Silicon-oxygen-carbon composite material and preparation method thereof, secondary battery

By forming a Si@SiOx@C composite material with SiOx and carbon layers on the surface of silicon particles, the volume expansion and conductivity problems of silicon anode materials are solved, and the high capacity and fast charging performance are improved.

CN122314795APending Publication Date: 2026-06-30ENVISION DYNAMICS TECH (JIANGSU) CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411979662.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-12-30
Publication Date
2026-06-30

AI Technical Summary

Technical Problem

The theoretical specific capacity of graphite, a traditional lithium-ion battery anode material, limits its performance in high capacity and fast charging. Silicon anode materials face cycle life issues caused by volume expansion and SEI film recombination in applications.

Method used

A one-pot, single-step synthesis method was used to prepare Si@SiOx@C composite materials. By forming SiOx and carbon layers on the surface of silicon particles, volume expansion was buffered and conductivity was improved.

Benefits of technology

It effectively inhibits silicon particle expansion, improves conductivity, enhances electrochemical performance, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005221491250000101
    Figure BDA0005221491250000101
  • Figure BDA0005221491250000111
    Figure BDA0005221491250000111
Patent Text Reader

Abstract

This invention belongs to the field of battery active materials technology, specifically disclosing a silicon-oxygen-carbon composite material, its preparation method, and a secondary battery. The silicon-oxygen-carbon composite material is prepared using silicon powder, a carbon source, and an oxygen-generating agent as raw materials via a one-pot, single-step synthesis method, comprising the following processes: heating to a first preset temperature, decomposing the oxygen-generating agent to produce oxygen, oxidizing the silicon on the surface of the silicon particles to form a silicon oxide coating layer, and obtaining Si@SiO. x Particles, 0.5≤x≤2; heated to the second preset temperature, in the Si@SiO x A carbon coating layer is formed on the surface of the particles to obtain the silicon-oxygen-carbon composite material. This invention achieves this by forming a tightly wrapped SiO2 layer on the surface of silicon particles. x The thin film of the silicon layer and the carbon layer effectively buffers the volume expansion of silicon particles during the charging and discharging process, improves the conductivity of the silicon anode, and effectively avoids the side reaction between silicon particles and electrolyte. As an anode material, it exhibits considerable lithium storage capacity and excellent electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery active materials technology, and in particular to a silicon-oxygen-carbon composite material, its preparation method, and a secondary battery. Background Technology

[0002] Lithium-ion batteries have been widely used in portable electronic devices, large-scale energy storage devices, and electric vehicles in recent years. Traditional lithium-ion battery anode materials are mainly carbon-based, but the theoretical specific capacity of graphite materials (372 mAh / g) significantly limits their application in next-generation lithium-ion batteries, especially in meeting the requirements for high capacity and fast charging performance. Compared to traditional graphite anode materials, silicon anode materials have significant research and application potential due to their high theoretical discharge specific capacity (4200 mAh / g), low discharge potential (0.4 V vs. Li+ / Li), and abundant reserves on Earth. They have become a key research focus for major lithium battery material manufacturers and battery manufacturers in recent years.

[0003] The lithium storage mechanism of silicon anodes involves an alloying reaction with lithium. During this reaction, various alloy phases are formed, exhibiting significant differences in morphology and structure. When lithium is intercalated into silicon, the resulting massive volume expansion induces cracks in the silicon particles, leading to pulverization and the exposure of new interfaces. This process consumes electrolyte and results in the loss of active lithium, impacting the cell's cycle life. Furthermore, with continued cycling, the solid-electrolyte interface (SEI) film is continuously damaged and remodeled, leading to further loss of active lithium and a rapid decline in capacity. Therefore, silicon anodes still face significant challenges in practical applications. Summary of the Invention

[0004] In view of the shortcomings of the prior art described above, the purpose of this invention is to provide a silicon-oxygen-carbon composite material and its preparation method, as well as a secondary battery, through a one-pot single-step synthesis method to prepare Si@SiO. x In the @C composite electrode material, the SiOx layer and carbon layer on the surface of silicon particles can synergistically suppress the volume expansion of silicon particles, and the outermost carbon layer can improve the conductivity of the silicon anode, thereby improving the electrochemical performance of the silicon anode material.

[0005] To achieve the above and other related objectives, this invention provides a method for preparing silicon-oxygen-carbon composite materials. Using silicon powder, carbon source, and oxygen-generating agent as raw materials, a one-pot, single-step synthesis method is employed to prepare the silicon-oxygen-carbon composite material, comprising the following steps:

[0006] When the temperature is raised to the first preset temperature, the oxygen-generating agent decomposes to produce oxygen, and the silicon on the surface of the silicon oxide particles forms a silicon oxide coating layer, thus obtaining Si@SiO. x Particles, wherein 0.5 ≤ X ≤ 2;

[0007] The temperature is raised to the second preset temperature, in the Si@SiO x A carbon coating layer is formed on the surface of the particles to obtain the silicon-oxygen-carbon composite material;

[0008] The first preset temperature is lower than the second preset temperature.

[0009] Furthermore, the oxygen-generating agent is selected from at least one of liquid carbon dioxide, hydrogen peroxide, or ammonium bicarbonate.

