Preparation method and application of triazole phosphate type corrosion and scale inhibitor

The preparation of triazole phosphate-based corrosion and scale inhibitors has solved the shortcomings of existing technologies that combine scale inhibitors and corrosion inhibitors, achieving high-efficiency scale inhibition and corrosion inhibition under high temperature and high pressure conditions. It has good environmental friendliness and ease of operation, and is suitable for the protection of metal pipelines in the petroleum industry.

CN122080067APending Publication Date: 2026-05-26SOUTHWEST PETROLEUM UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202610536063.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-04-22
Publication Date
2026-05-26

AI Technical Summary

Technical Problem

In existing technologies, conventional physical compounding of scale inhibitors and corrosion inhibitors suffers from poor synergistic effect, unstable molecular structure, poor environmental friendliness, narrow applicable operating conditions, and complex operation, making it difficult to effectively protect oil and metal pipelines under conditions of high mineralization, high hardness, and high temperature.

Method used

A triazole phosphate-type corrosion and scale inhibitor was prepared by a specific three-step synthesis method. By combining phosphate groups and triazole groups, it was designed as a single compound to achieve molecular-level synergy between scale inhibition and corrosion inhibition, forming a stable protective film.

Benefits of technology

It provides a more efficient, stable, economical and convenient pipeline protection solution, with excellent corrosion inhibition and scale inhibition performance, and exhibits catalytic activity for photocatalytic carbon dioxide reduction under both room temperature and high temperature conditions, making it suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122080067A_ABST
    Figure CN122080067A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a triazole phosphate type corrosion and scale inhibitor, and relates to the technical field of industrial water treatment chemicals. The compound is prepared by a three-step synthesis method which comprises the following steps: firstly, preparing an amino methylene phosphonic acid compound with one-NH reaction site from n ethylene (n + 1) amine, phosphorous acid and formaldehyde; secondly, preparing a triazole derivative from ethylene glycol glycidyl ether and triazole; and reacting the two products with sodium bicarbonate to obtain a target product. The target molecule contains a sodium phosphate group and a triazole group at the same time, through the synergistic effect of functional groups, intramolecular synergy of scale inhibition and corrosion inhibition functions is achieved, and the corrosion inhibition performance higher than that of a DETPMP scale and corrosion inhibitor used commercially is shown. The triazole phosphate type corrosion and scale inhibitor has good catalytic activity on photocatalytic carbon dioxide reduction under the conditions of room temperature and high temperature, the TON (carbon monoxide conversion number) can reach 1206, and the selectivity is 100%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of industrial water treatment chemicals, specifically to a triazole phosphate-type corrosion and scale inhibitor for petroleum industry metal pipelines. Its core lies in a novel compound prepared by a specific three-step synthesis method, which contains both phosphonic acid (sodium) groups and triazole groups in its molecular structure. The invention also discloses the preparation method of this compound and its application in the protection of petroleum metal pipelines. Background Technology

[0002] During oil extraction, transportation, and water injection, metal pipelines and equipment are in long-term contact with formation water or reinjection water with high mineralization, high hardness, and high temperature, facing the dual challenges of scaling and corrosion. Scale (mainly calcium carbonate, calcium sulfate, barium sulfate, etc.) significantly increases fluid transport resistance and energy consumption, and may even cause pipeline blockage; while corrosion directly damages the structural integrity of the pipeline, potentially leading to serious safety accidents such as perforation and leakage.

