Transparent copolyester, preparation method thereof and product prepared from copolyester
By employing pressure suppression and gradual pressure reduction methods during the preparation of transparent copolyester, side reactions are reduced, the problems of insufficient color and light transmittance of copolyester are solved, and copolyester products with high transparency and heat resistance are achieved.
Patent Information
- Application Number
- CN202511678623.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-11-17
- Publication Date
- 2026-01-16
AI Technical Summary
Existing transparent copolyesters are prone to thermal-oxidative side reactions during synthesis, resulting in poor color, insufficient light transmittance, and poor heat resistance.
In the esterification or transesterification stage, a pressure-locking reaction is carried out to increase the boiling point of excess monomer and reduce monomer vaporization; in the pre-condensation reaction stage, the pressure is gradually reduced to a high vacuum to remove excess monomer and its impurities, thereby reducing the occurrence of side reactions.
It effectively improves the color of copolyester, increases light transmittance and heat resistance, and the prepared copolyester products have light color, high transmittance and good heat resistance.
Abstract
Description
TECHNICAL FIELD
[0001] The present application belongs to the field of polyester, and particularly relates to a transparent copolyester, a preparation method thereof and an article prepared from the copolyester. BACKGROUND
[0002] Poly(1,4-cyclohexylenedimethylene terephthalate) (PCT) is a kind of transparent heat-resistant copolyester resin with excellent performance, which is obtained by esterification-polycondensation reaction of terephthalic acid (PTA) and 1,4-cyclohexanedimethanol (CHDM) or by ester exchange-polycondensation reaction of dimethyl terephthalate (DMT) and 1,4-cyclohexanedimethanol (CHDM). PCT has the characteristics of high melting point and fast crystallization rate, and the material is opaque. In order to reduce the crystallization rate and melting point of PCT and obtain colorless and transparent heat-resistant material, it is usually copolymerized with other diol monomers such as 2,2,4,4-tetramethyl-1,3-cyclobutanediol (CBDO), isosorbide (ISB) and neopentyl glycol (NPG), which can inhibit the crystallization of PCT and obtain transparent products. Among them, the copolyester obtained by copolymerization with CBDO is not only transparent, but also has high glass transition temperature and good impact resistance, and has wide application in the fields of water cups, electronic cigarettes and small household appliances.
[0003] The copolyester is prone to thermal oxygen side reactions during synthesis to generate impurities and color, affecting the color and light transmittance of the product. Patent CN101300285A mentions that the copolyester is prone to yellowing, and even if a stabilizer is added, a light yellow product can be obtained. One of the important reasons for the yellowing of the copolyester is that the polymerization monomers decompose by side reactions during polymerization, affecting the subsequent polymerization process and introducing unnecessary impurities. In addition, in order to promote the reaction during synthesis, one of the monomers, such as diol, is often excessive, which undoubtedly aggravates the situation.
[0004] In summary, the current transparent copolyester still has the problems of poor color, insufficient light transmittance and heat resistance, which need to be solved. SUMMARY
[0005] One of the purposes of the present application is to provide a copolyester preparation method and a copolyester prepared by the method. The copolyester preparation method of the present application can effectively reduce the side reactions during synthesis, improve the color of the copolyester product, and increase the light transmittance and reduce the haze.
[0006] Another purpose of the present application is to provide an article prepared from the copolyester prepared by the preparation method, and the article prepared from the copolyester, such as bottle material, sheet material, plate material and film material, has the characteristics of light color, high transmittance and good heat resistance.
[0007] To achieve the above-mentioned purposes of the application, the technical solutions adopted by the present application are as follows:
[0008] A method for preparing a transparent copolyester, the method comprising the following steps:
[0009] S1: Dicarboxylic acid or its ester reacts with diol under a pressure of 5–300 kPaG to undergo esterification or transesterification to obtain esterified or transesterified products.
[0010] S2: The system is restored to normal pressure, and the pressure is gradually reduced to <0.1 kPaA at the esterification or transesterification reaction temperature to carry out the prepolymerization reaction and obtain the prepolymer;
[0011] S3: Increase the temperature to carry out the final polycondensation reaction and obtain the target copolyester.