[0010] Furthermore, when the oxygen-generating agent is selected from liquid carbon dioxide or ammonium bicarbonate, the first preset temperature is 50°C to 70°C.

[0011] Furthermore, when the oxygen-generating agent is selected from hydrogen peroxide, the first preset temperature is 115℃~170℃.

[0012] Furthermore, the second preset temperature is 600℃~1000℃.

[0013] Furthermore, the process of heating to the second preset temperature adopts a gradient heating method with a heating rate of 3℃ / min to 8℃ / min.

[0014] Furthermore, after heating to the second preset temperature, the heat preservation time is 6h to 12h.

[0015] Furthermore, the temperature is increased to a second preset temperature, in the Si@SiO x The process of forming a carbon coating on the particle surface is carried out under a protective atmosphere.

[0016] Furthermore, the mass ratio of the silicon powder, carbon source, and oxygen-generating agent is 1:0.05-0.5:0.05-0.15.

[0017] Furthermore, the particle size D50 of the silicon powder is 100nm to 200nm.

[0018] Furthermore, the carbon source is selected from organic carbon sources, which are selected from at least one of sucrose, glucose, maltose, lactose, starch, formaldehyde, acetaldehyde, propionaldehyde, phenolic resin, epoxy resin, polyethylene glycol, cellulose, lignin, polyvinyl alcohol, polyvinyl chloride, polyethylene oxide, polyurethane, polyfurfural, citric acid, or cyclodextrin.

[0019] Furthermore, the silicon powder and carbon source are dispersed in an alcohol as a solvent to form a mixture A, wherein the alcohol is selected from at least one of methanol, ethanol, benzyl alcohol, ethylene glycol or isopropanol.

[0020] Furthermore, when preparing the mixture A, 3g to 8g of silicon powder is added to every 100ml of the solvent alcohol.

[0021] Furthermore, the silicon-oxygen-carbon composite material is prepared by a one-pot single-step synthesis method using silicon powder, carbon source and oxygen-generating agent as raw materials, and also includes the following process: after heating to the first preset temperature, when the pressure is increased to the preset pressure, stirring is performed.

[0022] Furthermore, the preset pressure is 7MPa to 10MPa.

[0023] Furthermore, the stirring speed is 500 rpm to 600 rpm.

[0024] Furthermore, the stirring time is 1 hour to 6 hours.

[0025] The present invention also provides a silicon-oxygen-carbon composite material prepared according to the method described above, the silicon-oxygen-carbon composite material comprising spherical Si@SiO x @C particles, the Si@SiO x @C particles include Si@SiO x Particles and coatings of the Si@SiO x The carbon layer of the particles; the Si@SiO x The particles include core silicon and SiO2 coating the core silicon. x layer.

[0026] The present invention also provides a secondary battery, including a negative electrode sheet, the negative electrode sheet including a negative current collector and a negative active material layer coated on at least one side surface of the negative current collector, the negative active material layer including a negative active material, the negative active material including the silicon-oxygen-carbon composite material as described above.

[0027] As described above, the silicon-oxygen-carbon composite material, its preparation method, and the secondary battery of the present invention have the following beneficial effects:

[0028] This invention synthesizes Si@SiO using silicon powder, carbon source, and oxygen-generating agent as raw materials via a one-pot, single-step synthesis method. x @C composite material, through the formation of tightly wrapped SiO on the surface of silicon particles x The thin film of the silicon layer and the carbon layer effectively buffers the volume expansion of silicon particles during the charging and discharging process, improves the conductivity of the silicon anode, and effectively avoids the side reaction between silicon particles and electrolyte. As an anode material, it exhibits considerable lithium storage capacity and excellent electrochemical performance.

[0029] This invention employs a one-pot, single-step synthesis method to prepare Si@SiO. x @C composite materials have a simple preparation process, are easy to operate, and are suitable for large-scale production. Detailed Implementation

[0030] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.

[0031] In this invention, unless otherwise stated, the term "multiple" means two or more.

[0032] The character " / " indicates that the objects before and after it are in an "or" relationship. For example, A / B means: A or B.

[0033] The term "and / or" describes an association between objects, indicating that three relationships can exist. For example, A and / or B means: A or B, or A and B.

[0034] One embodiment of the present invention provides a method for preparing a silicon-oxygen-carbon composite material, which uses silicon powder, carbon source and oxygen-generating agent as raw materials and adopts a one-pot single-step synthesis method to prepare the silicon-oxygen-carbon composite material, including the following processes:

[0035] When the temperature is raised to the first preset temperature, the oxygen-generating agent decomposes to produce oxygen, and the silicon on the surface of the silicon oxide particles forms a silicon oxide coating layer, thus obtaining Si@SiO. x Particles, where 0.5 ≤ x ≤ 2;

[0036] The temperature is raised to the second preset temperature, in the Si@SiO x A carbon coating layer is formed on the surface of the particles to obtain the silicon-oxygen-carbon composite material;

[0037] The first preset temperature is lower than the second preset temperature.