[0003] Currently, industrial applications commonly employ chemical agents for protection. To simultaneously inhibit scale formation and corrosion, the conventional approach involves physically combining specialized scale inhibitors and corrosion inhibitors. Common scale inhibitors include organophosphonic acid compounds such as aminotrimethylphosphonic acid (ATMP) and hydroxyethylidene diphosphonic acid (HEDP), which primarily inhibit scale formation through chelation and lattice distortion. Common corrosion inhibitors include nitrogen-containing heterocyclic compounds such as benzotriazole (BTA) and methylbenzotriazole (TTAA), which adsorb onto metal surfaces to form a protective film. However, this simple physical mixing of different functional agents suffers from the following long-standing, unresolved core technical defects: First, poor synergistic effect: different agent molecules may compete for adsorption or exhibit functional antagonism at the solution system and metal interface, resulting in overall protective efficacy often falling short of expectations, i.e., a "1+1500" effect. Under harsh conditions such as high chloride concentrations (mg / L) and high temperatures (e.g., >80°C), the molecular structure of benzotriazole corrosion inhibitors is unstable, easily decomposing or forming insoluble calcium gels with calcium ions, leading to the failure of their scale inhibition function under critical conditions. First, under high chloride ion concentrations or fluid shear forces, the adsorption film formed by benzotriazole corrosion inhibitors is not dense enough or is easily damaged, resulting in a sharp decline in corrosion inhibition performance. Second, their environmental friendliness is poor: traditional agents have high phosphorus content, and some components have poor biodegradability, conflicting with increasingly stringent environmental regulations. Third, their applicable operating range is narrow: existing compound systems have poor adaptability to water quality fluctuations (such as changes in pH and ionic strength), and their performance is unstable under extreme water quality conditions. Fourth, their operation and management are complex: separate storage, transportation, and precise control of the addition of multiple agents are required, increasing system complexity and the risk of human error.

[0004] Therefore, there is an urgent need in this field for a fundamental technological breakthrough: the development of a novel single compound whose molecular structure is designed to simultaneously carry highly efficient scale inhibitor and corrosion inhibitor functional groups, achieving efficient synergy between the two at the molecular level. This would provide a more efficient, stable, economical, and user-friendly pipeline protection solution. In view of this, this patent application is hereby filed. Summary of the Invention

[0005] Therefore, the technical solution provided by the present invention is as follows: A method for preparing a triazole phosphate-based corrosion and scale inhibitor, characterized by comprising the following steps: (1) Different n-ethylene(n+1)amine(n+2)methylenephosphoric acid compounds were prepared by adding n-ethylene(n+1)amine, phosphorous acid and formaldehyde solution to acid solution and heating reaction; wherein one -NH reaction site must be retained in the obtained compound; (2) Triazole derivatives were prepared by adding ethylene glycol glycidyl ether, triazole and catalyst to dimethyl sulfoxide and heating. (3) The triazole phosphate type corrosion and scale inhibitor can be prepared by heating the n-ethylene(n+1)amine(n+2)methylene phosphate compound prepared in step (1) and the triazole derivative prepared in step (2) in an aqueous solution. The R=H in the compound structure can be reacted to R=Na by neutralization with sodium bicarbonate.

[0006] A triazole phosphate-based corrosion and scale inhibitor, characterized in that the chemical structural formula of the triazole phosphate-based corrosion and scale inhibitor is as follows: ; In the chemical structural formula, n = 1, 2, 3, 4, 5 or 6; R = H or Na; Preferably, the acid solution in step (1) is a hydrochloric acid solution; the heating reaction conditions are: heating temperature of 80-100℃ and reaction time of 5-12h.

[0007] Preferably, the molar ratio of n-ethylene(n+1)amine, phosphorous acid and formaldehyde in step (1) is 1:n+2:2(n+2).

[0008] Preferably, the triazole mentioned in step (2) is a sterically hindered triazole, and more preferably o-methylbenzotriazole.

[0009] Preferably, the catalyst in step (2) is one of triphenylphosphine or triethylamine.

[0010] Preferably, the molar ratio of the n-ethylene(n+1)amine(n+2)methylenephosphonic acid compound to the triazole derivative in step (3) is 1:1.

[0011] Preferably, the heating reaction conditions in step (3) are: heating temperature of 80-100℃, reaction time of 5-12h, and reaction pH of 7.

