Non-flammable sodium-ion batteries

By using electrolytes of NaBF4 and glycol ether solvents in sodium-ion batteries, combined with specific materials, the efficiency and stability problems of existing batteries under low and high voltage conditions are solved, and high Coulombic efficiency and long cycle life are achieved. And improve the safety of the battery.

CN110140253BInactive Publication Date: 2024-10-15NATIONAL UNIVERSITY OF SINGAPORE
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN201780080508.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2016-10-26
Filing Date
2017-10-26
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing sodium-ion battery electrolytes have stability problems under low and high voltage conditions, resulting in low Coulombic efficiency and short cycle life. At the same time, flammability also poses safety risks.

Method used

Using an electrolyte including NaBF4 and glycol ether solvent, combined with specific cathode and anode materials, a sodium-ion battery with high Coulombic efficiency and long cycle life is formed. The average voltage of the electrolyte ranges from 1.5V to 6.0V, and can be charged after 5 times. /Coulombic efficiency reaches at least 90% after discharge cycle.

Benefits of technology

High Coulombic efficiency and long cycle life under low and high voltage conditions are achieved. At the same time, due to the use of non-flammable electrolytes, the safety of the battery is improved, and energy density loss and production costs are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110140253B_ABST
    Figure CN110140253B_ABST
Patent Text Reader

Abstract

Disclosed herein is a non-flammable sodium ion battery having a cathode and an anode and using an electrolyte comprising NaBF4 and a glycol ether solvent, wherein the battery has an average voltage of from 1.5 V to 6.0 V and a coulombic efficiency of at least 90% after 5 charge / discharge cycles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the formation of non-flammable sodium-ion batteries. More specifically, the present invention relates to the use of glycol ether-based electrolytes in sodium-ion batteries. Background Art

[0002] The listing or discussion of a prior-published document in this specification should not necessarily be taken as an admission that the document is part of the prior art or is common general knowledge.

[0003] Due to the increasing demand for energy, energy generation and storage technology is an important area of ​​current scientific research. The large-scale adoption of renewable energy can help meet this high demand for energy while also reducing environmental problems associated with burning fossil fuels. However, renewable energy sources tend to generate energy when energy demand is low and / or only intermittently. Therefore, in order to make renewable energy more commercially viable, it is necessary to find ways to store renewable energy so that it can be easily obtained during periods of high demand. Large-scale electrochemical energy storage (EES) devices or grid storage batteries are the most convenient and practical tools for storing and releasing intermittent energy generated by renewable energy. The comprehensive cost of power plants and their associated storage systems may be a decisive factor in whether to choose renewable energy instead of fossil fuel plants in the short and medium term. In addition to low production costs, the most ideal performance indicators of EES batteries are long cycle life (e.g., thousands of cycles), high storage / release efficiency, and high safety. The weight and volume energy density of such batteries are only secondary factors because space and weight are not major considerations.

[0004] Sodium ion batteries (NIBs) are a very attractive option for large-scale EES applications because sodium is more than a thousand times more abundant than lithium in the earth's crust, which means that as NIBs become more and more popular, the cost of NIBs is expected to drop significantly. However, in order to minimize the raw material costs of such batteries, it is necessary to use other abundant earth element resources, such as Fe, Mn and Ti, for the cathode and anode of NIBs for gate storage batteries. If the electrode materials show air and water stability and can be formed by using environmentally safe, non-toxic and cheap chemicals and avoiding large-scale synthesis processes that require high-temperature calcination, the cost can be further reduced. In addition, it is commercially desirable that NIBs show good thermal and chemical stability at room temperature under different charge / discharge states. The above materials and manufacturing options will ultimately reduce the costs associated with NIB manufacturing, production, maintenance and management processes, which will significantly affect the cost during the life of the battery. Although these requirements are quite stringent, there are already some promising NIB electrode materials that are reported to meet most of the above requirements for gate storage batteries.

[0005] While much effort has been put into the development of electrode materials for NIBs, relatively little effort has been put into finding electrolytes for use with the electrodes. However, since the electrolyte is the interface between the electrodes and directly affects the performance and safety of the battery, it is clear that choosing a suitable electrolyte is important for making an operational NIB. As such, determining a suitable electrolyte is an integral part of developing high-performance NIBs. Some important criteria for a good electrolyte are:

[0006] (1) High electrochemical stability;

[0007] (2) High chemical stability;

[0008] (3) High ionic conductivity;

[0009] (4) Low cost; and

[0010] (5) Safe to use.

[0011] So far, organic electrolyte solutions based on carbonate solvents have been mainly used to develop NIBs. This is because these materials exhibit a large potential window, high ionic conductivity, and good temperature characteristics. Some of the more commonly used carbonate solvents are ethylene carbonate, propylene carbonate, and dimethyl carbonate. However, such solvents are not suitable for use with low voltages (less than 1 V vs Na / Na + ) anodes present a major performance limitation as they are unable to withstand voltages below 1 V vs Na / Na + , resulting in a very low Coulombic efficiency. When the promising low-voltage anode Na2Ti3O7 is used in the approach, the first cycle Coulombic efficiency is only about 33% when using these carbonate solvents. In this case, the material cost of the NIB is significantly increased because if such a low-voltage electrode is used, two or three times the amount of cathode must be consumed in the first cycle to offset this low Coulombic efficiency, increasing the cost and resulting in a significant loss of energy density.

[0012] The same research group also reported the use of NaBF4 in tetraglyme as a NIB electrolyte in a half-cell configuration (where the cathode / anode cycled as a counter electrode relative to Na metal) ((a) I.-H.Jo, et al., Mater. Res. Bull., 2014, 58, 74-77; and (b) C.Kim, et al., J. Power Sources, 2016, 317, 153-158). Those disclosures were limited to a brief discussion of the sodium storage performance of the cathode (α-NaMnO2; reference (a)) and anode (Sn; reference (b)) vs Na metal. These disclosures demonstrated that this electrolyte performs well at high voltages (up to 4.0 V vs Na / Na + ) and low voltage to 0.001V vs Na / Na + Although this electrolyte is expected to decompose completely at reduced voltages <1 V vs Na / Na + (based on glyme), but the main problem with glyme-based electrolytes is their anodic stability, as they tend to decompose at higher voltages. As expected, from a Coulombic efficiency point of view, the + The reported performance of the α-NaMnO2 cathode is unsatisfactory (showing a stable Coulombic efficiency approaching only 80% over 20 cycles in reference (a)). From a practical point of view, such efficiency is unacceptable as it would lead to full cell failure in just a few cycles, such as 5 or 10, if the Coulombic efficiency of its cathode is only 80 or 90%, respectively. In fact, the authors only demonstrated 20 cycles with this electrolyte. Thus, there is no disclosure in these articles that the use of NaBF4 in tetraglyme as a NIB electrode material at high voltages (>3 V vs Na / Na + ) provide satisfactory performance (cycle life of at least 50 or 100 cycles).

[0013] In addition, conventional carbonate-based electrolytes currently used in lithium-ion batteries (LIBs) and NIBs are highly flammable. This poses a serious safety hazard as it may cause fire or explosion. Therefore, there is still a need to utilize electrolytes that are non-flammable and compatible with both low-voltage anodes and high-voltage cathodes to obtain high-voltage NIBs (average discharge voltage at least above 1.5 V) that show good performance and high cycle life.

[0014] Therefore, there remains a need for improved electrolytes for NIBs. Summary of the invention

[0015] Surprisingly, it was found that a battery using an electrolyte comprising NaBF4 and a glycol ether solvent solves many of the problems. Accordingly, various aspects and embodiments of the present invention are provided in the following numbered clauses.

[0016] 1. Non-flammable sodium-ion batteries, including:

[0017] cathode for sodium-ion batteries;

[0018] Anodes for sodium-ion batteries;

[0019] Diaphragm; and

[0020] An electrolyte comprising a salt and a glycol ether solvent, wherein:

[0021] Salts include NaBF4;

[0022] The battery has an average voltage of from 1.5V to 6.0V; and

[0023] The coulombic efficiency is at least 90% after 5 charge / discharge cycles.

[0024] 2. A battery according to clause 1, wherein the average voltage is from 1.75 to 5.5V, such as from 2.0 to 5.0V, such as from 2.5 to 5.0V.

[0025] 3. A battery according to clause 1 or clause 2, wherein the battery has a cycle life of from 50 cycles to 50,000 charge / discharge cycles, such as from 100 to 25,000 cycles, such as from 300 to 10,000 charge / discharge cycles.