[0038] In this invention, the oxygen generated by the decomposition of the oxygen-generating agent upon heating interacts with Si particles to form a continuous and uniformly coated SiO₂. x The layer can effectively buffer the volume expansion of Si during lithium insertion / extraction. This invention also includes Si@SiO x A thin carbon film was deposited on the outer layer of the particles through high-temperature carbonization, which improved the conductivity of the silicon anode. Simultaneously, SiO... x The tight encapsulation of the carbon layer and the silicon layer prevents direct contact between the Si particles and the electrolyte, reducing side reactions. Furthermore, this invention employs a one-pot, single-step synthesis method to prepare Si@SiO. x @C composite materials have a simple preparation process, are easy to operate, and are suitable for large-scale production.

[0039] In some embodiments, the oxygen-generating agent is selected from at least one of liquid carbon dioxide, hydrogen peroxide, or ammonium bicarbonate. The decomposition of these three compounds produces oxygen and other byproducts, but these byproducts are gases or carbon, easily separated, and do not introduce impurities into the finished product.

[0040] The chemical equation involved in the process of carbon dioxide decomposing to produce oxygen is: 2CO2(g)→2CO(g)+O2(g);

[0041] The chemical equation involved in the thermal decomposition of hydrogen peroxide to produce oxygen is: 2H2O2(l)→2H2O(l)+O2(g);

[0042] The chemical equations involved in the thermal decomposition of ammonium bicarbonate to produce oxygen are: NH4HCO3(s)→NH3(g)+CO2(g)+H2O(l), 2CO2(g)→2CO(g)+O2(g).

[0043] In some embodiments, when the oxygen-generating agent is selected from liquid carbon dioxide, the first preset temperature is 50°C to 70°C. Within this temperature range, liquid carbon dioxide is first vaporized and then decomposed to produce oxygen after being heated.

[0044] In some embodiments, when the oxygen-generating agent is selected from hydrogen peroxide, the first preset temperature is 115°C to 170°C. Within this temperature range, hydrogen peroxide decomposes into water and oxygen upon heating.

[0045] In some embodiments, when the oxygen-generating agent is selected from ammonium bicarbonate, the first preset temperature is 50°C to 70°C. Within this temperature range, ammonium bicarbonate decomposes into ammonia, carbon dioxide, and water upon heating, and the carbon dioxide further decomposes to produce oxygen.

[0046] In some embodiments, the second preset temperature is 600℃~1000℃, and high-temperature carbonization is performed at this temperature in Si@SiO x A thin carbon film is deposited on the outer layer of the particles.

[0047] In some embodiments, the process of heating to the second preset temperature employs a gradient heating method with a heating rate of 3°C / min to 8°C / min; after heating to the second preset temperature, the holding time is 6h to 12h; after heating to the second preset temperature, in the Si@SiO x The process of forming a carbon coating on the particle surface is carried out under a protective atmosphere, which is selected from at least one of nitrogen, argon, or hydrogen to provide an inert environment for the carbonization process.

[0048] In some embodiments, the mass ratio of silicon powder, carbon source, and oxygen-generating agent is 1:0.05–0.5:0.05–0.15. The amount of carbon source and oxygen-generating agent added respectively affects the carbon layer and SiO₂. x The thickness of the coating layer affects the electrochemical performance of the material, and the amount of both should not be too high.

[0049] In some embodiments, the particle size D50 of the silicon powder is 100nm to 200nm. The smaller the silicon powder particle size, that is, the smaller the silicon particles, the more difficult it is to coat. However, the method provided by the present invention can effectively coat small-diameter silicon particles. At the same time, the present invention also found that if the silicon powder particle size is too large, it will increase the volume expansion of silicon particles during charging and discharging, and deteriorate the cycle performance.

[0050] In some embodiments, the carbon source is selected from organic carbon sources, which are selected from at least one of sucrose, glucose, maltose, lactose, starch, formaldehyde, acetaldehyde, propionaldehyde, phenolic resin, epoxy resin, polyethylene glycol, cellulose, lignin, polyvinyl alcohol, polyvinyl chloride, polyethylene oxide, polyurethane, polyfurfural, citric acid, or cyclodextrin.

[0051] In some embodiments, the silicon powder and carbon source are dispersed in an alcohol as a solvent to form a mixture A, wherein the alcohol is selected from at least one of methanol, ethanol, benzyl alcohol, ethylene glycol, or isopropanol. The dispersion process may include, for example, a combination of one or more of ultrasonication, stirring, or centrifugation.

[0052] In some embodiments, when preparing the mixture A, 3g to 8g of silicon powder is added to every 100ml of the solvent alcohol. The amount of alcohol used also affects the particle size of the finished material, so the amount of alcohol used should not be too high; at the same time, the amount of alcohol used should not be too low, otherwise it will be difficult to disperse evenly, or the mixture A will be too viscous, which is not conducive to the subsequent reaction.

[0053] In some embodiments, a silicon-oxygen-carbon composite material is prepared by a one-pot, single-step synthesis method using silicon powder, carbon source, and oxygen-generating agent as raw materials. The method further includes the following steps: after heating to a first preset temperature, stirring is performed when the pressure reaches a preset pressure. The oxygen-generating agent decomposes upon heating to produce oxygen, causing an increase in the pressure inside the reactor. When the pressure inside the reactor reaches the preset pressure, stirring is initiated, causing the carbon source to decompose and coat the particle surface. Then, high-temperature carbonization is performed to form a uniformly coated carbon layer.

