Regulation and control method for efficiently and rapidly improving concentration of manganese ions in zinc electrolytic solution
By adding reducing agents and synergistically controlling electrolysis parameters in the wet leaching process, the problem of insufficient manganese ions in zinc electrolysis was solved, and the concentration of manganese ions in the zinc electrolysis solution was rapidly increased. This ensured the stability of the anode protective film and the qualification rate of zinc products, and reduced the waste of manganese resources.
Patent Information
- Application Number
- CN202511345803.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-19
- Publication Date
- 2025-12-23
AI Technical Summary
Existing technologies lack a synergistic control mechanism between electrolysis and wet processes, resulting in insufficient manganese ion concentration, failure of the anode protective film during zinc electrolysis, excessive lead content in zinc, and in severe cases, failure to produce qualified zinc ingots, as well as serious waste of manganese resources.
By adding reducing substances such as zinc particles and zinc concentrate in the wet leaching process, manganese dioxide is reduced to soluble Mn2+. Combined with the coordinated control of electrolysis parameters, such as controlling current density, extending the electrolysis cycle and temperature, using manual scraping to protect the anode plate, and adjusting the dosage of reducing agent through dynamic monitoring and feedback, the concentration of manganese ions can be rapidly increased.
It significantly increased the concentration of manganese ions in the zinc electrolytic solution, reduced the manganese content in the lead-silver slag, ensured a 100% yield of 0# zinc, reduced manganese salt consumption, and achieved efficient utilization of manganese resources and stability of the electrolysis process.
Smart Images

Figure CN121183376A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of zinc electrolysis technology, and in particular to a method for efficiently and rapidly increasing the concentration of manganese ions in a zinc electrolysis solution. Background Technology
[0002] In the hydrometallurgical zinc smelting process, manganese ions play a crucial role in maintaining anode stability. Mn2+ in the electrolyte... + The anode is oxidized to form a protective MnO2 film, which prevents corrosion of the lead-silver alloy anode plate. If the manganese ion concentration is insufficient (<2g / L), the protective film will loosen and fail, causing lead from the anode to dissolve and migrate to the cathode, resulting in excessive lead content in the precipitated zinc, and in severe cases, preventing the production of #0 zinc ingots. Traditional manganese ion control mainly relies on adding materials such as manganese carbonate and manganese ore powder in the wet process, but there are two major bottlenecks in actual production:
[0003] Firstly, when there is an increase in oxidizing substances or a lack of reducing substances in the system, a large amount of manganese enters the lead-silver slag (containing Mn > 2%) in the form of insoluble MnO2, resulting in a waste of manganese resources and system depletion.
[0004] Secondly, parameters such as current density and temperature in the electrolysis process are strongly correlated with the MnO2 deposition efficiency at the anode, while existing technologies lack a synergistic control mechanism between the electrolysis and wet processes.
[0005] In March 2023, a zinc smelter experienced a continuous depletion of manganese ions (Mn < 1 g / L in the electrolyte). Despite adding 139 tons of manganese carbonate, it was still unable to prevent the zinc and lead content from exceeding the standard. Only after adopting a reducing agent to enhance dissolution and linking the electrolysis parameters was the manganese concentration increased from 0.6 g / L to over 1.6 g / L within 7 days.
[0006] In summary, developing a rapid manganese extraction method that integrates efficient utilization of reducing agents, optimization of the electrolysis process, and real-time feedback is of great significance for ensuring the stability of zinc electrolysis production. Therefore, this application proposes a method for efficiently and rapidly increasing the concentration of manganese ions in the zinc electrolysis solution. Summary of the Invention
[0007] The purpose of this invention is to address the problem in the prior art of lacking a synergistic control mechanism for electrolysis and wet processes, and to propose a method for efficiently and rapidly increasing the concentration of manganese ions in zinc electrolytic solutions.
[0008] The technical solution of this invention: A method for efficiently and rapidly increasing the concentration of manganese ions in a zinc electrolytic solution, comprising the following steps:
[0009] A. Reducing agent addition: In the wet leaching process, a reducing agent is added to the material system containing manganese dioxide to reduce manganese dioxide to soluble Mn. 2+The reducing agent is zinc particles and / or contains Fe2+. + Zinc concentrate;
[0010] B. Coordinated control of electrolysis parameters: During the electrolysis process, the current density is controlled between 100 and 300 A / m. 2 The electrolysis cycle is extended to 36-48 hours, the electrolyte temperature is controlled at 34-36℃, and the cathode plate loading is reduced to less than 44 plates / tank.