[0012] The aforementioned triazole phosphate corrosion and scale inhibitors are used in the protection of metal pipelines in the petroleum industry.

[0013] Preferably, the application involves adding the compound to an aqueous medium with a mineralization greater than 10,000 mg / L, a calcium ion concentration greater than 500 mg / L, and a temperature between 60-100°C.

[0014] The specific principles of this invention are as follows: The triazole phosphate-type corrosion and scale inhibitor designed in this invention first synthesizes different n-ethylene(n+1)amine(n+2)methylenephosphonic acid systems via the Moedritzer–Irani reaction, retaining a -NH reaction site to allow the corresponding molecule to further react with triazole derivatives. Then, ethylene glycol glycidyl ether is reacted with triazole, and the amount of reactants is precisely controlled to obtain a triazole derivative with a single-sided ring-opening of ethylene glycol glycidyl ether. Finally, the triazole phosphate-type corrosion and scale inhibitor is prepared by a ring-opening addition reaction between n-ethylene(n+1)amine(n+2)methylenephosphonic acid and the triazole derivative. Neutralization with sodium bicarbonate can be used to change the R=H in the compound's structural formula to R=Na. The phosphate groups in the prepared triazole phosphate-type corrosion and scale inhibitor molecule can chelate with calcium ions in the aquatic environment to prevent calcium salt precipitation; while the triazole groups can adsorb onto the surface of metal pipes to form a protective film, thus achieving a corrosion inhibition effect.

[0015] The beneficial effects of this invention are as follows: 1) The preparation method of the triazole phosphate type corrosion and scale inhibitor provided by the present invention is simple and efficient, the reaction conditions are mild, no high temperature and high pressure are required, no special equipment is required, and it is suitable for large-scale industrial production. The yield of the triazole phosphate type corrosion and scale inhibitor can be as high as 83%. 2) The triazole phosphate-type corrosion and scale inhibitor provided by this invention not only has excellent corrosion inhibition performance but also good scale inhibition performance; 3) The triazole phosphate-type corrosion and scale inhibitor synthesized in this invention exhibits excellent catalytic activity for photocatalytic carbon dioxide reduction under both room temperature and high temperature conditions, with a carbon monoxide conversion number (TON) reaching 1206 and a selectivity of 100%. This not only realizes the recycling of carbon dioxide but also provides an ideal artificial photosynthesis simulation system, showing promising prospects for industrial applications. Attached Figure Description

[0016] Figure 1This is a diagram illustrating the synthesis reaction of diethylenetriaminetetramethylenephosphoric acid.

[0017] Figure 2 The diagram shows the synthesis reaction of triethylenetetramine pentamethylphosphoric acid.

[0018] Figure 3 The diagram shows the synthesis reaction of tetraethylenepentamine hexamethylphosphoric acid.

[0019] Figure 4 This is a diagram showing the synthesis reaction of triazole derivatives.

[0020] Figure 5 The diagram shows the synthesis reaction of sodium (((2-((di(phosphonomethyl)amino)ethyl)(phosphonomethyl)amino)ethyl)(2-hydroxy-3-(2-(2-hydroxy-3-(1H-1,2,4-triazol-1-yl)propoxy)ethoxy)propyl)amino)methyl)phosphonate.

[0021] Figure 6 The diagram shows the synthesis reaction of sodium 2-(2-hydroxy-3-(2-(2-hydroxy-3-(1H-1,2,4-triazol-1-yl)propoxy)ethoxy)propyl)-5,8,11-tris(phosphonomethyl)-2,5,8,11-tetraazadodecane-1,12-dimethylbisphosphonate.

[0022] Figure 7 The diagram shows the synthesis reaction of sodium 2-(2-hydroxy-3-(2-(2-hydroxy-3-(1H-1,2,4-triazol-1-yl)propoxy)ethoxy)propyl)-5,8,11,14-tetra(phosphonomethyl)-2,5,8,11,14-pentazopentadecane-1,15-dimethylbisphosphonate.