[0026] 4. A battery according to any preceding clause, wherein the battery has a coulombic efficiency of at least 95%, such as at least 97%, after 5 charge / discharge cycles.

[0027] 5. A battery according to any of the preceding clauses, wherein NaBF4 is provided at a concentration of from greater than 0 to less than or equal to 2.5 M in a glycol ether solvent, such as from 0.5 to less than or equal to 2.5 M, such as 1 M in a glycol ether solvent.

[0028] 6. A battery according to any of the preceding clauses, wherein the glycol ether solvent is selected from one or more of the group consisting of ethylene glycol dimethyl ether (monoglyme), diglyme, triglyme, tetraglyme, methyl perfluorobutyl ether (MFE) and the like.

[0029] 7. The battery according to clause 6, wherein the glycol ether solvent is tetraglyme.

[0030] 8. The battery according to any one of the preceding clauses, wherein the glycol ether solvent further comprises one or more solvents selected from the group consisting of cyclic carbonates, linear carbonates, cyclic esters, linear esters, cyclic ethers or linear ethers other than glycol ethers, nitriles, dioxolanes or their derivatives, thietanes, sulfolanes, and sultones or their derivatives.

[0031] 9. The battery according to clause 8, wherein the glycol ether solvent further comprises one or more selected from the group consisting of propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, methyl ethyl carbonate, tetrahydrofuran, sulfolane, and acetonitrile.

[0032] 10. The battery according to any one of the preceding clauses, wherein the salt further comprises one or more salts selected from the group consisting of NaCN, NaClO4, NaAsF6, NaPF6, NaPF 6-x (C n F 2n+1 ) x (1 < x < 6, n = 1 or 2), NaSCN, NaBr, NaI, Na2SO4, Na2B 10 Cl 10 , NaCl, NaF, NaPF4, NaOCN, Na(CF3SO3), NaN(CF3SO2)2, NaN(FSO2), NaN(C2F5SO2)2, NaN(CF3SO2)(C4F9SO2), NaC(CF3SO2)3, NaC(C2F5SO2)3, (CH3)4NBF4, (CH3)4NBr, (C2H5)4NClO4, (C2H5)4NI, (C3H7)4NBr, (n-C4H9)4NClO4, (n-C4H9)4NI, (C2H5)4N - maleate, (C2H5)4N - benzoate, (C2H5)4N - phthalate, sodium stearylsulfonate, sodium octylsulfonate, and sodium dodecylbenzenesulfonate.

[0033] 11. The battery according to clause 10, wherein the salt further comprises one or more salts selected from the group consisting of NaClO4, NaPF6, NaSCN, NaBr, NaI, NaCl, NaOCN, Na(CF3SO3), NaN(CF3SO2)2, and NaCN.

[0034] 12. The battery according to clause 10 or clause 11, wherein each of the one or more salts of clause 10 or clause 11, when present, is provided at a concentration greater than 0 to 2.5 M.

[0035] 13. The battery according to any one of the preceding clauses, wherein the cathode comprises one selected from the group consisting of Na a [Cu bFe c Mn d Ni e Ti f M g ]O2 (wherein: 0≤a≤1; 0≤b≤0.3; 0≤c≤0.5; 0≤d≤0.6; 0≤e≤0.3; 0≤f≤0.2; and 0≤g≤0.4, and M is selected from one or more of the group consisting of Mo, Zn, Mg, Cr, Co, Zr, Al, Ca, K, Sr, Li, H, Sn, Te, Sb, Nb, Sc, Rb, Cs and Na), M-Na2Fe2(CN)6.2H2O; R-Na2Fe2(CN)6, Na3V2(PO4)3(NVP) and Na4Mn3(PO4)2(P2O7) The active material is one or more of the group consisting of.

[0036] 14. A battery according to any of the preceding clauses, wherein the anode comprises a material selected from TiO2 or more specifically Pathway, Na2Ti6O 13 , graphite, hard carbon and sodium metal as an active material.

[0037] 15. A battery according to any of the preceding clauses, wherein the cathode and the anode comprise a member selected from the group consisting of: M-Na2Fe2(CN)6.2H2O / / TiO2, R-Na2Fe2(CN)6 / / TiO2, NVP / / TiO2, Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / Graphite, Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / Na2Ti6O 13 、Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / TiO2, Na4Mn3(PO4)2(P2O7) / / TiO2, Pathway, Na a [Cu b Fe c Mn d Nie Ti f M g ]O2 / / Hard carbon, Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / sodium metal; or more particularly Pathway; M-Na2Fe2(CN)6.2H2O / / Na2Ti6O 13 ; M-Na2Fe2(CN)6.2H2O / / graphite; M-Na2Fe2(CN)6.2H2O / / hard carbon; M-Na2Fe2(CN)6.2H2O / / sodium metal; Pathway; R-Na2Fe2(CN)6 / / Na2Ti6O 13 ; R-Na2Fe2(CN)6 / / graphite; R-Na2Fe2(CN)6 / / hard carbon; R-Na2Fe2(CN)6 / / sodium metal; Pathway: NVP / / Na2Ti6O 13 ; NVP / / graphite; NVP / / hard carbon; NVP / / sodium metal; Pathway: Na4Mn3(PO4)2(P2O7) / / Na2Ti6O 13 ; Na4Mn3(PO4)2(P2O7) / / graphite; Na4Mn3(PO4)2(P2O7) / / hard carbon; and Na4Mn3(PO4)2(P2O7) / / sodium metal, wherein (wherein: 0≤a≤1; 0≤b≤0.3; 0≤c≤0.5; 0≤d≤0.6; 0≤e≤0.3; 0≤f≤0.2; and 0≤g≤0.4, and M is selected from one or more of the group consisting of Mo, Zn, Mg, Cr, Co, Zr, Al, Ca, K, Sr, Li, H, Sn, Te, Sb, Nb, Sc, Rb, Cs and Na) a group of active material pairs.

[0038] 16. The battery according to clause 15, wherein the cathode and the anode are selected from the group consisting of: Pathway; M-Na2Fe2(CN)6.2H2O / / Na2Ti6O 13 ; M-Na2Fe2(CN)6.2H2O / / graphite; M-Na2Fe2(CN)6.2H2O / / hard carbon; M-Na2Fe2(CN)6.2H2O / / sodium metal; Pathway; R-Na2Fe2(CN)6 / / Na2Ti6O 13; R-Na2Fe2(CN)6 / / graphite; R-Na2Fe2(CN)6 / / hard carbon; R-Na2Fe2(CN)6 / / sodium metal; Pathway: NVP / / Na2Ti6O 13 ; NVP / / graphite; NVP / / hard carbon; NVP / / sodium metal; Pathway: Na4Mn3(PO4)2(P2O7) / / Na2Ti6O 13 ; Na4Mn3(PO4)2(P2O7) / / graphite; Na4Mn3(PO4)2(P2O7) / / hard carbon; and Na4Mn3(PO4)2(P2O7) / / sodium metal.

[0039] 17. A battery according to clause 15, wherein the cathode and the anode are selected from the group consisting of: M-Na2Fe2(CN)6.2H2O / / graphite, M-Na2Fe2(CN)6.2H2O / / Na2Ti6O 13 、R-Na2Fe2(CN)6 / / graphite、R-Na2Fe2(CN)6 / / Na2Ti6O 13 、NVP / / Graphite、NVP / / Na2Ti6O 13 , M-Na2Fe2(CN)6.2H2O / / TiO2, R-Na2Fe2(CN)6 / / TiO2, NVP / / TiO2, Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / Graphite, Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / Na2Ti6O 13 and Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / TiO2.

[0040] 18. A battery according to clause 17, wherein the cathode and the anode are selected from the group consisting of: M-Na2Fe2(CN)6.2H2O / / graphite, M-Na2Fe2(CN)6.2H2O / / Na2Ti6O 13、R-Na2Fe2(CN)6 / / graphite、R-Na2Fe2(CN)6 / / Na2Ti6O 13 , NVP / / graphite and NVP / / Na2Ti6O 13 .