[0054] In some embodiments, the preset pressure is 7MPa to 10MPa, the stirring rate is 500rpm to 600rpm, and the stirring time is 1h to 6h.

[0055] In some embodiments, the method for preparing the silicon-oxygen-carbon composite material includes the following steps:

[0056] S1. A liquid-phase system is prepared using silicon powder, carbon source and oxygen generator as raw materials;

[0057] S2. The temperature is raised to the first preset temperature. The oxygen-generating agent in the liquid phase system decomposes to produce oxygen. The silicon on the surface of the silicon oxide particles forms a silicon oxide coating layer, thus obtaining Si@SiO. x After granulation, the reaction solution undergoes solid-liquid separation, washing, and drying to obtain precursor powder. The drying temperature is, for example, 60℃~80℃, and the drying time is, for example, 8h~16h, until the moisture content is less than 0.5%.

[0058] S3. The temperature is raised to the second preset temperature to perform high-temperature carbonization treatment on the precursor powder, in the Si@SiO x A carbon coating layer is formed on the surface of the particles to obtain the silicon-oxygen-carbon composite material.

[0059] Furthermore, it should be noted that the chemical reaction process involved in the preparation method of the present invention is carried out in a closed reaction vessel, such as a high-pressure reactor or a tube furnace. For example, steps S2 and S3 in the above embodiments are carried out in different reactors, i.e., in two reactors. The precursor preparation process in step S2 can be carried out, for example, in a high-pressure reactor, and the high-temperature carbonization process in step S3 can be carried out, for example, in a tube furnace.

[0060] Another embodiment of the present invention provides a silicon-oxygen-carbon composite material prepared according to the method described above, the silicon-oxygen-carbon composite material comprising spherical Si@SiO x @C particles, the Si@SiO x @C particles include Si@SiO x Particles and coatings of the Si@SiO x The carbon layer of the particles; the Si@SiO x The particles include core silicon and SiO2 coating the core silicon. x Layer. Using the preparation method of this invention, a tightly and uniformly coated SiO layer can be formed on the surface of silicon particles. x The layer and carbon coating layer, thus obtaining Si@SiO x @C particles are spherical, and good particle sphericity is beneficial to improving electrochemical performance.

[0061] Another embodiment of the present invention provides a secondary battery, including a negative electrode sheet, the negative electrode sheet including a negative electrode current collector and a negative electrode active material layer coated at least on one surface of the negative electrode current collector, the negative electrode active material layer including a negative electrode active material, the negative electrode active material including the silicon-oxygen-carbon composite material as described above. The silicon-oxygen-carbon composite material provided by the present invention, as a negative electrode material, exhibits considerable lithium storage capacity and excellent electrochemical performance. The negative electrode current collector is selected, for example, from any one of copper foil current collectors, composite copper foil current collectors, carbon current collectors, foamed copper current collectors, or stainless steel current collectors, the thickness of the negative electrode current collector being, for example, 8 μm to 15 μm, and the single-sided coating thickness of the negative electrode active material layer being, for example, 10 μm to 80 μm. In a specific embodiment, the negative electrode current collector is, for example, copper foil, and the thickness of the copper foil is, for example, 13 μm, and the single-sided coating thickness of the negative electrode active material layer is 50 μm.

[0062] In some embodiments, the negative electrode active material layer includes a negative electrode active material, a conductive agent, a binder, etc., and the mass ratio of the negative electrode active material, the conductive agent, and the binder can be, for example, 80-96:2-10:2-10. The negative electrode active material includes the silicon-oxygen-carbon composite material described above, and further includes compounds capable of intercalating and deintercalating lithium ions, such as graphite, soft carbon, hard carbon, artificial graphite, natural graphite, silicon, and silicon oxides (SiO₂). x The conductive agent is selected from at least one of the following: (0 < x < 2), silicon carbide compounds, or lithium titanate. The conductive agent is selected from any one or more of conductive carbon black, acetylene black, Ketjen black, carbon nanotubes, and graphene. The binder is selected from any one or more of polyvinylidene fluoride, polyethylene oxide, polyamide, polypropylene, polyacrylate, polyethylene ether, polymethyl methacrylate, polyhexafluoropropylene, or styrene-butadiene rubber.

[0063] In one specific embodiment, the negative electrode active material is selected, for example, from the silicon-oxygen-carbon composite material described above; the conductive agent is selected, for example, from conductive carbon black; and the binder is selected, for example, from polyacrylate. The negative electrode active material, conductive agent, and binder are mixed, for example, at a mass ratio of 8:1:1, and deionized water is added. The mixture is then stirred evenly under vacuum to obtain a negative electrode slurry. The negative electrode slurry is coated onto a copper foil, then air-dried at room temperature and transferred to an oven for drying. After cold pressing and slitting, the negative electrode sheet is obtained. In other embodiments, the negative electrode sheet can also be obtained by any other method of forming a negative electrode sheet.

[0064] In some embodiments, the secondary battery may be, for example, a lithium-ion battery, a sodium-ion battery, a potassium-ion battery, etc., but is not limited thereto.