[0023] Figure 8 The image shows a steel sheet after it has been cleaned following 140 hours of application of a 100ppm scale and corrosion inhibitor. Detailed Implementation

[0024] The present invention will now be described in further detail with reference to the accompanying drawings and embodiments. It should also be understood that the following embodiments are only for further illustration of the present invention and should not be construed as limiting the scope of protection of the present invention. Specific mass, reaction time, temperature, process parameters, etc., in the examples are merely examples within a suitable range. Any non-essential improvements and adjustments made by those skilled in the art based on the above description of the present invention are within the scope of protection of the present invention.

[0025] Example 1: The synthesis of the triazole phosphate-type corrosion and scale inhibitor of the present invention includes the following steps: 1) Synthesis of tetraethylenepentamine hexamethylphosphonic acid: 10 mmol of tetraethylenepentamine was added to 30 ml of deionized water and stirred until homogeneous. Then, 60 mmol of phosphorous acid was added and stirred until homogeneous. Subsequently, 6.8 ml of concentrated hydrochloric acid (37%) was added dropwise. When the reaction temperature was raised to 90℃, 9 ml of formaldehyde aqueous solution (37%~40%) with a formaldehyde content of 120 mmol was added dropwise. The temperature was then raised to 100℃ and reacted for 6 hours to obtain the initial product, tetraethylenepentamine hexamethylphosphonic acid. The synthesis reaction formula of tetraethylenepentamine hexamethylphosphonic acid is as follows: Figure 3 As shown; add saturated sodium bicarbonate solution (concentration of 1.0~1.1mol / L) to the obtained primary product to neutralize until no bubbles are generated. Then remove unreacted formaldehyde and excess water in the reaction system by rotary evaporator, and filter out the precipitated sodium chloride through filter paper to finally prepare sodium tetraethylenepentamine hexamethylidene phosphate. 2) Synthesis of triazole derivatives: 10 mmol of triazole (solid) and 10 mmol of ethylene glycol glycidyl ether (liquid) were ultrasonically mixed at a molar ratio of 1:1 for 2 min, and then reacted slowly at 70 °C for 120 min to generate the triazole derivative intermediate (1-(2-(epoxypropane-2-ylmethoxy)ethoxy)-3-(1H-1,2,4-triazol-1-yl)prop-2-ol) to be added to the target reaction molecule. 3) The sodium tetraethylenepentamine hexamethylidene phosphate obtained in step 1) and the triazole derivative obtained in step 2) are mixed in a 1:1 ratio under neutral aqueous solvent conditions, and the reaction temperature is raised to 100℃ for 6 hours to obtain the final product 2-(2-hydroxy-3-(2-2-(2-hydroxy-3-(2-(2-hydroxy-3-(1H-1,2,4-triazol-1-yl)propoxy)ethoxy)propyl)-5,8,11,14-tetra(phosphonomethyl)-2,5,8,11,14-pentazapentadecan-1,15-dimethyldiphosphonate sodium salt. After removing excess water by rotary evaporation and drying in an oven at 105℃ for 24 hours, the yield was calculated to be 83% by the weight reduction method. The specific reaction formula is as follows. Figure 7 As shown.

[0026] Example 2: The synthesis steps of the scale inhibitor sodium phosphonate (((2-((di(phosphonomethyl)amino)ethyl)(phosphonomethyl)amino)ethyl)(2-hydroxy-3-(2-(2-hydroxy-3-(1H-1,2,4-triazol-1-yl)propoxy)ethoxy)propyl)amino)methyl) are the same as in Example 1, except that tetraethylenepentamine in step 1) is replaced with diethylenetriamine; wherein, the synthesis reaction formula of diethylenetriamine tetramethylenephosphonic acid is as follows. Figure 1As shown, the synthetic reaction formula for sodium (((2-((di(phosphonomethyl)amino)ethyl)(phosphonomethyl)amino)ethyl)(2-hydroxy-3-(2-(2-hydroxy-3-(1H-1,2,4-triazol-1-yl)propoxy)ethoxy)propyl)amino)methyl)phosphonate is as follows Figure 5 As shown.