[0041] 19. The battery according to clause 15, wherein the cathode and the anode are selected from the group consisting of: Pathway, M-Na2Fe2(CN)6.2H2O / / hard carbon, M-Na2Fe2(CN)6.2H2O / / sodium metal, Pathway, R-Na2Fe2(CN)6 / / hard carbon, R-Na2Fe2(CN)6 / / sodium metal, NVP / / Pathway, NVP / / Hard Carbon, NVP / / Sodium Metal, Pathway, Na4Mn3(PO4)2(P2O7) / / Na2Ti6O 13 Na4Mn3(PO4)2(P2O7) / / graphite, Na4Mn3(PO4)2(P2O7) / / hard carbon, Na4Mn3(PO4)2(P2O7) / / sodium metal, Na4Mn3(PO4)2(P2O7) / / TiO2, Pathway, Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / Hard Carbon and Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / Sodium metal.

[0042] 20. The battery according to clause 19, wherein the cathode and the anode are selected from the group consisting of: Pathway, M-Na2Fe2(CN)6.2H2O / / hard carbon, M-Na2Fe2(CN)6.2H2O / / sodium metal, Pathway, R-Na2Fe2(CN)6 / / hard carbon, R-Na2Fe2(CN)6 / / sodium metal, Pathway, NVP / / Hard Carbon, NVP / / Sodium Metal, Pathway, Na4Mn3(PO4)2(P2O7) / / Na2Ti6O 13Na4Mn3(PO4)2(P2O7) / / graphite, Na4Mn3(PO4)2(P2O7) / / hard carbon and Na4Mn3(PO4)2(P2O7) / / sodium metal.

[0043] 21. The battery according to any of the preceding clauses, wherein the electrolyte further comprises one or more additives selected from the group consisting of fluoroethylene carbonate (FEC), vinylene carbonate (VC), vinylethylene carbonate (VEC) and adiponitrile. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 Depicted are cyclic voltammetry curves of an aluminum working electrode versus sodium metal disk as counter and reference electrodes in 1 M NaBF4 in tetraglyme and 1 M NaClO4 in EC-PC.

[0045] Figure 2 Depicted are Na2Ti3O7 anodes in 1M NaBF4 tetraglyme and 1M NaClO4 EC-PC (for First cycle Coulombic efficiency curve of deep discharge path).

[0046] Figure 3 Depicts the Na half-cell Sodium storage performance of the sodium storage pathway anode: (a) the first galvanostatic cycle at C / 2 rate using 1 M NaBF4 tetraglyme electrolyte compared to 1 M NaClO4 EC-PC electrolyte with all other experimental conditions being the same; rate performance of this pathway at different rates using a C / 5 discharge rate, with (b) cycling curves and (c) obtained charge capacity versus cycle number; and (d) after 100 long-term cycles at C / 2 rate, showing negligible capacity loss for this pathway using the proposed electrolyte, with a stable Coulombic efficiency greater than 99%.

[0047] Figure 4 The sodium storage performance of graphite electrode relative to Na metal in 1M NaBF4 tetraethylene glycol dimethyl ether electrolyte solution is depicted: (a) cycling curves at different rates using a C / 5 discharge rate; (b) the obtained charge capacity versus cycle number (assuming the theoretical sodium storage capacity of graphite is 100 mAh / g); and (c) 100% capacity retention after 200 long-term cycles at a C / 2 rate.

[0048] Figure 5The sodium storage performance of the M-Na2Fe2(CN)6.2H2O cathode in 1M NaBF4 tetraglyme electrolyte solution is depicted: (a) cycling curves at different rates using a C / 5 charge rate; (b) the obtained discharge capacity versus cycle number; and (c) long-term cycling of the M-Na2Fe2(CN)6.2H2O cathode at 2C rate, again showing negligible capacity loss with a stable Coulombic efficiency of around 99.5%.

[0049] Figure 6 Plotted at 3.9–3.0 V vs Na / Na + Sodium storage performance of the R-Na2Fe2(CN)6 cathode in 1M NaBF4 tetraglyme electrolyte solution after 200 cycles: (a) first cycle curve; (b) tenth cycle curve at 1C rate; and (c) long-term cycling of the R-Na2Fe2(CN)6 cathode at 1C rate, showing good capacity retention after 200 cycles with a stable Coulombic efficiency of greater than 99%.

[0050] Figure 7 Depicted are representative C / 2 cycles of a full cell with graphite as anode, 1 M NaBF4 in tetraglyme as electrolyte, and (a) M-Na2Fe2(CN)6.2H2O as cathode; and (b) R-Na2Fe2(CN)6 as cathode cycled within its upper charge-discharge plateau. Figure 7 c depicts long-term cycling of these two full cells for 300 cycles, showing the efficiency of these two types of NIBs.

[0051] Figure 8 Depicted: (a) 1M NaBF4 in tetraethylene glycol dimethyl ether as the electrolyte, with the cathode cycling in its upper charge-discharge plateau Representative C / 2 cycle of a full cell; and (b) long term cycling of the full cell for 40 cycles.

[0052] Fig. 9 Depicted are: (a) Na in 1M NaBF4 tetraglyme electrolyte at C / 5 rate 0.9 [Cu 0.22 Fe 0.30 Mn 0.48 ] Cycling curve of O2 half-cell; and (b) Coulombic efficiency and discharge capacity of the half-cell within 150 cycles. Fig. 9 c depicts the Na in 1M NaBF4 tetraglyme electrolyte at C / 5 rate. 0.9 [Cu 0.12 Ni 0.10 Fe 0.30 Mn0.43 Ti 0.05 ]O2 half-cell cycle curve, and Fig. 9 d plots the Coulombic efficiency and discharge capacity of the half-cell over 50 cycles.

[0053] Fig.10 Depicted are: (a) comparison of the 1st cycle Coulombic efficiency of hard carbon half-cells in 1 M NaBF4 in tetraglyme and in 1 M NaClO4 in EC-PC at C / 20 rate; and (b) the Coulombic efficiency and charge capacity of hard carbon half-cells in the two types of electrolytes over 30 cycles.

[0054] Fig.11 Representative cycling profiles and long-term cycling stability of R-Na2Fe2(CN)6 / / hard carbon full cells using 1 M NaBF4 tetraglyme electrolyte over 100 cycles at C / 4 rate are depicted.

[0055] Fig.12 Depicted are: (a) Na at C / 8.5 rate using 1M NaBF4 in tetraglyme electrolyte 0.9 [Cu 0.12 Ni 0.10 Fe 0.30 Mn 0.43 Ti 0.05 ]Representative cycling curve of O2 / / hard carbon full cell; and (b) Coulombic efficiency and discharge capacity of the full cell in 10 cycles.

[0056] Fig.13 Depicted are flammability tests conducted in ambient air by exposing various electrolyte solutions to an open flame. The electrolyte solutions were: (a) 1M NaBF4 in tetraglyme; (b) 1M NaPF6 in commercially available EC-DMC; and (c) 0.6M NaPF6 in diglyme. Fig.13 In ac, "t = 0 s" refers to the moment when the flame first contacts the electrolyte solution. For 1M NaBF4 in tetraglyme, the flame comes from a lighter as shown. Fig.13 d depicts the DSC temperature rise curves of various electrolytes under argon atmosphere, indicating that the 1M NaBF4 tetraethylene glycol dimethyl ether electrolyte solution has excellent thermal stability. DETAILED DESCRIPTION

[0057] Surprisingly, it has been found that the use of a glycol ether-based electrolyte comprising sodium tetrafluoroborate as a salt can provide a non-flammable sodium ion battery having excellent cycling and coulombic efficiency characteristics. Thus, a non-flammable sodium ion battery is provided, comprising:

[0058] cathode for sodium-ion batteries;

[0059] Anodes for sodium-ion batteries;

[0060] Diaphragm; and

[0061] An electrolyte comprising a salt and a glycol ether solvent, wherein:

[0062] The salt includes NaBF4;

[0063] The battery has an average voltage of from 1.5V to 6.0V; and

[0064] The coulombic efficiency is at least 90% after 5 charge / discharge cycles.

[0065] In certain embodiments that may be mentioned herein, the cathode does not include α-NaMnO 2 as a positive electrode active material and / or the anode does not include a tin-based material as a negative electrode active material.

[0066] It should be appreciated that the sodium ion battery can be provided in any suitable configuration. Examples of suitable configurations include, but are not limited to, cylindrical batteries, prismatic batteries, button / coin batteries, soft pack batteries, etc.

[0067] Advantages associated with the disclosed battery are discussed below.

[0068] The batteries disclosed herein have improved safety due to the use of a thermally stable, non-flammable electrolyte (glycol ether solvent, such as tetraglyme). In contrast, current prior art lithium ion battery (LIB) and sodium ion battery (NIB) electrolytes are flammable. This is a serious safety hazard as it can lead to (and has led to) explosions. Using the specific electrolytes detailed herein, the disclosed NIBs will not catch fire even if directly exposed to an open flame. This is a significant safety advantage.

