Process for crystallizing metal sulfates

JP2023551108A5Pending Publication Date: 2024-11-12HATCH LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023527332
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-11-03
Filing Date
2021-11-03
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The presence of calcium, magnesium, and lithium impurities in raw materials for battery production leads to processing difficulties, including contamination of the final product, higher energy consumption, and undesirable solids formation due to low solubility of calcium sulfate salts, which results in supersaturated process streams.

Method used

A processing method involving pretreatment of feedstock with a leaching agent to selectively extract impurities, followed by purification and crystallization of metal sulfates, using basic metal salts as neutralizing agents to control impurity crystallization and enhance purity.

Benefits of technology

The method effectively reduces impurity levels, improving the purity and yield of crystallized metal sulfates, reducing energy consumption, and minimizing equipment contamination, thereby enhancing the quality of battery materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A process for crystallizing metal sulfates, comprising pretreating a feedstock containing calcium, magnesium, and / or lithium impurities by pre-leaching the feedstock in the presence of a lixiviant, selectively extracting a first portion of any of the impurities from the feedstock, and forming a leach solution containing non-crystallized metal sulfates and any remaining impurities; and / or purifying the leach solution and removing a second portion of any of the remaining impurities; and crystallizing the non-crystallized metal sulfates from the leach solution to form crystallized metal sulfates. The crystallized metal sulfates thus processed may be battery grade or electroplating grade.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This application claims priority to U.S. Provisional Patent Application No. 63 / 109,227, filed on 3 November 2020, the contents of which provisional patent application are incorporated herein by reference in their entirety.

[0002] This disclosure generally relates to processing methods. More specifically, this disclosure relates to processing methods for crystallizing metal sulfates. [Background technology]

[0003] Continuous technological advancements, such as the electrification of transportation, have increased the demand for batteries, including lithium-ion batteries. This increased demand for batteries has led to increased demand for battery components, such as crystalline metal sulfates.

[0004] However, the presence of calcium, magnesium, and / or lithium in the raw materials used to manufacture battery materials can lead to processing difficulties. Such processing difficulties may include contamination of the final product, higher energy consumption, and / or greater process emissions. In sulfate-based processes, calcium can cause further problems due to the low solubility of calcium sulfate salts. This low solubility can lead to a supersaturated process flow with calcium sulfate, resulting in undesirable solid formation within the processing apparatus. [Overview of the project] [Problems that the invention aims to solve]

[0005] There is a need for improved processing methods to address impurities in the manufacturing of battery materials such as crystalline metal sulfates. [Means for solving the problem]

[0006] Herein, embodiments of the present disclosure are described merely as examples with reference to the attached figures. [Brief explanation of the drawing]

[0007] [Figure 1] This invention describes a method for crystallizing metal sulfates, involving a Co intermediate raw material containing calcium and / or magnesium impurities. [Figure 2] This describes a single-stage pre-leaching process as part of a treatment method for crystallizing metal sulfates, involving raw materials containing calcium and / or magnesium impurities. [Figure 3] This describes a parallel multi-stage pre-leaching process as part of a treatment method for crystallizing metal sulfates, involving raw materials containing calcium and / or magnesium impurities. [Figure 4] This describes a countercurrent multi-stage pre-leaching process as part of a treatment method for crystallizing metal sulfates, involving raw materials containing calcium and / or magnesium impurities. [Figure 5] This shows a purification and impurity removal step as part of a process for crystallizing metal sulfates, involving raw materials containing calcium and / or magnesium impurities. [Figure 6] This describes a treatment method for crystallizing metal sulfates, involving a black mass raw material containing lithium impurities that emphasizes the pre-leaching process. [Figure 7] This paper describes a treatment method for crystallizing metal sulfates containing black lumps as raw materials, emphasizing a direct lithium extraction process. [Figure 8] A flowchart of a common method for producing crystalline metal sulfates is shown. [Figure 9] This invention describes a method for crystallizing metal sulfates, involving a mixed hydroxide precipitate intermediate raw material containing calcium and / or magnesium impurities. [Modes for carrying out the invention]

[0008] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which this invention pertains.

[0009] As used herein and in the claims, the singular forms "a," "an," and "it" include plural references unless otherwise specified in the context.

[0010] As used herein, the term “including” means that the following list is not exhaustive and may include, or may not include, any other further suitable items as needed, such as one or more further features, components and / or ingredients.

[0011] As used herein, “NMC” refers to nickel, manganese, and / or cobalt. As used herein, “metal sulfate” refers to any one or a combination of nickel sulfate, cobalt sulfate, and / or manganese sulfate. Furthermore, “metal hydroxide” refers to any one or a combination of nickel hydroxide, cobalt hydroxide, and / or manganese hydroxide.

[0012] As used herein, “crystallization,” “to crystallize,” or “crystallized” refers to the process of selectively and slowly forming a crystalline network from a metal sulfate in a leaching solution (or PLS), resulting in a pure crystalline compound (as indicated by X-ray diffraction). In contrast, as used herein, “precipitation” refers to a process characterized by the addition of a precipitation or basicizing agent and the formation of a crystalline or amorphous solid from a solution. As used herein, “cocrystallize” or “to cocrystallize” refers to the crystallization of two or more components (e.g., a metal sulfate, an impurity, etc.) from a solution together (e.g., simultaneously). As used herein, when referring to “selectively crystallizing” or “selectively cocrystallizing” a metal sulfate, “selective” means crystallizing the metal sulfate away from most, if not all, impurities or other components; in other words, “selective” means forming a pure crystalline metal sulfate.

[0013] As used herein, "raw material" or "pre-leached raw material" refers to a solid containing at least some materials that are desirable to extract / isolate from said solid for further processing and / or use in a final product, such as metals desirable in the manufacture of battery materials.

[0014] As used herein, "treatment method" refers to a process that may include a pretreatment step (e.g., pre-leaching), a purification step of treating the leaching solution to remove impurities (e.g., fluoride precipitation, direct lithium extraction), or a combination of both.

[0015] As used herein, "impurity" refers to a component of the raw material that is not a metal sulfate as described herein or does not contribute to the formation of the metal sulfates or crystallized metal sulfates as described herein. As used herein, an "impurity" may be a useful, beneficial, or desirable material when isolated from the raw material.

[0016] Treatment method for raw materials containing impurities Generally, the present disclosure provides a treatment method for crystallizing metal sulfates, comprising pretreating a raw material containing calcium, magnesium, and / or lithium impurities by pre-leaching the raw material in the presence of a leaching agent, selectively extracting a first portion of the impurities from the raw material, and forming a pre-leached raw material; purifying the pre-leached raw material and forming a leaching solution containing non-crystallized metal sulfates, wherein purifying optionally includes removing a second portion of the impurities from the leaching solution if the leaching solution containing non-crystallized metal sulfates further contains impurities; and crystallizing the non-crystallized metal sulfates from the leaching solution to form crystallized metal sulfates.

[0017] The present disclosure generally relates to a treatment method for crystallizing metal sulfates, which comprises pretreating a raw material containing calcium, magnesium and / or lithium impurities, the pretreatment including pre-leaching the raw material in the presence of a leaching agent, selectively extracting a first portion of the impurities from the raw material, and forming a pre-leached raw material; purifying the pre-leached raw material and forming a leaching solution containing amorphous metal sulfate, the purification optionally including removing a second portion of the impurities from the leaching solution if the leaching solution containing amorphous metal sulfate further contains impurities; crystallizing the amorphous metal sulfate from the leaching solution to form a crystallized metal sulfate in a mother liquor containing the remaining amorphous metal sulfate; separating the crystallized metal sulfate from the mother liquor; basifying a portion of the mother liquor to convert the remaining amorphous metal sulfate into a basic metal salt; and using the basic metal salt upstream of the crystallization of the metal sulfate.

[0018] Furthermore, the present disclosure generally relates to a treatment method for crystallizing metal sulfates, which comprises leaching a raw material containing calcium, magnesium and / or lithium impurities and forming a leaching solution containing amorphous metal sulfate as well as calcium, magnesium and / or lithium impurities; purifying the leaching solution, the purification including removing a portion of the impurities; and crystallizing the amorphous metal sulfate from the leaching solution to form a crystallized metal sulfate.

[0019] This disclosure further provides a method for crystallizing metal sulfates, generally comprising: leaching a raw material containing calcium, magnesium, and / or lithium impurities to form an leaching solution containing amorphous metal sulfates and calcium, magnesium, and / or lithium impurities; purifying the leaching solution, including removing a portion of the impurities; crystallizing the amorphous metal sulfates from the leaching solution to form crystalline metal sulfates in a mother liquor containing the remaining amorphous metal sulfates; separating the crystalline metal sulfates from the mother liquor; basicizing a portion of the mother liquor to convert the remaining amorphous metal sulfates into basic metal salts; and using basic metal salts upstream of the crystallization of metal sulfates.

[0020] In one or more embodiments of the present disclosure, crystallizing an amorphous metal sulfate from an leaching solution to form a crystalline metal sulfate includes: crystallizing the amorphous metal sulfate from the leaching solution to form a crystalline metal sulfate in a mother liquor containing the remaining amorphous metal sulfate; separating the crystalline metal sulfate from the mother liquor; basicizing a portion of the mother liquor to convert the remaining amorphous metal sulfate into a basic metal salt; and using a basic metal salt upstream of the crystallization of the metal sulfate.

[0021] In one or more embodiments of the present disclosure, using a basic metal salt upstream includes converting the basic metal salt back to residual amorphous metal sulfate. In one or more embodiments, converting the basic metal salt back to residual amorphous metal sulfate includes using the basic metal salt as a neutralizing agent to neutralize the acid upstream of the crystallization of the metal sulfate. In one or more embodiments, basicizing a portion of the mother liquor to convert the residual amorphous metal sulfate back to a basic metal salt further includes releasing the mother liquor and controlling the release rate to produce an amount of basic metal salt that is at least approximately equal to the amount of acid neutralized upstream of the crystallization of the metal sulfate.

[0022] In one or more embodiments, one or more processing methods of the present disclosure further include crystallizing the residual amorphous metal sulfate.

[0023] In one or more embodiments of the present disclosure, crystallizing a metal sulfate further includes controlling the release rate from the crystallizer such that the mother liquor is released and the crystallization of impurities is selectively inhibited. In one or more embodiments, crystallizing a metal sulfate further includes controlling the amount of free water in the crystallizer by controlling the rate of water evaporation from the crystallizer and controlling the addition of water to the crystallizer, such that the crystallization of impurities is selectively inhibited.

[0024] In one or more embodiments of this disclosure, the impurity includes sodium or potassium, etc. In one or more embodiments of this disclosure, the metal sulfate includes nickel sulfate, cobalt sulfate, or manganese sulfate. In one or more embodiments of this disclosure, the basic metal salt includes a metal hydroxide. In one or more embodiments, the metal hydroxide includes nickel hydroxide, cobalt hydroxide, or manganese hydroxide.

[0025] In one or more embodiments of the processing methods of the present disclosure, the processing method shown in Figure 8 is provided, wherein the leaching and purification step comprises pre-treating the raw materials described herein to form a pre-leached raw material, and subjecting the pre-leached raw material to the leaching and purification step to form a purified leaching solution containing amorphous metal sulfates; the crystallization step comprises introducing the purified leaching solution into a crystallizer, forming crystalline metal sulfates (e.g., nickel sulfate, manganese sulfate and / or cobalt sulfate) in a mother liquor containing residual amorphous metal sulfates, and separating the crystalline metal sulfates from the mother liquor; the basicization step comprises basicizing a portion of the mother liquor to convert the residual amorphous metal sulfates into basic metal salts; for example, using a basic metal salt upstream of the crystallization of metal sulfates as a neutralizing agent to neutralize an acid upstream of the crystallization of metal sulfates.

[0026] Method for processing raw materials containing calcium and / or magnesium impurities In one or more embodiments of this disclosure, a method for crystallizing a metal sulfate, Pretreatment of a raw material containing calcium and / or magnesium impurities, comprising pre-leaching the raw material in the presence of a leaching agent, selectively extracting a first portion of the calcium and / or magnesium impurities from the raw material, and forming a pre-leached raw material; The process involves purifying the pre-leached raw material and forming an leaching solution containing amorphous metal sulfates; The process involves crystallizing amorphous metal sulfates from the leachate and forming crystalline metal sulfates in the mother liquor containing the remaining amorphous metal sulfates; To separate crystalline metal sulfates from the mother liquor; This involves basicizing a portion of the mother liquor and converting the remaining amorphous metal sulfates into basic metal salts; Using a basic metal salt upstream of the crystallization of metal sulfates A processing method including this is provided.

[0027] In one or more embodiments of this disclosure, a method for crystallizing a metal sulfate, Pretreatment of raw materials containing calcium and / or magnesium impurities, Pre-leaching of raw materials in the presence of an extractant, Selective extraction of a first portion of calcium and / or magnesium impurities from the raw material, and Forming pre-leached raw materials This includes pre-processing; The process involves purifying the pre-leached raw material and forming an leaching solution containing amorphous metal sulfates; Crystallization of amorphous metal sulfates from the leaching solution to form crystalline metal sulfates. A processing method including this is provided.