[0012] To reduce side reactions, the inventors discovered through extensive research that pressurizing the reaction (5–300 kPaG) during the esterification or transesterification stage can increase the boiling point of excess monomer, thereby reducing monomer vaporization and minimizing side reactions caused by direct heating of the monomer at high temperatures. It also prevents oxygen from entering, further reducing the occurrence of side reactions. In the pre-polymerization stage (step S2), maintaining the esterification temperature and gradually reducing the pressure during S2 allows for better removal of excess monomer and its 0.3 wt% impurities. This effectively reduces subsequent high-temperature side reactions during final polycondensation, achieving the goals of improving color, increasing light transmittance, and enhancing heat resistance and processability.
[0013] In one embodiment of the present invention, the reaction pressure in S1 is preferably 50-200 kPaG, the reaction temperature is 190-240℃, preferably 210-230℃, and the reaction time is 120-240 min, preferably 150-180 min.
[0014] In one embodiment of the present invention, the reaction temperature in S2 is 190-240°C, preferably 210-230°C, the reaction pressure is gradually reduced from atmospheric pressure to <0.1 kPaA, preferably <0.05 kPaA, the pressure reduction rate is 1.68-3.36 kPa / min, preferably 2.02-2.52 kPa / min, and excess diol monomer and its impurities are removed. Preferably, the mass content of monomer and impurities in the system is less than 0.3 wt%, preferably less than 0.2 wt%.
[0015] In one embodiment of the present invention, the reaction temperature in S3 is 250-270°C, preferably 260-265°C, the absolute pressure of the reaction is below 0.1 kPaA, preferably below 0.05 kPaA, and the reaction time is 120-300 min, preferably 150-210 min.
[0016] In one embodiment of the present invention, the ester of the dicarboxylic acid is a dimethyl ester of the dicarboxylic acid.
[0017] Preferably, the dicarboxylic acid or ester of the dicarboxylic acid in S1 is one or more of terephthalic acid or its dimethyl ester, isophthalic acid or its dimethyl ester, phthalic acid or its dimethyl ester, biphenyl dicarboxylic acid or its dimethyl ester, naphthalenedicarboxylic acid or its dimethyl ester, furanic acid or its dimethyl ester, thiophene dicarboxylic acid or its dimethyl ester, and cyclohexanedicarboxylic acid or its dimethyl ester, more preferably terephthalic acid or its dimethyl ester and / or isophthalic acid or its dimethyl ester.
[0018] In one embodiment of the present invention, the diol in S1 is a C2-C20 aliphatic diol and / or aromatic diol, preferably 1,4-cyclohexanediol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, isosorbide, ethylene glycol, 1,3-propanediol, 2-methyl-1,3-propanediol, 1,2-propanediol, 1,4-butanediol, 2,3-butanediol, 1,2-pentanediol, 1,4-pentanediol, 1,5-pentanediol, neopentanediol, 3-methyl... The diol is selected from one or more of 1,5-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, diethylene glycol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, spirocyclodiol, and tricyclodecanediethanol, more preferably 1,4-cyclohexanediethanol and / or 2,2,4,4-tetramethyl-1,3-cyclobutanediol; preferably, the molar ratio of the diol to the diacid or the ester of the diacid is (1.1-1.5):1, more preferably (1.2-1.4):1.
[0019] In one embodiment of the present invention, a catalyst is further added in S1; preferably, the catalyst is one or more of the following: dibutyltin oxide, dimethyltin oxide, monobutyltriisooctanoate, dibutyldimethoxytin, stannous octanoate, stannous oxalate, dibutyltin diacetate, dibutyltin dilaurate, tetrabutyl titanate, isopropyl titanate, titanium glycolate, lithium acetate, potassium acetate, calcium acetate, magnesium acetate, barium acetate, zinc acetate, cobalt acetate, antimony acetate, lead acetate, manganese acetate, and germanium dioxide, preferably dibutyltin oxide and / or tetrabutyl titanate; preferably, the amount of catalyst added is 200-500 ppm of the total mass of the diol and diacid or the ester of the diacid, preferably 300-400 ppm.