[0065] In some embodiments, the secondary battery is a lithium-ion battery, including an electrolyte, a casing, and a bare cell disposed within the casing. The bare cell includes a positive electrode, a separator, and a negative electrode.

[0066] In one specific embodiment, the method for preparing the secondary battery includes the following steps: stacking a positive electrode, a separator, and a negative electrode sequentially, ensuring that a separator is present between any positive and negative electrode; obtaining a multi-layered stack by winding; and inserting this stack as a bare cell into a battery casing. Finally, injecting electrolyte into the casing once or in multiple stages, so that the bare cell is completely immersed in the electrolyte. In other words, the electrolyte is injected and fills the entire internal space of the battery, and the positive electrode, separator, and negative electrode are completely immersed in the electrolyte.

[0067] In one specific embodiment, the preparation method of the secondary battery includes the following steps: adding electrolyte to both sides of the separator, and assembling the positive electrode shell, positive electrode plate, separator, negative electrode plate and negative electrode shell in sequence in a glove box to form a button half battery.

[0068] In some embodiments, the positive electrode includes a positive current collector and a positive active material layer coated at least on one surface of the positive current collector. The positive current collector is, for example, a foil formed by surface treatment of materials such as nickel, titanium, aluminum, silver, stainless steel, or carbon. Besides foil, the positive current collector can also be used in any combination of one or more forms such as film, mesh, porous, foam, or nonwoven fabric. The thickness of the positive current collector is, for example, 8 μm to 15 μm, and the single-sided coating thickness of the positive active material layer is, for example, 20 μm to 100 μm. Further, in one specific embodiment, the positive current collector is, for example, an aluminum foil, and the thickness of the aluminum foil is, for example, 13 μm, and the single-sided coating thickness of the positive active material layer is 50 μm. In other embodiments, the positive electrode is, for example, a lithium metal sheet.

[0069] In some embodiments, the positive electrode active material layer includes a positive electrode active material, a binder, and a conductive agent, etc., and the mass ratio of the positive electrode active material, the conductive agent, and the binder can be, for example, 90-98:1-5:1-5. The positive electrode active material, for example, has the chemical formula Li. x [Ni y Co z Mn t M (1-y-z-t) ]O 2-δThe material, wherein M is selected from at least one of Cr, Zr, Ca, Mg, Cu, Ti, Al, Mo, W or Zn, 0.9 < x < 1.1, 0.65 ≤ y < 1.0, 0 ≤ z < 0.5, 0 ≤ t < 0.5, 0 ≤ δ ≤ 0.1. The binder is selected, for example, from any one or more of polyvinylidene fluoride (PVDF), poly(ethylene oxide) (PEO), polyamide (PA), polyacrylonitrile (PAN), polyacrylate, polyvinyl ether, polymethyl methacrylate (PMMA), ethylene-propylene-diene terpolymer (EPDM), polyhexanefluoropropylene (Polyhexafluoropropylene), or polymerized styrene-butadiene rubber (SBR). The conductive agent is selected from any one or more of conductive carbon black (Super P), acetylene black, carbon nanotubes, and graphene.

[0070] In one specific embodiment, the positive electrode active material is, for example, lithium iron phosphate, the binder is, for example, polyvinylidene fluoride, and the conductive agent is, for example, conductive carbon black. The positive electrode active material, conductive agent, and binder are mixed, for example, in a mass ratio of 98:1:1, and an organic solvent is added. The mixture is stirred under vacuum until the system is homogeneous to obtain a positive electrode slurry. The organic solvent is, for example, N-methylpyrrolidone (NMP). The positive electrode slurry is uniformly coated onto aluminum foil, then air-dried at room temperature and transferred to an oven for drying. After cold pressing and slitting, a positive electrode sheet is obtained. In other embodiments, the positive electrode sheet can also be obtained by any other method of forming a positive electrode sheet.

[0071] In some embodiments, the electrolyte includes an electrolyte lithium salt, a solvent, and additives. In secondary batteries, the electrolyte plays a role in conducting ions, providing ion channels, and maintaining chemical stability. The various components in the electrolyte can be categorized according to their function and dosage as electrolyte lithium salt, solvent, and additives. Lithium salt is primarily used to provide lithium ions to form ion channels. In the entire electrochemical system of the battery, the directional movement of lithium ions and electrons generates electricity. Lithium salt has a significant impact on the energy density, power density, wide electrochemical window, cycle life, and safety performance of lithium batteries. The solvent is used to dissolve the lithium salt and additives. Additives, added in small amounts to the electrolyte, are numerous and each plays a different role, for example, they can improve the battery's high and low temperature performance, cycle performance, and film-forming properties.

[0072] In some embodiments, the electrolyte lithium salt is selected from at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethyl)sulfonylimide, lithium acetate, lithium methanesulfonate, or lithium trifluoromethylsulfonate, and the mass percentage of the electrolyte lithium salt is 12% to 16% based on the total mass of the electrolyte. This invention does not limit the type of lithium salt; a single lithium salt or a mixture of lithium salts can be used.