[0028] In one or more embodiments of the present disclosure, a processing method is provided, wherein the leaching solution containing an amorphous metal sulfate further contains a second portion of calcium and / or magnesium impurities from the raw material, and the purification method comprises adding a fluoride source to the leaching solution, selectively reacting the fluoride source with the second portion of calcium and / or magnesium impurities to form a calcium and / or magnesium fluoride compound, and precipitating the calcium and / or magnesium fluoride compound from the leaching solution.

[0029] In one or more embodiments of the present disclosure, a processing method is provided, wherein the leaching solution containing an amorphous metal sulfate further comprises a second portion of calcium and / or magnesium impurities from the raw material, and the purification method comprises a solvent extraction step of selectively extracting at least the second portion of calcium and / or magnesium impurities from the leaching solution onto or into a solvent extraction reagent. In one or more embodiments, the solvent extraction step further comprises scrubbing the calcium and / or magnesium impurities from the solvent extraction reagent.

[0030] In one or more embodiments of this disclosure, a method for crystallizing a metal sulfate, Leaving a raw material containing calcium and / or magnesium impurities, and forming a leaching solution containing amorphous metal sulfates and calcium and / or magnesium impurities; This involves purifying the leachate. Adding a fluoride source to the leachate, To selectively react a fluoride source with some of the calcium and / or magnesium impurities, and to form a calcium and / or magnesium fluoride compound, and Precipitate calcium and / or magnesium fluoride compounds from the leachate. Including purification; The process involves crystallizing amorphous metal sulfates from the leachate and forming crystalline metal sulfates in the mother liquor containing the remaining amorphous metal sulfates; To separate crystalline metal sulfates from the mother liquor; This involves basicizing a portion of the mother liquor and converting the remaining amorphous metal sulfates into basic metal salts; Using a basic metal salt upstream of the crystallization of metal sulfates A processing method including this is provided.

[0031] In one or more embodiments of this disclosure, a method for crystallizing a metal sulfate, Leaving a raw material containing calcium and / or magnesium impurities, and forming a leaching solution containing amorphous metal sulfates and calcium and / or magnesium impurities; This involves purifying the leachate. Adding a fluoride source to the leachate, To selectively react a fluoride source with some of the calcium and / or magnesium impurities, and to form a calcium and / or magnesium fluoride compound, and Precipitate calcium and / or magnesium fluoride compounds from the leachate. Including purification; Crystallization of amorphous metal sulfates from the leaching solution to form crystalline metal sulfates. A processing method including this is provided.

[0032] In one or more embodiments of a method for treating calcium and / or magnesium impurities, the raw material includes an intermediate raw material. The intermediate raw material is a raw material pre-treated from the original or raw material. In one or more embodiments, the intermediate raw material may contain impurities at a lower concentration after pre-treatment than the original raw material. In one or more embodiments, the intermediate raw material consists of concentrates. In one or more embodiments, the intermediate raw material includes a metal-containing intermediate raw material. In one or more embodiments, the metal-containing intermediate raw material consists of metal hydroxides and / or mixed hydroxide precipitates (MHP). In one or more embodiments, the metal-containing intermediate raw material contains metals desirable in the manufacture of battery materials, such as cobalt, manganese and / or nickel, in addition to impurities such as calcium and / or magnesium. In one or more embodiments, the intermediate raw material includes nickel, manganese and / or cobalt intermediate raw materials. In one or more embodiments, the cobalt intermediate raw material consists of Co(OH)2 and / or mixed hydroxide precipitates (MHP). In one or more embodiments, the cobalt intermediate raw material contains metals desirable in the production of battery materials, such as cobalt, manganese, and / or nickel, in addition to impurities such as calcium and / or magnesium. In one or more embodiments, the manganese intermediate raw material consists of Mn(OH)2 and / or mixed hydroxide precipitate (MHP). In one or more embodiments, the manganese intermediate raw material contains metals desirable in the production of battery materials, such as manganese, cobalt, and / or nickel, in addition to impurities such as calcium and / or magnesium. In one or more embodiments, the nickel intermediate raw material contains Ni(OH)2 and / or mixed hydroxide precipitate. In one or more embodiments, the nickel intermediate raw material contains metals desirable in the production of battery materials, such as nickel, manganese, and / or cobalt, in addition to impurities such as calcium and / or magnesium.

[0033] In one or more embodiments of the processing method, the method comprises pre-treating a raw material containing calcium and / or magnesium impurities, the pre-treatment comprising pre-leaching the raw material in the presence of a leaching agent, selectively extracting a first portion of the calcium and / or magnesium impurities from the raw material, and forming a pre-leached raw material. In one or more embodiments, the leaching agent comprises an acidic aqueous solution. In one or more embodiments, the leaching agent is formed by adding acid to the raw material in water until the pH is in the range of about 5 to about 9, or about 5 to about 8, or about 5 to about 7, or about 6 to about 7. In one or more embodiments, the acid is sulfuric acid. In one or more embodiments of the method, the leaching agent is a concentrated cobalt sulfate solution. In one or more embodiments of the method, the concentrated cobalt sulfate solution has a concentration of ≥10 g / L, ≥20 g / L, ≥30 g / L, ≥40 g / L, ≥50 g / L, ≥60 g / L, ≥70 g / L, ≥80 g / L, ≥90 g / L, ≥100 g / L, ≥120 g / L, ≥140 g / L, ≥160 g / L, ≥180 g / L, or ≥200 g / L, or any concentration between approximately 10 g / L and 200 g / L, or any concentration within a range between approximately 10 g / L and 200 g / L.

[0034] In one or more embodiments of the processing method, the method comprises pre-leaching a raw material containing calcium and / or magnesium impurities, the pre-leaching being carried out at a pH of about 5 to about 9, or about 5 to about 8, or about 5 to about 7; or at any pH of about 5 to about 9; or at any range of pH of about 5 to about 9. In one or more embodiments, the pH of the pre-leaching may be maintained by adding further acid during the process. In one or more embodiments, the pre-leaching is carried out at a temperature of approximately ambient temperature to about 100°C, or about 60°C to about 100°C, or about 80°C to about 100°C, or about 80°C to about 95°C; or at any temperature of approximately ambient temperature to about 100°C; or at any range of temperature of approximately ambient temperature to about 100°C.

[0035] In one or more embodiments of the processing method, the method comprises pre-treating a raw material containing calcium and / or magnesium impurities, the pre-treatment being carried out as a single-stage pre-leaching process. In one or more embodiments, the single-stage pre-leaching process comprises adding an acid to the raw material in water to form an acidic aqueous leaching agent; pre-leaching the raw material at a suitable temperature (e.g., approximately ambient temperature to about 100°C) and a suitable pH (e.g., about 5 to about 9); forming a solution containing the pre-leached raw material and a first portion of the calcium and / or magnesium impurities; filtering and separating the pre-leached raw material from the impurity-containing solution; and washing the pre-leached raw material.

[0036] In one or more embodiments of the processing method, the method includes pre-treating a raw material containing calcium and / or magnesium impurities, the pre-treating being carried out as a multi-stage pre-leaching process. In one or more embodiments, the multi-stage pre-leaching process includes a series of single-stage pre-leaching processes, each single-stage process including the steps of forming a leaching agent, pre-leaching the raw material, forming a solution containing the pre-leached raw material and a first portion of the calcium and / or magnesium impurities, and filtering and washing the pre-leached raw material, wherein the pre-leached raw material from one single-stage process is supplied to the next single-stage process. In one or more embodiments, the multi-stage pre-leaching process includes two or three single-stage processes. In one or more embodiments, the multi-stage pre-leaching process is carried out in parallel flow, which involves bringing the raw material and leaching into contact and flowing in the same direction. In one or more embodiments, the multi-stage pre-leaching process is carried out in counterflow flow, which involves bringing the raw material and leaching into contact and flowing in opposite directions.

[0037] In one or more embodiments of the processing method, the method comprises pre-leaching a raw material containing calcium and / or magnesium impurities, wherein the calcium and / or magnesium impurities are extracted from the raw material during pre-leaching and dissolved in an aqueous leaching agent solution and / or an acidic aqueous solution, so as to form a solution containing a first portion of the calcium and / or magnesium impurities. In one or more embodiments, the pH and temperature of the single-stage or multi-stage pre-leaching process are selected to selectively extract the calcium and / or magnesium impurities in the pre-leached raw material while leaving at least a majority of the material desirable for the manufacture of batteries, such as metallic cobalt, manganese, and / or nickel. In one or more embodiments of the method, selective extraction of the first portion of calcium and / or magnesium impurities removes the corresponding portion of the impurities from the raw material, thereby forming a cleaner / purer pre-leached raw material that can be subsequently used in the manufacture of battery materials, such as crystalline metal sulfates, that meet purity requirements. In one or more embodiments, the method provides crystalline metal sulfates that meet the purity requirements of the impurity calcium and / or magnesium. In one or more embodiments, the crystalline metal sulfates include crystalline nickel sulfate, manganese sulfate, and / or cobalt sulfate. In one or more embodiments of the method, selective extraction of a first portion of calcium and / or magnesium impurities from a raw material includes selective extraction of about 50% to about 99%, or about 60% to about 99%, or about 70% to about 99%, or about 80% to about 99% of the calcium and / or magnesium impurities in the raw material.

[0038] In one or more embodiments of the processing method, the method comprises pre-leaching a raw material containing calcium and / or magnesium impurities, wherein small amounts of material desirable for the manufacture of batteries, such as metallic cobalt, manganese, and / or nickel, may be extracted from the raw material during pre-leaching and dissolved in a solution containing a first portion of the calcium and / or magnesium impurities. To recover these metals, the solution may be treated with a base such as a metal hydroxide (e.g., KOH or NaOH) to precipitate cobalt, manganese, and / or nickel as Co(OH)2, Mn(OH)2, and / or Ni(OH)2. The Co(OH)2, Mn(OH)2, and / or Ni(OH)2 can then be isolated and reintroduced into the process, while the remaining solution containing a first portion of the calcium and / or magnesium impurities may be sent for further processing or waste disposal.

[0039] In one or more embodiments of the processing method, the method comprises pre-treating a raw material containing calcium and / or magnesium impurities, further comprising purifying the pre-leached raw material and forming a leaching solution containing amorphous metal sulfates. In one or more embodiments, purifying the pre-leached raw material comprises leaching the pre-leached raw material under conditions that form a leaching solution containing amorphous metal sulfates. In one or more embodiments, leaching the pre-leached raw material under conditions that form a leaching solution comprises leaching under conditions that form a sulfate matrix-impregnated leaching solution (PLS). There are several leaching conditions that may be suitable for forming a leaching solution (or PLS). Based on the type or source of the raw material to be processed, a person skilled in the art will know which leaching conditions to select and test in order to confirm the selection and specify the particular conditions. For example, leaching may be carried out above ambient temperature or ambient temperature and / or ambient pressure. For raw materials containing MHP or black lumps, leaching may be carried out at a temperature of about 65°C and atmospheric pressure, for example, with the addition of acids and reducing agents.

[0040] In one or more embodiments of a method for treating calcium and / or magnesium impurities, the method comprises leaching a pre-leached raw material, followed by purifying the pre-leached raw material, the purification of the pre-leached raw material may further comprise subjecting the leaching solution (or PLS) containing amorphous metal sulfates to a series of component removal steps to form a purified leaching solution containing amorphous metal sulfates. The type and amount of components removed depends at least in part on the type of raw material from which the leaching solution is formed. When manufacturing materials for battery manufacturing, such as producing crystalline metal sulfates, there are specific product specifications (e.g., limitations) for such components that are acceptable; any such components present in the process raw materials, water, or reagents in amounts exceeding the said product specifications will need to have their concentrations reduced. Examples of components to be removed include, but are not limited to, sodium (Na), aluminum (Al), iron (Fe), copper (Cu), zinc (Zn), cobalt (Co), nickel (Ni), or manganese (Mn). There are many preferred methods for removing components from the leaching solution (or PLS). Such methods include, but are not limited to, precipitation, atmospheric pressure leaching or pressurized leaching, sulfidation, solvent extraction, ion exchange, and cementation. The selection of an appropriate method (and its operating conditions) depends at least in part on the type and amount of components to be removed and the specifications of the final product (e.g., crystalline metal sulfates) produced by the process. For example, a leached solution may be subjected to a series of component removal steps to remove components such as Cu (e.g., by solvent extraction, cementation, ion exchange, etc.), Fe and Al (e.g., by precipitation, etc.), and Zn (e.g., by solvent extraction, ion exchange, etc.).

[0041] In one or more embodiments of the processing method, the method comprises pre-treating a raw material containing calcium and / or magnesium impurities, and pre-treating the raw material does not require the removal of all calcium and / or magnesium impurities; therefore, the leaching solution containing amorphous metal sulfates may further contain a second portion of calcium and / or magnesium impurities from the raw material. Accordingly, in one or more embodiments of the method, purifying the pre-leached raw material further comprises subjecting the purified leaching solution containing amorphous metal sulfates and a second portion of calcium and / or magnesium impurities to a purification and de-impurity step to remove at least a portion of the remaining calcium and / or magnesium impurities. In one or more embodiments, the purification and de-impurity step comprises adding a fluoride source to the leaching solution, selectively reacting the fluoride source with the second (e.g., residual) portion of calcium and / or magnesium impurities to form a calcium and / or magnesium fluoride compound, and precipitating the calcium and / or magnesium fluoride compound from the leaching solution. In one or more embodiments, the purification, impurity removal step includes a solvent extraction step of selectively extracting at least a second portion of calcium and / or magnesium impurities from the leaching solution onto or into a solvent extraction reagent. In one or more embodiments, the solvent extraction step further includes scrubbing the calcium and / or magnesium impurities from the solvent extraction reagent.