[0069] The NIBs herein can be high voltage NIBs, which is a result of the wide voltage window of the electrolyte. Due to the use of different types of cathodes and anodes operating at different potentials, the NIBs disclosed herein can have discharge platforms varying from 1.8 to 3.9 V. Such flexibility is possible here because the electrolyte is very suitable for very low voltage anodes (<1 V vs Na / Na + ) and (unexpectedly) high voltage cathodes (>3 V vs Na / Na + ) performed equally well. Most electrolytes used in sodium-ion batteries do not display such a wide voltage window.

[0070] The non-flammable electrolytes disclosed herein have excellent sodium storage properties for both NIB cathodes and anodes. In other words, the disclosed electrolytes show remarkable performance metrics in terms of efficiency, rate performance, and cycle life for low voltage anodes and (unexpectedly) for high voltage cathodes, and the resulting batteries outperform current state-of-the-art NIB electrolytes in these metrics, while being safe, non-flammable, and inexpensive.

[0071] The NIBs disclosed herein are highly efficient due to the high Coulombic efficiency of the high voltage cathode and particularly the very low voltage anode using the disclosed electrolyte. Currently used NIB electrolyte solvents (e.g., ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC)) have a high efficiency at voltages <1 V vs Na / Na + , resulting in very low first cycle Coulombic efficiency (e.g., for promising NIB anodes, This means that more than two or even almost three times the amount of cathode needs to be used in a NIB full cell using such a low voltage anode and a previous state-of-the-art electrolyte (e.g., EC:PC of NaPF6 or EC:PC of NaClO4), resulting in a significant loss in energy density. The new electrolyte proposed in this patent shows a significantly higher first cycle Coulombic efficiency (≈73% for approach) and almost 100% when a graphite anode is used.

[0072] Furthermore, it is unusual that graphite can be used as an anode because it cannot be used with conventional NIB electrolytes (e.g., EC:PC of NaPF6 or EC:DMC of NaPF6). However, using the electrolyte disclosed herein, graphite performs very well as a low-cost, low-voltage, safe, environmentally friendly, and efficient medium-to-high capacity NIB anode.

[0073] Finally, the cathode and anode active materials used herein are inexpensive and can be manufactured using water-based and scalable syntheses. In addition, the electrolytes disclosed herein actually utilize one of the cheapest salt and non-flammable solvent combinations for non-aqueous NIB electrolytes.

[0074] When used herein, "average voltage" refers to the weighted average of the voltage when the total output capacity of the full cell during the discharge cycle is considered. In fact, the average voltage can be calculated by calculating the area under the voltage-to-capacity curve of the discharge cycle (the calculated area will be the specific energy density output by the full cell), and then dividing this value by the specific capacity (specific energy density = specific capacity * average voltage). When used herein, "Coulombic efficiency" refers to the efficiency of transferring charge (electrons) in the system to promote electrochemical reactions. In the full cell configuration, the coulombic efficiency is the ratio of the discharge capacity to the charge capacity of the full cell. In the cathode half-cell configuration, the coulombic efficiency will be the ratio of the discharge to the charge capacity, and in the half-cell configuration, the coulombic efficiency of the anode will be the ratio of the charge to the discharge capacity.

[0075] As described above, the sodium ion battery (NIB) according to the present invention shows an average voltage of from 1.5V to 6.0V, and a coulombic efficiency of at least 90% after 5 charge / discharge cycles. The NIB disclosed herein may have an average voltage of from 1.75V to 6.0V, from 2.0V to 6.0V, from 2.5V to 6.0V, from 3.0V to 6.0V, from 1.5V to 5.5V, from 1.75V to 5.5V, from 2.0V to 5.5V, from 2.5V to 5.5V, from 3.0V to 5.5V, from 2.0V to 5.0V, from 1.75V to 5.0V, from 2.0V to 5.0V, from 2.5V to 5.0V, from 3.0V to 5.0V. In the same or separate embodiments, the coulombic efficiency after 5 charge / discharge cycles may be at least 95%, at least 97%, or at least 99%.

[0076] As used herein, "cycle life" refers to the number of cycles at which a battery can deliver 20% of the capacity it was able to deliver in the initial cycles.

[0077] The NIB disclosed herein may have a cycle life of from 50 cycles to 50,000 charge / discharge cycles, such as from 100 cycles to 25,000 charge / discharge cycles, such as from 300 cycles to 10,000 charge / discharge cycles. Other suitable cycle lives may be from 50 to 5,000 charge / discharge cycles, such as from 100 cycles to 4,000 charge / discharge cycles, such as from 300 cycles to 3,000 charge / discharge cycles. It should be appreciated that any low-end range value here (e.g., 50, 100, 300) can be combined with a higher range value (e.g., 3000, 4000, 5000, 10000, 25000, 50000) to provide other preferred ranges.

[0078] The cathode of the present invention may include a current collector having thereon an active material layer, the layer including at least one binder and, if necessary, a conductive material in addition to the active material.

[0079] The current collector may be any suitable conductor for the cathode, for example, aluminum (Al), stainless steel, nickel-plated steel, and / or the like.

[0080] Active materials that can be used for the cathode include but are not limited to Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 (wherein: 0≤a≤1; 0≤b≤0.3; 0≤c≤0.5; 0≤d≤0.6; 0≤e≤0.3; 0≤f≤0.2; and 0≤g≤0.4, and M is selected from one or more of the group consisting of Mo, Zn, Mg, Cr, Co, Zr, Al, Ca, K, Sr, Li, H, Sn, Te, Sb, Nb, Sc, Rb, Cs and Na), or more particularly, M-Na2Fe2(CN)6.2H2O; R-Na2Fe2(CN)6, NVP and Na4Mn3(PO4)2(P2O7). It should be appreciated that the above substances can be used alone. That is, the cathode can contain only one of the above active substances. However, it is also possible for a single cathode to contain a combination of more than one of the above substances. When the above active substances are used in combination, any suitable weight ratio can be used. For example, the weight ratio of the two active materials in a single cathode can range from 1:100 to 100:1, such as from 1:50 to 50:1, for example 1:1. In additional or alternative embodiments, the battery may include more than one cathode. When the battery includes more than one cathode (e.g., from two to 10, such as from 2 to 5 cathodes), the active material can be selected from the above materials, and each cathode can independently include only one cathode active material or a combination of two or more active materials, as described above.

[0081] For the R-Na2Fe2(CN)6 cathode active material, both its 3.9-2.0V cycle (two moles of sodium storage per mole of R-Na2Fe2(CN)6 gives a theoretical capacity of 170.85 mAh / g) and its 3.9-3.0V cycle are intended to be covered herein by reference to the active material.

[0082] When the active substance is selected from free Na a [Cu b Fe c Mn d Ni e Ti f Mg ]O2, it should be recognized that the values ​​of ag and M are selected so as to maintain charge balance. a [Cu b Fe c Mn d Ni e Ti f M g Examples of active substances of O2 include Na 0.9 [Cu 0.22 Fe 0.30 Mn 0.48 ]O2 and Na 0.9 [Cu 0.12 Ni 0.10 Fe 0.30 Mn 0.43 Ti 0.05 ]O2.

[0083] When Na3V2(PO4)3 (NVP) is used as the positive electrode active material, it can be used as undoped NVP or as doped NVP (e.g., up to 10% dopant(s)), where the dopant(s) can be selected from any suitable metal, such as one or more of the group including but not limited to Mg, Zn, Al, etc. A specific NVP that may be mentioned herein is NVP doped with Zn. It should be clearly intended that the above-mentioned undoped NVP and doped NVP can be used in any cathode and anode active material combination mentioned herein, whether or not NVP is mentioned. A specific combination of cathode and anode active materials that may be mentioned is Zn-doped NVP / / hard carbon (e.g., in a tetraglyme-based electrolyte).

[0084] The binder improves the bonding properties of the positive electrode active material particles (e.g., M-Na2Fe2(CN)6.2H2O or R-Na2Fe2(CN)6) to each other and the current collector. The binder can be a non-aqueous binder, an aqueous binder, or a combination thereof. As long as the positive electrode active material and the conductive material are bonded to the current collector and have (or both) antioxidant properties and electrolyte stability to the high potential cathode, the binder is not particularly limited.

[0085] The non-aqueous binders that may be mentioned herein include, but are not limited to, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamide, polyimide, or a combination thereof.