[0073] In some embodiments, the solvent is selected from at least one of carbonate solvents, carboxylic acid ester solvents, ether solvents, or nitrile solvents, and the solvent accounts for 70% to 80% of the total mass of the electrolyte. Examples of carbonate solvents include ethylene carbonate, ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, fluoroethylene carbonate, and polycarbonate; examples of carboxylic acid ester solvents include ethyl formate, ethyl acetate, propyl acetate, ethyl propionate, and propyl propionate; examples of ether solvents include ethylene glycol dimethyl ether and diethanol diethyl ether; and examples of nitrile solvents include acetonitrile, propionitrile, butyronitrile, and valerate. This invention does not limit the type of solvent; a single solvent or a mixture of solvents can be used.

[0074] In some embodiments, the additive is selected from at least one of vinylene carbonate (VC), methylene methanedisulfonate (MMDS), propylene sulfite (PS), ethylene sulfate (1,3,2-dioxathiolane 2,2-dioxide (DTD)), and ethylenesulfite (ES), and the additive is present in a mass percentage of 0.1% to 5% based on the total mass of the electrolyte. This invention does not limit the type of additive; a single additive or a mixture of additives may be used.

[0075] In some embodiments, the diaphragm is, for example, a polyethylene (PE) membrane, a polypropylene (PP) membrane, a glass fiber membrane, or a composite membrane, and the thickness of the diaphragm is, for example, 9 μm to 15 μm.

[0076] The following specific examples illustrate the present invention in detail. It should also be understood that the following examples are only for specific illustrative purposes and should not be construed as limiting the scope of protection of the present invention. Any non-essential improvements and adjustments made by those skilled in the art based on the above description of the present invention are within the scope of protection of the present invention. The specific process parameters, etc., in the following examples are merely examples within a suitable range; that is, those skilled in the art can make appropriate selections within the appropriate range based on the description herein, and are not intended to be limited to the specific values ​​in the examples below.

[0077] Example 1

[0078] This embodiment provides a Si@SiO x The preparation method of the @C composite material is as follows:

[0079] 1. The particle size of silicon powder (average diameter of 2.1 μm) was reduced by ball milling, resulting in a D50 of 120 nm for the silicon powder.

[0080] 2. Using glucose and polyethylene glycol as carbon sources, disperse silicon powder and 30wt% carbon source (meaning the carbon source mass is 30wt% of the silicon powder mass) in ethanol and perform ultrasonic dispersion treatment for 20 minutes to form mixture A.

[0081] 3. Using liquid CO2 as the oxygen-generating agent, the mixture A and 8 wt% liquid CO2 (meaning the oxygen-generating agent is 8 wt% of the silicon powder mass) are transferred to a high-pressure reactor. Ethanol is miscible with liquid CO2 and they serve as a co-solvent.

[0082] 4. Raise the temperature inside the reactor in step 3 to 60°C to vaporize the liquid CO2 inside the reactor. At this time, the pressure inside the reactor gradually increases. When the pressure inside the reactor reaches 8.5 MPa, stir vigorously at a speed of 600 rpm for 3 hours.

[0083] 5. Collect the powder obtained in step 4 and dry it in an oven at 60°C for 12 hours to obtain SiO2. x And carbon-coated precursor powder.

[0084] 6. Place the precursor powder obtained in step 5 into a tube furnace and carbonize it at 900℃ for 6 hours under an argon atmosphere to obtain Si@SiO. x @C composite material.

[0085] Example 2

[0086] This embodiment provides a Si@SiO x The preparation method of the @C composite material differs from that of Example 1 in that the amount of carbon source added in step 2 is 5 wt%. All other steps and parameters are the same as in Example 1.

[0087] Example 3

[0088] This embodiment provides a Si@SiO x The preparation method of the @C composite material differs from that of Example 1 in that the amount of carbon source added in step 2 is 10 wt%. All other steps and parameters are the same as in Example 1.

[0089] Example 4

[0090] This embodiment provides a Si@SiO x The preparation method of the @C composite material differs from that of Example 1 in that the amount of carbon source added in step 2 is 20 wt%. All other steps and parameters are the same as in Example 1.

[0091] Example 5

[0092] This embodiment provides a Si@SiO x The preparation method of the @C composite material differs from that of Example 1 in that the amount of carbon source added in step 2 is 40 wt%. All other steps and parameters are the same as in Example 1.

[0093] Example 6

[0094] This embodiment provides a Si@SiO x The preparation method of the @C composite material differs from that of Example 1 in that the amount of carbon source added in step 2 is 50 wt%. All other steps and parameters are the same as in Example 1.

[0095] Example 7

[0096] This embodiment provides a Si@SiO x The preparation method of the @C composite material differs from that of Example 1 in that the amount of liquid CO2 added in step 3 is 5 wt%. All other steps and parameters are the same as in Example 1.

[0097] Example 8

[0098] This embodiment provides a Si@SiO x The preparation method of the @C composite material differs from that of Example 1 in that the amount of liquid CO2 added in step 3 is 10 wt%. All other steps and parameters are the same as in Example 1.

