An organic solvent-resistant recyclable supported palladium catalyst, and a preparation method and application thereof
By modifying the mesoporous metal oxide-activated carbon composite support to support palladium catalysts, the problems of unrecoverable homogeneous palladium catalysts and poor solvent resistance of supported catalysts were solved, achieving efficient and stable Suzuki-Miyaura coupling reaction, reducing costs and improving product purity.
Patent Information
- Application Number
- CN202610686280.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-05-19
- Publication Date
- 2026-07-24
AI Technical Summary
Existing homogeneous palladium catalysts cannot be recovered, resulting in waste of palladium resources and high costs. Furthermore, existing supported catalysts have poor resistance to organic solvents, insufficient thermal stability, and low catalytic activity, making it difficult to meet the requirements of efficient coupling reactions.
A supported palladium catalyst, suitable for the Suzuki-Miyaura coupling reaction, was prepared by loading palladium active components onto a modified mesoporous metal oxide-activated carbon composite support and modifying it with a silane coupling agent.
The catalyst is stable and does not swell in organic solvents, does not collapse at high temperatures, has high catalytic activity, is easy to separate and recover, is stable for recycling, reduces reaction costs and improves product purity.
Smart Images

Figure CN122441498A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of catalyst preparation technology, specifically to a recoverable supported palladium catalyst resistant to organic solvents, its preparation method, and its application. Background Technology
[0002] The Suzuki-Miyaura coupling reaction is an important organic synthesis reaction for constructing carbon-carbon bonds. It is widely used in pharmaceutical synthesis, fine chemicals, materials chemistry and other fields. Its core is the coupling reaction between arylboronic acid (or borate ester) and aryl halide (or alkenyl halide) catalyzed by palladium catalyst to generate biaryl or alkenylaryl compounds.
[0003] Currently, homogeneous palladium catalysts are mainly used in Suzuki-Miyaura coupling reactions, commonly including tetra(triphenylphosphine)palladium, palladium acetate, and bis(triphenylphosphine)palladium dichloride. These homogeneous palladium catalysts can efficiently catalyze various coupling reactions and are the most widely used catalyst type in laboratory and industrial production.
[0004] However, homogeneous palladium catalysts have significant technical drawbacks in practical applications: on the one hand, since the homogeneous palladium catalyst and the reaction system are in the same phase, it is difficult to separate and recover them from the reaction products after the reaction, resulting in a serious waste of palladium resources—palladium is a precious metal and expensive, and the inability to recycle it will significantly increase the reaction cost; on the other hand, unrecovered palladium catalyst will remain in the product, affecting the purity of the product. Especially in the field of drug synthesis, heavy metal residues will cause the product to fail to meet quality standards, requiring additional separation and purification steps, which will further increase production costs.
[0005] To address the problem of unrecoverable homogeneous palladium catalysts, existing technologies have attempted to support palladium catalysts on supports to prepare heterogeneous supported palladium catalysts for separation and recovery. However, existing supported palladium catalysts still have many shortcomings: some supports (such as ordinary silica gel and resin) have poor resistance to organic solvents, and long-term immersion in commonly used organic solvents can easily lead to swelling and degradation, resulting in catalyst detachment and reduced catalytic activity and recovery stability; some supports lack thermal stability and are prone to structural collapse under high-temperature reaction conditions, making them unsuitable for catalyst regeneration processes requiring high-temperature treatment; some supported catalysts have uneven palladium loading and poor dispersion, resulting in catalytic activity far lower than that of homogeneous catalysts, making it difficult to meet the requirements of efficient coupling reactions; in addition, some supported catalysts are difficult to separate, requiring complex operations such as centrifugation and filtration, and the catalytic activity decreases significantly after recovery, making them unsuitable for repeated recycling.