[0086] The aqueous binders that may be mentioned herein include, but are not limited to, rubber-based binders or polymer resin binders. The rubber-based binder may be selected from styrene-butadiene rubber, acrylated styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, and combinations thereof. The polymer resin binder may be selected from ethylene-propylene copolymer, epichlorohydrin, polyphosphazene, polyacrylonitrile, polystyrene, ethylene-propylene-diene copolymer, polyvinyl pyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, and combinations thereof.

[0087] Cellulose-based compounds can be used as binders (or used in combination with other substances). Examples of suitable cellulose-based materials include, but are not limited to, one or more of carboxymethyl cellulose, hydroxypropyl methylcellulose, methylcellulose, or their alkali metal salts. The alkali metal can be Na, K, or Li. Based on 100 parts by weight of the active substance, the amount of such cellulose-based compounds included can be from about 0.1 parts by weight to about 20 parts by weight. The specific cellulose-based binder that may be mentioned herein is the sodium salt of carboxymethyl cellulose.

[0088] The conductive substance improves the conductivity of the electrode. Any substance that can conduct electricity can be used as the conductive substance unless it causes chemical changes, and examples thereof may be natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber and / or similar carbon-based substances; copper, nickel, aluminum, silver and / or similar metal powders or metal fibers and / or similar metal-based substances; polyphenylene derivatives and / or similar conductive polymers; and / or mixtures thereof.

[0089] The cathode of the present invention can be manufactured using the following method. First, the active material (one or more), the conductive material and the binder are mixed in a desired ratio (for example, the ratio of active material (one or more): additive: binder is from 70:20:10 to 96:2:2, and the specific ratios that may be mentioned include but are not limited to 85:10:5 and 90:5:5), and dispersed in an aqueous solution and / or an organic solvent (such as N-methyl-2-pyrrolidone) to form a slurry. Additionally or alternatively, the amount of active material in the cathode can be from 70 to 96wt%, the amount of additive (such as conductive carbon) can be from 2 to 20wt%, and the amount of binder can also be from 2 to 10wt%. Subsequently, the slurry is coated on the current collector and then dried to form an active material layer. Here, the coating method is not particularly limited, and can be, for example, a knife coating method (such as a scraper coating), a concave coating method and / or a similar method. Then, the active material layer is pressed to a desired thickness using a press (such as a roller press) to manufacture an electrode. The thickness of the active material layer is not particularly limited and can be any suitable thickness applicable to a positive active material layer of a rechargeable lithium or sodium battery. The active material loading can be from 1 to 50 mg cm -2 , for example, the active substance loading can be from 5 to 40 mg cm -2 , such as from 8 to 30 mg cm -2 .

[0090] The anode can be formed in a manner similar to that described above, that is, the anode can include a negative electrode active material, and can also include a binder and a conductive additive.

[0091] The negative electrode active material layer can be any suitable negative electrode active material layer for a full battery cell (e.g., NIB). For example, the negative electrode active material may include a carbon-based material, a silicon-based material, a tin-based material, an antimony-based material, a lead-based material, a metal oxide (e.g., lithium or sodium metal oxide), a sodium metal, and / or the like, which can be used alone or as a mixture of two or more. The carbon-based material can be, for example, a soft carbon or a hard carbon or a graphite-based material, such as artificial graphite, natural graphite, a mixture of artificial graphite and natural graphite, natural graphite coated with artificial graphite, and / or the like. The silicon-based material can be, for example, silicon, silicon oxide, a silicon-containing alloy, a mixture of a graphite-based material and the above-mentioned materials, and / or the like. Silicon oxide can be SiO x(0 < x ≤ 2). The silicon-containing alloy can be an alloy that includes silicon in the maximum amount of total metal elements based on the total amount of the alloy (e.g., silicon is the metal element with the largest amount among all metal elements), for example, Si-Al-Fe alloy. The tin-based material can be, for example, tin, tin oxide, tin-containing alloy, graphite-based material, mixtures of the above materials, and / or similar materials. The same applies to antimony and lead-based materials. The lithium metal oxide can be, for example, titanium oxide compounds such as Li4Ti5O 12 、Li2Ti6O 13 or Li2Ti3O7. The sodium metal oxide can be, for example, titanium oxide compounds such as Na2Ti3O7 or Na2Ti6O 13 . Other suitable metal oxides that may be mentioned in this article include but are not limited to TiO2, Fe2O3, MoO3. According to one embodiment, graphite can further improve the cycle life characteristics of the NIB. In certain embodiments mentioned in this article, the negative electrode active material is not a tin-based material.

[0092] It should be recognized that the above negative electrode active materials can be used alone. That is, the anode can contain only one of the above negative electrode active materials. However, it is also possible that a single anode contains a combination of more than one of the above materials. When the above active materials are used in combination, any suitable weight ratio can be used. For example, the range of the weight ratio of two active materials in a single anode can be from 1:100 to 100:1, such as from 1:50 to 50:1, for example 1:1. In additional or alternative embodiments, the battery can include more than one anode. When the battery contains more than one anode (e.g., from two to 10, such as from 2 to 5 cathodes), the active material can be selected from the above active materials, and each anode can independently contain only one anode active material or a combination of two or more active materials, as described above.

[0093] More particularly, the negative electrode active material can be selected from the group consisting of TiO2 or more specifically ways, Na2Ti6O 13 , graphite, hard carbon, and sodium metal.

[0094] The binder and conductive additive (if any) are not particularly limited and can be the same as those of the cathode.

[0095] The weight ratio of the negative electrode active material to the binder is not particularly limited and can be the weight ratio of the related art NIB.

[0096] The anode can be manufactured as follows. The negative electrode active material (one or more), the conductive additive (if necessary) and the binder are mixed in a desired proportion, and the mixture is dispersed in a suitable solvent (such as water and / or a similar solvent) to prepare a slurry. The slurry is then coated on a current collector and dried to form a negative electrode active material layer. Then, the negative electrode active material layer is pressed to a desired thickness using a press to manufacture the anode. Here, the negative electrode active material layer has no particular thickness restrictions, but may have any suitable thickness that the negative electrode active material layer of a rechargeable lithium (or sodium) ion battery may have. In addition, when metallic sodium is used as the negative electrode active material layer, the metallic sodium may overlap with the current collector (e.g., laminated or coated on the current collector).

[0097] It should be appreciated that the cathode and anode active materials described above can be paired together to provide cathode and anode active material pairs. Thus, the battery disclosed herein can have a cathode and an anode comprising an active material pair selected from the group consisting of: M-Na2Fe2(CN)6.2H2O / / TiO2, R-Na2Fe2(CN)6 / / TiO2, NVP / / TiO2, Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / Graphite, Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / Na2Ti6O 13 、Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / TiO2, Na4Mn3(PO4)2(P2O7) / / TiO2, Pathway, Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / Hard carbon, Na a [Cu b Fe c Mn d Ni e Tif M g ]O2 / / Sodium metal, M-Na2Fe2(CN)6.2H2O / / Pathway; M-Na2Fe2(CN)6.2H2O / / Na2Ti6O 13 ; M-Na2Fe2(CN)6.2H2O / / graphite; M-Na2Fe2(CN)6.2H2O / / hard carbon; M-Na2Fe2(CN)6.2H2O / / sodium metal; Pathway; R-Na2Fe2(CN)6 / / Na2Ti6O 13 ; R-Na2Fe2(CN)6 / / graphite; R-Na2Fe2(CN)6 / / hard carbon; R-Na2Fe2(CN)6 / / sodium metal; Pathway: NVP / / Na2Ti6O 13 ; NVP / / graphite; NVP / / hard carbon; NVP / / sodium metal; Pathway: Na4Mn3(PO4)2(P2O7) / / Na2Ti6O 13 ; Na4Mn3(PO4)2(P2O7) / / graphite; Na4Mn3(PO4)2(P2O7) / / hard carbon; and Na4Mn3(PO4)2(P2O7) / / sodium metal, wherein: 0≤a≤1; 0≤b≤0.3; 0≤c≤0.5; 0≤d≤0.6; 0≤e≤0.3; 0≤f≤0.2; and 0≤g≤0.4, and M is one or more selected from the group consisting of Mo, Zn, Mg, Cr, Co, Zr, Al, Ca, K, Sr, Li, H, Sn, Te, Sb, Nb, Sc, Rb, Cs and Na.

