A flexible dual-mode carbon-based sensing patch, its preparation method, and its application in monitoring oyster freshness.

By employing a biodegradable electrospun substrate membrane and a temperature and impedance sensing unit attached with conductive silver paste in oyster freshness detection, the problems of non-degradable sensors and single-parameter monitoring are solved, enabling real-time, non-destructive, dual-parameter monitoring of oyster freshness, which is suitable for moist and irregular surfaces.

CN122361529APending Publication Date: 2026-07-10BOHAI UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202610766836.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-05-29
Publication Date
2026-07-10

AI Technical Summary

Technical Problem

Existing technologies for detecting oyster freshness suffer from limitations such as non-degradable sensor substrates, difficulty in comprehensively reflecting the spoilage process due to single-parameter monitoring, and difficulty in achieving non-destructive monitoring of moist and irregular surfaces.

Method used

A biodegradable electrospun substrate film is used, combined with a temperature sensing unit and an impedance sensing unit attached with conductive silver paste. The temperature sensing unit and the impedance sensing unit are respectively composed of a composite conductive film of graphene and carbon nanotubes and a carbon nanotube conductive network. Through vacuum filtration deposition and connection with conductive silver wires, dual-parameter signal acquisition is achieved.

Benefits of technology

It enables real-time, non-destructive, dual-parameter monitoring of oyster freshness. The sensor is highly reliable, environmentally friendly, and suitable for moist, irregular surfaces, as well as for cold chain logistics and warehousing management of shellfish meat.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122361529A_ABST
    Figure CN122361529A_ABST
Patent Text Reader

Abstract

This invention discloses a flexible dual-mode carbon-based sensing patch, its preparation method, and its application in monitoring oyster freshness. It belongs to the field of flexible electronic sensors and non-destructive testing technology for food. The sensing patch includes a biodegradable electrospun substrate membrane, and a temperature sensing unit and an impedance sensing unit attached to the substrate membrane via conductive silver paste. The temperature sensing unit is a composite conductive film formed by vacuum filtration deposition of a graphene-carbon nanotube blend, and the impedance sensing unit is a conductive network film formed by vacuum filtration deposition of carbon nanotubes. The temperature sensing unit and the impedance sensing unit are respectively connected to conductive silver wires via conductive silver paste for signal transmission. This invention features a simple structure, controllable preparation process, stable sensing performance, and good compatibility with biodegradable substrates, providing a high-performance, integrable sensing solution for real-time, non-destructive monitoring of oyster freshness after death.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of flexible electronic sensors and non-destructive testing technology for food, specifically involving a flexible dual-mode carbon-based sensing patch, its preparation method, and its application in monitoring the freshness of oysters. Background Technology

[0002] Oysters, as a high-value, perishable aquatic product, spoil rapidly after harvesting due to their high water and protein content. Freshness directly impacts food safety and commercial value. Currently, oyster freshness testing primarily relies on sensory evaluation and laboratory physicochemical analysis, such as volatile basic nitrogen (TVB-N) determination and total bacterial count. However, these traditional methods have significant drawbacks: sensory evaluation is highly subjective and lacks standardized criteria; while physicochemical testing is accurate, it is time-consuming, labor-intensive, and destructive to samples, failing to achieve real-time, online, and non-destructive monitoring during cold chain logistics, thus hindering the need for precise quality control.

[0003] In recent years, with the rapid development of flexible electronics and sensing technology, non-destructive testing of food based on multi-parameter sensing has become a research hotspot. Among existing technologies, researchers have developed oyster freshness monitoring systems based on electronic noses, achieving quality assessment by detecting volatile organic compounds; other studies have used acoustic vibration technology combined with machine learning to achieve non-destructive testing of closed oysters; and hydrogel fluorescent patches based on upconversion materials can monitor biogenic amines in food through color changes. These studies provide various technical pathways for non-destructive testing of food, but dual-parameter in-situ monitoring of oyster soft tissue has yet to be reported.

[0004] Bioimpedance technology can sensitively reflect changes in muscle tissue cell integrity, ionic state, and moisture distribution, and has been proven to be useful for assessing quality changes in aquatic products. Temperature, as a key driver of spoilage rates, is fundamentally supported by in-situ monitoring for predicting shelf life. Therefore, a dual-parameter sensing system integrating temperature and bioimpedance offers a technological possibility for real-time reflection of aquatic product quality degradation.