[0011] C. Anode plate protection operation: The anode plates are manually scraped instead of mechanically flattened. The anode plates are then loaded into the electrolytic cell within 10 minutes after scraping.
[0012] D. Dynamic monitoring and feedback:
[0013] ① The manganese concentration of the electrolyte is detected after filtration through a filter membrane, and the manganese content of the lead-silver slag is monitored daily;
[0014] ② When the manganese content of lead-silver slag is >1% and the manganese concentration of the middle and upper clarifiers is <2g / L, increase the amount of reducing agent added;
[0015] ③ When the manganese concentration in the waste electrolyte is <1.5g / L, add manganese sulfate or manganese carbonate to the clean electrolyte section.
[0016] Optionally, the amount of zinc particles added in step A is 60–100 kg / h, and must simultaneously meet the following conditions: slurry flow rate > 150 m³ / h, slurry pH = 2.0–2.5, Fe... 3+ >10g / L, copper ion concentration in solution ≥1g / L.
[0017] Optionally, the amount of zinc concentrate added in step A is 4.5–9 tons / day, and its Fe2+ + Content ≥15wt%, S 2 - Content ≥ 8wt%.
[0018] Optionally, the reducing agent in step A can be added in the following way:
[0019] When the system manganese concentration is <1g / L, zinc particles and zinc concentrate are added together, with zinc particles at 80-100kg / h and zinc concentrate at 6-9 tons / day;
[0020] When the system manganese concentration is 1-2 g / L, zinc concentrate is added as a single agent at a dosage of 4.5-6 tons / day.
[0021] Stop adding reducing agent when the system manganese concentration is >2g / L.
[0022] Optionally, in step A, the residual sulfur content of the roasted sand is simultaneously controlled to be 1.0% to 1.5%, specifically by: lowering the roasting temperature when the manganese concentration of the supernatant is <2g / L to increase the residual sulfur content to 1.0% to 1.5%; and raising the roasting temperature when the manganese concentration of the supernatant is ≥3g / L to reduce the residual sulfur content to 0.7% to 1.0%.
[0023] Optionally, the current density control in step B adopts a staged strategy:
[0024] When the manganese concentration is <1 g / L, the current density drops to 100-200 A / m. 2 ;
[0025] When the manganese concentration is 1–1.5 g / L, the current density increases to 200–300 A / m. 2 ;
[0026] When the manganese concentration is >1.5 g / L, the current density recovers to 400 A / m. 2 above.
[0027] Optionally, step D may also include:
[0028] The manganese concentration in the pre- and post-liquid sluices of the electrolytic cell was measured twice a week, and the manganese depletion amount ΔMn was calculated.
[0029] When ΔMn>1000mg / L, initiate the electrolysis parameter adjustment in step B.
[0030] Optionally, in step D, the amount of manganese sulfate added is 2 to 3 tons / day, and the amount of manganese carbonate added is 3 to 8 tons / day.
[0031] Compared with the prior art, this application includes at least one of the following beneficial technical effects:
[0032] 1. This invention solves the problem of manganese resource waste: through a composite reduction system of metallic zinc particles and zinc concentrate, the manganese content of lead-silver slag is reduced from more than 2% in traditional processes to 0.3% to 0.5%, which greatly improves the manganese leaching efficiency and significantly reduces the amount of purchased manganese salts such as manganese carbonate.
[0033] 2. By using a current density gradation control strategy and dynamic matching with the residual sulfur content of roasted sand, the excessive precipitation of MnO2 at the anode is suppressed by low current density when the manganese concentration is <1g / L, which greatly shortens the system recovery time.
[0034] 3. Using manual scraping plates instead of mechanical flattening avoids lead contamination caused by damage to the anode protective film, allowing the 0# zinc compliance rate to recover from 0% during the accident period to 100%, reducing tank shutdown losses.
[0035] 4. Using the manganese content of lead-silver slag and the electrolytic depletion amount ΔMn as dual feedback signals, the real-time optimization of the reducing agent dosage and current density is driven to achieve long-term stability of manganese balance.