[0042] In one or more embodiments of the treatment method for calcium and / or magnesium impurities, purifying the pre-leached raw material involves adding a fluoride source to the leaching solution, and the precipitated calcium and / or magnesium fluoride compound may include CaF2 and / or MgF2. In one or more embodiments, the calcium and / or magnesium fluoride compound precipitates due to their low solubility in aqueous solution. In one or more embodiments, the added fluoride source is soluble in aqueous solution. In one or more embodiments, the added fluoride source is hydrogen fluoride, sodium fluoride, cobalt fluoride, ammonium fluoride, or a combination thereof. In one or more embodiments, the amount of fluoride source added may depend on the amount of calcium and / or magnesium impurities remaining in the leaching solution and / or the corrosion properties of the fluoride compound and the process's resistance (e.g., equipment's resistance to corrosion). In one or more embodiments, the amount of fluoride source added may be selected to selectively precipitate calcium and / or magnesium impurities while leaving most, if not all, of the metals and / or materials desirable for further downstream processing and / or isolation, such as amorphous metal sulfates (e.g., amorphous cobalt sulfate, manganese sulfate, and / or nickel sulfate) for the manufacture of batteries.

[0043] In one or more embodiments of a method for treating calcium and / or magnesium impurities, the purification of the pre-leached raw material includes solvent extraction, which may include the use of an organic extractant, a solvent extraction reagent, or a combination thereof. In one or more embodiments, the organic extractant, solvent extraction reagent comprises the organic phase of the solvent extraction. In one or more embodiments, the organic extractant or solvent extraction reagent may be selective for the extraction of one or a combination of calcium and / or magnesium, base metals (e.g., copper, aluminum, zinc), and / or transition metals (e.g., nickel, cobalt, manganese, etc.). In one or more embodiments, the solvent extraction reagent may be Cyanex 272® or an equivalent. In one or more embodiments, the solvent extraction may be carried out at an acidic pH. In one or more embodiments, the pH may be about 4.5 to about 6 or about 5 to about 5.5. In one or more embodiments, the solvent extraction further includes scrubbing, which may be accompanied by a scrubbing solution. In one or more embodiments, the scrubbing solution may include a sulfate solution. In one or more embodiments, the sulfate solution may include a metal sulfate solution, and the metal may be the same or identical metal that is extracted when the pre-leached raw material is purified. In one or more embodiments, scrubbing conditions may be selected to selectively scrub and remove calcium and / or magnesium impurities from the organic extractant or solvent extractant while leaving most, if not all, of the metal and / or material desired for further downstream processing and / or isolation, such as amorphous metal sulfates (e.g., amorphous cobalt sulfate, manganese sulfate, and / or nickel sulfate). In one or more embodiments, the metal and / or material desired for further downstream processing and / or isolation may be stripped from the organic extractant or solvent extractant using a dilute acidic solution, such as a dilute sulfuric acid solution. In one or more embodiments, stripping may be performed at a pH of about 2 to about 4 or about 3 to about 3.5. In one or more embodiments, after extraction, scrubbing, and then stripping, the desired metal and / or material may be isolated so as to be substantially free of calcium and / or magnesium impurities.

[0044] In one or more embodiments of a method for treating calcium and / or magnesium impurities, the method comprises purifying a pre-leached raw material, the purification, impurity removal step may be carried out at a pH of about 3 to about 9, or about 3 to about 7, or about 3 to about 5; or about 3 to about 4; or about 3 to about 3.5; or about 5 to about 6; or about 5 to about 5.5; or any pH of about 3 to about 9; or any range of pH of about 3 to about 9. In one or more embodiments, the pH of the purification, impurity removal step may be maintained by adding further acid during the process. In one or more embodiments, the purification, impurity removal step may be carried out at a temperature of approximately ambient temperature to about 100°C, or about 20°C to about 80°C, or about 20°C to about 60°C, or about 20°C to about 40°C; or any temperature of about 20°C to about 100°C; or any range of temperature of about 20°C to about 100°C.

[0045] In one or more embodiments of a method for treating calcium and / or magnesium impurities, the method comprises purifying a pre-leached raw material, selectively forming and precipitating calcium and / or magnesium fluoride compounds, or selectively solvent-extracting calcium and / or magnesium impurities, the purification and impurity removal step removes at least a portion of the calcium and / or magnesium impurities (i.e., the second portion of calcium and / or magnesium impurities) that may remain in the pre-leached raw material after pretreatment and subsequently extracted into the leaching solution containing amorphous metal sulfates. In one or more embodiments of the method, selective removal of at least the second portion of calcium and / or magnesium impurities removes the corresponding portion of the impurities from the leaching solution that originally originated from the raw material and remained in the pre-leached raw material, thereby forming a cleaner / pureer leaching solution that satisfies purity requirements and can be subsequently used in the manufacture of battery materials, such as crystalline metal sulfates. In one or more embodiments, selective removal of a second portion of calcium and / or magnesium impurities includes selectively removing about 50% to about 99%, or about 60% to about 99%, or about 70% to about 99%, or about 80% to about 99% of the calcium and / or magnesium impurities in the leaching solution that originally originated from the raw material and remained in the pre-leached raw material.

[0046] In one or more embodiments of a method for treating calcium and / or magnesium impurities, the method comprises purifying the pre-leached raw materials so that the calcium and / or magnesium fluoride compounds precipitate from the leaching solution, which may then be filtered, optionally washed, and further processed downstream or sent to waste disposal. After the removal of the calcium / or magnesium fluoride compounds, the leaching solution containing amorphous metal sulfates may continue to be processed further.

[0047] In one or more embodiments of a method for treating calcium and / or magnesium impurities, the method comprises purifying a pre-leached raw material, further comprising removing a residual fluoride source from the leaching solution. In one or more embodiments, removal of the residual fluoride source comprises selectively reacting the residual fluoride source with a calcium source to form a calcium fluoride compound, and precipitating the calcium fluoride compound from the leaching solution. In one or more embodiments, the residual fluoride source is at least partially or completely removed. In one or more embodiments, the calcium fluoride compound comprises CaF2. In one or more embodiments, the calcium source comprises limestone, lime, gypsum, or a combination thereof. In one or more embodiments, the method further comprises removing the residual calcium source by ion exchange, solvent extraction, or a combination thereof.

[0048] In one or more embodiments of a method for treating calcium and / or magnesium impurities, the method comprises purifying a pre-leached raw material, the amount of fluoride source added may be selected to remove calcium and / or magnesium impurities to a level acceptable for downstream processes. In one or more embodiments, the amount of fluoride source remaining in the leaching solution (e.g., residual fluoride source) is then removed by adding a calcium compound (e.g., calcium source) such as limestone, lime, or gypsum that is substantially free of magnesium. In one or more embodiments, any excess calcium compound remaining (if present) can then be separated from amorphous metal sulfates in the leaching solution, for example by ion exchange, solvent extraction, or a combination thereof.

[0049] In one or more embodiments of a method for treating calcium and / or magnesium impurities, the method comprises purifying a pre-leached raw material, further comprising removing a residual fluoride source, the removal comprising combining a solution containing a first portion of the calcium and / or magnesium impurities from the pre-leaching step with a crystallizer discharge stream (described in more detail below) containing the residual fluoride source, selectively reacting the residual fluoride source with the first portion of the calcium and / or magnesium impurities to form a calcium and / or magnesium fluoride compound, and precipitating the calcium and / or magnesium fluoride compound from the discharge stream. In one or more embodiments, the residual fluoride source is at least partially or completely removed. In one or more embodiments, the calcium fluoride compound comprises CaF2.

[0050] In one or more embodiments of the processing method, the method comprises leaching a raw material containing calcium and / or magnesium impurities to form a leaching solution containing amorphous metal sulfates and calcium and / or magnesium impurities. In one or more embodiments of the method, leaching the raw material comprises leaching under conditions that form a leaching solution containing amorphous metal sulfates and calcium and / or magnesium impurities. In one or more embodiments, leaching the raw material under conditions that form a leaching solution comprises leaching under conditions that form a sulfate matrix-impregnated leaching solution (PLS). There are several leaching conditions that may be suitable for forming a leaching solution (or PLS). Based on the type or source of the raw material to be processed, a person skilled in the art will know which leaching conditions to select and test in order to confirm the selection and specify the particular conditions.

[0051] In one or more embodiments of the processing method, the method comprises leaching a raw material containing calcium and / or magnesium impurities, and the method further comprises purifying the leaching solution containing amorphous metal sulfates and calcium and / or magnesium impurities. In one or more embodiments of the method, the purification of the leaching solution may comprise subjecting the leaching solution (or PLS) containing amorphous metal sulfates and calcium and / or magnesium impurities to a series of component removal steps to form a purified leaching solution. The type and amount of components removed depends at least in part on the type of raw material from which the leaching solution is formed. When manufacturing materials for battery manufacturing, such as producing crystallized metal sulfates, there are specific product specifications (e.g., limitations) on such components that are permissible; any such components present in the process raw materials, water, or reagents in amounts exceeding the said product specifications will need to have their concentrations reduced. Examples of components to be removed include, but are not limited to, sodium (Na), aluminum (Al), iron (Fe), copper (Cu), zinc (Zn), cobalt (Co), nickel (Ni), or manganese (Mn). There are many suitable methods for removing components from leaching solutions (or PLS). Such methods include, but are not limited to, precipitation, atmospheric pressure leaching or pressurized leaching, sulfidation, solvent extraction, ion exchange, and cementation. The selection of a suitable method (and its operating conditions) depends at least in part on the type and amount of component to be removed and the specifications of the final product (e.g., crystalline metal sulfate) produced by the process. For example, a leaching solution may be subjected to a series of component removal steps to remove components such as Cu (e.g., by solvent extraction, cementation, ion exchange, etc.), Fe and Al (e.g., by precipitation, etc.), and Zn (e.g., by solvent extraction, ion exchange, etc.).

[0052] In one or more embodiments of the processing method, the method comprises purifying a leaching solution containing amorphous metal sulfates and calcium and / or magnesium impurities, wherein the purification of the leaching solution further comprises subjecting the purified leaching solution containing amorphous metal sulfates and calcium and / or magnesium impurities to a purification and impurity removal step to remove at least a portion of the calcium and / or magnesium impurities. In one or more embodiments, the purification and impurity removal step comprises adding a fluoride source to the leaching solution, selectively reacting the fluoride source with a portion of the calcium and / or magnesium impurities to form a calcium and / or magnesium fluoride compound, and precipitating the calcium and / or magnesium fluoride compound from the leaching solution.

[0053] In one or more embodiments of the processing method, the method comprises purifying a leaching solution containing amorphous metal sulfates and calcium and / or magnesium impurities, wherein the precipitated calcium and / or magnesium fluoride compounds include CaF2 and / or MgF2. In one or more embodiments, the calcium and / or magnesium fluoride compounds precipitate due to their low solubility in aqueous solutions. In one or more embodiments, the fluoride source added is soluble in aqueous solutions. In one or more embodiments, the fluoride source added is hydrogen fluoride, sodium fluoride, cobalt fluoride, ammonium fluoride, or a combination thereof. In one or more embodiments, the amount of fluoride source added may depend on the amount of calcium and / or magnesium impurities in the leaching solution and / or the corrosion properties of the fluoride compounds and the process's resistance (e.g., equipment's resistance to corrosion). In one or more embodiments, the amount of fluoride source added may be selected to selectively precipitate calcium and / or magnesium impurities while leaving at least a majority of the material desirable for the manufacture of the battery, such as amorphous metal sulfates (e.g., amorphous cobalt sulfate, manganese sulfate, and / or nickel sulfate).

[0054] In one or more embodiments of the processing method, the method comprises purifying a leaching solution containing amorphous metal sulfates and calcium and / or magnesium impurities, wherein the purification and de-impurity step is carried out at a pH of about 3 to about 9, or about 3 to about 7, or about 3 to about 5; or at any pH of about 3 to about 9; or at any range of pH of about 3 to about 9. In one or more embodiments, the pH of the purification and de-impurity step may be maintained by adding further acid during the process. In one or more embodiments, the purification and de-impurity step is carried out at a temperature of approximately ambient temperature to about 100°C, or about 20°C to about 80°C, or about 20°C to about 60°C, or about 20°C to about 40°C; or at any temperature of about 20°C to about 100°C; or at any range of temperature of about 20°C to about 100°C.