[0020] In one embodiment of the present invention, a heat stabilizer is further added to S1; preferably, the heat stabilizer is a phosphate ester compound, preferably an alkyl phosphate ester and / or an aryl phosphate ester, more preferably a triphenyl phosphate ester and / or a triethyl phosphate ester; preferably, the amount of the heat stabilizer added is 300 to 600 ppm of the total mass of the diol and the diacid or the diester of the diacid, more preferably 300 to 400 ppm.
[0021] Another object of the present invention is to provide a transparent copolyester prepared by the above method. The copolyester is a light-colored, highly transparent, and heat-resistant copolyester.
[0022] Another object of the present invention is to provide a transparent copolyester product, such as bottle material, sheet material, plate material and film material, which is processed from the above copolyester and has the characteristics of light color, high transparency and good heat resistance.
[0023] In one embodiment of the present invention, the copolyester has an intrinsic viscosity > 0.6 dL / g, an optical sample color difference L value > 90, an absolute value of a value < 1, an absolute value of b value < 1, a light transmittance > 90%, and a haze < 1%; after the granules are heated at 270°C for 10 min, the injection molded sample Δ tensile strength < 2 MPa, and the optical sample color difference Δb value < 0.2.
[0024] Compared with the prior art, the positive effects of the technical solution of the present invention are as follows:
[0025] (1) The preparation method of the light-colored high-transparency heat-resistant copolyester involved in this invention increases the boiling point of the excess monomer by performing a pressure (5-300 kPaG) reaction during the reaction esterification or transesterification stage, so as to weaken the monomer vaporization and reduce the side reactions that occur when directly heated at high temperature.
[0026] (2) The preparation method of light-colored high-transparency heat-resistant copolyester involved in this invention, in the pre-shrinking stage, keeps the esterification temperature unchanged, and gradually reduces the pressure to high vacuum through a certain pressure reduction rate, which can stably and effectively remove excess monomer and its generated impurity content of 0.3wt%, weaken the side reaction at high temperature in the subsequent final polycondensation, improve color and increase light transmittance.
[0027] (3) The method for preparing light-colored, high-transparency, heat-resistant copolyester involved in this invention produces a copolyester with good heat resistance. After heating at 270°C for 10 minutes, the tensile strength and color difference of the injection-molded sample remain good. Detailed Implementation
[0028] The present invention will be further described below with reference to specific embodiments. It should be noted that the embodiments are only used to illustrate the present invention and do not constitute a limitation on the scope of protection of the present invention.
[0029] The raw materials—diols, diacids or their dimethyl esters, catalysts, and heat stabilizers—were all commercially available and of analytical grade. Dimethyl terephthalate, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, and 1,4-cyclohexanediethanol were purchased from Beijing Inokai Technology Co., Ltd., with a purity of 99%. Dibutyltin oxide and triphenyl phosphate were purchased from Shanghai Maclean Biochemical Technology Co., Ltd., with a purity of 98%.
[0030] The equipment and methods used in this invention are all common in the field.
[0031] Intrinsic viscosity: The intrinsic viscosity of the sample at 25℃ was measured using a Nanjing Tenghui Ubbelohde viscometer. The solvent was phenol / tetrachloroethane (mass ratio w / w = 3 / 2), and the sample concentration was 0.005 g / mL.
[0032] Excess monomer and its impurities: Using an Agilent 7890B gas chromatograph, 0.1 g of sample was added to hexafluoroisopropanol as solvent to prepare a mixed standard solution with a standard volume concentration of 10 g / L, and quantification was performed using the external standard method.
[0033] Optical performance: 25mm diameter and 1.5mm thick circular wafers were prepared using a Haake MiniJet II micro-injection molding machine. Transmittance and haze (H) were measured using a CS-821N benchtop spectrophotometer. Color difference was measured as L / a / b (representing brightness or black / white intensity, green / red intensity, and blue / yellow intensity, respectively).
[0034] Mechanical properties: Tensile strength was tested using a HaakeMiniJet II micro injection molding machine to prepare dumbbell-shaped specimens with a width of 4 mm and a thickness of 2 mm. The specimens were tested using a mechanical testing machine (Instron 5960) at a tensile speed of 50 mm / min.