[0036] In summary, this invention significantly increases the concentration of manganese ions in the solution in a short time by using a combination of wet slurry and electrolysis, thereby greatly reducing the manganese content in lead-silver slag and achieving a 100% compliance rate for 0# zinc. At the same time, it significantly reduces the consumption of manganese salts, achieving good technical results and economic benefits. Attached Figure Description
[0037] Figure 1 A graph showing the relationship between the yield of Mn in the first system, the Mn in the second system, and the 0# zinc after manganese extraction and the change over time.
[0038] Figure 2 This is a graph showing the relationship between the first-system Mn, the second-system Mn, and the precipitated zinc Pb over time in a wet process.
[0039] Figure 3 This is a graph showing the relationship between the Mn content in the lead-silver slag and time in this invention;
[0040] Figure 4 This is a graph showing the relationship between manganese concentration at various points in the wet process and time.
[0041] Figure 5 A graph showing the relationship between the first system Mn, the second system Mn, and the precipitated zinc Pb over time after manganese extraction;
[0042] Figure 6 A schematic diagram of the anode plate before it is flattened;
[0043] Figure 7 This is a schematic diagram of the anode plate after it has been flattened. Detailed Implementation
[0044] The technical solution of the present invention will be further described below with reference to the accompanying drawings and specific embodiments.
[0045] Example 1
[0046] This invention proposes a method for efficiently and rapidly increasing the concentration of manganese ions in a zinc electrolytic solution, comprising the following steps:
[0047] A. Reducing agent addition: In the wet leaching process, a reducing agent is added to the material system containing manganese dioxide to reduce manganese dioxide to soluble Mn. 2+ The reducing agent is zinc particles and / or contains Fe2+. + Zinc concentrate;
[0048] In step A, the amount of zinc particles added is 60–100 kg / h, and it must simultaneously meet the following conditions: slurry flow rate > 150 m³ / h, slurry pH = 2.0–2.5 > 2.0, and Fe... 3+ >10g / L, copper ion concentration in solution ≥1g / L.
[0049] In step A, the amount of zinc concentrate added is 4.5–9 tons / day, and its Fe2+ + Content ≥15wt%, S2- content ≥8wt%.
[0050] The method of adding the reducing substance in step A is as follows:
[0051] When the system manganese concentration is <1g / L, zinc particles and zinc concentrate are added together, with 80kg / h of zinc particles and 6 tons / day of zinc concentrate.
[0052] When the system manganese concentration is 1 g / L, zinc concentrate is added as a single agent at a rate of 4.5 tons / day.
[0053] Stop adding reducing agent when the system manganese concentration is >2g / L.
[0054] In step A, the residual sulfur content of the roasted sand is controlled to be 1.0% simultaneously. Specifically, when the manganese concentration in the supernatant is <2g / L, the roasting temperature is lowered to increase the residual sulfur content to 1.0%; when the manganese concentration in the supernatant is ≥3g / L, the roasting temperature is increased to reduce the residual sulfur content to 0.7%.
[0055] B. Coordinated control of electrolysis parameters: During the electrolysis process, the current density is controlled at 200 A / m. 2 The electrolysis cycle was extended to 36 hours, and the electrolyte temperature was controlled at 34℃.
[0056] Current density control employs a staged strategy:
[0057] When the manganese concentration is <1 g / L, the current density drops to 100 A / m. 2 ;
[0058] When the manganese concentration is 1–1.5 g / L, the current density increases to 200 A / m. 2 ;
[0059] When the manganese concentration is >1.5 g / L, the current density recovers to 400 A / m. 2 above
[0060] C. Anode plate protection operation: The anode plates are manually scraped instead of mechanically flattened. The anode plates are then loaded into the electrolytic cell within 10 minutes after scraping.
[0061] D. Dynamic monitoring and feedback:
[0062] ① The manganese concentration of the electrolyte is detected after filtration through a filter membrane, and the manganese content of the lead-silver slag is monitored daily;
[0063] ② When the manganese content of lead-silver slag is >1% and the manganese concentration of the middle and upper clarifiers is <2g / L, increase the amount of reducing agent added;
[0064] ③ When the manganese concentration in the waste electrolyte is <1.5g / L, add manganese sulfate or manganese carbonate to the clean electrolyte section.
[0065] The manganese concentration in the pre- and post-liquid sluices of the electrolytic cell was measured twice a week, and the manganese depletion amount ΔMn was calculated.
[0066] When ΔMn>1000mg / L, initiate the electrolysis parameter adjustment in step B.
[0067] The daily replenishment of manganese sulfate is 2 tons, and the daily replenishment of manganese carbonate is 3 tons.
