-mentioned indolocarbazole compounds is to prepare compound 10 according to the preparation method of compound 18 in Example 3, except that 2-bromoethylbenzene in S1 of Example 3 is replaced with 1-bromobenzene and 1,4-dibromobutane in S2 is replaced with 1,2-dibromoethane.
[0071] Example 12 An indole-carbazole compound, namely compound 13, has the following structural formula: .
[0072] The preparation method of the above-mentioned indolocarbazole compounds is to prepare compound 13 according to the preparation method of compound 18 in Example 3, except that 2-bromoethylbenzene in S1 of Example 3 is replaced with 1-bromobenzene and 1,4-dibromobutane in S2 is replaced with 1,3-dibromopropane.
[0073] Example 13 An indole-carbazole compound, namely compound 16, has the following structural formula: .
[0074] The preparation method of the above-mentioned indolocarbazole compounds is to prepare compound 16 according to the preparation method of compound 18 in Example 3, except that 2-bromoethylbenzene in S1 of Example 3 is replaced with 1-bromobenzene.
[0075] Example 14 An indole-carbazole compound, namely compound 11, has the following structural formula: .
[0076] The preparation method of the above-mentioned indolocarbazole compounds is to prepare compound 11 according to the preparation method of compound 18 in Example 3, except that 2-bromoethylbenzene in S1 of Example 3 is replaced with bromomethylbenzene and 1,4-dibromobutane in S2 is replaced with 1,2-dibromoethane.
[0077] Example 15 An indole-carbazole compound, namely compound 12, has the following structural formula: .
[0078] The preparation method of the above-mentioned indolocarbazole compounds is to prepare compound 12 according to the preparation method of compound 18 in Example 3, except that 1,4-dibromobutane in S2 of Example 3 is replaced with 1,2-dibromoethane.
[0079] Example 16 An indole-carbazole compound, namely compound 14, has the following structural formula: .
[0080] The preparation method of the above-mentioned indolocarbazole compounds is to prepare compound 14 according to the preparation method of compound 18 in Example 3, except that 2-bromoethylbenzene in S1 of Example 3 is replaced with bromomethylbenzene, and 1,4-dibromobutane in S2 is replaced with 1,3-dibromopropane.
[0081] Example 17 An indole-carbazole compound, namely compound 15, has the following structural formula: .
[0082] The preparation method of the above-mentioned indolocarbazole compounds is to prepare compound 15 according to the preparation method of compound 18 in Example 3, except that 1,4-dibromobutane in S2 of Example 3 is replaced with 1,3-dibromopropane.
[0083] Example 18 An indole-carbazole compound, namely compound 17, has the following structural formula: .
[0084] The preparation method of the above-mentioned indolocarbazole compounds is to prepare compound 17 according to the preparation method of compound 18 in Example 3, except that 2-bromoethylbenzene in S1 of Example 3 is replaced with bromomethylbenzene.
[0085] Application Example 1 A perovskite solar cell comprises, from bottom to top, a bottom electrode, a hole transport layer, a perovskite light-absorbing layer, a passivation layer, an electron transport layer, and a top electrode.
[0086] The above-mentioned method for preparing perovskite solar cells includes the following steps: S1, Treatment of the bottom electrode: Using conductive glass FTO or ITO as the bottom electrode, clean it with washing solution, ultrapure water, ethanol and ultrasonic for 20 minutes respectively. Then dry the conductive glass with an air gun and store it in a drying cabinet. Before use, place the cleaned conductive glass in an ultraviolet ozone cleaner for 30 minutes to enhance the wettability of the conductive glass surface.
[0087] S2, Preparation of hole transport layer: Compound 7 prepared in Example 1 was used as the material of hole transport layer. Compound 7 prepared in Example 1 was mixed with anhydrous ethanol to obtain a coating solution with a concentration of 5 mg / mL. 100 μL of the coating solution was taken onto the bottom electrode by pipetting and spin-coated at 3000 rpm for 30 s. After spin-coating, the solution was annealed on a hot plate at 100 ℃ for 10 min and then naturally cooled to obtain hole transport layer.
[0088] S3, Preparation of the perovskite light-absorbing layer: Dissolve 1.1 mol / L PbI2, 0.2 mol / L MABr, 0.2 mol / L PbBr2, 1 mol / L FAI, and 0.06 mol / L CsI in 1250 μL of a mixed solution of N,N-dimethylformamide and dimethyl sulfoxide in a volume ratio of 4:1. Shake at room temperature for 3 h to obtain a perovskite precursor solution with a concentration of 1.8 mol / L. Drop the perovskite precursor solution onto the hole transport layer, let it stand, and spin coat at 5000 rpm for 40 s. Add 150 μL of chlorobenzene antisolvent 10 s before the end of spin coating. After spin coating, anneal on a hot plate at 200℃ for 50 min to obtain the perovskite light-absorbing layer.