[0055] In one or more embodiments of the processing method, the method comprises purifying a leachate containing amorphous metal sulfates and calcium and / or magnesium impurities, wherein the purification and impurity removal step selectively forms and precipitates calcium and / or magnesium fluoride compounds, thereby removing at least a portion of the calcium and / or magnesium impurities from the leachate containing amorphous metal sulfates and calcium and / or magnesium impurities. In one or more embodiments of the method, selective removal of at least a portion of the calcium and / or magnesium impurities removes the corresponding portion of the impurities from the leachate that originally originated from the raw materials, thereby forming a cleaner / pureer leachate that satisfies purity requirements and can be subsequently used in the manufacture of battery materials, such as crystalline metal sulfates. In one or more embodiments, selective removal of a portion of the calcium and / or magnesium impurities includes selectively removing about 50% to about 99%, or about 60% to about 99%, or about 70% to about 99%, or about 80% to about 99% of the calcium and / or magnesium impurities that originally existed in the leachate.

[0056] In one or more embodiments of the processing method, the method comprises purifying a leachate containing amorphous metal sulfates and calcium and / or magnesium impurities, wherein the calcium and / or magnesium fluoride compounds precipitate from the leachate, which may then be filtered, optionally washed, and further processed downstream or sent to waste disposal. After the removal of the calcium and / or magnesium fluoride compounds, the leachate containing amorphous metal sulfates may continue to be processed further.

[0057] In one or more embodiments of a method for treating calcium and / or magnesium impurities, the method comprises purifying a leachate containing amorphous metal sulfates and calcium and / or magnesium impurities, further comprising removing a residual fluoride source from the leachate. In one or more embodiments, removal of the residual fluoride source comprises selectively reacting the residual fluoride source with a calcium source to form a calcium fluoride compound, and precipitating the calcium fluoride compound from the leachate. In one or more embodiments, the residual fluoride source is at least partially or completely removed. In one or more embodiments, the calcium fluoride compound comprises CaF2. In one or more embodiments, the calcium source comprises limestone, lime, gypsum, or a combination thereof. In one or more embodiments, the method further comprises removing the residual calcium source by ion exchange, solvent extraction, or a combination thereof.

[0058] In one or more embodiments of a method for treating calcium and / or magnesium impurities, the method comprises purifying a leachate containing amorphous metal sulfates and calcium and / or magnesium impurities, wherein the amount of fluoride source added may be selected to remove calcium and / or magnesium impurities to a level acceptable for downstream processes. In one or more embodiments, any amount of fluoride source remaining in the leachate (e.g., residual fluoride source) is then removed by adding a calcium compound (e.g., calcium source) such as substantially magnesium-free limestone, or lime, or gypsum. In one or more embodiments, any excess calcium compound remaining (if present) can then be separated from the amorphous metal sulfates in the leachate, for example, by ion exchange, solvent extraction, or a combination thereof.

[0059] In one or more embodiments of a method for treating calcium and / or magnesium impurities, the method further comprises crystallizing amorphous metal sulfates from a leachate to form crystalline metal sulfates. In one or more embodiments, crystallizing amorphous metal sulfates comprises introducing a purified leachate containing amorphous metal sulfates into a crystallizer under conditions sufficient to selectively crystallize the amorphous metal sulfates. In one or more embodiments, selective crystallizing amorphous metal sulfates may involve selectively crystallizing one or a combination of NiSO4, CoSO4, and / or MnSO4 from a solution (for example, in a forced-circulation crystallizer under reduced pressure, depending on the feed material, such as for manganese) to produce crystalline metal sulfates in the mother liquor. These crystalline metal sulfates can then be discharged from the crystallizer, thereby isolating them from the mother liquor. If one crystallization cycle (e.g., using one crystallizer) is insufficient to produce the crystallized metal sulfate (e.g., this may occur with more contaminated feed material), the crystals discharged from the crystallizer may be dissolved in pure water and then introduced into a second crystallization cycle (e.g., using a second crystallizer) for recrystallization.

[0060] Various types of crystallizers may be suitable for influencing the selective crystallization of amorphous metal sulfates from leaching solutions. Such crystallizers include, but are not limited to, evaporative crystallizers, forced-circulation (FC) crystallizers, indirect forced-circulation (IFC) crystallizers, and draft-tube baffle (DTB) crystallizers. The conditions and operating parameters for such crystallizers may be selected depending on the type and purity of the metal sulfate to be crystallized and / or the type and concentration of impurities in the leaching solution. For example, the release of mother liquor from the crystallizer during crystallization and the rate at which the release occurs may affect the purity of the crystallized metal sulfate, for example, by selectively inhibiting the crystallization of impurities. Selecting a release rate to selectively inhibit the crystallization of a particular impurity means setting the crystallizer release rate within a range of possible release rates that inhibit the crystallization of a specific impurity rather than inhibiting the crystallization of different impurities. The release rate may be selected to maximize the inhibition of the crystallization of a particular impurity. Impurities may include sodium, potassium, etc. Using a higher release rate of the mother liquor helps maintain lower concentrations of impurities and other components in the mother liquor that may affect the purity of the crystallized metal sulfate. Furthermore, the solubility of impurities may be temperature-dependent; therefore, selecting the crystallizer temperature and crystallizer release rate may be effective in controlling the purity of the crystallized metal sulfate. The solubility of impurities may also depend on the amount of free water present in the leaching solution and / or mother liquor; therefore, controlling the level of water in the crystallizer may be an effective means of controlling the purity of the crystallized metal sulfate. For example, in some cases, metal sulfate crystallizes from solution as metal sulfate hydrate (i.e., crystallized metal sulfate and water molecules combine in distinct ratios as essential parts of the crystal), which reduces the concentration of water in the mother liquor. By reducing the concentration of free water, the concentration of impurities in the mother liquor (e.g., sodium, potassium, etc.) may also increase to the point where they crystallize from solution and affect the purity of the crystallized metal sulfate.However, if a sufficient amount of water is added to the mother liquor when it is present in the leachate and / or crystallizer, or if an excess amount of water remains in the leachate after upstream processing (for example, at least the amount of water that would be expected to be lost by hydrate formation), the presence of such free water may inhibit the crystallization of impurities from the solution.

[0061] After crystallization, the mother liquor may still contain undesirable salts / metals (e.g., Li2SO4, Mg, Na, etc.) and residual amorphous metal sulfates. To selectively recover residual amorphous metal sulfates from the undesirable materials remaining in the solution, the mother liquor is "released" from the crystallizer and basicized so that the amorphous metal sulfates are converted into insoluble basic metal salts (e.g., metal hydroxides such as Ni(OH)2, Co(OH)2, Mn(OH)2, etc.). The resulting basic metal salts (e.g., metal hydroxides) precipitate from the mother liquor and can be isolated from the mother liquor by filtration. For example, the basic metal salts can be recovered by filtration, concentration and filtration or centrifugation. The resulting precipitated metal hydroxide may be washed or repulped to form a slurry, but is then used upstream to neutralize an acid introduced in the leaching and / or component removal stage of the process, thereby converting the metal hydroxide back to an amorphous metal sulfate, which can then be isolated by downstream crystallization. Using a basic metal salt (e.g., metal hydroxide) as a neutralizing agent reduces and / or eliminates the need to introduce an external neutralizing agent; this reduces the use of reagents (and associated costs) and introduces further sources of impurities that could affect the purity of the product (e.g., cation Na from an external neutralizing agent), which would otherwise require a higher crystallization apparatus discharge rate to avoid coprecipitation of impurities and contamination of the crystallized metal sulfate. + , K + Li + Ca 2+ Mg 2+) is reduced and / or eliminated. In some cases, to ensure that there is a sufficient amount of basic metal salt, e.g., metal hydroxide available for use as a neutralizing agent, the rate at which the mother liquor is released from the crystallizer and basicized to form metal hydroxide can be controlled so that the amount of metal hydroxide formed is at least approximately equal to or approximately equal to the amount of acid introduced in the leaching and / or purification steps. Furthermore, using a basic metal salt (e.g., metal hydroxide) as a neutralizing agent converts the basic metal salt back into metal sulfate in the leaching solution. The leaching solution containing the converted metal sulfate then proceeds to the crystallizer, where the converted metal sulfate can be crystallized and isolated from the mother liquor. This loop of isolating and basicizing the mother liquor to convert the amorphous metal sulfate in the solution into basic metal salts, and then using those basic metal salts as neutralizing agents to convert the basic metal salts back into metal sulfate that can later be isolated by crystallization, can improve the yield of isolated crystallized metal sulfate obtained from specific raw materials.

[0062] In one or more embodiments of a method for treating calcium and / or magnesium impurities, crystallizing amorphous metal sulfates includes: crystallizing metal sulfates from an leaching solution to form crystalline metal sulfates in a mother liquor containing residual amorphous metal sulfates; separating the crystalline metal sulfates from the mother liquor; basicizing a portion of the mother liquor to convert the residual amorphous metal sulfates into basic metal salts; and using a basic metal salt upstream of the crystallization of metal sulfates. In one or more embodiments, using a basic metal salt upstream includes converting the basic metal salt back to amorphous metal sulfates. In one or more embodiments, converting the basic metal salt back to amorphous metal sulfates includes using a basic metal salt to neutralize an acid upstream of the crystallization of metal sulfates. In one or more embodiments, the basic metal salt includes a metal hydroxide. In one or more embodiments, the metal hydroxide includes one or a combination of nickel hydroxide, cobalt hydroxide, or manganese hydroxide.

[0063] In one or more embodiments of a method for treating calcium and / or magnesium impurities, the method comprises pre-treating a raw material and purifying a pre-leached raw material, wherein the leaching solution formed by purifying the pre-leached raw material, containing amorphous metal sulfates, may include the purified leaching solution introduced into the crystallizer; or it may be the mother liquor discharged from the crystallizer. Thus, in one or more embodiments of the method, the purification and impurity removal step for selectively forming and precipitating calcium and / or magnesium fluoride compounds may be carried out in the leaching solution before the leaching solution is introduced into the crystallizer; or it may be carried out in the mother liquor.

[0064] In one or more embodiments of a method for treating calcium and / or magnesium impurities, the method comprises leaching a raw material and purifying the leaching solution containing amorphous metal sulfates and calcium and / or magnesium impurities, wherein the leaching solution may include the purified leaching solution introduced into a crystallizer; or it may be the mother liquor discharged from the crystallizer. Thus, in one or more embodiments of the method, the purification and impurity removal steps for selectively forming and precipitating calcium and / or magnesium fluoride compounds may be carried out in the leaching solution before it is introduced into the crystallizer; or it may be carried out in the mother liquor.

[0065] In one or more embodiments of the processing method, the method comprises pre-leaching a raw material containing calcium and / or magnesium impurities, and the processing method shown in Figure 1 is provided, wherein the raw material is an intermediate raw material containing Co; the raw material is pre-leached to remove a first portion of calcium and / or magnesium impurities to form a solution containing the pre-leached raw material and calcium and / or magnesium impurities; the impurity-containing solution is basicized to precipitate Ca(OH)2 for use upstream of the process; the pre-leached raw material is then leached and subjected to a component removal step; the purified leached solution containing amorphous metal sulfates is introduced into a crystallizer to crystallize CoSO4; and a purification and impurity removal step is performed in the mother liquor discharged from the crystallizer to selectively form and precipitate calcium and / or magnesium fluoride compounds to remove a second portion of calcium and / or magnesium impurities.

[0066] In one or more embodiments of the processing method, the method comprises pre-leaching a raw material containing calcium and / or magnesium impurities, and a single-stage pre-leaching process is provided as shown in Figure 2, in which an intermediate raw material containing Co(OH)2 is mixed with a leaching agent in a pre-leaching reactor to form a pre-leached raw material containing a pre-leached Co(OH)2 cake and a pre-leached solution containing at least a first portion of calcium and / or magnesium impurities.

[0067] In one or more embodiments of the processing method, the method comprises pre-leaching a raw material containing calcium and / or magnesium impurities, and a parallel-flow, multi-stage pre-leaching process is provided as shown in Figure 3, in which an intermediate raw material containing Co(OH)2 is mixed with a leaching agent across a series of single-stage pre-leaching reactors to form a pre-leached raw material containing a pre-leached Co(OH)2 cake and a pre-leached solution containing at least a first portion of calcium and / or magnesium impurities.

[0068] In one or more embodiments of the processing method, the method comprises pre-leaching a raw material containing calcium and / or magnesium impurities, and a countercurrent, multi-stage pre-leaching process is provided as shown in Figure 4, in which an intermediate raw material containing Co(OH)2 is mixed countercurrently with a Co solution leaching agent across a series of single-stage pre-leaching reactors to form a pre-leached raw material containing a pre-leached Co(OH)2 cake and a pre-leached solution containing at least a first portion of calcium and / or magnesium impurities.

[0069] In one or more embodiments of a method for treating calcium and / or magnesium impurities, a purification and impurity removal step is provided, as shown in Figure 5, for selectively forming and precipitating calcium and / or magnesium fluoride compounds, where the raw material solution is mixed with a fluoride solution under acidic and / or basic conditions in a precipitation reactor to form a purified leachate (e.g., purified solution) and a precipitated CaF2 and / or MgF2 cake.