[0005] However, existing non-destructive monitoring technologies still have the following shortcomings: (1) The sensor substrates are mostly made of non-degradable materials, which are not environmentally friendly; (2) Most studies focus on monitoring a single parameter, which is difficult to fully reflect the putrefaction process; (3) There is still a lack of research on special flexible sensor patches for the moist and irregular surface of the soft tissue of dead oysters. Summary of the Invention

[0006] The purpose of this section is to outline some aspects of embodiments of the present invention and to briefly describe some preferred embodiments. Simplifications or omissions may be made in this section, as well as in the abstract and title of this application, to avoid obscuring the purpose of these documents; however, such simplifications or omissions should not be construed as limiting the scope of the invention.

[0007] In view of the problems existing in the above and / or prior art, the present invention is proposed.

[0008] Therefore, the purpose of this invention is to overcome the shortcomings of the prior art and provide a flexible dual-mode carbon-based sensing patch.

[0009] To solve the above-mentioned technical problems, the present invention provides the following technical solution: including, Biodegradable electrospun substrate membrane; A temperature sensing unit is attached to the base film via conductive silver paste. The temperature sensing unit is a composite conductive film formed by vacuum filtration deposition of a blend of monolayer graphene and carboxylated multi-walled carbon nanotubes. An impedance sensing unit is attached to the base film via conductive silver paste. The impedance sensing unit is a conductive network film formed by vacuum filtration and deposition of carbon nanotubes. And conductive silver wires connected to the temperature sensing unit and the impedance sensing unit respectively via conductive silver paste.

[0010] As a preferred embodiment of the flexible dual-mode carbon-based sensing patch of the present invention, wherein the mass ratio of monolayer graphene to carboxylated multi-walled carbon nanotubes in the temperature sensing unit is 5:1 to 3:1.

[0011] As a preferred embodiment of the flexible dual-mode carbon-based sensing patch of the present invention, the thickness of the temperature sensing unit is 20~40 μm, and the thickness of the impedance sensing unit is 20~40 μm.

[0012] As a preferred embodiment of the flexible dual-mode carbon-based sensing patch of the present invention, the temperature coefficient of resistance of the temperature sensing unit is -0.536% / ℃ to -0.780% / ℃.

[0013] As a preferred embodiment of the flexible dual-mode carbon-based sensing patch of the present invention, the conductive silver paste is a low-temperature curing silver paste with a curing temperature ≤80℃.

[0014] As a preferred embodiment of the flexible dual-mode carbon-based sensing patch of the present invention, wherein the impedance sensing unit has an impedance response range of 0 kΩ to 7 kΩ when detecting the freshness of oysters. Another object of the present invention is to provide a method for preparing a flexible dual-mode carbon-based sensing patch.

[0015] To solve the above-mentioned technical problems, the present invention provides the following technical solution: including, A temperature sensing unit was obtained by blending a single-layer graphene dispersion with a carboxylated multi-walled carbon nanotube dispersion and depositing the mixture into a film through vacuum filtration. An impedance sensing unit was obtained by depositing a carboxylated multi-walled carbon nanotube dispersion into a film through vacuum filtration. Conductive silver paste is coated on a predetermined area of ​​a biodegradable electrospun substrate film. Temperature sensing unit and impedance sensing unit are attached to the conductive silver paste respectively and cured at 20~40℃ for 6~12h to fix the sensing unit to the substrate. Conductive silver paste is coated on the electrode leads of the temperature sensing unit and the impedance sensing unit, and conductive silver wires are embedded in the silver paste. The mixture is cured at 60~80℃ for 0.5~3 hours to complete the electrode connection and obtain a flexible dual-mode carbon-based sensing patch.

[0016] In a preferred embodiment of the preparation method of the flexible dual-mode carbon-based sensing patch of the present invention, the concentration of the dispersion is 0.5~10 mg / mL, the dispersion medium is water, and a surfactant is added and ultrasonic treatment is assisted during the dispersion process.

[0017] In a preferred embodiment of the preparation method of the flexible dual-mode carbon-based sensing patch of the present invention, an organic filter membrane with a pore size of 0.22-0.45 μm is used as a support during the vacuum filtration process.