[0035] Example 1
[0036] (1) 1000g of dimethyl terephthalate, 295g of 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 596g of 1,4-cyclohexanediol, 0.38g of dibutyltin oxide and 0.57g of triphenyl phosphate were added to the reaction vessel and subjected to transesterification reaction at 190℃ and a pressure of 5kPaG for 240min.
[0037] (2) Then the system is restored to normal pressure, the temperature is kept constant at 190℃, and the vacuum is gradually reduced to below 0.1kPaA at a depressurization rate of 1.68kPa / min. The mass content of excess diol 2,2,4,4-tetramethyl-1,3-cyclobutanediol and its impurities (such as 1-(1-butenoxy)pentane) is ≤0.3%.
[0038] (3) Maintain a vacuum below 0.1 kPaA and react at 250℃ for 300 min to obtain copolyester 1. After water cooling and pelletizing, copolyester granules are obtained with an intrinsic viscosity of 0.681 dL / g, a light transmittance of 91%, a haze of 0.5%, and optical sample color difference L value of 95, a value of -0.5, and b value of 0.6. The tensile strength of the granule injection molded sample is 44 MPa. After heating at 270℃ for 10 min, the tensile strength of the injection molded sample is 43 MPa, and the optical sample color difference b value is 0.7.
[0039] Example 2
[0040] (1) Add 856g of terephthalic acid, 295g of 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 596g of 1,4-cyclohexanediethanol, 0.95g of dibutyltin oxide and 1.14g of triphenyl phosphate to a reaction vessel and carry out transesterification reaction at 240℃ and 300kPaG for 120min.
[0041] (2) Then the system is restored to normal pressure, the temperature is kept constant at 240℃, and the vacuum is gradually reduced to below 0.05kPaA at a depressurization rate of 3.36kPa / min. The mass content of excess diol 2,2,4,4-tetramethyl-1,3-cyclobutanediol and its impurities (such as 1-(1-butenoxy)pentane) is ≤0.2%.
[0042] (3) Maintain a vacuum below 0.05 kPa and react at 270°C for 120 min to obtain copolyester 2. After water cooling and pelletizing, copolyester granules are obtained with an intrinsic viscosity of 0.688 dL / g, a light transmittance of 91%, a haze of 0.4%, and optical sample color difference L value of 95, a value of -0.5, and b value of 0.6. The tensile strength of the granule injection molded sample is 45 MPa. After heating at 270°C for 10 min, the tensile strength of the injection molded sample is 44 MPa, and the optical sample color difference b value is 0.7.
[0043] Example 3
[0044] (1) 1000g of dimethyl terephthalate, 295g of 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 596g of 1,4-cyclohexanediol, 0.57g of dibutyltin oxide and 0.57g of triphenyl phosphate were added to the reaction vessel and the transesterification reaction was carried out at 210℃ and 50kPaG for 180min.
[0045] (2) Then the system is restored to normal pressure, the temperature is kept constant at 210℃, and the vacuum is gradually reduced to below 0.05kPaA at a depressurization rate of 2.02kPa / min. The mass content of excess diol 2,2,4,4-tetramethyl-1,3-cyclobutanediol and its impurities (such as 1-(1-butenoxy)pentane) is ≤0.2%.
[0046] (3) Maintain a vacuum below 0.05 kPa and react at 260℃ for 210 min to obtain copolyester 3. After water cooling and pelletizing, copolyester granules are obtained with an intrinsic viscosity of 0.692 dL / g, a light transmittance of 92%, a haze of 0.3 wt%, and optical sample color difference L value of 96, a value of -0.3, and b value of 0.4. The tensile strength of the granule injection molded sample is 47 MPa. After heating at 270℃ for 10 min, the tensile strength of the injection molded sample is 46 MPa, and the optical sample color difference b value is 0.4.
[0047] Example 4
[0048] (1) Add 856g of terephthalic acid, 295g of 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 596g of 1,4-cyclohexanediol, 0.76g of dibutyltin oxide and 0.76g of triphenyl phosphate to a reaction vessel and carry out transesterification reaction at 230℃ and 200kPaG for 150min.