[0068] Example 2
[0069] This invention proposes a method for efficiently and rapidly increasing the concentration of manganese ions in a zinc electrolytic solution, comprising the following steps:
[0070] A. Reducing agent addition: In the wet leaching process, a reducing agent is added to the material system containing manganese dioxide to reduce manganese dioxide to soluble Mn. 2+ The reducing agent is zinc particles and / or contains Fe2+. + Zinc concentrate;
[0071] In step A, the amount of zinc granules added is 100 kg / h, and the following conditions must be met simultaneously: slurry flow rate > 150 m³ / h. 3 / h, pulp pH 2.0-2.5, Fe 3+ >10g / L, copper ion concentration in solution ≥1g / L.
[0072] In step A, the amount of zinc concentrate added is 9 tons / day, and its Fe... 2+ Content ≥15wt%, S 2 - Content ≥ 8wt%.
[0073] The method of adding the reducing substance in step A is as follows:
[0074] When the system manganese concentration is <1g / L, zinc particles and zinc concentrate are added together, with 100kg / h of zinc particles and 9 tons / day of zinc concentrate.
[0075] When the system manganese concentration is 2 g / L, zinc concentrate is added as a single agent at a dosage of 6 tons / day.
[0076] Stop adding reducing agent when the system manganese concentration is >2g / L.
[0077] In step A, the residual sulfur content of the roasted sand is controlled to be 1.5% simultaneously. Specifically, when the manganese concentration in the supernatant is <2g / L, the roasting temperature is lowered to increase the residual sulfur content to 1.5%; when the manganese concentration in the supernatant is ≥3g / L, the roasting temperature is increased to reduce the residual sulfur content to 1.0%.
[0078] Coordinated control of electrolysis parameters: During the electrolysis process, the current density is controlled at 300 A / m. 2 The electrolysis cycle was extended to 48 hours, and the electrolyte temperature was controlled at 36℃.
[0079] Current density control employs a staged strategy:
[0080] When the manganese concentration is <1 g / L, the current density drops to 200 A / m. 2 ;
[0081] When the manganese concentration is 1–1.5 g / L, the current density increases to 300 A / m. 2 A;
[0082] When the manganese concentration is >1.5 g / L, the current density recovers to 400 A / m. 2 above
[0083] C. Anode plate protection operation: The anode plates are manually scraped instead of mechanically flattened. The anode plates are then loaded into the electrolytic cell within 10 minutes after scraping.
[0084] D. Dynamic monitoring and feedback:
[0085] The manganese concentration of the electrolyte was detected after filtration through a filter membrane, and the manganese content of the lead-silver slag was monitored daily.
[0086] When the manganese content of lead-silver slag is >1% and the manganese concentration of the middle and upper clarifiers is <2g / L, the amount of reducing agent added should be increased.
[0087] When the manganese concentration in the waste electrolyte is <1.5g / L, manganese sulfate or manganese carbonate should be added to the clean electrolyte section.
[0088] The manganese concentration in the pre- and post-liquid sluices of the electrolytic cell was measured twice a week, and the manganese depletion amount ΔMn was calculated.
[0089] When ΔMn>1000mg / L, initiate the electrolysis parameter adjustment in step B.
[0090] The daily replenishment of manganese sulfate is 3 tons, and the daily replenishment of manganese carbonate is 8 tons.
[0091] Example 3
[0092] Since March 11, excessive Pb content in the precipitated zinc has prevented the normal production of No. 0 zinc ingots and some zinc alloys in the smelting and casting section. Analysis revealed that the main factor causing the widespread excessive Pb content in the precipitated zinc was the low Mn ion content in the electrolyte.
[0093] After taking a series of manganese extraction measures, such as Figure 1As shown, it should be noted that the test results for #0 zinc were delayed by one day compared to the production date. In early April, the manganese ion content in the system rebounded, causing the Pb content in the precipitated zinc to decrease and stabilize at normal levels. From April 6th onwards, all zinc ingots produced met the #0 zinc standard, and the #0 zinc production rate remained at 100% thereafter. A detailed summary is as follows:
[0094] Cause Analysis and Control Measures: During electrolysis, Mn ions in the electrolyte are oxidized at the anode to generate MnO2, which is adsorbed onto the anode surface to form a protective film, preventing corrosion of the anode lead (the anode plate is a Pb-Ag alloy material). When the concentration of Mn ions in the electrolyte is too low, the generated MnO2 is loose and difficult to adsorb onto the anode plate surface, failing to provide protection. As a result, the anode plate surface is continuously corroded into the electrolyte, causing the deposited zinc to contain excessive Pb.