[0018] Another object of the present invention is to provide an application of a flexible dual-mode carbon-based sensing patch in monitoring the freshness of oysters.

[0019] Beneficial effects of this invention: (1) The present invention adopts a functionally separated dual-mode design. The temperature sensing unit and the impedance sensing unit adopt different carbon-based material formulations. The temperature unit uses graphene and carbon nanotubes to achieve a high-sensitivity temperature response, while the impedance unit uses pure carbon nanotubes to construct a stable conductive network to achieve sensitive detection of tissue electrical properties. The two sensing units complement each other and do not interfere with each other. They can synchronously and in situ collect temperature changes and multi-frequency bioimpedance signals of oyster soft tissue.

[0020] (2) The present invention integrates independently prepared sensing units onto a biodegradable substrate by attaching conductive silver paste, thereby realizing the modular combination of sensing functional layer and supporting substrate. This avoids problems such as interface stress, material incompatibility, and high temperature damage to the substrate that may be caused by directly preparing the sensing layer on the substrate, while giving full play to the environmental advantages of biodegradable substrate.

[0021] (3) In this invention, the sensing unit adopts vacuum filtration to form a film with uniform thickness and controllable structure. The film thickness can be precisely controlled by adjusting the concentration of dispersion and the filtration volume. The bonding process is mild and the curing temperature is not higher than 80°C, so it will not damage the substrate and sensing material. The conductive silver paste connecting the silver wires ensures the reliability of signal transmission.

[0022] (4) The flexible patch prepared by the present invention can be closely attached to the moist and irregular curved surface of oyster soft tissue, which solves the problem of traditional rigid sensors being difficult to adapt. The hydrophobic properties of the base film and the flexibility of the sensing unit together ensure long-term stable attachment and signal acquisition in a humid environment.

[0023] (5) In this invention, the substrate material is a biodegradable polymer and the sensing unit is a carbon-based material. The overall solution conforms to the green electronic design concept and avoids the problem of persistent electronic waste generated after the disposal of traditional non-degradable sensors.

[0024] (6) The patch prepared by the present invention can simultaneously collect temperature and impedance dual parameter signals, and the accuracy of predicting oyster freshness is 0.9497. It has broad application prospects in the fields of shellfish cold chain logistics, warehousing management, and quality traceability. Attached Figure Description

[0025] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. Wherein: Figure 1 This is a scanning electron microscope image of the temperature sensing unit prepared in Embodiment 1 of the present invention; Figure 2 This is a scanning electron microscope image of the impedance sensing unit obtained in Embodiment 1 of the present invention; Figure 3 This is a schematic diagram of the structure of the flexible dual-mode carbon-based sensing patch prepared in Embodiment 1 of the present invention; Figure 4 The resistance-temperature response curve of the temperature sensing unit in the flexible dual-mode carbon-based sensing patch prepared in Example 1 of this invention. Figure 5 The impedance response diagrams of the impedance sensing unit in the flexible dual-mode carbon-based sensing patch prepared in Embodiment 1 of the present invention under different freshness conditions are shown. Figure 6 This is a correlation diagram between the impedance and oyster TVB-N in the flexible dual-mode carbon-based sensing patch prepared in Example 1 of this invention. Detailed Implementation

[0026] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the examples in the specification.

[0027] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.

[0028] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The phrase "in one embodiment" appearing in different places in this specification does not necessarily refer to the same embodiment, nor is it a single or selective embodiment that is mutually exclusive with other embodiments.

[0029] Unless otherwise specified, all raw materials used in this invention are commercially available in the field.

[0030] The carbon nanotubes are carboxylated multi-walled carbon nanotubes with a length of 5-15 nm, purchased from Pioneer Nano. The graphene is a single layer of graphene oxide with a size of 20 μm, purchased from Pioneer Nano. The conductive silver paste is Kingstar K-818.

[0031] The performance testing of the sensor patch in this invention is performed according to the following method: Temperature sensing was measured using linear sweep voltammetry (LSV) on an electrochemical workstation. Impedance induction testing was performed using electrochemical workstation AC impedance measurement (IMP). The reference electrode is an Ag / AgCl electrode, and the counter electrode is a platinum wire electrode.