[0006] Therefore, developing a supported palladium catalyst that can overcome the above-mentioned defects and possesses properties such as resistance to organic solvents, high temperature resistance, easy separation and recovery, high catalytic activity, and good cycle stability to replace the traditional homogeneous palladium catalyst in the Suzuki-Miyaura coupling reaction, thereby realizing the recovery and utilization of palladium resources, reducing reaction costs, and improving product purity, has significant industrial application value and practical significance. Summary of the Invention
[0007] In order to overcome the problems of existing technologies, such as the inability to recover homogeneous palladium catalysts used in the Suzuki-Miyaura coupling reaction, poor high-temperature resistance, high cost, and affected product purity, as well as the poor organic solvent resistance, low catalytic activity, and poor recovery stability of existing supported palladium catalysts, this invention provides an organic solvent-resistant and recyclable supported palladium catalyst, its preparation method, and its application.
[0008] This invention is achieved using the following technical solution: A solvent-resistant, recyclable supported palladium catalyst, characterized in that it comprises a support and a palladium active component supported on the surface and within the pores of the support, wherein the support is a modified mesoporous metal oxide-activated carbon composite support resistant to organic solvents, the palladium active component is a palladium complex, and the modified mesoporous metal oxide-activated carbon composite support is composed of mesoporous metal oxide and activated carbon modified by a silane coupling agent, wherein the silane coupling agent is an amino- or phosphine-containing silane coupling agent.
[0009] Furthermore, the loading of the palladium active component is 0.5%-5% of the carrier mass.
[0010] Furthermore, the mesoporous metal oxide is one or more of mesoporous titanium dioxide, mesoporous alumina, and mesoporous zirconium oxide, and the specific surface area of the mesoporous metal oxide is 100-500 m². 2 / g, with a pore size of 2-50 nm; the activated carbon is coconut shell activated carbon, activated by 5%-10% dilute nitric acid, with a specific surface area of 800-1500 m² / g. 2 / g, with a pore size of 1-100 nm.
[0011] Furthermore, the silane coupling agent is one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, and diphenylphosphinopropyltrimethoxysilane, and the amount of silane coupling agent used is 1%-5% of the total mass of the mesoporous metal oxide and activated carbon.
[0012] Furthermore, the palladium complex is one or two of bis(triphenylphosphine)palladium dichloride, tetra(triphenylphosphine)palladium, and bis(tritert-butylphosphine)palladium.
[0013] Furthermore, the organic solvent resistance index of the supported palladium catalyst is: no swelling or degradation after soaking in dioxane, toluene, DMF or ethanol for 72 h, and the catalyst shedding rate is ≤0.5%; the high temperature resistance index of the supported palladium catalyst is: no structural collapse after calcination at 400℃ for 2 h, and the catalytic activity remains stable.
[0014] A method for preparing a recoverable supported palladium catalyst, such as one resistant to organic solvents, includes the following steps: S1. Preparation of modified mesoporous metal oxide-activated carbon composite support, specifically including: S1.1 Activation of activated carbon: pulverize coconut shell activated carbon to 100-200 mesh, add 5%-10% dilute nitric acid solution, boil for 2-4 h, wash with deionized water until neutral, and dry at 80-120℃ for 4-12 h to obtain activated carbon. S1.2 Pretreatment of mesoporous metal oxides: calcining the mesoporous metal oxides at 300-500℃ for 2-6 h, and cooling to room temperature for later use; S1.3, Composite and Modification: Activated carbon and pretreated mesoporous metal oxide are mixed at a mass ratio of 1:1-5, added to organic solvent I, and ultrasonically dispersed for 30-60 min to obtain a mixed suspension; silane coupling agent is added, and the mixture is stirred at 50-80℃ for 4-8 h. After filtration, washing, and drying, the modified mesoporous metal oxide-activated carbon composite carrier is obtained. S2, Palladium-supported active components, specifically including: S2.1 Preparation of palladium source solution: Dissolve the palladium complex in organic solvent II and stir until homogeneous to obtain palladium source solution; S2.2 Impregnation and loading: The modified mesoporous metal oxide-activated carbon composite support prepared in step S1 is added to the palladium source solution and impregnated by stirring at 25-60℃ for 6-12 h. After filtration, washing and drying, the supported palladium catalyst is obtained.
[0015] Further, the organic solvent I in step S1.3 is toluene or xylene; the organic solvent II in step S2.1 is methanol, ethanol or dichloromethane, and the concentration of the palladium source solution is 0.01-0.1 mol / L.