[0099] Example 9

[0100] This embodiment provides a Si@SiO x The preparation method of the @C composite material differs from that of Example 1 in that: in step 3, H2O2 is used as the oxygen-generating agent, and the mass of H2O2 is 6.2 wt% of the mass of silicon powder; in step 4, the temperature inside the reactor is raised to 160°C. Other steps and parameters are the same as in Example 1.

[0101] Example 10

[0102] This embodiment provides a Si@SiO x The preparation method of the @C composite material differs from that of Example 1 in that: in step 3, solid NH4HCO3 is used as the oxygen-generating agent, and the mass of NH4HCO3 is 14.4 wt% of the mass of silicon powder; in step 4, the temperature inside the reactor is raised to 60°C. All other steps and parameters are the same as in Example 1.

[0103] Comparative Example 1

[0104] This comparative example provides a Si@SiO x The preparation steps of the composite material are as follows:

[0105] 1. The particle size of silicon powder (average diameter of 2.1 μm) was reduced by ball milling, resulting in a D50 of 120 nm for the silicon powder.

[0106] 2. Disperse silicon powder in ethanol and perform ultrasonic dispersion treatment for 20 minutes to form mixture A.

[0107] 3. Using liquid CO2 as the oxygen-generating agent, the mixture A and 8 wt% liquid CO2 (meaning the oxygen-generating agent is 8 wt% of the silicon powder mass) are transferred to a high-pressure reactor. Ethanol is miscible with liquid CO2 and they serve as a co-solvent.

[0108] 4. Raise the temperature inside the reactor in step 3 to 60°C to vaporize the liquid CO2 inside the reactor. At this time, the pressure inside the reactor gradually increases. When the pressure inside the reactor reaches 8.5 MPa, stir vigorously at a speed of 600 rpm for 3 hours.

[0109] 5. Collect the powder obtained in step 4 and dry it in an oven at 60°C for 12 hours to obtain Si@SiO. x Composite materials.

[0110] Comparative Example 2

[0111] This comparative example provides a Si@C composite material, the preparation method of which is as follows:

[0112] 1. The particle size of silicon powder (average diameter of 2.1 μm) was reduced by ball milling, resulting in a D50 of 120 nm for the silicon powder.

[0113] 2. Using glucose and polyethylene glycol as carbon sources, disperse silicon powder and 30wt% carbon source (meaning the carbon source mass is 30wt% of the silicon powder mass) in ethanol and perform ultrasonic dispersion treatment for 20 minutes to form mixture A.

[0114] 3. Transfer mixture A to a high-pressure reactor.

[0115] 4. Raise the temperature inside the reactor from step 3 to 60°C and stir vigorously at a speed of 600 rpm for 3 hours.

[0116] 5. Collect the powder obtained in step 4 and dry it. Dry the powder in an oven at 60°C for 12 hours to obtain carbon-coated precursor powder.

[0117] 6. Place the precursor powder obtained in step 5 into a tube furnace and carbonize it at 900°C for 6 hours under an argon atmosphere to obtain the Si@C composite material.

[0118] To verify the performance of the materials prepared in Example 1N10 and Comparative Example 1N2, the materials prepared in Examples 1-10 and Comparative Examples 1-2 were mixed with binder polyacrylate and conductive carbon black in a mass ratio of 8:1:1 to form a slurry. This slurry was coated onto copper foil, dried, and cut into negative electrode sheets with a diameter of 12 mm. A lithium metal sheet was used as the positive electrode sheet, and a Celgard 2400 polypropylene (PP) membrane was used as the separator. An electrolyte with a LiPF6 concentration of 1.0 mol / L was prepared using ethylene carbonate and diethyl carbonate in a volume ratio of 1:1 as solvents and LiPF6 as the lithium salt. 35 μL of electrolyte was added to each side of the separator, and CR2016 coin cell half-cells were assembled in a glove box. The cells were tested, with a voltage range of 0.01 V to 1.5 V and a charge / discharge current of 0.5 A / g. The results are shown in Table 1.

[0119] Table 1 Electrochemical performance

[0120]

[0121]

[0122] As can be seen from the table above, SiO x The carbon coating improves the cycle stability of the silicon anode.

[0123] Comparative studies of Examples 1-6 show that as the amount of carbon source added increases, the carbon coating amount and carbon layer thickness gradually increase, while the initial discharge specific capacity of the electrode gradually decreases. This is because the increased carbon coating thickness reduces the proportion of silicon in the electrode, thereby reducing the electrode's specific capacity. Meanwhile, the cycle stability of the electrode gradually improves because the carbon coating enhances the conductivity of the silicon anode, reducing the polarization of the redox reaction. Simultaneously, the carbon film ensures both uniform coating and effective carbon encapsulation. However, when the carbon source addition exceeds 30 wt%, the increase in capacity retention after 100 cycles significantly decreases. Therefore, the amount of carbon source added should not be too high, meaning the carbon coating layer should not be too thick.