[0032] Example 1 This embodiment provides a method for preparing a flexible dual-mode carbon-based sensing patch, specifically: 1) Fabrication of the temperature sensing unit: Weigh 100 mg of carboxylated multi-walled carbon nanotubes, add 100 mL of ultrapure water, and then add sodium dodecylbenzenesulfonate (C... 18 H 29 300 mg of NaO3S (carboxylated multi-walled carbon nanotubes and sodium dodecylbenzenesulfonate in a mass ratio of 1:3) was ultrasonically dispersed for 240 minutes and magnetically stirred for 4 hours to obtain a carbon nanotube dispersion of 1 mg / mL. Weigh 100 mg of monolayer graphene oxide, add 100 mL of ultrapure water, sonicate for 240 minutes, and magnetically stir for 4 hours to obtain a 1 mg / mL monolayer graphene dispersion. The graphene dispersion and carbon nanotube dispersion were mixed evenly to achieve a mass ratio of 4:1 for graphene and carbon nanotubes in the mixed dispersion. The mixed dispersion was then vacuum filtered to form a film, dried under vacuum at 50°C for 2 hours, and trimmed into a circle to obtain a temperature sensing unit with a film thickness of 25 μm.

[0033] Figure 1 The image shows a scanning electron microscope (SEM) image of the temperature sensing unit obtained in this step. It can be seen that the graphene is laid out in a sheet structure, with carbon nanotubes interspersed between the graphene sheets to form a continuous and dense three-dimensional conductive network. There is no obvious agglomeration, and the specific surface area is large, which matches the signal transmission requirements of temperature sensing.

[0034] 2) Fabrication of the impedance sensing unit: Weigh 10 mg of carboxylated multi-walled carbon nanotubes, add 100 mL of ultrapure water, add 300 mg of sodium dodecylbenzenesulfonate, sonicate for 240 minutes, and magnetically stir for 3 hours. Then add sodium dodecylbenzenesulfonate (C 18 H 29 300 mg of NaO3S (carboxylated multi-walled carbon nanotubes and sodium dodecylbenzenesulfonate in a mass ratio of 1:3) was used to form a film by vacuum filtration of 100 ml of the dispersion. The film was dried under vacuum at 50 °C for 2 hours and then trimmed into a circle to obtain an impedance sensing unit with a film thickness of 25 μm.

[0035] Figure 2 The image shown is a scanning electron microscope image of the impedance sensing unit obtained in this step. It can be seen that carbon nanotubes rely on their high aspect ratio to interweave and overlap each other, forming a uniform and unbroken conductive path, which can stably capture the impedance signal of biological tissue.

[0036] 3) Substrate preparation: A biodegradable electrospun substrate membrane was prepared using electrospinning technology. The substrate membrane has a PLA-CS / PEO-PLA sandwich structure and was synthesized according to Example 1 of the published patent CN121650324A.

[0037] 4) Attachment Integration: Conductive silver paste is applied to a predetermined area of ​​the base film. Circular temperature sensing units and circular impedance sensing units are then attached to the conductive silver paste and cured at 25°C for 8 hours. Conductive silver paste is then applied to the electrode leads of the temperature and impedance sensing units, and conductive silver wires are embedded in the paste. The mixture is cured at 60°C for 0.5 hours, completing the electrode connection. The resulting structural diagram is shown below. Figure 3 The flexible dual-mode carbon-based sensing patch shown is Figure 3In the diagram, 1 represents the bioimpedance sensing area, 2 represents the temperature sensing area, 3 represents the substrate, 4 represents the working electrode, 5 represents the counter electrode, and 6 represents the working electrode.

[0038] Figure 4 The nonlinear change of the sensor patch resistance in this embodiment with temperature within the range of -20 to 60°C shows that the resistance initially decreases rapidly with increasing temperature, reaches a minimum value between 30 and 40°C, and then slowly recovers. The experimental data were fitted with an exponential function, R0. 2 =0.974, the model can accurately describe its resistance-temperature response characteristics.