[0095] In recent years, the manganese ion concentration in the zinc system has continued to decline. Although measures such as adding zinc concentrate (containing reducing substances) and manganese carbonate in the wet process have been taken, the manganese concentration is still decreasing.
[0096] like Figure 2 As shown, starting in March, the concentration of Mn ions in the electrolyte had dropped below 1.5 g / L, and remained around 1.2 g / L in the latter half of March. However, according to feedback from laboratory personnel, there were a significant amount of manganese dioxide particles in the electrolyte recently, interfering with the test results. On March 30th, after filtering the electrolyte, the measured Mn ion concentration was only 0.6 g / L (indicating that the Mn ion concentration in the electrolyte was already below 1 g / L in mid-March or even earlier). The graph shows that the excessively low manganese ion concentration (<1 g / L) is the main reason for the widespread exceedance of Pb in the deposited zinc since mid-March. From March 30th onwards, the Mn ion concentration in the electrolyte was measured using a method of filtering before analysis.
[0097] After identifying the cause, a series of manganese reduction measures were implemented, mainly in two categories: increasing the manganese supplementation in the wet process and reducing manganese deposition in the electrolytic zinc process. According to research data, the main factors affecting the anode MnO2 deposition efficiency are:
[0098] ① Current density: As the current density increases, the MnO2 deposition efficiency at the anode decreases;
[0099] ②Temperature: As the temperature increases, the MnO2 precipitation efficiency at the anode increases;
[0100] ③ Mn ion concentration: When the manganese ion concentration is below 2 g / L, a protective film of MnO2 cannot be formed on the anode surface, and the MnO2 precipitation efficiency of the anode increases with the increase of Mn ion concentration; when the manganese ion concentration is 2-3 g / L, a protective film of MnO2 is formed on the anode surface, and the MnO2 precipitation efficiency of the anode decreases with the increase of Mn ion concentration; when the manganese ion concentration is above 3 g / L, the entire anode surface is covered by a protective film of MnO2, and the MnO2 precipitation efficiency of the anode increases with the increase of Mn ion concentration. Therefore, it is more appropriate to control the Mn ion concentration at 2-3 g / L.
[0101] The specific manganese extraction measures are as follows:
[0102] 1. Complete the manganese concentration detection data at each point in the system, increase the manganese concentration detection frequency, establish the manganese balance of the system, adjust the addition amount of each material according to the manganese balance, and predict and track the trend of manganese concentration in the system.
[0103] 2. Add manganese carbonate to supplement Mn 2+ Starting March 15th, manganese carbonate was added at a rate of 6 tons per day; starting March 24th, the rate was 8 tons per day; starting March 28th, the rate was 5 tons per day; and on April 7th, the rate was 3 tons per day. (A total of 139 tons of manganese carbonate were added from March 15th to April 7th.)
[0104] 3. Zinc concentrate, utilizing its reducing properties (Fe2+) 2+ S 2- (etc.) reduce manganese powder and MnO2 in anode mud to Mn 2+ Zinc concentrate was added daily at a rate of 1 bucket (approximately 1.7 tons) starting January 6th, 3 buckets (4.4 tons) daily starting March 29th, 6 buckets (approximately 9 tons) daily starting April 2nd, 5 buckets (approximately 8 tons) daily starting April 7th, 4 buckets (approximately 6 tons) daily starting April 8th, and finally reverted to 3 buckets (approximately 4.5 tons) daily starting April 9th. A total of 226 tons of leached zinc concentrate were added.
[0105] 4. Adding zinc particles follows the same principle as adding zinc concentrate. Zinc particles were added at a rate of 60 kg per hour starting on the 26th, 80 kg per hour starting on the 31st, and 100 kg per hour on April 2nd. Adding was suspended during the night shift on April 7th. A total of 23.5 tons of zinc particles were added.
[0106] like Figure 3 It can be seen that after adding zinc particles, the Mn content in the lead-silver slag decreased from about 2% to below 1%, indicating that the addition of zinc particles has a very significant effect on manganese supplementation.
[0107] 5. Add manganese sulfate to supplement Mn 2+ Starting on April 6th, during the day shift, 3 tons of manganese sulfate were added to the first stage of the purified solution daily.