[0049] (2) Then the system is restored to normal pressure, the temperature is kept constant at 230℃, and the vacuum is gradually reduced to below 0.05kPaA at a depressurization rate of 2.52kPa / min. The mass content of excess diol 2,2,4,4-tetramethyl-1,3-cyclobutanediol and its impurities (such as 1-(1-butenoxy)pentane) is ≤0.2%.
[0050] (3) Maintain a vacuum below 0.05 kPa and react at 260°C for 150 min to obtain copolyester 4. After water cooling and pelletizing, copolyester granules are obtained with an intrinsic viscosity of 0.691 dL / g, a light transmittance of 91%, a haze of 0.4%, and optical sample color difference L value of 95, a value of -0.3, and b value of 0.5. The tensile strength of the granule injection molded sample is 45 MPa. After heating at 270°C for 10 min, the tensile strength of the injection molded sample is 45 MPa, and the optical sample color difference b value is 0.6.
[0051] Example 5
[0052] (1) 1000g of dimethyl terephthalate, 223g of 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 594g of 1,4-cyclohexanediol, 0.57g of dibutyltin oxide and 0.57g of triphenyl phosphate were added to the reaction vessel and the transesterification reaction was carried out at 210℃ and 50kPaG for 180min.
[0053] (2) Then the system is restored to normal pressure, the temperature is kept constant at 210℃, and the vacuum is gradually reduced to below 0.05kPaA at a depressurization rate of 2.02kPa / min. The excess diol 2,2,4,4-tetramethyl-1,3-cyclobutanediol and its impurities (1-(1-butenoxy)pentane, etc.) have a mass content ≤0.2%.
[0054] (3) Maintain a vacuum below 0.05 kPa and react at 260℃ for 210 min to obtain copolyester 5. After water cooling and pelletizing, copolyester granules are obtained with an intrinsic viscosity of 0.691 dL / g, a light transmittance of 92%, a haze of 0.3 wt%, and optical sample color difference L value of 95, a value of -0.3, and b value of 0.5. The tensile strength of the granule injection molded sample is 46 MPa. After heating at 270℃ for 10 min, the tensile strength of the injection molded sample is 45 MPa, and the optical sample color difference b value is 0.5.
[0055] Example 6
[0056] (1) 1000g of dimethyl terephthalate, 520g of 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 594g of 1,4-cyclohexanediol, 0.57g of dibutyltin oxide and 0.57g of triphenyl phosphate were added to the reaction vessel and subjected to transesterification reaction at 210℃ and a pressure of 50kPaG for 180min.
[0057] (2) Then the system is restored to normal pressure, the temperature is kept constant at 210℃, and the vacuum is gradually reduced to below 0.05kPaA at a depressurization rate of 2.02kPa / min. Excess diol 2,2,4,4-tetramethyl-1,3-cyclobutanediol and its impurities (1-(1-butenoxy)pentane, etc.) are removed. The mass content of monomers and impurities is ≤0.2%.
[0058] (3) Maintain a vacuum below 0.05 kPa and react at 260℃ for 210 min to obtain copolyester 6. After water cooling and pelletizing, copolyester granules are obtained with an intrinsic viscosity of 0.688 dL / g, light transmittance of 91%, haze of 0.4%, and optical sample color difference L value of 95, a value of -0.4, and b value of 0.5. The tensile strength of the granule injection molded sample is 45 MPa. After heating at 270℃ for 10 min, the tensile strength of the injection molded sample is 44 MPa, and the optical sample color difference b value is 0.6.
[0059] Comparative Example 1
[0060] (1) 1000g of dimethyl terephthalate, 295g of 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 596g of 1,4-cyclohexanediol, 0.57g of dibutyltin oxide and 0.57g of triphenyl phosphate were added to the reaction vessel and the transesterification reaction was carried out at 210℃ and 50kPaG for 180min.
[0061] (2) Then the system is restored to normal pressure, the temperature is kept constant at 210℃, and the vacuum is directly (within about 1 minute) drawn to below 0.05 kPaA. The reaction is carried out for 50 minutes. The excess diol 2,2,4,4-tetramethyl-1,3-cyclobutanediol and its generated impurities (1-(1-butenoxy)pentane, etc.) have a mass content of 0.5%.