[0039] The impedance response of the flexible dual-mode carbon-based sensing patch prepared in this embodiment to oyster samples of different freshness grades was measured, and the results are as follows: Figure 5 As shown, the impedance response of the sensor of this invention to oyster samples of different freshness grades varies significantly. As the freshness of the oysters gradually deteriorates from freshest to sub-fresh, moderately fresh, spoiled, and finally rotten, the impedance value measured by the sensor exhibits a continuous and significant decreasing trend. The impedance value of fresh oyster samples is approximately 7000Ω, while the impedance value of completely rotten samples drops to nearly 39Ω. This result demonstrates that the sensor of this invention can accurately and quantitatively distinguish different freshness grades of oysters through changes in impedance signals, providing reliable technical support for rapid, non-destructive, and on-site detection of oyster freshness.

[0040] The flexible dual-mode carbon-based sensing patch prepared in this embodiment was used to measure bioimpedance values ​​of oysters at storage time and sampling time for the determination of physicochemical indicators (volatile basic nitrogen content). The correlation between changes in bioimpedance values ​​and TVB-N content was obtained, and the results are as follows: Figure 6 As shown in the figure, within the experimental testing range, the impedance value of oysters showed a significant negative linear correlation with the TVB-N content, where y represents the TVB-N content of the oyster sample (unit: mg / 100g), and x represents the impedance value of the corresponding sample (unit: Ω). The coefficient of determination R of this fitting model is... 2 =0.9497, indicating a high linear correlation between impedance value and TVB-N content. The change in impedance value can be used to quantitatively predict the TVB-N content of oysters, providing a quantitative basis for non-destructive testing of oyster freshness.

[0041] In summary, the temperature sensing unit exhibits optimal overall performance with a graphene to carbon nanotube mass ratio of 4:1, achieving a temperature coefficient of resistance of -0.780 / ℃ and good linearity. The impedance sensing unit, prepared by filtration of a 1.0 mg / mL CNT dispersion, demonstrates stable performance at a thickness of approximately 25 μm. A curing temperature of 60℃ is optimal for the conductive silver paste, ensuring good curing while avoiding thermal damage. The flexible dual-mode carbon-based sensing patch prepared using this optimized method can stably and sensitively acquire temperature and impedance signals simultaneously, making it suitable for real-time monitoring of oyster freshness.

[0042] Comparative Example 1 The difference between this comparative example and Example 1 is that the temperature sensing unit contains only carbon nanotubes, specifically: Fabrication of temperature sensing unit: Weigh 100 mg of carboxylated multi-walled carbon nanotubes and 300 mg of sodium dodecylbenzenesulfonate (the mass ratio of carboxylated multi-walled carbon nanotubes to sodium dodecylbenzenesulfonate is 1:3), add 100 mL of ultrapure water, sonicate for 240 minutes, and magnetically stir for 4 hours to obtain a carbon nanotube dispersion of 1 mg / mL. The dispersion is then vacuum filtered to form a film, and vacuum dried at 50 °C for 8 hours to obtain a pure CNT temperature sensing unit.

[0043] The remaining steps and processes were all performed according to Example 1 to obtain the flexible carbon-based sensing patch of this comparative example.

[0044] Comparative Example 2 The difference between this comparative example and Example 1 is that the temperature sensing unit contains only graphene. Specifically: Fabrication of temperature sensing unit: Weigh 100 mg of monolayer graphene, add 100 mL of ultrapure water, ultrasonically disperse for 240 minutes, and magnetically stir for 4 hours to obtain a 1 mg / mL graphene dispersion. The dispersion is then vacuum filtered to form a film, and vacuum dried at 50°C for 8 hours to obtain a pure graphene temperature sensing unit.

[0045] The remaining steps and processes were all performed according to Example 1 to obtain the flexible carbon-based sensing patch of this comparative example.

[0046] Comparative Example 3 The difference between this comparative example and Example 1 is that the graphene in the temperature sensing unit is replaced with carbon black. Specifically: Fabrication of temperature sensing unit: Weigh 1 g of carbon black (CB) and 100 mg of sodium dodecylbenzenesulfonate (the mass ratio of carbon black to sodium dodecylbenzenesulfonate is 10:1), add 100 mL of ultrapure water, sonicate for 240 minutes, and magnetically stir for 4 hours to obtain a carbon black dispersion of 1 g / 100 mL. Mix the carbon black dispersion with the carbon nanotube dispersion at a mass ratio of 1:1. Take 100 mL of the mixture and filter it under vacuum to form a film. Dry it under vacuum at 50 °C for 8 hours to obtain the CB / CNTs temperature sensing unit.