[0098] As mentioned above, when the active material of the cathode is selected from the free Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2, the material can be used in combination with any negative electrode active material disclosed herein. For example, the cathode and anode active material pair can be selected from Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / TiO2, Pathway, Na a [Cu b Fec Mn d Ni e Ti f M g ]O2 / / Na2Ti6O 13 、Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / Graphite, Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / Hard carbon, Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / Sodium metal, Na 0.9 [Cu 0.12 Ni 0.10 Fe 0.30 Mn 0.43 Ti 0.05 ]O2 / / TiO2, Pathway, Na 0.9 [Cu 0.12 Ni 0.10 Fe 0.30 Mn 0.43 Ti 0.05 ]O2 / / Na2Ti6O 13 、Na 0.9 [Cu 0.12 Ni 0.10 Fe 0.30 Mn 0.43 Ti 0.05 ]O2 / / Graphite, Na 0.9 [Cu 0.12 Ni 0.10 Fe 0.30 Mn 0.43 Ti 0.05 ]O2 / / Hard Carbon and Na 0.9 [Cu 0.12 Ni 0.10 Fe 0.30 Mn 0.43 Ti 0.05 ]O2 / / sodium metal. For example, when the active material of the cathode is selected from the free form Na a [Cub Fe c Mn d Ni e Ti f M g ]O2, the cathode and anode active material pair can be Na 0.9 [Cu 0.12 Ni 0.10 Fe 0.30 Mn 0.43 Ti 0.05 ]O2 / / Hard carbon.

[0099] A particular cathode and anode active material pair can operate within a defined average voltage window. Thus, the NIBs disclosed herein can be grouped according to the average voltage produced by these cathode and anode pairs in a battery comprising an electrolyte disclosed herein, which groupings can be average voltages from 1.5 V to less than 2.5 V, 2.5 V, and higher (e.g., to 6.0 V).

[0100] The cathode and anode pairs herein operating at an average voltage from 1.5 V to less than 2.5 V include M-Na2Fe2(CN)6.2H2O / / graphite, M-Na2Fe2(CN)6.2H2O / / Na2Ti6O 13 、R-Na2Fe2(CN)6 / / graphite、R-Na2Fe2(CN)6 / / Na2Ti6O 13 、NVP / / Graphite、NVP / / Na2Ti6O 13 , M-Na2Fe2(CN)6.2H2O / / TiO2, R-Na2Fe2(CN)6 / / TiO2, NVP / / TiO2, Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / Graphite, Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / Na2Ti6O 13 and Na a [Cu b Fe c Mn d Ni e Ti f M g]O2 / / TiO2. Specific pairs that may be mentioned for this voltage range include M-Na2Fe2(CN)6.2H2O / / graphite, M-Na2Fe2(CN)6.2H2O / / Na2Ti6O 13 、R-Na2Fe2(CN)6 / / graphite、R-Na2Fe2(CN)6 / / Na2Ti6O 13 ,NVP / / graphite and NVP / / Na2Ti6O 13 .

[0101] The cathode and anode pairs herein operating from an average voltage of 2.5 V and higher include Pathway, M-Na2Fe2(CN)6.2H2O / / hard carbon, M-Na2Fe2(CN)6.2H2O / / sodium metal, Pathway, R-Na2Fe2(CN)6 / / hard carbon, R-Na2Fe2(CN)6 / / sodium metal, Pathway, NVP / / Hard Carbon, NVP / / Sodium Metal, Pathway, Na4Mn3(PO4)2(P2O7) / / Na2Ti6O 13 Na4Mn3(PO4)2(P2O7) / / graphite, Na4Mn3(PO4)2(P2O7) / / hard carbon, Na4Mn3(PO4)2(P2O7) / / sodium metal, Na4Mn3(PO4)2(P2O7) / / TiO2, Pathway, Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / Hard Carbon and Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 / / sodium metal. Specific pairs that may be mentioned for this voltage range include Pathway, M-Na2Fe2(CN)6.2H2O / / hard carbon, M-Na2Fe2(CN)6.2H2O / / sodium metal, Pathway, R-Na2Fe2(CN)6 / / hard carbon, R-Na2Fe2(CN)6 / / sodium metal, Pathway, NVP / / Hard Carbon, NVP / / Sodium Metal, Pathway, Na4Mn3(PO4)2(P2O7) / / Na2Ti6O13 Na4Mn3(PO4)2(P2O7) / / graphite, Na4Mn3(PO4)2(P2O7) / / hard carbon and Na4Mn3(PO4)2(P2O7) / / sodium metal.

[0102] The sodium ion battery also includes a separator. The separator is not particularly limited and can be any suitable separator for a sodium ion battery. For example, a porous layer or nonwoven fabric showing excellent high rate discharge performance and / or similar performance can be used alone or as a mixture (e.g., in a laminate structure).

[0103] The substrate of the diaphragm may include, for example, polyolefin-based resins, polyester-based resins, polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymers, vinylidene fluoride-perfluorovinyl ether copolymers, vinylidene fluoride-tetrafluoroethylene copolymers, vinylidene fluoride-trifluoroethylene copolymers, vinylidene fluoride-vinyl fluoride copolymers, vinylidene fluoride-hexafluoroacetone copolymers, vinylidene fluoride-ethylene copolymers, vinylidene fluoride-propylene copolymers, vinylidene fluoride-trifluoropropylene copolymers, vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene copolymers, vinylidene fluoride-ethylene-tetrafluoroethylene copolymers and / or the like. The polyolefin-based resin may be polyethylene, polypropylene and / or the like; and the polyester-based resin may be polyethylene terephthalate, polybutylene terephthalate and / or the like.

[0104] The porosity of the separator is not particularly limited, and may be any suitable porosity that a separator for a sodium ion battery may have.

[0105] The separator may include a coating containing an inorganic filler, which may be formed on at least one side of the substrate. The inorganic filler may include Al2O3, Mg(OH)2, SiO2 and / or the like. The coating including the inorganic filler may prevent direct contact between the positive electrode and the separator, prevent oxidation and decomposition of the electrolyte on the surface of the positive electrode during storage at high temperatures, and inhibit the generation of gas, which is a decomposition product of the electrolyte. A suitable separator that may be mentioned herein is a glass fiber separator.

[0106] It will be appreciated that any of the above-described membranes may be used in various aspects and embodiments of the present invention, provided they are a technically reasonable choice.

[0107] As described above, the electrolyte includes a salt and a glycol ether solvent, where the salt includes NaBF4. NaBF4 can be present at any suitable concentration, such as greater than 0 to less than or equal to 2.5 M in the glycol ether solvent. Suitable concentrations of NaBF4 include, but are not limited to, from 0.5 to less than or equal to 2.5 M, from 0.75 to 2.5 M, from 1.0 to 2.5 M, from 1.5 to 2.5 M, from 2.0 to 2.5 M, from 0.5 to 2.0 M, from 0.5 to 1.5 M, from 0.5 to 1.0 M, and from 0.5 to 0.75 M in the glycol ether solvent. For example, NaBF4 can be present at a concentration of 1 M in the glycol ether solvent. For the avoidance of doubt, when "M" is used herein in relation to concentration, it refers to molar concentration (i.e., moles per liter of solvent).

[0108] The salt may further include those selected from NaCN, NaClO4, NaAsF6, NaPF6, NaPF 6-x (C n F 2n+1 ) x (1 < x < 6, n = 1 or 2), NaSCN, NaBr, NaI, Na2SO4, Na2B 10 Cl 10, NaCl, NaF, NaPF4, NaOCN, Na(CF3SO3), NaN(CF3SO2)2, NaN(FSO2), NaN(C2F5SO2)2, NaN(CF3SO2)(C4F9SO2), NaC(CF3SO2)3, NaC(C2F5SO2)3, (CH3)4NBF4, (CH3)4NBr, (C2H5)4NClO4, (C2H5)4NI, (C3H7)4NBr, (n-C4H9)4NClO4, (n-C4H9)4NI, (C2H5)4N-maleate, (C2H5)4N-benzoate, (C2H5)4N-phthalate, sodium stearyl sulfonate, sodium octyl sulfonate and sodium dodecylbenzene sulfonate. In certain embodiments that may be mentioned herein, the salt may also include one or more salts selected from the group consisting of NaClO4, NaPF6, NaSCN, NaBr, NaI, NaCl, NaOCN, Na(CF3SO3), NaN(CF3SO2)2 and NaCN. When any of these additional salts are included in the electrolyte composition, each salt may be provided at a suitable concentration. Suitable concentrations of each of these additional salts include, but are not limited to, from 0.5 to less than or equal to 2.5M, from 0.75 to 2.5M, from 1.0 to 2.5M, from 1.5 to 2.5M, from 2.0 to 2.5M, from 0.5 to 2.0M, from 0.5 to 1.5M, from 0.5 to 1.0M and from 0.5 to 0.75M in a glycol ether solvent. For example, each additional salt (when present) may be present at a concentration of 1M in a glycol ether solvent. The above salts may be present in any suitable ratio relative to NaBF4.