[0108] like Figure 4 As shown, through the above adjustments, the manganese ion concentration at various points in the wet process increased significantly, by about 100% (from 1.2-1.4 g / L on March 11 to 2.6-2.8 g / L on April 9).
[0109] 6. Increase the amount of new electrolyte used to accelerate the increase of Mn ions in the waste liquid. From March 30th to April 4th for System 1, and from March 30th (day shift) to April 5th for System 2, increase the amount of new electrolyte added to 70-80 m³ / h to replace the electrolyte with new electrolyte of high Mn ion concentration.
[0110] 7. In low-current, long-cycle electrolysis production, the anode MnO2 deposition efficiency decreases with increasing current density. However, if high-current-density production is adopted when the Mn ion concentration is too low, a large amount of zinc with excessive Pb content will be produced. On the one hand, the surface of the zinc deposited at high current density is rougher and more easily adsorbs a large amount of lead; on the other hand, high-current-density production results in a larger daily zinc deposition output and a greater total amount of MnO2. Therefore, low-current production is more suitable before the manganese concentration is increased. Thus, the zinc sheet production cycle, which was originally 24 hours, was extended to 36 hours starting March 29th, so that the 36-hour cycle was followed for three days from the 29th to the 31st. On the 30th, the current in both systems dropped to a minimum of 100 A / m. 2 (Anode plate coating was performed to reduce Pb corrosion.) Subsequently, due to insufficient current, the zinc plates in the system tank burned. Therefore, the minimum current of the system was adjusted to 300A / m. 2 The current in the second system increased to 200 A / m 2 Considering that both systems need to be unloaded on the 31st, the highest current of system one only reached 400A / m at night. 2 The second system was upgraded to 250A / m 2 After the tank was removed from the tank on April 3, the second system underwent another 48-hour low-current production cycle.
[0111] 8. Control the electrolyte temperature, keeping it within a low temperature range, approximately 34–36°C.
[0112] 9. Reduce the number of cathode plates in the cells to decrease zinc precipitation. Starting from April 3rd for System 1 and April 4th for System 2, the number of cathode plates per electrolytic cell was reduced from 48 to 44, reducing the production of anode mud (MnO2) and thus reducing manganese ion consumption.
[0113] 10. The flattening machine for anode plates was suspended, and manual scraping was switched to the new system. Because the manganese dioxide protective film on the anode plates is prone to dehydration and peeling off when exposed to air for extended periods, causing the surface protection to fail and allowing Pb ions to enter the electrolyte, the flattening machine personnel switched from night shifts to daytime shifts. Each span was manually flattened and scraped, and the treated anode plates were directly placed into the electrolytic cell, reducing their exposure time to air. In just 30 days, one system per day was used to flatten 4 rows of anode plates, totaling 108 cells, demonstrating high efficiency.
[0114] Summary of manganese extraction: After taking the above measures, the concentration of Mn ions in the electrolyte increased rapidly. At the end of March, it was only 0.6 g / L at its lowest point, but by April 9, it had reached 1.6-1.7 g / L. The content of zinc Pb in the precipitated zinc also decreased accordingly and stabilized within the normal range. From April 6 onwards, all zinc ingots produced met the 0# zinc standard, and the 0# zinc yield remained at 100%.
[0115] like Figure 5 As shown in the analysis, the main reasons for manganese ion depletion in the system, based on the system's manganese ion balance and considering the factors affecting the anodic MnO2 precipitation efficiency mentioned above, are as follows:
[0116] 1. The amount of MnO2 deposited at the anode during the electrolysis process is too large.
[0117]
[0118] The data in the table above shows that the Mn ion depletion value after the electrolysis process is approximately 1.1 g / L, while based on historical experience, the Mn ion depletion value during normal electrolysis is approximately 0.4 g / L. Assuming a daily waste liquid volume of 3300 m³, and currently 3.63 tons of Mn are released daily, this means an increase of 2.31 tons of Mn released daily compared to normal conditions. The increased Mn ion depletion value during electrolysis can be attributed to the following two factors:
[0119] (1) When the manganese ion concentration is below 2 g / L, a protective film of MnO2 cannot be formed on the anode surface, the MnO2 precipitation efficiency of the anode is high, and the amount of MnO2 precipitated is large;
[0120] In this situation, the amount of Pb corroded into the electrolyte increases, and the probability of Pb being reduced and deposited at the cathode or mixed into the deposited zinc also increases. Therefore, the lead content of the deposited zinc will increase or even exceed the standard. In severe cases, it will lead to a significant decrease in the yield of 0# zinc or even the inability to produce 0# zinc.