[0047] The remaining steps and processes were all performed according to Example 1 to obtain the flexible carbon-based sensing patch of this comparative example.

[0048] Example 2 The difference between this embodiment and embodiment 1 is that the mass ratio of graphene dispersion to carbon nanotube dispersion in step 1) of the temperature sensing unit preparation process is adjusted to 3:1, so that the mass ratio of graphene to carbon nanotube in the mixed dispersion is 3:1. The remaining steps are the same as in embodiment 1, and the flexible dual-mode carbon-based sensing patch of this embodiment is obtained.

[0049] Example 3 The difference between this embodiment and embodiment 1 is that the mass ratio of graphene dispersion to carbon nanotube dispersion in step 1) of the temperature sensing unit preparation process is adjusted to 5:1, so that the mass ratio of graphene to carbon nanotube in the mixed dispersion is 5:1. The remaining steps are the same as in embodiment 1, and the flexible dual-mode carbon-based sensing patch of this embodiment is obtained.

[0050] The temperature coefficient of resistance of the temperature sensing units of Comparative Examples 1 to 3 and Comparative Examples 1 to 2 was measured, and the results are shown in Table 1.

[0051] Table 1

[0052] As can be seen, the temperature sensing units of the flexible dual-mode carbon-based sensing patches prepared in the various embodiments of the present invention show a significant improvement in sensitivity compared to the comparative examples. Comparative Example 2, due to its poor film formation, lacks a stable electrical signal and therefore cannot measure the temperature coefficient of resistance. The temperature coefficient of resistance of the temperature sensing unit in Comparative Example 1 is -0.40% / ℃, with poor continuity of the conductive network and unstable resistance value. Comparative Example 3 aims to achieve near-zero TCR to meet stability requirements, rather than pursuing high sensitivity; therefore, it is not suitable for the high-sensitivity temperature sensor design of this work.

[0053] Example 4 The difference between this embodiment and Embodiment 1 is that the concentration of the carbon nanotube (CNT) dispersion in step 2) during the preparation of the impedance sensing unit is adjusted to 0.5 mg / mL, 1.0 mg / mL, and 1.5 mg / mL, respectively. 100 mL of the dispersion is vacuum filtered to form a film, and then vacuum dried at 50°C for 8 hours to obtain impedance sensing units of different thicknesses. The remaining steps are the same as in Embodiment 1, resulting in flexible dual-mode carbon-based sensing patches with different impedance sensing unit concentrations in this embodiment.

[0054] Testing revealed that when the CNT dispersion concentration was 0.5 mg / mL and the sensing unit thickness was approximately 10 μm, the carbon nanotube concentration was too low, resulting in sparse overlap between the tubes and the failure to form a complete percolation conductive network. Conversely, at a concentration of 1.5 mg / mL and a sensing unit thickness of approximately 50 μm, the excessive concentration exacerbated entanglement and aggregation between the tubes. Both of these undesirable concentrations led to an uneven conductive network, resulting in significant fluctuations in resistance values ​​and unstable signals when measured with a multimeter, making it impossible to obtain specific values. When the CNT dispersion concentration was 1.0 mg / mL and the filtration volume was 100 mL, the resulting impedance sensing unit thickness was approximately 25 μm, and the impedance response was stable within the 1-100 kHz range.

[0055] Example 5 The difference between this embodiment and embodiment 1 is that, in step 4) of the bonding and integration process, the conductive silver wire is embedded in the silver paste, and the curing temperature is 20℃, 40℃, 60℃, and 80℃ respectively. The remaining steps and processes are the same as in Example 1, resulting in flexible dual-mode carbon-based sensing patches with different bonding and curing temperatures in this example.

[0056] Tests showed that when the curing temperature was 20-40℃, the conductive silver paste curing reaction was incomplete and the conductive silver paste was not fully fixed. When the curing temperature was further increased to 80℃, although the crosslinking density was further increased, the interfacial internal stress caused by curing shrinkage increased significantly, which could easily cause microcracks in the sensing film. The curing state was better under the curing condition of 60℃, and it would not cause thermal damage to the substrate and sensing material.