[0109] The glycol ether solvent may be selected from one or more of the group consisting of ethylene glycol dimethyl ether (monoglycol dimethyl ether), diglycol dimethyl ether, triglycol dimethyl ether, tetraglycol dimethyl ether, methyl perfluorobutyl ether (MFE) and analogs thereof. Analogs of tetraglycol dimethyl ether (CH3(O(CH2)2)4OCH3) that may be mentioned include, but are not limited to, one or both of its CH3 terminal members may be modified to -C2H5 or -CH2CH2Cl or other similar substituents. In certain embodiments of the present invention that may be mentioned herein, the glycol ether solvent is tetraglycol dimethyl ether.

[0110] Although the glycol ether solvent may include only glycol dimethyl ether type solvents, in certain embodiments, it may also include additional suitable solvents that are compatible with being used in sodium ion batteries. Suitable solvents that may be mentioned herein include, but are not limited to, cyclic carbonates (such as propylene carbonate, ethylene carbonate, diethyl carbonate, butylene carbonate, fluoroethylene carbonate, chloroethylene carbonate, vinylene carbonate and / or the like), linear carbonates (such as dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, etc.), cyclic esters (such as γ-butyrolactone, γ-valerolactone, etc.), linear esters (such as methyl formate, methyl acetate, methyl butyrate, etc.), cyclic or linear ethers other than glycol ethers (such as tetrahydrofuran and its derivatives), 1,3-dioxane, 1,4-dioxane, 1,2-dimethoxyethane, 1,4-dibutoxyethane, etc.), nitriles (such as acetonitrile, benzonitrile and / or the like), dioxolanes or their derivatives, ethylene sulfide, sulfolane and sultones or their derivatives. These solvents may be used in any suitable weight ratio relative to glycol ethers (e.g., tetraglyme). For example, the additional solvent may be one or more selected from the group consisting of propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, tetrahydrofuran, sulfolane, and acetonitrile.

[0111] The electrolyte may also include various suitable additives, such as negative electrode SEI (solid electrolyte interface) forming agents, surfactants and / or similar additives. Such additives may be, for example, succinic anhydride, lithium bis(oxalate) borate, sodium bis(oxalate) borate, lithium tetrafluoroborate, dinitrile compounds, propane sultone, butane sultone, propene sultone, 3-cyclobutene sulfone, fluorinated allyl ether, fluorinated acrylate, carbonate, such as vinyl carbonate, vinyl ethylene carbonate and fluoroethylene carbonate and / or similar substances. The concentration of the additive may be any suitable concentration used in general NIBs. The specific additive that may be included in the electrolyte is one or more additives selected from the group consisting of fluoroethylene carbonate (FEC), vinyl carbonate (VC), vinyl ethylene carbonate (VEC) and adiponitrile. The above-mentioned additives may be present in any suitable weight ratio.

[0112] In NIB, the separator can be disposed between the positive electrode and the negative electrode to manufacture an electrode structure, and the electrode structure is processed to have a desired shape, such as a cylinder, a prism, a laminate, a button shape, and / or the like, and inserted into a container having the same shape. Then, a non-aqueous electrolyte is injected into the container, and the electrolyte is impregnated in the pores of the separator, thereby manufacturing a rechargeable sodium or sodium ion battery.

[0113] Below, the embodiments of the present invention are described in more detail with reference to the following examples. However, the present disclosure is not limited thereto. In addition, the contents not described in the present disclosure can be fully understood by those skilled in the art and will not be described herein.

[0114] Example

[0115] Synthesis of Sodium Titanate (Na2Ti3O7)

[0116] Na2Ti3O7 is synthesized by stirring appropriate amounts of sodium hydroxide and titanium isopropoxide in Milli-Q water to which a certain amount of ascorbic acid is added. After stirring for several hours, the solution is dried on a hot plate or in an oven to remove the water. The resulting dry powder is ground and then burned in a tube furnace at 850°C in flowing Ar gas for 6 hours. The resulting black powder is the desired Na2Ti3O7 species embedded in a carbon matrix (called Na2Ti3O7 / C ), having a morphology similar to that described in A. Rudola, N. Sharma, and P. Balaya, Electrochem. Commun., 2015, 61, 10-13.

[0117] Synthesis of M-Na2Fe2(CN)6.2H2O

[0118] In a typical synthesis, 5 mmol of Na4Fe(CN)6 and 22.5 mmol of ascorbic acid are added to 100 mL of Milli-Q water in a round-bottom flask. The flask is immersed in a silicone oil bath and maintained at 140°C. The solution is stirred for 4 hours while refluxing, so that the reflux temperature of the solution measured by a thermometer immersed in the solution is about 107°C (the solution always shows violent boiling (bubbling)). The flask is then removed from the oil bath and allowed to cool to room temperature, followed by a white precipitate obtained under a yellow solution. The precipitate can be recovered by centrifugation or filtration (the precipitate recovery method does not change the phase purity). During this process, the white precipitate exhibits a light cyan color. The precipitate is then dried in air at 70°C for 3h to obtain the final compound.

[0119] Synthesis of R-Na2Fe2(CN)6

[0120] Based on the conversion of M-Na2Fe2(CN)6.2H2O to R-Na2Fe2(CN)6, R-Na2Fe2(CN)6 is synthesized by heating M-Na2Fe2(CN)6.2H2O (in electrode form or other form), as described in PCT Application No. PCT / SG2017 / 050203 and J.Electochem.Soc.2017,164,A1098-A1109.

[0121] Electrode preparation, cell assembly, and electrochemical evaluation

[0122] Composite electrodes were prepared using the synthesized material as active material, Ketjen black (KB) (Lion) as a conductive additive, and sodium salt of carboxymethyl cellulose CMC (Alfa Aesar) as a binder in a weight ratio of 85:10:5. To prepare the slurry, CMC was first dissolved in Milli-Q water, to which a hand-ground mixture of M-Na2Fe2(CN)6.2H2O and KB was added. After stirring at 1200 rpm for 2 h, the slurry was coated on Al foil using a doctor blade technique and then dried at 120°C overnight under a vacuum of 1 mbar. After drying, the coated electrode was pressed by double rollers at a pressure of 37 psi. The electrode was thus coated with active material with a loading of 3-4 mg cm -2 Between. A 2016-type coin cell (MTI) made with such an electrode was used as the working electrode, sodium metal (Merck) was used as the counter electrode and reference electrode, and glass fiber (Whatman, GF / A grade) was used as the separator layer. Before the battery assembly, the electrode was dried at 120°C in a vacuum of 1 mbar and placed in a glove box (MBraun, Germany) filled with Ar with H2O and O2 <5 ppm.

[0123] The coin cells were cycled in a computer controlled Arbin battery tester (model BT2000, USA) at room temperature.

[0124] Full battery evaluation

[0125] Graphite slurry was prepared using graphite (MCMB graphite, TB-17 type, from MTI) with CMC as binder in a weight ratio of 95:5 (no external conductive additive was used). As described above, Na2Ti3O7 / C was synthesized by a scaled-up modified version of the synthesis reported in our previous report (A. Rudola, N. Sharma, and P. Balaya, Electrochem. Commun., 2015, 61, 10-13) using water as the solution medium with an in-situ C content of about 14 wt%. Na2Ti3O7 / C slurry was prepared using Super P carbon black (as a conductive additive) and CMC as a binder in a weight ratio of 90:5:5, so that the final weight in the slurry was as follows - Na2Ti3O7: in-situ and ex-situ carbon: CMC = 76:19:5.