[0027] Example 3: The synthesis steps of the scale inhibitor sodium 2-(2-hydroxy-3-(2-(2-hydroxy-3-(1H-1,2,4-triazol-1-yl)propoxy)ethoxy)propyl)-5,8,11-tris(phosphonomethyl)-2,5,8,11-tetraazadodecane-1,12-dimethylbisphosphonate were the same as in Example 1, except that tetraethylenepentamine in step 1) was replaced with triethylenetetramine; wherein, the synthesis reaction formula of triethylenetetraminepentimide phosphoric acid is as follows. Figure 2 As shown, the synthetic reaction formula for sodium 2-(2-hydroxy-3-(2-(2-hydroxy-3-(1H-1,2,4-triazol-1-yl)propoxy)ethoxy)propyl)-5,8,11-tris(phosphonomethyl)-2,5,8,11-tetraazadodecane-1,12-dimethylbisphosphonate is as follows: Figure 6 As shown.

[0028] Example 4: The corrosion inhibition performance of the prepared scale and corrosion inhibitor was tested according to "SYT 0026.1-2024 Determination of Corrosion Rate of Metallic Materials in Oil and Gas Field Media Part 1: Corrosion Coating Method". The specific conditions and steps are as follows: The metal sample used in the test was Q235 steel, with dimensions of 5cm in length, 2.5cm in width, 0.2cm in thickness, and a surface area of ​​28cm². 2 ; The test conditions were: the temperature of the plate was 40℃, and the test time was 133.5h (50ppm) and 140h (100ppm). The testing equipment and instruments included: a constant temperature water bath (temperature range 30℃~90℃, temperature control accuracy). 0.1℃), balance (sensitivity 0.0001g), thermometer (0~100℃, scale division 1℃), 500ml hanging reagent bottle, raw material tape, ultrasonic cleaner, glass rod, measuring cylinder, tweezers, and several beakers; The specific test steps are as follows: (1) Prepare simulated oilfield water: Prepare simulated oilfield water (700mL) and simulated oilfield water (700mL) with corresponding scale inhibitors and corrosion inhibitors according to the standard, and affix labels. The oilfield water is prepared by mixing produced water A and river water B in a 1:1 ratio. The components are as follows: Produced water A solution contains 0.73 g / L sodium sulfate, 0.048 g / L sodium bicarbonate, 227.378 g / L sodium chloride, 2.519 g / L potassium chloride, 23.891 g / L magnesium chloride hexahydrate, 38.081 g / L anhydrous calcium chloride, and 2.721 g / L strontium chloride hexahydrate; River water B solution contains 37.619 g / L sodium chloride, 0.789 g / L potassium chloride, 18.899 g / L magnesium chloride hexahydrate, 2.502 g / L anhydrous calcium chloride, 11.196 g / L sodium sulfate, 0.199 g / L sodium bicarbonate, and 0.061 g / L strontium chloride hexahydrate. First, prepare solutions A and B separately. First, add the corresponding amount of the final scale and corrosion inhibitor molecules from Example 2 or the commercial DETPMP scale and corrosion inhibitor molecules to solution B, and then mix them in a 1:1 ratio. The concentration of the scale and corrosion inhibitor molecules is 50 ppm / 100 ppm. (2) Sample preparation: Take out the steel sheet and put it into a beaker. Add an appropriate amount of petroleum ether to the beaker to completely immerse the steel sheet. Then sonicate for 3 minutes to remove all the oil film on the surface of the steel sheet. Then take out the steel sheet, wash it with deionized water and anhydrous ethanol, and dry it with cold air for later use. (3) Weighing: Weigh the steel sheet samples prepared in step (3) in a balance and record their grade and corresponding weight. Weigh each sheet three times and take the average weight. (4) Hanging the strips: Cut the raw material tape into strips no less than 10cm long and twist them by hand; then pass the prepared raw material tape through the round hole of the steel sample and tie a knot 3cm above it; then hang the steel samples that have been tied on into the corresponding reagent