[0057] In summary, this invention discloses a flexible dual-mode carbon-based sensing patch, its preparation method, and its application in monitoring oyster freshness. It belongs to the field of flexible electronic sensors and non-destructive testing technology for food. The sensing patch includes a biodegradable electrospun substrate membrane, and a temperature sensing unit and an impedance sensing unit attached to the substrate membrane via conductive silver paste. The temperature sensing unit is a composite conductive film formed by vacuum filtration deposition of a graphene-carbon nanotube blend, and the impedance sensing unit is a conductive network film formed by vacuum filtration deposition of carbon nanotubes. The temperature sensing unit and the impedance sensing unit are respectively connected to conductive silver wires via conductive silver paste for signal transmission. This invention features a simple structure, controllable preparation process, stable sensing performance, and good compatibility with biodegradable substrates, providing a high-performance, integrable sensing solution for real-time, non-destructive monitoring of oyster freshness after death.

[0058] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.

Claims

1. A flexible dual-mode carbon-based sensing patch, characterized in that: include, Biodegradable electrospun substrate membrane; A temperature sensing unit is attached to the base film via conductive silver paste. The temperature sensing unit is a composite conductive film formed by vacuum filtration deposition of a blend of monolayer graphene and carboxylated multi-walled carbon nanotubes. An impedance sensing unit is attached to the base film via conductive silver paste. The impedance sensing unit is a conductive network film formed by vacuum filtration and deposition of carbon nanotubes. And conductive silver wires connected to the temperature sensing unit and the impedance sensing unit respectively via conductive silver paste.

2. The flexible dual-mode carbon-based sensing patch as described in claim 1, characterized in that: The mass ratio of monolayer graphene to carboxylated multi-walled carbon nanotubes in the temperature sensing unit is 5:1 to 3:

1.

3. The flexible dual-mode carbon-based sensing patch as described in claim 2, characterized in that: The thickness of the temperature sensing unit is 20~40 μm, and the thickness of the impedance sensing unit is 20~40 μm.

4. The impedance sensing unit as described in claim 3, characterized in that: The temperature coefficient of resistance of the temperature sensing unit is -0.536% / ℃ to -0.780% / ℃.

5. The flexible dual-mode carbon-based sensing patch as described in claim 1, characterized in that: The conductive silver paste is a low-temperature curing type, with a curing temperature ≤80℃.

6. The flexible dual-mode carbon-based sensing patch as described in claim 3, characterized in that: The impedance sensing unit has an impedance response range of 0 kΩ to 7 kΩ when detecting the freshness of oysters.

7. The method for preparing the flexible dual-mode carbon-based sensing patch as described in any one of claims 1 to 6, characterized in that: include, A temperature sensing unit was obtained by blending a single-layer graphene dispersion with a carboxylated multi-walled carbon nanotube dispersion and depositing the mixture into a film through vacuum filtration. An impedance sensing unit was obtained by depositing a carboxylated multi-walled carbon nanotube dispersion into a film through vacuum filtration. Conductive silver paste is coated on a predetermined area of ​​a biodegradable electrospun substrate film. Temperature sensing unit and impedance sensing unit are attached to the conductive silver paste respectively and cured at 20~40℃ for 6~12h to fix the sensing unit to the substrate. Conductive silver paste is coated on the electrode leads of the temperature sensing unit and the impedance sensing unit, and conductive silver wires are embedded in the silver paste. The mixture is cured at 60~80℃ for 0.5~3 hours to complete the electrode connection and obtain a flexible dual-mode carbon-based sensing patch.

8. The method for preparing the flexible dual-mode carbon-based sensing patch as described in claim 7, characterized in that: The concentration of the dispersion is 0.5~10 mg / mL, the dispersion medium is water, and a surfactant is added and ultrasonic treatment is assisted during the dispersion process.

9. The method for preparing the flexible dual-mode carbon-based sensing patch as described in claim 7, characterized in that: The vacuum filtration process uses an organic filter membrane with a pore size of 0.22~0.45 μm as a support.

10. The application of the flexible dual-mode carbon-based sensing patch as described in any one of claims 1 to 6 in monitoring the freshness of oysters.

Citation Information

Patent Citations

  • Biodegradable flexible conductive high-hydrophobicity composite film as well as preparation method and application thereof