[0089] S4, Preparation of passivation layer: Dissolve 2-phenylethylamine hydroiodate in isopropanol to obtain a passivation solution with a concentration of 0.5 mg / mL. Use a pipette to measure 50 μL of the solution and drop it onto the surface of the perovskite light-absorbing layer. Spin-coat at 5000 rpm for 30 s using a dynamic coating method. Anneal at 100℃ for 5 min to obtain the passivation layer.
[0090] S5, Fabrication of the electron transport layer: An electron transport layer material is deposited on the passivation layer using vacuum evaporation to form the electron transport layer; C60 and BCP are used as the electron transport layer materials, and the mixture is deposited at 5×10⁻⁶... -4 With a vacuum of Pa and an evaporation rate of 0.1 A / s to 0.2 A / s, the electron transport layer material was deposited onto the passivation layer to obtain an electron transport layer with a thickness of 250 nm.
[0091] S6, Fabrication of the top electrode: The top electrode material is deposited on the electron transport layer using vacuum evaporation to form the top electrode; silver is used as the top electrode material, and the deposition process is carried out at 5 × 10⁻⁶. -4 With a vacuum of Pa and an evaporation rate of 1 A / s to 2 A / s, silver was deposited onto the electron transport layer to obtain a top electrode with a thickness of 1200 nm.
[0092] Application Example 2 The difference compared to Application Example 1 is that in S2, a coating solution with a concentration of 4 mg / mL is obtained.
[0093] A perovskite solar cell comprises, from bottom to top, a bottom electrode, a hole transport layer, a perovskite light-absorbing layer, a passivation layer, an electron transport layer, and a top electrode.
[0094] The above-mentioned method for preparing perovskite solar cells includes the following steps: S1, Treatment of the bottom electrode: Same as in Application Example 1.
[0095] S2, Preparation of hole transport layer: Compound 9 prepared in Example 2 was used as the material of hole transport layer. Compound 9 prepared in Example 1 was mixed with anhydrous ethanol to obtain a coating solution with a concentration of 4 mg / mL. 100 μL of the coating solution was taken onto the bottom electrode by pipetting and spin-coated at 3000 rpm for 30 s. After spin-coating, the solution was annealed on a hot plate at 100°C for 10 min and then naturally cooled to obtain hole transport layer.
[0096] S3 to S6 are the same as in Application Example 1.
[0097] Application Example 3 The difference compared to Application Example 1 is that in S2, a coating solution with a concentration of 6 mg / mL is obtained.
[0098] A perovskite solar cell comprises, from bottom to top, a bottom electrode, a hole transport layer, a perovskite light-absorbing layer, a passivation layer, an electron transport layer, and a top electrode.
[0099] The above-mentioned method for preparing perovskite solar cells includes the following steps: S1, Treatment of the bottom electrode: Same as in Application Example 1.
[0100] S2, Preparation of hole transport layer: Compound 18 prepared in Example 3 was used as the material of hole transport layer. Compound 18 prepared in Example 3 was mixed with anhydrous ethanol to obtain a coating solution with a concentration of 6 mg / mL. 100 μL of the coating solution was taken onto the bottom electrode by pipetting and spin-coated at 3000 rpm for 30 s. After spin-coating, the solution was annealed on a hot plate at 100°C for 10 min and then naturally cooled to obtain hole transport layer.
[0101] S3 to S6 are the same as in Application Example 1.
[0102] Application Example 4 The difference compared to Application Example 1 is that in S2, a coating solution with a concentration of 8 mg / mL is obtained.
[0103] A perovskite solar cell comprises, from bottom to top, a bottom electrode, a hole transport layer, a perovskite light-absorbing layer, a passivation layer, an electron transport layer, and a top electrode.
[0104] The above-mentioned method for preparing perovskite solar cells includes the following steps: S1, Treatment of the bottom electrode: Same as in Application Example 1.
[0105] S2, Preparation of hole transport layer: Compound 1 prepared in Example 4 is used as the material of hole transport layer. Compound 1 prepared in Example 4 is mixed with anhydrous ethanol to obtain a coating solution with a concentration of 8 mg / mL. 100 μL of the coating solution is taken onto the bottom electrode by pipetting and spin-coated at 3000 rpm for 30 s. After spin-coating, it is annealed on a hot plate at 100°C for 10 min and then naturally cooled to obtain hole transport layer.