bottles of simulated oilfield water and fix them with rubber bands, and then screw on the caps; heat the water bath to 40°C and place the above reagent bottles into the water bath and let them stand. The water in the water bath needs to cover the bottle body up to the cap opening. (5) Take out the test piece: Take the reagent bottle out of the water bath, then take out the test piece from the reagent bottle, cut the raw material tape, rinse the steel sheet with deionized water and gently brush the surface of the steel sheet with a brush to remove the scale crystals on the surface, then place it on the recording paper to take a picture. After taking the picture, select the steel sheet with the most severe corrosion and the hardest scale crystals on the surface, put it into the pickling solution (300mL hydrochloric acid + 5g hexamethylenetetramine and deionized water to make 1000mL) for ultrasonic cleaning, and continuously observe its surface. When its surface is smooth and free of scale crystals, take it out and record the cleaning time of the process to obtain the steel sheet after being cleaned with pickling solution. After rinsing the steel sheet with the pickling solution using deionized water, immerse it in NaOH solution (60g / L) for 30 seconds, then rinse it with deionized water. Dry the steel sheet and immerse it in anhydrous ethanol for 3 minutes. Remove it and dry it with cold air. Weigh each dried steel sheet in a balance and record the weight according to its grade. Weigh each sheet three times and take the average weight. Take a new steel sheet and repeat all the above experimental steps, record its weight, calculate the weight difference, and eliminate errors in the experimental process. (6) Data processing According to "SYT 0026.1-2024 Determination of Corrosion Rate of Metallic Materials in Oil and Gas Field Media - Part 1: Corrosion Coating Method", corrosion rate is used as the expression form of the test results, and the uniform corrosion rate is calculated according to the following formula: ; In the formula — Uniform corrosion rate (mm / a); —Sample mass (g) before the test; —Sample mass after the test (g); —Total surface area of ​​the sample (cm²) 2 ); —Test time (h); —Density of the sample material (g / cm³) 3 ); Furthermore, according to SY / T5329-94 "Recommended Indicators and Analytical Methods for Water Quality in Injection of Clastic Rock Reservoirs", the requirement for corrosivity of injection water is that the corrosion rate of carbon steel must be less than 0.076 mm / a. The results of the plate-coated corrosion inhibitor tests are shown in Tables 1 and 2. From the results in Tables 1 and 2, it can be seen that when the scale and corrosion inhibitor dosage is 50 ppm, the final corrosion rate of the scale and corrosion inhibitor molecules in Example 2 is 0.071 mm / a, while the corrosion rate of the commercial DETPMP scale and corrosion inhibitor molecules is 0.076 mm / a. When the scale and corrosion inhibitor dosage is 100 ppm, the final corrosion rate of the scale and corrosion inhibitor molecules in Example 2 is 0.0529 mm / a, and the corrosion rate of the DETPMP scale and corrosion inhibitor molecules is 0.0602 mm / a, both lower than the corrosion rate without scale and corrosion inhibitor (0.094 mm / a), thus achieving a corrosion inhibition effect. It can be seen that the synthesized scale and corrosion inhibitor molecules have higher corrosion inhibition performance than the commercial DETPMP molecules, and when at least 50 ppm of Y1 scale and corrosion inhibitor is added, the corrosion rate of Q235 steel in oilfield water meets the standard requirements (less than 0.076 mm / a). Figure 8 The image shows a steel sheet after it has been cleaned following 140 hours of application of a 100ppm scale and corrosion inhibitor.