[0062] (3) Then, while maintaining a vacuum below 0.05 kPa, the mixture was heated to 260°C and reacted for 210 min to obtain copolyester 7. After water cooling and pelletizing, copolyester granules were obtained with an intrinsic viscosity of 0.687 dL / g, a light transmittance of 90%, a haze of 0.6%, and optical sample color difference L value of 94, a value of -0.6, and b value of 0.8. The tensile strength of the granule injection-molded sample was 46 MPa. After heating at 270°C for 10 min, the tensile strength of the injection-molded sample was 44 MPa, and the optical sample color difference b value was 0.9.
[0063] Comparative Example 2
[0064] (1) 1000g of dimethyl terephthalate, 295g of 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 596g of 1,4-cyclohexanediol, 0.57g of dibutyltin oxide and 0.57g of triphenyl phosphate were added to the reaction vessel and the transesterification reaction was carried out at 210℃ and 50kPaG for 180min.
[0065] (2) Then the system is restored to normal pressure, the temperature is raised to 245℃, and the vacuum is directly (within about 1 minute) drawn to below 0.05 kPaA. The reaction is carried out for 50 minutes, and excess diol 2,2,4,4-tetramethyl-1,3-cyclobutanediol and its impurities (1-(1-butenoxy)pentane, etc.) are added until the mass content of monomer and impurities is 0.6%.
[0066] (3) Then, maintaining a vacuum below 0.05 kPa, the reaction was carried out at 260°C for 210 min to obtain copolyester 8. After water cooling and pelletizing, copolyester granules were obtained with an intrinsic viscosity of 0.686 dL / g, a light transmittance of 90%, a haze of 0.6%, and optical sample color difference L value of 94, a value of -0.6, and b value of 0.9. The tensile strength of the granule injection molded sample was 45 MPa. After heating at 270°C for 10 min, the tensile strength of the injection molded sample was 43 MPa, and the optical sample color difference b value was 1.0.
[0067] Comparative Example 3
[0068] (1) 1000g of dimethyl terephthalate, 295g of 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 596g of 1,4-cyclohexanediol, 0.57g of dibutyltin oxide and 0.57g of triphenyl phosphate were added to the reaction vessel and the transesterification reaction was carried out at 210℃ and atmospheric pressure for 180min.
[0069] (2) Keep the temperature constant at 210℃ and gradually evacuate to below 0.05kPaA at a pressure reduction rate of 2.02kPa / min. The excess diol 2,2,4,4-tetramethyl-1,3-cyclobutanediol and its impurities (1-(1-butenoxy)pentane, etc.) have a mass content of 0.4%.
[0070] (3) Then, while maintaining a vacuum below 0.05 kPa, the mixture was heated to 260°C and reacted for 210 min to obtain copolyester 9. After water cooling and pelletizing, copolyester granules were obtained with an intrinsic viscosity of 0.687 dL / g, a light transmittance of 90%, a haze of 0.6%, and optical sample color difference L value of 94, a value of -0.6, and b value of 0.7. The tensile strength of the granule injection molded sample was 46 MPa. After heating at 270°C for 10 min, the tensile strength of the injection molded sample was 44 MPa, and the optical sample color difference b value was 0.8.
Claims
1. A method for producing a transparent copolyester, characterized by, The preparation method comprises the following steps: S1: binary acid or ester of binary acid and binary alcohol are first subjected to esterification or ester exchange reaction under 5-300 kPaG pressure to obtain esterification product or ester exchange product; S2: the system is returned to normal pressure, and pre-polycondensation reaction is carried out at the esterification or ester exchange reaction temperature by gradually reducing the pressure to <0.1 kPaA to obtain a prepolymer; S3: temperature is raised to carry out final polycondensation reaction to obtain the target copolyester.
2. The production method according to claim 1, characterized by, The reaction pressure in S1 is 50-200 kPaG; And / or, the reaction temperature in S1 is 190-240 DEG C, preferably 210-230 DEG C; And / or, the reaction time in S1 is 120-240 min, preferably 150-180 min.