[0121] (2) During the process of flattening the anode plate by the anode flattening machine, the MnO2 protective film on the anode surface is destroyed, resulting in a high MnO2 precipitation efficiency and a large amount of MnO2 precipitation before the MnO2 protective film is regenerated.
[0122] like Figure 6 and Figure 7 To reduce Mn ion depletion, two measures are needed: First, the Mn ion concentration in the electrolyte should be increased as quickly as possible and maintained at 2–3 g / L. Second, the anode flattening machine should be optimized, such as by appropriately increasing the stroke of the flattening head, reducing the speed of the flattening head, or changing the material of the flattening head to reduce the flattening force. This will ensure the effective removal of anode sludge while preventing the MnO2 protective film on the anode surface from being damaged and exposing the lead layer.
[0123] 2. The raw materials, zinc-containing materials, and auxiliary materials contain an increase in oxidizing substances or a decrease in reducing substances. The MnO2 in the manganese ore powder and anode mud added during the wet process must be reduced to Mn. 2+ Only then can it enter the solution. If the amount of oxidizing substances (manganese powder, nitrite, etc.) introduced into the wet process increases or the amount of reducing substances (ferrous iron, residual sulfur, etc.) decreases, the amount of manganese ions dissolved into the system will decrease. When the amount of manganese entering the system from the wet process is less than the amount of Mn precipitated from the electrolytic zinc process, Mn ion depletion will occur in the system.
[0124]
[0125]
[0126] Theoretically, all the anode mud from electrolysis should return to the wet process, and since manganese ore powder is added in the wet process, Mn depletion should not occur. However, in reality, a large amount of Mn from the manganese ore powder and anode mud does not dissolve and enters the system but is carried away by lead-silver slag and iron ore slag, thus causing Mn depletion. This indicates an increase in oxidizing substances or a decrease in reducing substances entering the wet process system. Furthermore, continuous monitoring and detection of oxides and reducing substances in raw materials, zinc-containing materials, and auxiliary materials are necessary in later stages.
[0127] The system manganese balance table shows that only when the amount of Mn in the manganese ore powder equals the amount of Mn carried away by the two slags can the system maintain manganese balance without supplementing manganese salts such as manganese carbonate and manganese sulfate. However, in reality, increasing the amount of manganese ore powder added cannot maintain manganese balance; it will only further increase the amount of manganese entering the lead-silver slag and iron ore slag, resulting in manganese waste. Only by increasing the amount of reducing substances introduced into the hydrometallurgical process (such as adding zinc concentrate, increasing residual sulfur in roasted sand, adding zinc particles, etc.) to reduce the Mn content in the lead-silver slag can the system achieve manganese balance.
[0128] like Figure 3 As shown, the Mn content curves of lead-silver slag before and after the addition of zinc particles in the wet process (starting from March 26) show that adding sufficient reducing substances can significantly reduce the Mn content of lead-silver slag from the original 2% to 0.5% (minimum 0.3%).
[0129]
[0130] If the Mn content in the lead-silver slag decreases to 0.5% in February and March, the new Mn balance is shown in the table above. This indicates that as long as there are sufficient reducing agents (such as zinc particles), it is entirely possible to maintain the Mn balance of the system without adding manganese carbonate or manganese sulfate.
[0131] It should be noted that the Mn content in the supernatant is maintained at 2–3 g / L, and the manganese content in the waste electrolyte is controlled at 1.5–2.5 g / L. This balance is maintained as follows:
[0132] 1) Appropriately increase the residual sulfur in calcined sand. When the concentration of Mn ions in the supernatant is close to or high, the residual sulfur in calcined sand can be appropriately reduced;
[0133] 2) The detection of Mn in the solution always follows the method of filtration before detection to improve the reliability of the results;
[0134] 3) Regularly test the Mn content in lead-silver slag, ideally 1-2 times per week. When the Mn content in the lead-silver slag exceeds 1%:
[0135] ① If the concentration of Mn ions in the middle and upper naphthalenes is too low, a process instruction should be given to increase the residual sulfur in the calcined sand;
[0136] ②If the concentration of Mn ions in the middle and upper naphthalenes is not too low, then the amount of manganese ore powder and anode mud used should be reduced appropriately;
[0137] ③ If the waste electrolyte contains less than 1500 mg / L of manganese, add manganese carbonate during leaching or add manganese sulfate to the purified solution.