[0029] Table 1. Results of 133.5h test of 50ppm scale and corrosion inhibitor tablets ; Table 2 Results of 140h test of 100ppm scale and corrosion inhibitor tablets .

[0030] Example 5: The scale inhibition performance of the prepared scale inhibitor was tested. The specific conditions and steps are as follows: (1) Preparation of cation solution: Add 0.73g sodium sulfate, 0.048g sodium bicarbonate, 227.378g sodium chloride, 2.519g potassium chloride, 23.891g magnesium chloride hexahydrate, 38.081g anhydrous calcium chloride, and 2.721g strontium chloride hexahydrate to 1 liter of deionized water and stir thoroughly to dissolve them, thus preparing a cation solution. The resulting solution is denoted as solution A. (2) Preparation of anionic solution: Add 37.619g sodium chloride, 0.789g potassium chloride, 18.899g magnesium chloride hexahydrate, 2.502g calcium chloride, 11.196g sodium sulfate, 0.199g sodium bicarbonate, and 0.061g strontium chloride hexahydrate to 1 liter of deionized water and stir thoroughly to dissolve them, thus preparing an anionic solution. The resulting solution is referred to as solution B. (3) Preparation of high-concentration scale inhibitor solution (1000ppm): Add 0.4g DETPMP (diethylenetriaminepentamethylphosphonic acid, active ingredient content 50%) to 100ml of step (2) to prepare solution B containing 1000ppm DTPMP. The resulting solution is recorded as solution S. (4) Add 0.4g of scale and corrosion inhibitor Y1 (corresponding to the final scale and corrosion inhibitor molecule in Example 2, with an effective ingredient content of 50%) to 200ml of solution B prepared in step (2) to obtain solution B containing 1000ppm of Y1. The resulting solution is recorded as solution Y. (5) Take 10 ml of S prepared in step (3), 10 ml of Y prepared in step (4), and 90 ml of B prepared in step (2) respectively, mix them to prepare an anionic solution with a scale inhibitor and corrosion inhibitor content of 100 ppm, and record the resulting solutions as S1 and Y1. (6) Take 100ml of solution A obtained in step (1) into three beakers and label them as A1, A2, and A3. Label 100ml of solution B obtained in step (2) as K. (7) Place the S1, Y1, K obtained in step (5) and the A1, A2, A3 obtained in step (6) into an oven preheated to 90°C. After heating for 1 hour, take them out and mix S1, Y1, K with A1, A2, A3 respectively to obtain 1 part of each solution containing 50 ppm scale inhibitor DTPMP and Y1, and 1 part of blank solution. After standing for 24 hours, the sample to be tested is obtained. (8) Take 1 ml of the supernatant from each of the samples prepared in step (7) and dilute it 10 times with 9 ml of deionized water. Measure the calcium ion concentration using ICP within 2 hours. Then calculate the scale inhibition efficiency using the following formula: ; In the formula: the concentration of calcium ion control sample is 6751 mg / L, and the concentration of calcium ion blank sample is 5442 mg / L; The scale inhibition efficiency is shown in Table 3. As can be seen from Table 3, at 90℃, the scale inhibition rate of scale inhibitor Y1 (content of 50ppm) for oilfield water is 85.63% after 24 hours, which is close to the scale inhibition rate (89.91%) of commercial scale inhibitor DETPMP (content of 50ppm). The reason why the scale inhibition rate of the synthesized scale inhibitor Y1 (the final scale inhibitor molecule in Example 2) is slightly lower than that of commercial scale inhibitor DETPMP may be that a phosphate scale inhibition group on commercial scale inhibitor DETPMP was changed to a triazole corrosion inhibition group, resulting in higher corrosion inhibition performance and slightly lower scale inhibition performance. However, both meet the qualified condition of scale inhibition rate greater than 85% in the scale inhibition performance test of GB / T 16632-2008 "Determination of Scale Inhibition Performance of Water Treatment Agents - Calcium Carbonate Deposition Method". Table 3 Scale Inhibition Rate Test Results ; The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.