[0070] In one or more embodiments of the processing method, the method comprises pre-leaching a raw material containing calcium and / or magnesium impurities, and the processing method shown in Figure 9 is provided, where the raw material is an intermediate raw material comprising a mixed hydroxide precipitate; the raw material is pre-leached to remove a first portion of calcium and / or magnesium impurities to form a pre-leached raw material; the pre-leached raw material is then leached and subjected to a component removal step, the component removal step comprising an impurity removal step and a solvent extraction step, for example a Co solvent extraction step, to remove a second portion of calcium and / or magnesium impurities; and non-crystalline metal sulfur A purified leachate containing the salt is introduced into a crystallizer, and metal sulfates such as nickel sulfate are crystallized; the mother liquor is released from the crystallizer, basicized to form Ni, Mn and / or Co hydroxides, which are used as neutralizing agents upstream or downstream of the crystallizer for further processing; a purification and de-impurity step to selectively extract calcium and / or magnesium impurities is further accompanied by a scrubbing step to remove the extracted second portion of calcium and / or magnesium impurities and a stripping step to isolate desired materials such as cobalt sulfate, which can be further crystallized later.

[0071] For example, a Co solvent extraction (SX) step may involve using a solvent extraction (SX) reagent to extract cobalt, such as Cyanex 272® or an equivalent; and loading the SX reagent with calcium and / or magnesium impurities, as well as cobalt, so that the pH is raised to about 5–5.5. In some cases, a smaller proportion, such as nickel (e.g., about 10%), may also be loaded into the reagent. As part of the SX, calcium and / or magnesium and possibly nickel may be scrubbed from the SX reagent in a scrubbing step (e.g., the pH may be lower than in the extraction step), for example, using a cobalt sulfate solution as a scrubbing solution which may or may not be slightly acidified. The scrubbing step may remove most, if not all, of the calcium and / or magnesium and possibly nickel, so that the aqueous liquid exiting the scrubbing step contains the scrubbed calcium and / or magnesium and possibly nickel, as well as any remaining cobalt from the scrubbing solution. This liquid may be sent to a nickel / cobalt recovery process, where nickel and cobalt can be precipitated and separated from calcium and / or magnesium and returned to the process circuit. The calcium and / or magnesium in this liquid may then be sent to a separate recovery process. The cobalt extracted into the SX reagent may be stripped from the reagent using a dilute acid, such as sulfuric acid, at a pH of approximately 3–3.5. The cobalt thus stripped is substantially free of calcium and / or magnesium and may be suitable for further purification before crystallization as cobalt sulfate.

[0072] In one or more embodiments of the method for treating calcium and / or magnesium impurities, the metal sulfate includes any combination of nickel sulfate, manganese sulfate, and / or cobalt sulfate. In one or more embodiments of the method, crystallizing the amorphous metal sulfate includes selectively crystallizing one or two of nickel sulfate, manganese sulfate, and cobalt sulfate from a leaching solution. In one or more embodiments of the method, crystallizing the amorphous metal sulfate includes selectively crystallizing any combination of nickel sulfate, manganese sulfate, and cobalt sulfate from a leaching solution. In one or more embodiments of the method, the crystallized metal sulfate is a battery-grade crystallized metal sulfate or an electroplating-grade crystallized metal sulfate.

[0073] In one or more embodiments of a method for treating calcium and / or magnesium impurities, a pre-leaching process, precipitation of calcium and / or magnesium fluoride compounds, and / or selective solvent extraction of calcium and / or magnesium impurities reduces or eliminates the level of calcium and / or magnesium impurities in the leaching solution containing amorphous metal sulfates, thereby increasing the single-stage product yield when the leaching solution is introduced into a crystallizer compared to cases where the pre-leaching process, precipitation of calcium and / or magnesium fluoride compounds, and / or selective solvent extraction of calcium and / or magnesium impurities are not performed. In one or more embodiments of the method for treating calcium and / or magnesium impurities, a pre-leaching process, precipitation of calcium and / or magnesium fluoride compounds, and / or selective solvent extraction of calcium and / or magnesium impurities reduces or eliminates the level of calcium and / or magnesium impurities in the leaching solution containing amorphous metal sulfates, thereby reducing the crystallization release rate when the leaching solution is introduced into a crystallizer compared to cases where the pre-leaching process, precipitation of calcium and / or magnesium fluoride compounds, and / or selective solvent extraction of calcium and / or magnesium impurities are not performed. In one or more embodiments, there is an increase in single-stage product yield or a decrease in crystallization release rate, and a reduction in CAPEX and OPEX costs. In one or more embodiments of the method, a pre-leaching process, precipitation of calcium and / or magnesium fluoride compounds, and / or selective solvent extraction of calcium and / or magnesium impurities reduces or eliminates the level of calcium and / or magnesium impurities in the leaching solution containing amorphous metal sulfates, thereby providing crystallized metal sulfates that meet the purity requirements for calcium and / or magnesium impurities.

[0074] Processing method for raw materials containing lithium impurities In one or more embodiments of this disclosure, a method for crystallizing a metal sulfate, This involves pre-treating raw materials containing lithium impurities, Pre-leaching of raw materials in the presence of an extractant, Selective extraction of the first portion of lithium impurities from the raw material, and Forming pre-leached raw materials This includes pre-processing; The process involves purifying the pre-leached raw material and forming an leaching solution containing amorphous metal sulfates; The process involves crystallizing amorphous metal sulfates from the leachate and forming crystalline metal sulfates in the mother liquor containing the remaining amorphous metal sulfates; To separate crystalline metal sulfates from the mother liquor; This involves basicizing a portion of the mother liquor and converting the remaining amorphous metal sulfates into basic metal salts; Using a basic metal salt upstream of the crystallization of metal sulfates A processing method including this is provided.

[0075] In one or more embodiments of this disclosure, a method for crystallizing a metal sulfate, Pretreatment of a raw material containing lithium impurities, comprising pre-leaching the raw material in the presence of a leaching agent, selectively extracting a first portion of the lithium impurities from the raw material, and forming a pre-leached raw material; The process involves purifying the pre-leached raw material and forming an leaching solution containing amorphous metal sulfates; Crystallization of amorphous metal sulfates from the leaching solution to form crystalline metal sulfates. A processing method including this is provided.

[0076] In one or more embodiments of the present disclosure, a processing method is provided in which the leaching solution containing an amorphous metal sulfate further contains a second portion of lithium impurities from the raw material, and the purification includes selectively extracting at least the second portion of lithium impurities by direct lithium extraction.

[0077] In one or more embodiments of this disclosure, a method for crystallizing a metal sulfate, The process involves leaching out a raw material containing lithium impurities and forming a leaching solution containing amorphous metal sulfates and lithium impurities; Purifying the aforementioned leachate, Selective extraction of some lithium impurities by direct lithium extraction. Including purification; The process involves crystallizing amorphous metal sulfates from the leachate and forming crystalline metal sulfates in the mother liquor containing the remaining amorphous metal sulfates; To separate crystalline metal sulfates from the mother liquor; This involves basicizing a portion of the mother liquor and converting the remaining amorphous metal sulfates into basic metal salts; Using a basic metal salt upstream of the crystallization of metal sulfates A processing method including this is provided.

[0078] In one or more embodiments of this disclosure, a method for crystallizing a metal sulfate, The process involves leaching out a raw material containing lithium impurities and forming a leaching solution containing amorphous metal sulfates and lithium impurities; Purifying the aforementioned leachate, Selective extraction of some lithium impurities by direct lithium extraction. Including purification; Crystallization of amorphous metal sulfates from the leaching solution to form crystalline metal sulfates. A processing method including this is provided.

[0079] In one or more embodiments of the treatment method for lithium impurities, the raw material includes battery raw material. In one or more embodiments, the raw material includes recycled battery raw material. In one or more embodiments, the raw material includes black lumps raw material from batteries. In one or more embodiments, any one of the battery raw materials includes, in addition to impurities such as lithium, a metal desirable in the manufacture of battery materials such as cobalt, manganese and / or nickel.

[0080] In one or more embodiments of the processing method, the method comprises pre-treating a raw material containing lithium impurities, the pre-treating comprising pre-leaching the raw material in the presence of a leaching agent, selectively extracting a first portion of the lithium impurities from the raw material, and forming a pre-leached raw material. In one or more embodiments, the leaching agent comprises an aqueous solution, an aqueous solution containing an oxidizing agent, an acidic aqueous solution, or an acidic aqueous solution containing an oxidizing agent. In one or more embodiments, the leaching agent is formed by adding an acid to the raw material in water with or without an oxidizing agent until the pH is in the range of about 5 to about 9, or about 5 to about 8, or about 5 to about 7, or about 6 to about 7. In one or more embodiments, the acid is sulfuric acid. In one or more embodiments, the oxidizing agent is sodium persulfate, ozone, or sodium hypochlorite. In one or more embodiments, the oxidizing agent is added in an amount of <1 mole of oxidizing agent per mole of a metal desired in the production of battery materials such as cobalt, manganese, and / or nickel. In one or more embodiments, the oxidizing agent is added in an amount of about 0.5 moles per mole of cobalt, manganese, and / or nickel; or in an amount of about 0.3 moles per mole of cobalt, manganese, and / or nickel.

[0081] In one or more embodiments of the processing method, the method comprises pre-leaching a raw material containing lithium impurities, the pre-leaching being carried out at a pH of about 5 to about 9, or about 5 to about 8, or about 5 to about 7; or at any pH of about 5 to about 9; or at any range of pH of about 5 to about 9. In one or more embodiments, the pH of the pre-leaching may be maintained by adding further acid during the process. In one or more embodiments, the pre-leaching is carried out at a temperature of approximately ambient temperature to about 100°C, or about 60°C to about 100°C, or about 80°C to about 100°C, or about 80°C to about 95°C; or at any temperature of approximately ambient temperature to about 100°C; or at any range of temperature of approximately ambient temperature to about 100°C.

[0082] In one or more embodiments of the processing method, the method comprises pre-treating a raw material containing lithium impurities, the pre-treatment being carried out as a single-stage pre-leaching process. In one or more embodiments, the single-stage pre-leaching process comprises adding an acid to the raw material in water with or without an oxidizing agent to form an acidic aqueous leaching agent; pre-leaching the raw material at a suitable temperature (e.g., approximately ambient temperature to about 100°C) and a suitable pH (about 5 to about 9); forming a solution containing the pre-leached raw material and a first portion of the lithium impurities; filtering and separating the pre-leached raw material from the impurity-containing solution; and washing the pre-leached raw material.

[0083] In one or more embodiments of the processing method, the method includes pre-treating a raw material containing lithium impurities, the pre-treatment being carried out as a multi-stage pre-leaching process. In one or more embodiments, the multi-stage pre-leaching process includes a series of single-stage pre-leaching processes, each single-stage process including the steps of forming a leaching agent, pre-leaching the raw material, forming a solution containing the pre-leached raw material and a first portion of the lithium impurities, and filtering and washing the pre-leached raw material, wherein the pre-leached raw material from one single-stage process is supplied to the next single-stage process. In one or more embodiments, the multi-stage pre-leaching process includes two or three single-stage processes. In one or more embodiments, the multi-stage pre-leaching process is carried out in parallel flow, which involves bringing the raw material and leaching into contact and flowing in the same direction. In one or more embodiments, the multi-stage pre-leaching process is carried out in counterflow flow, which involves bringing the raw material and leaching into contact and flowing in opposite directions.

[0084] In one or more embodiments of the processing method, the method comprises pre-leaching a raw material containing lithium impurities, wherein a solution containing a first portion of the lithium impurities is formed so that the lithium impurities are extracted from the raw material and dissolved in an aqueous leaching solution with or without an oxidizing agent, or in an acidic aqueous solution with or without an oxidizing agent during pre-leaching. In one or more embodiments, the pH and temperature of the single-stage or multi-stage pre-leaching process are selected to selectively extract the lithium impurities in the pre-leached raw material while leaving at least a majority of materials desirable for the manufacture of batteries, such as metallic cobalt, manganese, and / or nickel. In one or more embodiments of the method, selective extraction of a first portion of lithium impurities removes the applicable portion of the impurities from the raw material, thereby forming a cleaner / purer pre-leached raw material that can be subsequently used in the manufacture of battery materials, such as crystalline metal sulfates, that meet purity requirements. In one or more embodiments of the method, selective extraction of a first portion of lithium impurities from the raw material includes selective extraction of about 20% to about 70%, or about 30% to about 70%, or about 40% to about 70%, or about 50% to about 70%, or about 60% to about 70% of the lithium impurities in the raw material. In one or more embodiments, selective extraction of a first portion of lithium impurities includes selective extraction of about 20% to about 30% of the lithium impurities in the raw material when the leaching agent is an acidic aqueous solution. In one or more embodiments, selective extraction of a first portion of lithium impurities includes selective extraction of about 60% to about 70% of the lithium impurities in the raw material when the leaching agent is an acidic aqueous solution containing an oxidizing agent.

[0085] In one or more embodiments of the processing method, the method comprises pre-leaching a raw material containing lithium impurities, wherein small amounts of materials desirable for the manufacture of batteries, such as metallic cobalt, manganese, and / or nickel, may be extracted from the raw material during pre-leaching and dissolved in a solution containing a first portion of the lithium impurities. To recover these metals, the solution may be treated with a base such as a metal hydroxide (e.g., KOH or NaOH) to precipitate cobalt, manganese, and / or nickel as Co(OH)2, Mn(OH)2, and / or Ni(OH)2. The Co(OH)2, Mn(OH)2, and / or Ni(OH)2 can then be isolated and reintroduced into the process, while the remaining solution containing the first portion of the lithium impurities may be sent for further processing or waste disposal.