3. The production method according to claim 1 or 2, characterized by, The reaction temperature in S2 is 190-240 DEG C, preferably 210-230 DEG C; Preferably, the reaction pressure in S2 is gradually reduced from normal pressure to <0.05 kPaA; Preferably, the pressure reduction rate in S2 is 1.68-3.36 kPa / min, preferably 2.02-2.52 kPa / min; Preferably, the mass content of monomers and impurities in the system is 0.3 wt% or less, preferably 0.2 wt% or less.
4. The production method according to claim 1 or 2, characterized by, The reaction temperature in S3 is 250-270 DEG C, preferably 260-265 DEG C; And / or, the reaction pressure in S3 is 0.1 kPaA or less, preferably 0.05 kPaA or less; And / or, the reaction time in S3 is 120-300 min, preferably 150-210 min.
5. The method of any one of claims 1-4, wherein, The ester of binary acid is dimethyl ester of binary acid; Preferably, the binary acid or ester of binary acid in S1 is selected from one or more of terephthalic acid or dimethyl ester thereof, isophthalic acid or dimethyl ester thereof, phthalic acid or dimethyl ester thereof, diphenyl dicarboxylic acid or dimethyl ester thereof, naphthalene dicarboxylic acid or dimethyl ester thereof, furan dicarboxylic acid or dimethyl ester thereof, thiophene dicarboxylic acid or dimethyl ester thereof, and cyclohexane dicarboxylic acid or dimethyl ester thereof, more preferably terephthalic acid or dimethyl ester thereof and / or isophthalic acid or dimethyl ester thereof; Preferably, the binary alcohol in S1 is C2-C20 aliphatic diol and / or aromatic diol, preferably one or more of 1,4-cyclohexane dimethanol, 2,2,4,4-tetramethyl-1,3-cyclobutane diol, isosorbide, ethylene glycol, 1,3-propanediol, 2-methyl-1,3-propanediol, 1,2-propanediol, 1,4-butanediol, 2,3-butanediol, 1,2-pentanediol, 1,4-pentanediol, 1,5-pentanediol, neopentyl glycol, 3-methyl 1,5-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, diethylene glycol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, spiro glycol, tricyclodecane dimethanol, more preferably 1,4-cyclohexane dimethanol and / or 2,2,4,4-tetramethyl-1,3-cyclobutane diol; Preferably, the molar ratio of the binary alcohol to binary acid or ester of binary acid is (1.1-1.5):1, preferably (1.2-1.4):
1.
6. The method of any one of claims 1-5, wherein, A catalyst is further added in S1; Preferably, the catalyst is one or more of dibutyltin oxide, dimethyltin oxide, monobutyltin triisooctoate, dibutyltin dimethoxide, stannous octoate, stannous oxalate, dibutyltin diacetate, dibutyltin dilaurate, tetrabutyl titanate, isopropyl titanate, titanium glycolate, lithium acetate, potassium acetate, calcium acetate, magnesium acetate, barium acetate, zinc acetate, cobalt acetate, antimony acetate, lead acetate, manganese acetate, germanium dioxide, more preferably dibutyltin oxide and / or tetrabutyl titanate; Preferably, the catalyst is added in an amount of 200-500 ppm, preferably 300-400 ppm, based on the total mass of the dihydric alcohol and the diacid or diester of the diacid.
7. The method of any one of claims 1-6, wherein, A heat stabilizer is also added in S1; Preferably, the heat stabilizer is a phosphoric acid ester compound, preferably an alkyl phosphoric acid ester and / or an aryl phosphoric acid ester, more preferably triphenyl phosphate and / or triethyl phosphate; Preferably, the heat stabilizer is added in an amount of 300-600 ppm, preferably 300-400 ppm, based on the total mass of the dihydric alcohol and the diacid or diester of the diacid.
8. A transparent copolyester prepared according to the process of any one of claims 1-7.
9. An article of the transparent copolyester prepared according to the process of any one of claims 1-7, including a bottle, a sheet, a plate, and a film.
Citation Information
Patent Citations
Polyester compositions containing cyclobutanediol having high glass transition temperature and articles made therefrom
CN101300285A
Cited By
PETG (polyethylene terephthalate glycol) resin as well as preparation method and application thereof
CN122302233A