Claims

1. A method for preparing a triazole phosphate-based corrosion and scale inhibitor, characterized in that it specifically includes the following steps: (1) Different n-ethylene(n+1)amine(n+2)methylenephosphoric acid compounds were prepared by adding n-ethylene(n+1)amine, phosphorous acid and formaldehyde solution to acid solution and heating reaction; wherein one -NH reaction site must be retained in the obtained compound; (2) Triazole derivatives were prepared by adding ethylene glycol glycidyl ether, triazole and catalyst to dimethyl sulfoxide and heating. (3) The triazole phosphate type corrosion and scale inhibitor can be prepared by heating the n-ethylene(n+1)amine(n+2)methylene phosphate compound prepared in step (1) and the triazole derivative prepared in step (2) in an aqueous solution. The R=H in claim 1 can be reacted to R=Na by neutralization with sodium bicarbonate.

2. A method for preparing the triazole phosphate-type corrosion and scale inhibitor as described in claim 1, characterized in that, The chemical structural formula of the triazole phosphate type corrosion and scale inhibitor is as follows: In the chemical structural formula, n = 1, 2, 3, 4, 5 or 6; R = H or Na.

3. The preparation method of the triazole phosphate type corrosion and scale inhibitor according to claim 1, characterized in that, The acid solution mentioned in step (1) is a hydrochloric acid solution; the heating reaction conditions are: heating temperature of 80-100℃ and reaction time of 5-12h.

4. The preparation method of the triazole phosphate type corrosion and scale inhibitor according to claim 1, characterized in that, The molar ratio of n-ethylene(n+1)amine, phosphorous acid and formaldehyde mentioned in step (1) is 1:n+2:2(n+2).

5. The preparation method of the triazole phosphate type corrosion and scale inhibitor according to claim 1, characterized in that, The triazole mentioned in step (2) is a sterically hindered triazole, preferably o-methylbenzotriazole.

6. The preparation method of the triazole phosphate type corrosion and scale inhibitor according to claim 1, characterized in that, The catalyst mentioned in step (2) is either triphenylphosphine or triethylamine.

7. The preparation method of the triazole phosphate type corrosion and scale inhibitor according to claim 1, characterized in that, The molar ratio of the n-ethylene(n+1)amine(n+2)methylenephosphonic acid compound to the triazole derivative in step (3) is 1:

1.

8. The method for preparing the triazole phosphate-type corrosion and scale inhibitor according to claim 1, characterized in that, The heating reaction conditions described in step (3) are: heating temperature of 80-100℃, reaction time of 5-12h, and reaction pH of 7.

9. The preparation method of the triazole phosphate type corrosion and scale inhibitor as described in claim 1 and the application of the preparation method of the triazole phosphate type corrosion and scale inhibitor as described in any one of claims 3-8 in the protection of metal pipelines in the petroleum industry.

10. The application of the triazole phosphate-based corrosion and scale inhibitor according to claim 9, characterized in that, The application involves adding the compound to an aqueous medium with a mineralization greater than 10,000 mg / L, a calcium ion concentration greater than 500 mg / L, and a temperature between 60-100°C.

Citation Information

Patent Citations

  • Corrosion-inhibitive and anti-sludge agent compond of derivatives of thiophosphate ester and imidazoline phosphate ester

    CN1030263A

  • Efficient scale and corrosion inhibitor and preparation method thereof

    CN103819010A

  • Nitrogen-containing multipurpose metal corrosion inhibitor and preparation method thereof

    CN119980244A

  • Compound for scale and corrosion inhibitor and scale and corrosion inhibitor

    CN120209035A

  • Scale and corrosion inhibitors

    CN1427860A