[0106] S3 to S6 are the same as in Application Example 1.
[0107] Application Example 5 The difference compared to Application Example 1 is that in S2, a coating solution with a concentration of 10 mg / mL is obtained.
[0108] A perovskite solar cell comprises, from bottom to top, a bottom electrode, a hole transport layer, a perovskite light-absorbing layer, a passivation layer, an electron transport layer, and a top electrode.
[0109] The above-mentioned method for preparing perovskite solar cells includes the following steps: S1, Treatment of the bottom electrode: Same as in Application Example 1.
[0110] S2, Preparation of hole transport layer: Compound 6 prepared in Example 9 is used as the material of hole transport layer. Compound 6 prepared in Example 9 is mixed with anhydrous ethanol to obtain a coating solution with a concentration of 10 mg / mL. 100 μL of the coating solution is taken onto the bottom electrode by pipetting and spin-coated at 3000 rpm for 30 s. After spin-coating, it is annealed on a hot plate at 100°C for 10 min and then naturally cooled to obtain hole transport layer.
[0111] S3 to S6 are the same as in Application Example 1.
[0112] Application Example 6 The difference compared to Application Example 1 is that in S2, a coating solution with a concentration of 12 mg / mL is obtained.
[0113] A perovskite solar cell comprises, from bottom to top, a bottom electrode, a hole transport layer, a perovskite light-absorbing layer, a passivation layer, an electron transport layer, and a top electrode.
[0114] The above-mentioned method for preparing perovskite solar cells includes the following steps: S1, Treatment of the bottom electrode: Same as in Application Example 1.
[0115] S2, Preparation of hole transport layer: Using the material of the hole transport layer of compound 16 prepared in Example 13, compound 16 prepared in Example 13 was mixed with anhydrous ethanol to obtain a coating solution with a concentration of 12 mg / mL. 100 μL of the coating solution was taken onto the bottom electrode by pipetting and spin-coated at 3000 rpm for 30 s. After spin-coating, it was annealed on a hot plate at 100°C for 10 min and then naturally cooled to obtain the hole transport layer.
[0116] S3 to S6 are the same as in Application Example 1.
[0117] To further illustrate the technical effects of the present invention, a comparative example is also provided, as follows: Application Comparative Example 1 The difference from Application Example 1 is that in S2, the hole transport layer material is compound 4-(3,6-dimethyl-9H-carbazole-9-yl)butylphosphonic acid, namely Me-4PACz.
[0118] A perovskite solar cell comprises, from bottom to top, a bottom electrode, a hole transport layer, a perovskite light-absorbing layer, a passivation layer, an electron transport layer, and a top electrode.
[0119] The above-mentioned method for preparing perovskite solar cells includes the following steps: S1, Treatment of the bottom electrode: Same as in Application Example 1.
[0120] S2, Preparation of hole transport layer: Using compound Me-4PACz as the material of hole transport layer, compound Me-4PACz is mixed with anhydrous ethanol to obtain a coating solution with a concentration of 5 mg / mL. 100 μL of coating solution is taken onto the bottom electrode using a pipette and spin-coated at 3000 rpm for 30 s. After spin-coating, it is annealed on a hot plate at 100℃ for 10 min and then naturally cooled to obtain hole transport layer.
[0121] S3 to S6 are the same as in Application Example 1.
[0122] The performance of the perovskite solar cells prepared in the above application examples and application comparison example 1 was tested, and the results are shown in Table 1 below.
[0123] Table 1 Performance of the perovskite solar cell of the present invention As shown in Table 1, using the indole-carbazole compounds provided by this invention as the hole transport layer in perovskite solar cells effectively improves the hole transport rate and fill factor, thereby endowing perovskite solar cells with excellent photoelectric conversion efficiency. The perovskite solar cell prepared using Example 6 of this invention has a photoelectric conversion efficiency of 25.19%, and the perovskite solar cells obtained using compounds 1 to 18 of Examples 1 to 18 of this invention as hole transport layer materials all have photoelectric conversion efficiencies greater than 24.0%, reaching 24.25% to 25.19%. In contrast, the perovskite solar cell prepared using existing hole transport materials in Comparative Example 1 has a photoelectric conversion efficiency of only 23.19%. Therefore, it is evident that the indole-carbazole compounds provided by this invention, as small organic molecules, can significantly improve the photoelectric conversion efficiency of perovskite solar cells.