[0086] In one or more embodiments of the processing method, the method comprises pre-treating a raw material containing lithium impurities, further comprising purifying the pre-leached raw material and forming a leaching solution containing amorphous metal sulfates. In one or more embodiments, purifying the pre-leached raw material comprises leaching the pre-leached raw material under conditions that form a leaching solution containing amorphous metal sulfates. In one or more embodiments, leaching the pre-leached raw material under conditions that form a leaching solution comprises leaching under conditions that form a sulfate matrix-impregnated leaching solution (PLS). There are several leaching conditions that may be suitable for forming a leaching solution (or PLS). Based on the type or source of the raw material to be processed, a person skilled in the art will recognize which leaching conditions to select and test in order to confirm the selection and specify the particular conditions.

[0087] In one or more embodiments of a method for treating lithium impurities, the method comprises purifying a pre-leached raw material, and the purification of the pre-leached raw material after leaching may further comprise subjecting the leaching solution (or PLS) containing amorphous metal sulfates to a series of component removal steps to form a purified leaching solution containing amorphous metal sulfates. The type and amount of components removed depends at least in part on the type of raw material from which the leaching solution is formed. When manufacturing materials for battery manufacturing, such as producing crystalline metal sulfates, there are specific product specifications (e.g., limitations) on such components that are permissible; any such components present in the process raw materials, water, or reagents in amounts exceeding the said product specifications will need to have their concentrations reduced. Examples of components to be removed include, but are not limited to, sodium (Na), aluminum (Al), iron (Fe), copper (Cu), zinc (Zn), cobalt (Co), nickel (Ni), or manganese (Mn). There are many preferred methods for removing components from the leaching solution (or PLS). Such methods include, but are not limited to, precipitation, atmospheric pressure leaching or pressurized leaching, sulfidation, solvent extraction, ion exchange, and cementation. The selection of an appropriate method (and its operating conditions) depends at least in part on the type and amount of components to be removed and the specifications of the final product (e.g., crystalline metal sulfates) produced by the process. For example, a leached solution may be subjected to a series of component removal steps to remove components such as Cu (e.g., by solvent extraction, cementation, ion exchange, etc.), Fe and Al (e.g., by precipitation, etc.), and Zn (e.g., by solvent extraction, ion exchange, etc.).

[0088] In one or more embodiments of the processing method, the method comprises pre-treating a raw material containing lithium impurities, and pre-treating the raw material does not require the removal of most or all of the lithium impurities; therefore, the leaching solution containing amorphous metal sulfates may further contain a second portion of the lithium impurities from the raw material. Accordingly, in one or more embodiments of the method, purifying the pre-leached raw material further comprises subjecting the leaching solution containing amorphous metal sulfates to a purification and impurity removal step to remove at least a portion of the remaining lithium impurities. In one or more embodiments, the purification and impurity removal step comprises selectively extracting a second portion of the lithium impurities by direct lithium extraction.

[0089] In general, direct lithium extraction (DLE) is considered a type of recovery technique in which lithium is removed from brine or aqueous solution to produce a higher purity lithium concentrate for purification into, for example, battery-quality lithium chemical products. DLE generally depends on the chemical or physical selective characteristics of the material for removing lithium from brine while leaving other salts in the starting solution. In one or more embodiments of a method for treating lithium impurities, the method comprises purifying a pre-leached raw material, and the direct lithium extraction (DLE) comprises a selective extraction technique in which lithium impurities are removed from the leaching solution while leaving at least a majority of the material desirable for the manufacture of batteries, such as metallic cobalt, manganese, and / or nickel. In one or more embodiments, direct lithium extraction comprises selectively extracting lithium impurities using an ion exchange medium, an organic extractant, a membrane, or a combination thereof. In one or more embodiments, the ion exchange medium comprises a layered lithium aluminate adsorbent. In one or more embodiments, the layered lithium aluminate adsorbent selectively extracts lithium impurities under pH neutral or weakly acidic conditions. In one or more embodiments, the organic extractant selectively extracts lithium impurities from the leachate at a higher temperature and precipitates the lithium impurities at a lower temperature.

[0090] In one or more embodiments of a method for treating lithium impurities, the method comprises purifying a pre-leached raw material, and the purification, impurity removal step of direct lithium extraction removes from the raw material at least a portion, if not most, of the lithium impurities (i.e., the second portion of lithium impurities) that may remain in the pre-leached raw material after pretreatment and subsequently extracted into a leaching solution containing amorphous metal sulfates. In one or more embodiments of the method, selective removal of at least the second portion of lithium impurities removes the corresponding portion of the impurities from the leaching solution that originally originated from the raw material, thereby forming a cleaner / pureer leaching solution that can be subsequently used in the manufacture of battery materials, such as crystalline metal sulfates, that meets purity requirements. In one or more embodiments, selective removal of the second portion of lithium impurities includes selectively removing about 50% to about 99%, or about 60% to about 99%, or about 70% to about 99%, or about 80% to about 99%, of the lithium impurities in the leaching solution that originally originated from the raw material and remained in the pre-leached raw material.

[0091] In one or more embodiments of the method for treating lithium impurities, the method comprises purifying a pre-leached raw material, wherein the lithium impurities are selectively extracted from the leaching solution by direct lithium extraction, which can then be sent downstream for further processing or waste disposal. After the removal of lithium impurities, the leaching solution containing amorphous metal sulfates can continue to be processed. In one or more embodiments of the method, direct lithium extraction is performed before the purification and component removal steps. In one or more embodiments of the method, direct lithium extraction is performed after the purification and component removal steps.

[0092] In one or more embodiments of the processing method, the method includes leaching a raw material containing lithium impurities to form a leaching solution containing amorphous metal sulfates and lithium impurities. In one or more embodiments of the method, leaching the raw material includes leaching under conditions that form a leaching solution containing amorphous metal sulfates and lithium impurities. In one or more embodiments, leaching the raw material under conditions that form a leaching solution includes leaching under conditions that form a sulfate matrix-impregnated leaching solution (PLS). There are several leaching conditions that may be suitable for forming a leaching solution (or PLS). Based on the type or source of the raw material to be processed, a person skilled in the art will know which leaching conditions to select and test in order to confirm the selection and specify the particular conditions.

[0093] In one or more embodiments of the processing method, the method comprises leaching a raw material containing lithium impurities, and the method further comprises purifying the leaching solution containing amorphous metal sulfates and lithium impurities. In one or more embodiments of the method, the purification of the leaching solution may comprise subjecting the leaching solution (or PLS) containing amorphous metal sulfates and lithium impurities to a series of component removal steps to form a purified leaching solution. The type and amount of components removed depends at least in part on the type of raw material from which the leaching solution is formed. When manufacturing materials for battery manufacturing, such as producing crystalline metal sulfates, there are specific product specifications (e.g., limitations) on such components that are permissible; any such components present in the process raw materials, water, or reagents in amounts exceeding the said product specifications will need to have their concentrations reduced. Examples of components to be removed include, but are not limited to, sodium (Na), aluminum (Al), iron (Fe), copper (Cu), zinc (Zn), cobalt (Co), nickel (Ni), or manganese (Mn). There are many preferred methods for removing components from the leaching solution (or PLS). Such methods include, but are not limited to, precipitation, atmospheric pressure leaching or pressurized leaching, sulfidation, solvent extraction, ion exchange, and cementation. The selection of an appropriate method (and its operating conditions) depends at least in part on the type and amount of components to be removed and the specifications of the final product (e.g., crystalline metal sulfates) produced by the process. For example, a leached solution may be subjected to a series of component removal steps to remove components such as Cu (e.g., by solvent extraction, cementation, ion exchange, etc.), Fe and Al (e.g., by precipitation, etc.), and Zn (e.g., by solvent extraction, ion exchange, etc.).

[0094] In one or more embodiments of the processing method, the method comprises purifying a leaching solution containing amorphous metal sulfates and lithium impurities, further comprising subjecting the leaching solution containing amorphous metal sulfates and lithium impurities to a purification and impurity removal step to remove at least a portion of the lithium impurities. In one or more embodiments, the purification and impurity removal step comprises selectively extracting a portion of the lithium impurities by direct lithium extraction.

[0095] In one or more embodiments of the processing method, the method comprises purifying a leachate containing amorphous metal sulfates and lithium impurities, wherein direct lithium extraction (DLE) includes a selective extraction technique in which lithium impurities are removed from the leachate while leaving at least a large portion of the material desirable for the manufacture of batteries, such as metallic cobalt, manganese, and / or nickel. In one or more embodiments, direct lithium extraction comprises selectively extracting lithium impurities using an ion exchange medium, an organic extractant, a membrane, or a combination thereof. In one or more embodiments, the ion exchange medium comprises a layered lithium aluminate adsorbent. In one or more embodiments, the layered lithium aluminate adsorbent selectively extracts lithium impurities under pH neutral or weakly acidic conditions. In one or more embodiments, the organic extractant selectively extracts lithium impurities from the leachate at a higher temperature and releases the lithium impurities at a lower temperature.

[0096] In one or more embodiments of the processing method, the method comprises purifying a leachate containing amorphous metal sulfates and lithium impurities, wherein the purification, impurity removal step of direct lithium extraction removes at least a portion, if not most, of the lithium impurities in the leachate containing amorphous metal sulfates and lithium impurities. In one or more embodiments of the method, selective removal of at least a portion of the lithium impurities removes the corresponding portion of the impurities from the leachate that originally originated from the raw materials, thereby forming a cleaner / pureer leachate that satisfies purity requirements and can be subsequently used in the manufacture of battery materials, such as crystalline metal sulfates. In one or more embodiments, selective removal of a portion of the lithium impurities includes selectively removing about 50% to about 99%, or about 60% to about 99%, or about 70% to about 99%, or about 80% to about 99% of the lithium impurities in the leachate that originally existed in the raw materials.

[0097] In one or more embodiments of the processing method, the method comprises purifying a leachate containing amorphous metal sulfates and lithium impurities, wherein the lithium impurities are selectively extracted from the leachate by direct lithium extraction, and then they may be sent downstream for further processing or waste disposal. After the removal of lithium impurities, the leachate containing amorphous metal sulfates may continue to be processed. In one or more embodiments of the method, direct lithium extraction is performed before the purification and component removal steps. In one or more embodiments of the method, direct lithium extraction is performed after the purification and component removal steps.

[0098] In one or more embodiments of a method for treating lithium impurities, the method further comprises crystallizing amorphous metal sulfates from a leaching solution to form crystalline metal sulfates. In one or more embodiments, crystallizing amorphous metal sulfates comprises introducing a leaching solution containing amorphous metal sulfates into a crystallizer under conditions sufficient to selectively crystallize the amorphous metal sulfates. In one or more embodiments, selective crystallizing amorphous metal sulfates may involve selectively crystallizing one or a combination of NiSO4, CoSO4 and / or MnSO4 from a solution (for example, in a forced-circulation crystallizer under reduced pressure, depending on the feed material, such as for manganese) to produce crystalline metal sulfates in the mother liquor. These crystalline metal sulfates can then be discharged from the crystallizer to isolate them from the mother liquor. If one crystallization cycle (e.g., using one crystallizer) is insufficient to produce the crystallized metal sulfate (e.g., this may occur with more contaminated feed material), the crystals discharged from the crystallizer may be dissolved in pure water and then introduced into a second crystallization cycle (e.g., using a second crystallizer) for recrystallization.

[0099] Various types of crystallizers may be suitable for influencing the selective crystallization of amorphous metal sulfates from leaching solutions. Such crystallizers include, but are not limited to, evaporative crystallizers, forced-circulation (FC) crystallizers, indirect forced-circulation (IFC) crystallizers, and draft-tube baffle (DTB) crystallizers. The conditions and operating parameters for such crystallizers may be selected depending on the type and purity of the metal sulfate to be crystallized and / or the type and concentration of impurities in the leaching solution. For example, the release of mother liquor from the crystallizer during crystallization and the rate at which the release occurs may affect the purity of the crystallized metal sulfate, for example, by selectively inhibiting the crystallization of impurities. Selecting a release rate to selectively inhibit the crystallization of a particular impurity means setting the crystallizer release rate within a range of possible release rates that inhibit the crystallization of a specific impurity rather than inhibiting the crystallization of different impurities. The release rate may be selected to maximize the inhibition of the crystallization of a particular impurity. Impurities may include sodium, potassium, etc. Using a higher release rate of the mother liquor helps maintain lower concentrations of impurities and other components in the mother liquor that may affect the purity of the crystallized metal sulfate. Furthermore, the solubility of impurities can be temperature-dependent; therefore, selecting the crystallizer temperature and crystallizer release rate can be effective in controlling the purity of the crystallized metal sulfate. The solubility of impurities may also depend on the amount of free water present in the leaching solution and / or mother liquor; controlling the level of water in the crystallizer can be an effective means of controlling the purity of the crystallized metal sulfate. For example, in some cases, the metal sulfate crystallizes from the solution as a metal sulfate hydrate (i.e., the crystallized metal sulfate and water molecules combine in distinct ratios as essential parts of the crystal), which reduces the concentration of water in the mother liquor. By reducing the concentration of free water, the concentration of impurities in the mother liquor (e.g., sodium, potassium, etc.) can also increase to the point where they crystallize from the solution and affect the purity of the crystallized metal sulfate.However, when a sufficient amount of water is in the leaching solution and / or the crystallization apparatus, when added to the mother liquor, or when the corresponding amount of excess water remains in the leaching solution after upstream treatment (e.g., at least as much water as is expected to be lost by hydrate formation), the presence of the corresponding free water can inhibit the crystallization of impurities from the solution.