[0016] The application of a solvent-resistant, recyclable supported palladium catalyst in the Suzuki-Miyaura coupling reaction is as follows: using aryl halides and 3,4,5-trifluorophenylboronic acid as reaction substrates, the supported palladium catalyst as the catalyst, and a base as a co-catalyst, the reaction is carried out in organic solvent III at 60-120°C under inert gas protection for 4-12 h. After the reaction is completed, the catalyst is filtered out, washed, dried, and recycled.
[0017] Further, the aryl halide is o-chloroaniline or o-bromoaniline; the amount of catalyst used is 0.5%-5% of the molar amount of the aryl halide; the base is one or more of K2CO3 or Cs2CO3, and the amount used is 1.5-3.0 times the molar amount of the aryl halide; the organic solvent III is a mixed solvent of dioxane and water in a volume ratio of 4:1, a mixed solvent of ethanol and water in a volume ratio of 3:1, or toluene; the inert gas is nitrogen or argon.
[0018] This invention provides an organic solvent-resistant, recyclable supported palladium catalyst, its preparation method, and its application. Compared with the prior art, it has the following advantages: 1. This invention uses a modified mesoporous metal oxide-activated carbon composite support to load palladium active components. After the support is modified with a silane coupling agent, it shows no swelling or degradation after being soaked in commonly used organic solvents for Suzuki-Miyaura coupling reactions such as dioxane, toluene, DMF, and ethanol for 72 h, and the catalyst shedding rate is ≤0.5%. At the same time, the catalyst does not collapse in structure and maintains stable catalytic activity after being calcined at 400℃ for 2 h, which solves the problems of poor resistance to organic solvents and insufficient thermal stability of existing supports, and is suitable for the oxidation and regeneration process of catalysts.
[0019] 2. The supported palladium catalyst of the present invention is a heterogeneous catalyst, which can be recovered by simple filtration after the reaction. It has high separation efficiency and solves the problems of homogeneous palladium catalysts being unrecoverable, costly, and containing heavy metal residues in the product.
[0020] 3. The supported palladium catalyst of this invention achieves uniform dispersion of the palladium active component, and its catalytic activity is close to or even better than that of traditional homogeneous palladium catalysts. Examples show that when o-bromoaniline is used as a substrate, the yield of the coupling product can reach 93%, and the yield remains at 86% after six cycles of catalyst recycling, with no significant decrease in catalytic activity. This solves the problems of low catalytic activity and poor recovery stability of existing supported catalysts.
[0021] 4. The catalyst preparation method of the present invention is simple and convenient to operate, the raw materials used are readily available and low in cost, and no complicated equipment is required, making it suitable for large-scale industrial production. Attached Figure Description
[0022] Figure 1 This is the XRD pattern of the supported palladium catalyst prepared in Example 1 of this invention.
[0023] Figure 2 This is the XPS spectrum of the supported palladium catalyst prepared in Example 1 of this invention.
[0024] Figure 3 This is a SEM image (×200) of the supported palladium catalyst prepared in Example 1 of this invention.
[0025] Figure 4 This is a SEM image (×1000) of the supported palladium catalyst prepared in Example 1 of this invention. Detailed Implementation
[0026] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention. Example 1
[0027] An organic solvent-resistant, recyclable supported palladium catalyst includes a support and a palladium active component supported on the surface and within the pores of the support. The support is an organic solvent-resistant modified mesoporous metal oxide-activated carbon composite support, and the palladium active component is a palladium complex. In this embodiment, the palladium complex is bis(triphenylphosphine)palladium dichloride. The modified mesoporous metal oxide-activated carbon composite support is composed of mesoporous metal oxide and activated carbon modified with a silane coupling agent. In this embodiment, the mesoporous metal oxide is mesoporous alumina, and the silane coupling agent is 3-aminopropyltriethoxysilane.