[0138] 4) Regularly send samples to test the Mn ion concentration in the pre- and post-electrolytic zinc sluices. It is recommended to do this 1 to 2 times per week to track and analyze the changing trend of MnO2 deposition efficiency at the anode during the electrolysis process.
[0139] The above specific embodiments are merely several optional embodiments of the present invention. Based on the technical solutions of the present invention and the relevant teachings of the above embodiments, those skilled in the art can make various alternative improvements and combinations to the above specific embodiments.
Claims
1. A method for efficient and rapid regulation of the concentration of manganese ions in zinc electrolysis solution, characterized by, The method comprises the following steps: A. Reducing agent addition: In the wet leaching process, a reducing substance is added to the material system containing manganese dioxide, so that the manganese dioxide is reduced to soluble Mn 2+ ; the reducing substance is zinc metal particles and / or zinc concentrate containing Fe2 + ; B. Synergistic control of electrolysis parameters: In the electrolysis process, the current density is controlled to be less than 300 A / m 2 , the electrolysis cycle is extended to 36-48 hours, and the electrolyte temperature is controlled at 34-36℃; C. Anode plate protection operation: manual shovel plate is used to replace mechanical flat treatment of anode plate, and the anode plate is loaded into the electrolytic cell within 10 minutes after the shovel plate; D. Dynamic monitoring and feedback: The manganese concentration of the electrolyte is detected after filtration by filter membrane, and the manganese content of lead-silver residue is monitored regularly; When the manganese content of lead-silver residue is greater than 1% and the manganese concentration of supernatant is less than 2 g / L, the amount of reducing substance is increased; When the manganese concentration of waste electrolyte is less than 1.5 g / L, manganese sulfate or manganese carbonate is added in the clean liquid section.
2. The method according to claim 1, characterized in that, The amount of metal zinc particles added in step A is 60-100 kg / h, and it is necessary to simultaneously satisfy: slurry flow > 150 m3 / h, slurry pH = 2.0-2.5 = 2.0-2.5, Fe 3+ > 10 g / l, and the concentration of copper ions in the solution is > 1 g / L.
3. The method according to claim 2, characterized in that, The zinc concentrate addition in step A is 4.5-9 tons / day, with Fe2 + content > 15 wt%, S 2 content > 8 wt%.
4. The method of claim 1, wherein the method is characterized by, The adding mode of reducing substance in step A is as follows: When the manganese concentration of the system is less than 1 g / L, zinc particles and zinc concentrate are jointly added, the amount of zinc particles is 80-100 kg / h, and the amount of zinc concentrate is 6-9 tons / day; When the manganese concentration of the system is 1-2 g / L, zinc concentrate is added alone, and the amount is 4.5-6 tons / day; When the manganese concentration of the system is greater than 2 g / L, the addition of reducing agent is stopped.
5. The method of claim 1, wherein the method is characterized by, In step A, the residual sulfur content of calcine is simultaneously controlled to be 1.0%-1.5%, which is achieved by the following methods: when the manganese concentration of supernatant is less than 2 g / L, the roasting temperature is reduced to increase the residual sulfur content to 1.0%-1.5%; when the manganese concentration of supernatant is greater than or equal to 3 g / L, the roasting temperature is increased to reduce the residual sulfur content to 0.7%-1.0%.
6. The method of claim 1, wherein the method is characterized by, In step B, the current density is regulated by stages: Manganese concentration < 1 g / L, current density reduced to 100-200 A / m 2 ; Manganese concentration 1-1.5 g / L, current density increased to 200-300 A / m 2 ; The current density is restored to 400 A / m at a manganese concentration > 1.5 g / L 2 The above.
7. The method of claim 1, wherein the method is characterized by, In step D, the following is also included: The manganese concentration of the front liquid and the rear liquid of the electrolytic cell is detected twice a week, and the manganese depletion amount ΔMn is calculated; When ΔMn is greater than 1000 mg / L, the electrolytic parameter regulation of step B is started.
8. The method of claim 1, wherein the method is characterized by, In step D, the amount of manganese sulfate added is 2-3 tons / day, and the amount of manganese carbonate added is 3-8 tons / day.