[0124] Comparing Examples 1, 7, and 8, it can be seen that the initial efficiency of the battery decreases with increasing liquid CO2 content. The vaporization of CO2 promotes the formation of SiO2. x Layer formation, SiO x The increased thickness of the C layer leads to an increase in oxygen-containing groups on the surface of the silicon particles (some of the electrolyte permeates through the C layer and reacts with SiO). x (Due to reactions occurring in the layer), side reactions increase during SEI film formation, leading to increased lithium-ion consumption and reduced initial efficiency. Furthermore, when the liquid CO2 content increases, the SiO₂ on the silicon particle surface... x The layer also gradually thickens, forming SiO2 from silicon particles. x This will consume silicon, reducing the initial discharge capacity of the electrode. The highest capacity retention rate of the battery was achieved when the liquid CO2 content was 8 wt% (Example 1). At this point, SiO2 forms on the surface of the silicon particles. x The layer has a moderate thickness, which effectively suppresses the volume expansion of silicon particles while ensuring the effective utilization of the silicon particle capacity.

[0125] By comparing Examples 1, 9 and 10, it was found that the initial efficiency and cycle performance of H2O2 and NH4HCO3 as oxygen-generating agents were worse than those of CO2. This is due to the lower surface tension and excellent mass transfer performance of CO2 after it is vaporized.

[0126] By comparing Example 1, Comparative Example 1, and Comparative Example 2, it can be seen that SiO x Both the SiO2 and carbon coating layers play a crucial role in the cycling stability of the electrode. x The synergistic effect of the carbon and silicon layers effectively buffers the volume expansion of silicon particles, improves the conductivity of the silicon anode, and effectively avoids side reactions between silicon particles and the electrolyte, resulting in a superior Si@SiO2 anode. x @C composite materials exhibited considerable lithium storage capacity and excellent electrochemical performance.

[0127] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.

Claims

1. A method for preparing a silicon-oxygen-carbon composite material, characterized in that, Silicon-oxygen-carbon composite materials were prepared by a one-pot, single-step synthesis method using silicon powder, carbon source, and oxygen-generating agent as raw materials, including the following processes: When the temperature is raised to the first preset temperature, the oxygen-generating agent decomposes to produce oxygen, and the silicon on the surface of the silicon oxide particles forms a silicon oxide coating layer, thus obtaining Si@SiO. x Particles, where 0.5 ≤ x ≤ 2; The temperature is raised to the second preset temperature, in the Si@SiO x A carbon coating layer is formed on the surface of the particles to obtain the silicon-oxygen-carbon composite material; The first preset temperature is lower than the second preset temperature.

2. The method for preparing the silicon-oxygen-carbon composite material according to claim 1, characterized in that: The oxygen-generating agent is selected from at least one of liquid carbon dioxide, hydrogen peroxide, or ammonium bicarbonate. And / or, the second preset temperature is 600℃~1000℃; And / or, the process of heating to the second preset temperature adopts a gradient heating method with a heating rate of 3℃ / min to 8℃ / min; And / or, after heating to the second preset temperature, the holding time is 6h to 12h; And / or, heat to a second preset temperature, in the Si@SiO x The process of forming a carbon coating on the particle surface is carried out under a protective atmosphere.

3. The method for preparing the silicon-oxygen-carbon composite material according to claim 2, characterized in that: When the oxygen-generating agent is selected from liquid carbon dioxide or ammonium bicarbonate, the first preset temperature is 50℃~70℃; Alternatively, when the oxygen-generating agent is selected from hydrogen peroxide, the first preset temperature is 115℃~170℃.

4. The method for preparing the silicon-oxygen-carbon composite material according to claim 1, characterized in that: The mass ratio of silicon powder, carbon source, and oxygen-generating agent is 1:0.05-0.5:0.05-0.15; And / or, the particle size D50 of the silicon powder is 100nm to 200nm; And / or, the carbon source is selected from organic carbon sources.

5. The method for preparing the silicon-oxygen-carbon composite material according to claim 1, characterized in that: The silicon powder and carbon source are dispersed in an alcohol solvent to form a mixture A.

6. The method for preparing the silicon-oxygen-carbon composite material according to claim 5, characterized in that: When preparing the mixture A, 3g to 8g of silicon powder is added to every 100ml of the solvent alcohol.

7. The method for preparing the silicon-oxygen-carbon composite material according to any one of claims 1 to 6, characterized in that, Silicon-oxygen-carbon composite materials were prepared by a one-pot, single-step synthesis method using silicon powder, carbon source, and oxygen-generating agent as raw materials. Includes the following processes: After the temperature is raised to the first preset temperature, stirring is performed when the pressure is increased to the preset pressure.

8. The method for preparing the silicon-oxygen-carbon composite material according to claim 7, characterized in that: The preset pressure is 7MPa to 10MPa; And / or, the stirring speed is 500 rpm to 600 rpm; And / or, the stirring time is 1h to 6h.

9. A silicon-oxygen-carbon composite material prepared by the method according to any one of claims 1 to 8, characterized in that: The silicon-oxygen-carbon composite material includes spherical Si@SiO x @C particles, the Si@SiO x @C particles include Si@SiO x Particles and coatings of the Si@SiO x The carbon layer of the particles; the Si@SiO x The particles include core silicon and SiO2 coating the core silicon. x layer.

10. A secondary battery, characterized in that: The negative electrode includes a negative current collector and a negative active material layer coated on at least one side surface of the negative current collector. The negative active material layer includes a negative active material, which includes the silicon-oxygen-carbon composite material of claim 9.