Oilless and antirust production method of stainless steel band subjected to stress relief annealing
A technology for stress-relieving annealing and stainless steel strips is applied in the production field of oil-free and rust-proof stainless steel strips after stress-relieving annealing. Good anti-rust ability
Patent Information
- Authority / Receiving Office
- CN · China
- Current Assignee / Owner
- Publication Date
- 2014-09-17
Abstract
Description
technical field
[0001] The invention relates to a production method of a steel strip, in particular to a production method of an oil-free and rust-proof stainless steel strip after stress relief annealing. Background technique
[0002] It is known in the production industry of the stainless steel strip that in order to ensure the stable performance of the stainless steel strip and eliminate the internal stress of rolling, it is usually necessary to carry out stress relief annealing to the stainless steel strip during the production process. Stress relief annealing will destroy the passivation film on the surface of the stainless steel strip, thus making the stainless steel strip lose its antirust function. In order to regain the anti-rust function of the stainless steel strip after stress relief annealing, anti-rust treatment is required.
[0003] At present, the methods used in the industry for antirust treatment of stainless steel strips after stress relief annealing are ...
Examples
Embodiment 1
[0023] A kind of oil-free rust-proof production method of stainless steel strip after stress relief annealing of the present invention comprises the following steps:
[0024] First, roll up
[0025] Use the recoiling unit to wind the stainless steel strip after stress relief annealing onto the reel;
[0026] Next, create a
[0027] Put the stainless steel strip on the reel into the fourteen-high rolling mill for tensioning, the tension coefficient is 400N / mm 2 , at the same time, press down the squeeze roller on the rolling mill;
[0028] After that, spray
[0029] Using the spraying device, the rolling oil is directly sprayed onto the upper and lower surfaces of the stainless steel strip from four directions: up, down, front, back;
[0030] After that, carry out the spray rewinding of the tape
[0031] Start the rolling mill directly without using the work rolls on the rolling mill, so that the stainless ste...
Embodiment 2
[0037] A kind of oil-free rust-proof production method of stainless steel strip after stress relief annealing of the present invention comprises the following steps:
[0038] First, roll up
[0039] Use the recoiling unit to wind the stainless steel strip after stress relief annealing onto the reel;
[0040] Next, create a
[0041] Put the stainless steel strip on the reel into the 14-high rolling mill for tensioning, the tension coefficient is 600N / mm 2 , at the same time, press down the squeeze roller on the rolling mill;
[0042] After that, spray
[0043] Using the spraying device, the rolling oil is directly sprayed onto the upper and lower surfaces of the stainless steel strip from four directions: up, down, front, back;
[0044] After that, carry out the spray rewinding of the tape
[0045] Start the rolling mill directly without using the work rolls on the rolling mill, so that the tension of the stainless st...
Embodiment 3
[0051] A kind of oil-free rust-proof production method of stainless steel strip after stress relief annealing of the present invention comprises the following steps:
[0052] First, roll up
[0053] Use the recoiling unit to wind the stainless steel strip after stress relief annealing onto the reel;
[0054] Next, create a
[0055] Put the stainless steel strip on the reel into the 20-high rolling mill for tensioning, the tension coefficient is 500N / mm2, and at the same time, press the oil squeeze roller on the rolling mill;
[0056] After that, spray
[0057] Using the spraying device, the rolling oil is directly sprayed onto the upper and lower surfaces of the stainless steel strip from four directions: up, down, front, back;
[0058] After that, carry out the spray rewinding of the tape
[0059] Start the rolling mill directly without using the work rolls on the rolling mill, so that the stainless steel strip tensi...