[0028] The method for preparing the organic solvent-resistant, recyclable supported palladium catalyst in this embodiment includes the following steps: S1. Preparation of modified mesoporous metal oxide-activated carbon composite support, specifically including: S1.1 Activation of activated carbon: Take 10g of coconut shell activated carbon, crush it to 150 mesh, add 100 mL of 8% dilute nitric acid solution, boil for 3 h, then wash with deionized water until neutral, and dry at 100℃ for 8 h to obtain activated carbon.
[0029] S1.2 Pretreatment of mesoporous metal oxides: Take 20g of mesoporous alumina, calcine it at 400℃ for 4 h to remove impurities and moisture, and cool it to room temperature for later use.
[0030] S1.3, Composite and Modification: 10g of activated carbon and 20g of pretreated mesoporous metal oxide were mixed and added to 100 mL of toluene. The mixture was ultrasonically dispersed for 45 min to obtain a mixed suspension. Then, 1.5g of 3-aminopropyltriethoxysilane was added and stirred at 65℃ for 6 h. After the reaction was completed, the mixture was filtered, washed with toluene 4 times, and dried at 100℃ for 8 h to obtain the modified mesoporous metal oxide-activated carbon composite carrier.
[0031] S2, Palladium-supported active components, specifically including: S2.1 Preparation of palladium source solution: Dissolve 0.5 g of bis(triphenylphosphine)palladium dichloride in 50 mL of dichloromethane and stir until homogeneous to obtain palladium source solution.
[0032] S2.2 Impregnation and Loading: 10g of the modified mesoporous metal oxide-activated carbon composite support prepared in step S1 was added to the palladium source solution and impregnated at 30℃ for 10 h with stirring, so that the palladium dichloride bis(triphenylphosphine) combines with the amino groups on the support surface through the phosphine groups and is uniformly loaded on the support; after impregnation, it was filtered, washed with dichloromethane 4 times, and dried at 110℃ for 9 h to obtain the supported palladium catalyst Pd / Al2O3, wherein the loading amount of palladium active component is 2.5% of the support mass.
[0033] Organic solvent resistance test: The prepared supported palladium catalyst was immersed in dioxane, toluene, DMF and ethanol respectively, and kept at 120℃ for 72 h. The catalyst did not swell or degrade, and the catalyst shedding rate was 0.3%.
[0034] High temperature resistance test: The supported palladium catalyst was calcined at 400℃ for 2 h, and the structure did not collapse, and the catalytic activity remained stable.
[0035] The prepared supported palladium catalyst was characterized. Figure 1 The XRD patterns show characteristic diffraction peaks of metallic palladium (Pd) at 2θ = 39.8°, 46.2°, and 67.4° (consistent with JCPDS standard card 46-1043), and characteristic diffraction peaks of palladium oxide (PdO) at 2θ = 33.9° and 42.3° (consistent with JCPDS standard card 43-1024), indicating that palladium was successfully loaded onto the support and exists in both metallic palladium and palladium oxide forms.
[0036] like Figure 2 The XPS spectra show that Pd appears at binding energies of 334.8 eV and 340.3 eV. 0 3D 5 / 2 and 3D 3 / 2 Characteristic peaks were observed at binding energies of 335.8 eV and 343.1 eV, indicating the presence of Pd. 2+ 3D 5 / 2 and 3D 3 / 2 The characteristic peaks indicate that palladium in the catalyst exists in both zero-valent and +2-valent forms.
[0037] like Figure 3 As shown in the SEM image (×200), the catalyst particles are irregularly shaped lumps, uniformly dispersed, and without obvious agglomeration. Figure 4The SEM image (×1000) shows that the catalyst surface is rough and has abundant micron-sized pores. This structure is conducive to the diffusion of the reaction substrate and contact with the palladium active sites. Example 2
[0038] The supported palladium catalyst prepared in Example 1 was applied in the Suzuki-Miyaura coupling reaction. The specific application method is as follows: Under nitrogen protection, 1.0 mmol of o-chloroaniline, 1.2 mmol of 3,4,5-trifluorophenylboronic acid, 2.0 mmol of K2CO3, and 0.03 mmol of the prepared supported palladium catalyst were added to a dry three-necked flask. Then, 4 mL of dioxane and 1 mL of deionized water were added and stirred until homogeneous. The three-necked flask was placed in a 90°C oil bath and refluxed for 6 h. After the reaction was completed, the mixture was cooled to room temperature, filtered to separate the catalyst, washed with ethanol, dried at 100°C, and then used for further processing. The filtrate was extracted with ethyl acetate, the organic phase was washed with saturated brine, dried over anhydrous Na2SO4, concentrated by rotary evaporation, and purified by silica gel column chromatography to obtain the 3',4',5'-trifluorobiphenyl-2-amine product.