[0100] After crystallization, the mother liquor may still contain unwanted salts / metals (e.g., Li2SO4, Mg, Na, etc.) and residual non-crystallized metal sulfates. To selectively recover the residual non-crystallized metal sulfates from the remaining unwanted materials in the solution, the mother liquor is "discharged" from the crystallization apparatus and basified so that the non-crystallized metal sulfates are converted to insoluble basic metal salts (e.g., metal hydroxides such as Ni(OH)2, Co(OH)2, Mn(OH)2, etc.). The resulting basic metal salt (e.g., metal hydroxide) precipitates from the mother liquor and can be isolated from the mother liquor by filtration. For example, the basic metal salt can be recovered by filtration, concentration, and filtration or centrifugation. The resulting precipitated metal hydroxide can be washed or repulped to form a slurry, but is then used upstream to neutralize the acid introduced in the leaching and / or component removal stages of the process, thereby converting the metal hydroxide back to the non-crystallized metal sulfate, which can then be isolated by downstream crystallization. Using a basic metal salt (e.g., metal hydroxide) as a neutralizing agent reduces and / or eliminates the need to introduce an external neutralizing agent; this reduces the use (and associated costs) of reagents and may require a higher crystallization apparatus discharge rate to avoid co-precipitation of impurities and contamination of the crystallized metal sulfate, which can affect the purity of the product, and a further source of impurities (e.g., cations Na + 、K + 、Li + 、Ca 2+ 、Mg 2+) is reduced and / or eliminated. In some cases, to ensure that there is a sufficient amount of basic metal salt, e.g., metal hydroxide available for use as a neutralizing agent, the rate at which the mother liquor is released from the crystallizer and basicized to form metal hydroxide can be controlled so that the amount of metal hydroxide formed is at least approximately equal to or approximately equal to the amount of acid introduced in the leaching and / or purification steps. Furthermore, using a basic metal salt (e.g., metal hydroxide) as a neutralizing agent converts the basic metal salt back into metal sulfate in the leaching solution. The leaching solution containing the converted metal sulfate then proceeds to the crystallizer, where the converted metal sulfate can be crystallized and isolated from the mother liquor. This loop of isolating and basicizing the mother liquor to convert the amorphous metal sulfate in the solution into basic metal salts, and then using those basic metal salts as neutralizing agents to convert the basic metal salts back into metal sulfate that can later be isolated by crystallization, can improve the yield of isolated crystallized metal sulfate obtained from specific raw materials.

[0101] In one or more embodiments of a method for treating lithium impurities, crystallizing amorphous metal sulfates includes: crystallizing metal sulfates from a leaching solution to form crystalline metal sulfates in a mother liquor containing residual amorphous metal sulfates; separating the crystalline metal sulfates from the mother liquor; basicizing a portion of the mother liquor to convert the residual amorphous metal sulfates into basic metal salts; and using a basic metal salt upstream of the crystallization of metal sulfates. In one or more embodiments, using a basic metal salt upstream includes converting the basic metal salt back to amorphous metal sulfates. In one or more embodiments, converting the basic metal salt back to amorphous metal sulfates includes using a basic metal salt to neutralize an acid upstream of the crystallization of metal sulfates. In one or more embodiments, the basic metal salt includes a metal hydroxide. In one or more embodiments, the metal hydroxide includes one or a combination of nickel hydroxide, cobalt hydroxide, or manganese hydroxide.

[0102] In one or more embodiments of the processing method, the method comprises pre-leaching a raw material containing lithium impurities, and the processing method shown in Figure 6 is provided, where the raw material is a black lump raw material; the raw material is pre-leached to remove a first portion of the lithium impurities to form a solution containing the pre-leached raw material and the lithium impurities; the impurity-containing solution is basicized to precipitate nickel, manganese and / or cobalt hydroxide (i.e., NMC(OH)2) for use upstream of the process; the pre-leached raw material is then leached and subjected to a component removal step to form a purified leached solution containing amorphous metal sulfates; the purified leached solution is introduced into a crystallizer and the nickel, manganese and / or cobalt (NMC) sulfates are crystallized.

[0103] In one or more embodiments of the processing method, the method comprises purifying a leaching solution containing amorphous metal sulfates and lithium impurities, and the processing method shown in Figure 7 is provided, where the raw material is a black lump raw material; the raw material is leached to form a leaching solution containing amorphous metal sulfates and lithium impurities; the leaching solution is then subjected to a purification and impurity removal step with direct lithium extraction (DLE) to selectively extract some of the lithium impurities, and thereafter the leaching solution is subjected to a component removal step, and the extracted lithium impurities are sent downstream; the purified leaching solution containing amorphous metal sulfates is introduced into a crystallizer, and nickel, manganese and / or cobalt (NMC) sulfates are crystallized.

[0104] In one or more embodiments of the method for treating lithium impurities, the metal sulfate includes any combination of nickel sulfate, manganese sulfate, and / or cobalt sulfate. In one or more embodiments of the method, crystallizing the amorphous metal sulfate includes selectively crystallizing one or two of nickel sulfate, manganese sulfate, and cobalt sulfate from a leaching solution. In one or more embodiments of the method, crystallizing the amorphous metal sulfate includes selectively crystallizing any combination of nickel sulfate, manganese sulfate, and cobalt sulfate from an aqueous solution. In one or more embodiments of the method, the crystallized metal sulfate is a battery-grade crystallized metal sulfate or an electroplating-grade crystallized metal sulfate.

[0105] In one or more embodiments of the treatment method for lithium impurities, the pre-leaching process and / or direct lithium extraction reduces or eliminates the level of lithium impurities in the leaching solution containing amorphous metal sulfates, thereby increasing the single-stage product yield when the leaching solution is introduced into the crystallizer compared to when the pre-leaching process and / or direct lithium extraction is not performed. In one or more embodiments of the treatment method for lithium impurities, the pre-leaching process and / or direct lithium extraction reduces or eliminates the level of lithium impurities in the leaching solution containing amorphous metal sulfates, thereby potentially reducing the crystallizer discharge rate when the leaching solution is introduced into the crystallizer compared to when the pre-leaching process and / or direct lithium extraction is not performed. In one or more embodiments, there is an increase in single-stage product yield or a decrease in crystallizer discharge rate, resulting in a reduction in CAPEX and OPEX costs. In one or more embodiments of the method, a pre-leaching process and / or direct lithium extraction reduces or eliminates the level of lithium impurities in the leaching solution containing the amorphous metal sulfate, thereby providing a crystalline metal sulfate that satisfies the purity requirements of lithium impurities.

[0106] The embodiments described herein are intended to be illustrative only. Modifications, alterations, and variations of specific embodiments can be made by those skilled in the art. The claims should not be limited by any specific embodiment described herein, but should be construed to be consistent with the entire specification.

[0107] All publications, patents, and patent applications referenced herein represent the level of skill of a person skilled in the art to which the present invention relates, and each individual published patent or patent application is incorporated herein by reference to the same extent as each individual is specifically and individually indicated as being incorporated by reference.

[0108] Although the present invention is described in this manner, it will be apparent that it can be modified in many respects. Such modifications should not be considered departures from the spirit and scope of the invention, and all such modifications that would be apparent to those skilled in the art are intended to be included within the following claims.

Claims

1. 1. A process for crystallizing a metal sulfate, comprising the steps of: Pretreating a feedstock containing calcium and / or magnesium impurities, comprising: pre-leaching the feedstock in the presence of a leaching agent; selectively extracting a first portion of the calcium and / or magnesium impurities from the feedstock; and Forming the pre-leached feedstock and pretreating the purifying the pre-leached feedstock and forming a leach solution containing non-crystallized metal sulfates; crystallizing the non-crystallized metal sulfate from the leach solution to form a crystallized metal sulfate in a mother liquor containing the remaining non-crystallized metal sulfate; separating the crystallized metal sulfate from the mother liquor; basifying a portion of said mother liquor to convert said remaining non-crystallized metal sulfate salts to basic metal salts; using said basic metal salt upstream of the crystallization of said metal sulfate; A processing method comprising:

2. 2. The method of claim 1, wherein the first portion of the calcium and / or magnesium impurities from the feedstock comprises from about 50% to about 99% of the calcium and / or magnesium impurities in the feedstock.

3. 3. The method of claim 1 or 2, wherein the leaching agent is an acidic aqueous solution, a concentrated cobalt sulfate solution, or a combination thereof.

4. The method of claim 3 , wherein the aqueous acid solution comprises sulfuric acid.

5. The leach solution containing non-crystallized metal sulfate further comprises a second portion of the calcium and / or magnesium impurities from the feedstock, and the purifying step comprises: adding a fluoride source to the leach solution; selectively reacting the fluoride source with the second portion of the calcium and / or magnesium impurities and forming calcium and / or magnesium fluoride compounds; precipitating said calcium and / or magnesium fluoride compounds from said leach solution; The method according to any one of claims 1 to 4, comprising:

6. 6. The method of claim 5, wherein the fluoride source is hydrogen fluoride, sodium fluoride, cobalt fluoride, ammonium fluoride, or a combination thereof.

7. The method further includes removing residual fluoride sources from the leach solution, the removing comprising: selectively reacting the residual fluoride source with a calcium source and forming a calcium fluoride compound; precipitating said calcium fluoride compound from said leach solution; The method of claim 5 or 6, comprising:

8. 8. The method of claim 7, wherein the calcium source is limestone, lime, gypsum, or a combination thereof.

9. 9. The method of claim 7 or 8, further comprising removing the residual calcium source by ion exchange, solvent extraction, or a combination thereof.

10. The leach solution containing non-crystallized metal sulfate further comprises a second portion of the calcium and / or magnesium impurities from the feedstock, and the purifying step comprises: selectively solvent extracting the second portion of the calcium and / or magnesium impurities onto or into a solvent extraction reagent; scrubbing the calcium and / or magnesium impurities from the solvent extraction reagent; and / or removing said second portion of said calcium and / or magnesium impurities by ion exchange; The method according to any one of claims 1 to 4, comprising:

11. The purification step comprising: selectively solvent extracting said second portion of said calcium and / or magnesium impurities onto or into a solvent extraction reagent; scrubbing the calcium and / or magnesium impurities from the solvent extraction reagent; and / or removing said second portion of said calcium and / or magnesium impurities by ion exchange; The method according to any one of claims 5 to 9, further comprising:

12. 12. The method of any one of claims 1 to 11, wherein the second portion of calcium and / or magnesium impurities comprises from about 50% to about 99% of the calcium and / or magnesium impurities in the leach solution.

13. 1. A process for crystallizing a metal sulfate, comprising the steps of: leaching a feedstock containing calcium and / or magnesium impurities and forming a leach solution containing non-crystallized metal sulfates and said calcium and / or magnesium impurities; purifying the leach solution, adding a fluoride source to said leach solution; selectively reacting said fluoride source with a portion of said calcium and / or magnesium impurities and forming calcium and / or magnesium fluoride compounds; and precipitating said calcium and / or magnesium fluoride compounds from said leach solution; selectively solvent extracting a portion of said calcium and / or magnesium impurities onto or into a solvent extraction reagent and scrubbing said calcium and / or magnesium impurities from said solvent extraction reagent; and / or removing a portion of said calcium and / or magnesium impurities by ion exchange; and purifying the compound; crystallizing the non-crystallized metal sulfate from the leach solution to form a crystallized metal sulfate in a mother liquor containing the remaining non-crystallized metal sulfate; separating the crystallized metal sulfate from the mother liquor; basifying a portion of said mother liquor to convert said remaining non-crystallized metal sulfate salts to basic metal salts; using said basic metal salt upstream of the crystallization of said metal sulfate; A processing method comprising:

14. The purification step comprising: Selectively solvent extracting a portion of the calcium and / or magnesium impurities onto or into a solvent extraction reagent and scrubbing the calcium and / or magnesium impurities from the solvent extraction reagent; and / or removing a portion of said calcium and / or magnesium impurities by ion exchange; The method of claim 13, comprising:

15. 1. A process for crystallizing a metal sulfate, comprising the steps of: leaching a feedstock containing calcium and / or magnesium impurities and forming a leach solution containing non-crystallized metal sulfates and said calcium and / or magnesium impurities; purifying the leach solution, selectively solvent extracting a portion of said calcium and / or magnesium impurities onto or into a solvent extraction reagent and scrubbing said calcium and / or magnesium impurities from said solvent extraction reagent; and / or purifying the mixture, the purifying step comprising removing a portion of the calcium and / or magnesium impurities by ion exchange; crystallizing the non-crystallized metal sulfate from the leach solution to form a crystallized metal sulfate; A processing method comprising:

16. 16. The method of any one of claims 13 to 15, wherein the portion of calcium and / or magnesium impurities comprises from about 50% to about 99% of the calcium and / or magnesium impurities in the leach solution.