[0124] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. Therefore, if these modifications and variations fall within the scope of the claims of this invention and their equivalents, this invention also intends to include these modifications and variations.
Claims
1. An indolocarbazole compound, characterized in that, Its general structural formula is: Wherein, L1 and L2 are each independently C0 to C6 alkylene groups; R1 and R2 are each independently hydrogen atoms or C1 to C4 alkoxy groups.
2. The indolocarbazole compound according to claim 1, characterized in that, L1 is a C1-C4 alkylene group, L2 is a C0-C2 alkylene group, and R1 and R2 are each independently methoxy groups.
3. The indolocarbazole compound according to claim 1, characterized in that, The indolocarbazole compound is any one of the following structural formulas: , , , , , , , , , , , , , , , , , .
4. A method for preparing the indolocarbazole compound according to claim 1, characterized in that, Includes the following steps: Using compounds of Formula 1 and Formula 2 as raw materials, the compounds were dissolved in N,N-dimethylformamide at room temperature and subjected to a substitution reaction under the action of a base and a phase transfer catalyst to attach a brominated alkyl chain to the N atom of the indole-carbazole molecule, thus obtaining the compound of Formula 3. Using the compounds of Formula 3 and Formula 4 as raw materials, a reflux reaction was carried out at 140℃~180℃ to obtain the compound of Formula 5. Using the compound of formula 5 and trimethylbromosilane of formula 6 as starting materials, the compounds were dissolved in 1,4-dioxane and hydrolyzed at room temperature to yield the indole-carbazole compound of formula 7. The synthetic route is as follows: In this context, L1 and L2 are each independently C0 to C6 alkylene groups; R1 and R2 are each independently hydrogen atoms or C1 to C4 alkoxy groups.
5. The method for preparing indolocarbazole compounds according to claim 4, characterized in that, The molar ratio of the compound of Formula 1 to the compound of Formula 2 is 1:10 to 20; the molar ratio of the compound of Formula 3 to the compound of Formula 4 is 1:10 to 30; and the molar ratio of the compound of Formula 5 to the trimethylbromosilane of Formula 6 is 1:5 to 15.
6. A perovskite solar cell, comprising, from bottom to top, a bottom electrode, a hole transport layer, a perovskite light-absorbing layer, a passivation layer, an electron transport layer, and a top electrode, characterized in that, The hole transport layer is prepared using an indole-carbazole compound as described in any one of claims 1 to 3.
7. The perovskite solar cell according to claim 6, characterized in that, The hole transport layer is obtained by mixing an indole-carbazole compound with anhydrous ethanol to obtain a coating solution with a concentration of 4 mg / mL to 12 mg / mL, spin-coating the coating solution onto the bottom electrode at a speed of 1000 rpm to 5000 rpm, and annealing at 100℃ to 150℃.
8. The perovskite solar cell according to claim 7, characterized in that, The perovskite light-absorbing layer is prepared by spin-coating a perovskite precursor solution onto the hole transport layer at a rotation speed of 500 rpm to 8000 rpm and annealing at 100℃ to 300℃ to obtain the perovskite light-absorbing layer. The passivation layer is obtained by dissolving 2-phenylethylamine hydroiodate in isopropanol to obtain a passivation solution, spin-coating the passivation solution onto the surface of the perovskite light-absorbing layer, and annealing it at 100°C.
9. The perovskite solar cell according to claim 8, characterized in that, The perovskite precursor solution is prepared by dissolving PbI2, MABr, PbBr2, FAI and CsI in a mixed solution composed of N,N-dimethylformamide and dimethyl sulfoxide, and shaking at room temperature to obtain the perovskite precursor solution.
Citation Information
Patent Citations
Indolocarbazole-based self-assembled monomolecular layer hole transport material and synthesis method and application thereof
CN114874263A
Indole-containing phosphonic acid compound, application thereof and photoelectric device
CN117659085A
Indolo [2, 3-A] carbazole compound as well as preparation method and application thereof
CN118063511A
Perovskite cell and preparation method thereof, laminated cell and photovoltaic module
CN120224908A
Hole transport layer material for inverted perovskite solar cell, inverted perovskite solar cell and application
CN120365320A
Cited By
Crystalline silicon / perovskite laminated solar cell and preparation method thereof
CN121968884A
Indolocarbazole heterocyclic derivative, preparation method and trans-perovskite solar cell
CN122036802A