[0039] The product yield was 64% and the purity was 99.2% after testing. The separated catalyst was recycled 5 times, and the product yield could still reach 55%, and the catalytic activity remained stable. Example 3
[0040] This embodiment also applies the supported palladium catalyst prepared in Example 1 to the Suzuki-Miyaura coupling reaction. The difference from Example 2 is that o-chloroaniline is replaced with an equimolar mass of o-bromoaniline. The remaining steps and process parameters are the same as in Example 2, and 3',4',5'-trifluorobiphenyl-2-amine product is prepared.
[0041] The product yield was 93% and the purity was 99.5% after testing. The separated catalyst was recycled 6 times, and the product yield was still 86%, indicating that the catalytic activity remained stable. Comparative Example 1
[0042] Using tetra(triphenylphosphine)palladium as a catalyst, replacing the supported palladium catalyst prepared in this invention by an equal amount, the coupling reaction of Example 3 was repeated. All other steps and process parameters were the same as in Example 3, yielding the product. After the reaction, the product yield was 85%, but tetra(triphenylphosphine)palladium could not be separated and recovered from the reaction system, resulting in a palladium residue of 120 ppm in the product. Additional purification was required, increasing production costs. Comparative Example 2
[0043] Using ordinary silica gel as a support, the modified mesoporous metal oxide-activated carbon composite support in Example 1 was replaced by an equal mass, and a silica gel-supported palladium catalyst was prepared according to step S2 of Example 1. Then, the prepared silica gel-supported palladium catalyst was replaced by an equal mass of the supported palladium catalyst of this invention, and the coupling reaction of Example 3 was repeated. All other steps and process parameters were the same as in Example 3, yielding the product. During the reaction, the silica gel underwent slight swelling in dioxane. After the reaction, the catalyst shedding rate was 5.8%, and the product yield was 82%. After the catalyst was recycled three times, the product yield dropped to 70%, and the catalytic activity significantly decreased.
[0044] As can be seen from the above examples and comparative examples, the supported palladium catalyst of the present invention has the advantages of being resistant to organic solvents, easy to separate and recover, high catalytic activity, and good cycle stability. It can effectively replace the traditional homogeneous palladium catalyst in the Suzuki-Miyaura coupling reaction, solving the problems of homogeneous catalysts being unrecoverable, costly, and having low product purity. At the same time, it overcomes the defects of existing supported catalysts and has important industrial application value.
[0045] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A solvent-resistant, recyclable supported palladium catalyst, characterized in that: The invention includes a carrier and a palladium active component loaded on the surface and within the pores of the carrier. The carrier is a modified mesoporous metal oxide-activated carbon composite carrier resistant to organic solvents. The palladium active component is a palladium complex. The modified mesoporous metal oxide-activated carbon composite carrier is composed of mesoporous metal oxide and activated carbon modified by a silane coupling agent. The silane coupling agent is a silane coupling agent containing amino or phosphine groups.
2. The organic solvent-resistant, recyclable supported palladium catalyst according to claim 1, characterized in that: The loading of the palladium active component is 0.5%-5% of the carrier mass.
3. The organic solvent-resistant, recyclable supported palladium catalyst according to claim 1, characterized in that: The mesoporous metal oxide is one or more of mesoporous titanium dioxide, mesoporous alumina, and mesoporous zirconium oxide, and the specific surface area of the mesoporous metal oxide is 100-500 m². 2 / g, with a pore size of 2-50 nm; the activated carbon is coconut shell activated carbon, activated by 5%-10% dilute nitric acid, with a specific surface area of 800-1500 m² / g. 2 / g, with a pore size of 1-100 nm.