17. The method of any one of claims 13 to 16, wherein the fluoride source is hydrogen fluoride, sodium fluoride, cobalt fluoride, ammonium fluoride, or a combination thereof.

18. The method further includes removing residual fluoride sources from the leach solution, the removing comprising: selectively reacting the residual fluoride source with a calcium source and forming a calcium fluoride compound; precipitating said calcium fluoride compound from said leach solution; Including, The method according to any one of claims 13 to 17.

19. 20. The method of claim 18, wherein the calcium source is limestone, lime, gypsum, or a combination thereof.

20. 20. The method of claim 18 or 19, further comprising removing the residual calcium source by ion exchange, solvent extraction, or a combination thereof.

21. 1. A process for crystallizing a metal sulfate, comprising the steps of: Pretreating a feedstock containing lithium impurities, comprising: pre-leaching the feedstock in the presence of a leaching agent; selectively extracting a first portion of the lithium impurity from the feedstock; and Forming the pre-leached feedstock and pretreating the purifying the pre-leached feedstock and forming a leach solution containing non-crystallized metal sulfates; crystallizing the non-crystallized metal sulfate from the leach solution to form a crystallized metal sulfate in a mother liquor containing the remaining non-crystallized metal sulfate; separating the crystallized metal sulfate from the mother liquor; basifying a portion of said mother liquor to convert said remaining non-crystallized metal sulfate salts to basic metal salts; using said basic metal salt upstream of the crystallization of said metal sulfate; A processing method comprising:

22. 1. A process for crystallizing a metal sulfate, comprising the steps of: Pretreating a feedstock containing lithium impurities, comprising: pre-leaching the feedstock in the presence of a leaching agent; selectively extracting a first portion of the lithium impurity from the feedstock; and Forming the pre-leached feedstock and pretreating the purifying the pre-leached feedstock and forming a leach solution containing non-crystallized metal sulfates; crystallizing the non-crystallized metal sulfate from the leach solution to form a crystallized metal sulfate; A processing method comprising:

23. crystallizing the non-crystallized metal sulfate from the leach solution to form a crystallized metal sulfate; crystallizing the non-crystallized metal sulfate from the leach solution to form a crystallized metal sulfate in a mother liquor containing the non-crystallized metal sulfate; separating the crystallized metal sulfate from the mother liquor; basifying a portion of said mother liquor to convert said remaining non-crystallized metal sulfate salts to basic metal salts; using said basic metal salt upstream of the crystallization of said metal sulfate; 23. The method of claim 22, comprising:

24. 24. The method of any one of claims 21 to 23, wherein the first portion of lithium impurities comprises about 20% to about 70% of the lithium impurities in the feedstock.

25. The method according to any one of claims 21 to 24, wherein the leaching agent is water, an aqueous solution, an aqueous solution containing an oxidizing agent, an acidic aqueous solution or an acidic aqueous solution containing an oxidizing agent.

26. 26. The method of claim 25, wherein the aqueous acid solution comprises sulfuric acid.

27. 27. The method of claim 25 or 26, wherein the oxidizing agent comprises sodium persulfate, ozone or sodium hypochlorite.

28. The leach solution containing non-crystallized metal sulfate further comprises a second portion of the lithium impurities from the feedstock, and the purifying step comprises: selectively extracting said second portion of said lithium impurities by direct lithium extraction. The method according to any one of claims 21 to 27, comprising:

29. 30. The method of claim 28, wherein the second portion of the lithium impurities comprises about 50% to about 99% of the lithium impurities in the leach solution.

30. 30. The method of claim 28 or 29, wherein direct lithium extraction comprises selectively extracting the lithium impurity using an ion exchange medium, an organic extractant, or a membrane.

31. 31. The method of claim 30, wherein the ion exchange medium comprises a layered lithium aluminate adsorbent.

32. 1. A process for crystallizing a metal sulfate, comprising the steps of: leaching a feedstock containing lithium impurities and forming a leach solution containing non-crystallized metal sulfate and the lithium impurities; purifying the leach solution, Selectively extracting a portion of the lithium impurities by direct lithium extraction. and purifying the compound; crystallizing the non-crystallized metal sulfate from the leach solution to form a crystallized metal sulfate in a mother liquor containing the remaining non-crystallized metal sulfate; separating the crystallized metal sulfate from the mother liquor; basifying a portion of said mother liquor to convert said remaining non-crystallized metal sulfate salts to basic metal salts; using said basic metal salt upstream of the crystallization of said metal sulfate; A processing method comprising:

33. 33. The method of claim 32, wherein the portion of the lithium impurities comprises about 50% to about 99% of the lithium impurities in the leach solution.

34. 34. The method of claim 32 or 33, wherein direct lithium extraction comprises selectively extracting the lithium impurity using an ion exchange medium, an organic extractant, or a membrane.

35. 35. The method of claim 34, wherein the ion exchange medium comprises a layered lithium aluminate adsorbent.

36. 36. The method of any one of claims 1 to 35, wherein using the basic metal salt upstream comprises converting the basic metal salt back to the residual non-crystallized metal sulfate.

37. 37. The method of claim 36, wherein converting the basic metal salt back to the residual non-crystallized metal sulfate comprises using the basic metal salt as a neutralizing agent to neutralize acid upstream of crystallization of the metal sulfate.

38. basifying a portion of the mother liquor to convert the remaining non-crystallized metal sulfate to the basic metal salt; releasing said mother liquor and controlling the rate of release to produce an amount of said basic metal salt that is at least approximately equal to the amount of acid neutralized upstream of the crystallization of said metal sulfate salt. The method of any one of claims 1 to 37, further comprising:

39. 39. The method of any one of claims 1 to 38, further comprising crystallizing the remaining non-crystallized metal sulfate.

40. 40. The method of any one of claims 1 to 39, wherein crystallizing the metal sulfate further comprises controlling a discharge rate from a crystallizer to selectively inhibit crystallization of impurities when discharging the mother liquor and crystallizing the metal sulfate.

41. 41. The method of any one of claims 1 to 40, wherein crystallizing the metal sulfate further comprises controlling the amount of free water in the crystallizer by one or more of controlling the rate of water evaporation from a crystallizer and controlling the addition of water to the crystallizer so as to selectively inhibit crystallization of impurities when crystallizing the metal sulfate.

42. 42. The method of claim 40 or 41, wherein the impurities include sodium or potassium.

43. 43. The method of any one of claims 1 to 42, wherein the metal sulfate comprises nickel sulfate, cobalt sulfate or manganese sulfate.

44. 44. The method of any one of claims 1 to 43, wherein the basic metal salt comprises a basic nickel salt, a basic cobalt salt, or a basic manganese salt.

45. The method of any one of claims 1 to 44, wherein the basic metal salt comprises a metal hydroxide.

46. 46. ​​The method of claim 45, wherein the metal hydroxide comprises nickel hydroxide, cobalt hydroxide, or manganese hydroxide.

47. A method for preparing a leached metal sulfate solution useful in the manufacture of battery materials, comprising the steps of:

1. Pre-treating an intermediate material comprising metal hydroxide and / or mixed hydroxide precipitate (MHP), said intermediate material comprising calcium and / or magnesium impurities, comprising: pre-leaching the intermediate feedstock in the presence of a leaching agent; selectively extracting a first portion of the calcium and / or magnesium impurities from the intermediate feedstock; and Forming the pre-leached feedstock and pretreating the refining the pre-leached feedstock; and forming a leach solution containing metal sulfates, the leach solution containing calcium and / or magnesium impurities in concentrations suitable to meet purity requirements for the manufacture of battery materials; The method includes:

48. A method for preparing a leached metal sulfate solution useful in the manufacture of battery materials, comprising the steps of:

1. Pre-treating an intermediate material comprising metal hydroxide and / or mixed hydroxide precipitate (MHP), said intermediate material containing calcium and / or magnesium impurities, comprising: pre-leaching the intermediate feedstock in the presence of a leaching agent; selectively extracting a first portion of the calcium and / or magnesium impurities from the intermediate feedstock; and Forming the pre-leached feedstock and pretreating the compound; refining the pre-leached feedstock to form a leach solution containing a second portion of the calcium and / or magnesium impurities; The purifying step comprises: adding a fluoride source to the leach solution, selectively reacting the fluoride source with the second portion of the calcium and / or magnesium impurities to form calcium and / or magnesium fluoride compounds, and precipitating the calcium and / or magnesium fluoride compounds from the leach solution. selectively solvent extracting said second portion of said calcium and / or magnesium impurities onto or into a solvent extraction reagent and scrubbing said calcium and / or magnesium impurities from said solvent extraction reagent; and / or removing said second portion of said calcium and / or magnesium impurities by ion exchange. and purifying the compound; forming a leach solution containing metal sulfates, the leach solution containing calcium and / or magnesium impurities in concentrations suitable to meet purity requirements for the manufacture of battery materials; The method includes:

49. The method described in claim 47 or 48, wherein the first portion of the calcium and / or magnesium impurities from the raw material comprises from about 50% to about 99% of the calcium and / or magnesium impurities in the raw material.

50. The method of any one of claims 47 to 49, wherein the leaching agent is an acidic aqueous solution, a concentrated cobalt sulfate solution, or a combination thereof.

51. The method of claim 50, wherein the acidic aqueous solution contains sulfuric acid.

52. The method of any one of claims 47 to 51, wherein the fluoride source is hydrogen fluoride, sodium fluoride, cobalt fluoride, ammonium fluoride or a combination thereof.

53. The method of claim 52, further comprising removing a residual fluoride source from the leach solution, said removing comprising: selectively reacting the residual fluoride source with a calcium source and forming a calcium fluoride compound; precipitating the calcium fluoride compound from the leach solution; 53. The method of claim 52, comprising:

54. The method of claim 53, wherein the calcium source is a calcium compound.

55. The method of claim 53 or 54, wherein the calcium source is limestone, lime, gypsum or a combination thereof.

56. The method of any one of claims 53 to 55, further comprising removing residual calcium sources by ion exchange, solvent extraction or a combination thereof.

57. A method according to any one of claims 47 to 56, wherein the second portion of the calcium and / or magnesium impurities comprises from about 50% to about 99% of the calcium and / or magnesium impurities in the leach solution.

58. The method of any one of claims 47 to 57, wherein the intermediate raw material comprises cobalt hydroxide and / or mixed hydroxide precipitate (MHP).

59. A method for preparing a leached metal sulfate solution useful in the manufacture of battery materials, comprising the steps of:

1. A feedstock comprising a battery supply, the feedstock comprising lithium impurities, the feedstock being pre-treated, pre-leaching the feedstock in the presence of a leaching agent; Selectively extracting a first portion of the lithium impurities from the feedstock. forming a pre-leached feedstock; and pretreating the refining the pre-leached feedstock; and forming a leach solution containing a metal sulfate, the leach solution having a concentration of lithium impurities suitable to meet purity requirements for the manufacture of battery materials; The method includes:

60. A method for preparing a leached metal sulfate solution useful in the manufacture of battery materials, comprising the steps of:

1. A feedstock comprising a battery supply, the feedstock comprising lithium impurities, the feedstock being pre-treated, pre-leaching the feedstock in the presence of a leaching agent; selectively extracting a first portion of the lithium impurity from the feedstock; and forming a pre-leached feedstock; and pretreating the purifying the pre-leached feedstock to form a leach solution containing a second portion of the lithium impurities; The purifying step comprises: selectively extracting said second portion of said lithium impurities by direct lithium extraction. and forming a leach solution comprising a metal sulfate, said leach solution having a concentration of lithium impurities suitable to meet purity requirements for the manufacture of battery materials; The method includes:

61. The process of claim 59 or 60, wherein the first portion of the lithium impurities comprises about 20% to about 70% of the lithium impurities in the feedstock.

62. The method of any one of claims 59 to 61, wherein the leaching agent is water, an aqueous solution, an aqueous solution containing an oxidizing agent, an acidic aqueous solution or an acidic aqueous solution containing an oxidizing agent.

63. The method of claim 62, wherein the acidic aqueous solution contains sulfuric acid.

64. The method described in claim 62 or 63, wherein the oxidizing agent includes sodium persulfate, ozone or sodium hypochlorite.

65. The method of claim 64, wherein the second portion of the lithium impurities comprises from about 50% to about 99% of the lithium impurities in the leaching solution.

66. A method described in any one of claims 59 to 65, wherein direct lithium extraction comprises selectively extracting the lithium impurity using an ion exchange medium, an organic extractant or a membrane.

67. The method of claim 66, wherein the ion exchange medium comprises a layered lithium aluminate adsorbent.

68. The method of any one of claims 59 to 67, wherein the feedstock comprises a recycled battery supply, a black mass supply, or a combination thereof.

69. The method of any one of claims 47 to 68, wherein the metal sulfate comprises nickel sulfate, cobalt sulfate or manganese sulfate.