4. The organic solvent-resistant, recyclable supported palladium catalyst according to claim 1, characterized in that: The silane coupling agent is one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, and diphenylphosphinopropyltrimethoxysilane, and the amount of silane coupling agent used is 1%-5% of the total mass of the mesoporous metal oxide and activated carbon.
5. The organic solvent-resistant, recyclable supported palladium catalyst according to claim 1, characterized in that: The palladium complex is one or two of bis(triphenylphosphine)palladium dichloride, tetra(triphenylphosphine)palladium, and bis(tritert-butylphosphine)palladium.
6. The organic solvent-resistant, recyclable supported palladium catalyst according to claim 1, characterized in that: The organic solvent resistance index of the supported palladium catalyst is: no swelling or degradation after soaking in dioxane, toluene, DMF or ethanol for 72 h, and catalyst shedding rate ≤0.5%; the high temperature resistance index of the supported palladium catalyst is: no structural collapse after calcination at 400℃ for 2 h, and stable catalytic activity.
7. A method for preparing an organic solvent-resistant, recyclable supported palladium catalyst as described in any one of claims 1-6, characterized in that, Includes the following steps: S1. Preparation of modified mesoporous metal oxide-activated carbon composite support, specifically including: S1.1 Activation of activated carbon: Pulverize activated carbon to 100-200 mesh, add 5%-10% dilute nitric acid solution, boil for 2-4 hours, wash with deionized water until neutral, and dry at 80-120℃ for 4-12 hours to obtain activated activated carbon. S1.2 Pretreatment of mesoporous metal oxides: calcining the mesoporous metal oxides at 300-500℃ for 2-6 h, and cooling to room temperature for later use; S1.3, Composite and Modification: Activated carbon and pretreated mesoporous metal oxide are mixed at a mass ratio of 1:1-5, added to organic solvent I, and ultrasonically dispersed for 30-60 min to obtain a mixed suspension; silane coupling agent is added, and the mixture is stirred at 50-80℃ for 4-8 h. After filtration, washing, and drying, the modified mesoporous metal oxide-activated carbon composite carrier is obtained. S2, Palladium-supported active components, specifically including: S2.1 Preparation of palladium source solution: Dissolve the palladium complex in organic solvent II and stir until homogeneous to obtain palladium source solution; S2.2 Impregnation and loading: The modified mesoporous metal oxide-activated carbon composite support prepared in step S1 is added to the palladium source solution and impregnated by stirring at 25-60℃ for 6-12 h. After filtration, washing and drying, the supported palladium catalyst is obtained.
8. The method for preparing an organic solvent-resistant, recyclable supported palladium catalyst according to claim 7, characterized in that: In step S1.3, the organic solvent I is toluene or xylene; in step S2.1, the organic solvent II is methanol, ethanol or dichloromethane, and the concentration of the palladium source solution is 0.01-0.1 mol / L.
9. The application of an organic solvent-resistant, recyclable supported palladium catalyst as described in any one of claims 1-6 in the Suzuki-Miyaura coupling reaction, characterized in that, The specific application method is as follows: using aryl halides and 3,4,5-trifluorophenylboronic acid as reaction substrates, the supported palladium catalyst as catalyst, and a base as a co-catalyst, the reaction is carried out in organic solvent III at 60-120℃ under inert gas protection for 4-12 h. After the reaction is completed, the catalyst is filtered out, washed, dried and recycled.
10. The application of the organic solvent-resistant, recyclable supported palladium catalyst according to claim 9 in the Suzuki-Miyaura coupling reaction, characterized in that: The aryl halide is o-chloroaniline or o-bromoaniline; the amount of catalyst used is 0.5%-5% of the molar amount of the aryl halide; the base is one or more of K2CO3 or Cs2CO3, and the amount used is 1.5-3.0 times the molar amount of the aryl halide; the organic solvent III is a mixed solvent of dioxane and water in a volume ratio of 4:1, a mixed solvent of ethanol and water in a volume ratio of 3:1, or toluene; the inert gas is nitrogen or argon.