[0126] For the M-Na2Fe2(CN)6.2H2O / / graphite full cell, the weight ratio of active material in the anode to the cathode was 0.68:1 (excess cathode was used to compensate for the initial low Coulombic efficiency). For the R-Na2Fe2(CN)6 / / graphite full cell, the weight ratio of anode to cathode (active material) was 1.05:1 (excess cathode was used for the reasons described below), while for Full cells, anode to cathode (active material) weight ratio of 0.95:1. All full cells were directly assembled without any pre-cycling of the cathode or anode. For the R-Na2Fe2(CN)6 / / graphite full cells, discharge was controlled by time rather than voltage, while the charge cut-off voltage was 3.3V. Full battery, due to Flat Na + The ion insertion plateau, the upper cutoff voltage is dynamically increased by small increments in the initial cycles to compensate for the slight increase in cathode potential in each cycle due to the lower Coulombic efficiency in the initial cycles.

[0127] By utilizing such a modified cycling method for two full cells using R-Na2Fe2(CN)6 as the cathode, the slightly lower Coulombic efficiency in the initial cycle inherently causes the voltage to slide to the higher potential of the cathode, so that it eventually cycles within the charge-discharge plateau above it.

[0128] The average voltage of the full cell is calculated by calculating the area under the voltage vs. specific capacity curve of the discharge cycle (the calculated area is the specific energy density output by the full cell), and then dividing this value by the specific capacity (specific energy density = specific capacity * average voltage). The coulombic efficiency of the full cell is calculated by taking the ratio of the discharge capacity to the charge capacity.

[0129] Preparation of electrolyte

[0130] Solvents, ethylene carbonate (EC, Alfa Aesar), propylene carbonate (PC, Sigma Aldrich), dimethyl carbonate (DMC, Kishida chemicals), diethylene glycol dimethyl ether (Diglyme, anhydrous, 99.5%, SigmaAldrich) and tetraethylene glycol dimethyl ether (Tetraglyme, ≥99%, Sigma Aldrich) were obtained from commercial sources and used without further purification. EC-PC (1:1, v / v) and EC-DMC (1:1, v / v) mixtures were prepared in house accordingly.

[0131] Similarly, Na salts, NaClO4 (98+%, anhydrous, Alfa Aesar), NaPF6 (99+%, Alfa Aesar), NaBF4 (98%, Sigma Aldrich) were obtained from commercial sources and used without further purification. As an alternative to preparing 1M NaPF6 EC:DMC (1:1, v / v) electrolyte, it can be purchased from Kishida chemicals.

[0132] 1M NaBF4 in tetraglyme electrolyte is prepared by dissolving NaBF4 in the required amount of tetraglyme. The mixture is then stirred until the salt is completely dissolved. Typically, the salt dissolves within 10 to 15 min. Once prepared, the electrolyte can be directly added to NIBs with different combinations of cathodes and anodes (described in detail later) in any configuration (cylindrical cells, prismatic cells, button / coin cells, pouch cells, or any other configuration).

[0133] Flammability testing and DSC measurements of electrolytes

[0134] The flammability of all reported electrolytes was evaluated using standard methods. From the glove box, take exactly 400 μL of each electrolyte in a sealed Ar-filled vial. Then transfer them to a fume hood under ambient air. Pour each electrolyte onto a coin cell tank so that it completely fills the tank. Then, an open flame is brought into contact with the surface of the electrolyte, with t=0 s being the moment the flame contacts the electrolyte. The open flame is allowed to continue contacting the electrolyte until it ignites. The tetraglyme electrolyte of 1M NaBF4 was continuously exposed to an open flame for a full minute without ignition.

[0135] For differential scanning calorimetry (DSC) measurements, the electrolytes were sealed in aluminum capsules in an Ar-filled glove box and then measured at a heating rate of 10° C. / min using a TA Instruments 2920. No air exposure occurred during the DSC measurements.

[0136] In the following examples and Figure 1-12 The results detailed in show that 1 M NaBF4 in tetraglyme electrolyte works well with different types of high-voltage cathodes, low-voltage anodes, and combinations of these electrodes.

[0137] Example 1

[0138] Electrochemical stability of electrolyte

[0139] To examine the anodic stability of the electrolyte, cyclic voltammetry (CV) experiments were performed using bare aluminum (Al) foil as the working electrode (WE), sodium (Na) metal as the counter electrode (CE) and reference electrode (RE), and 1 M NaBF4 in tetraethylene glycol dimethyl ether as the electrolyte. + CV was performed between 10 and 150 μm to determine the voltage window of the electrolyte, and the results were as follows: Figure 1 For comparison, the CV curves in EC (ethylene carbonate)-PC (propylene carbonate) (volume ratio 1:1), one of the most widely used and stable NIB electrolytes, 1 M NaClO4, are also included.

[0140] During oxidation at high potential, tetraglyme in 1 M NaBF4 showed a significantly reduced oxidation current relative to that of EC-PC in 1 M NaClO4. In fact, the latter + The former shows a significant current spike after 4.8 V, while the latter shows a much reduced current spike after 4.8 V, indicating that 1 M NaBF4 tetraethylene glycol dimethyl ether may be more resistant to oxidation compared with 1 M NaClO4 EC-PC. + This leads to the formation of a stable solid electrolyte interface (SEI), which prevents further reduction of the electrolyte in subsequent cycles.

[0141] The CV results reported here do not refer to any specific cathode and show that the electrolyte can be used at high voltage cathodes (>3 V vs Na / Na + And of course good sodium storage performance can be obtained up to 4-4.2V).

[0142] Example 2

[0143] use Performance of low-voltage Na2Ti3O7 anode in different electrolytes

[0144] To determine the extent of first-cycle reduction of the electrolyte and how this will negatively affect the first-cycle Coulombic efficiency of the low-voltage anode, a formula of the form Low-voltage sodium titanate (Na2Ti3O7) anode for deep discharge pathway. Na2Ti3O7 has been well studied for use as a NIB anode due to its high capacity (177.8 mAh / g) and low average voltage (about 0.3 V vs Na / Na + ) (A. Rudola, et al., J. Mater. Chem. A, 2013, 1, 2653-2662).

[0145] Using the above two electrolytes and with all other conditions being the same, the C / 10 rate was 2.5-0.01 V vs Na / Na + The first cycle of the anode between Figure 2 As shown in Figure 2, the same charge (sodium deintercalation) capacity of 165 mAh / g was obtained in both electrolytes. However, the first discharge (sodium intercalation) capacity of EC-PC in 1M NaClO4 was 289 mAh / g, while that of tetraethylene glycol dimethyl ether in 1M NaBF4 was only 200 mAh / g. As mentioned earlier, this long first cycle discharge capacity is due to the low charge (sodium deintercalation) capacity of EC-PC at near 0.0 V vs Na / Na + Electrolyte reduction at reduced voltage. This electrolyte reduction is highly undesirable as it results in low first cycle Coulombic efficiency (ratio of charge to discharge capacity of the anode in a half-cell configuration), which will adversely affect the energy density of NIBs using this anode relative to a suitable cathode. For 1 M NaClO4 in EC-PC electrolyte, the first cycle Coulombic efficiency is very low at 56.8%, while for 1 M NaBF4 in tetraethylene glycol dimethyl ether electrolyte, the first cycle Coulombic efficiency is quite high at 82.4%.

[0146] Thus, using a low voltage insertion anode, such as Na2Ti3O7, with 1M NaBF4 in tetraethylene glycol dimethyl ether as the electrolyte, up to 90 mAh / g of irreversible capacity can be saved. This is a significant margin and will result in the use of a lighter corresponding cathode (i.e., lighter weight) since this irreversible capacity will need to be provided by the cathode in the full cell. In this way, this electrolyte can result in significant energy density gains for the same anode and cathode combination in NIBs. This is an extremely important advantage of this electrolyte over existing electrolytes in the field.

[0147] Example 3

[0148] use Pathway, Performance of Na2Ti3O7 Anode in 1M NaBF4 Tetraglyme Electrolyte

[0149] conventional The cycle life in the deep discharge pathway (in Example 2) is poor and is generally limited to about 100 cycles. Therefore, the use of such an anode is not desirable for large-scale grid storage batteries with an expected cycle life of several thousand cycles. Therefore, in order to test the sodium storage performance of Na2Ti3O7 using this new electrolyte, the recently discovered Na2Ti3O7 was selected. Sodium storage pathway, as it has a moderately high capacity of 88.9 mAh / g and a high conductivity at 0.2 V vs Na / Na+ A very low charge plateau at 1000 Å and a long cycle life of over 1,500 cycles (A. Rudola, et al., Electrochem. Commun., 2015, 61, 10-13 and PCT Application No. PCT / SG2016 / 050094).

[0150] Figure 3 a shows the use of two electrolytes The first galvanostatic cycle of the deep discharge pathway. While the same flat charge plateau at 0.2 V was obtained with both electrolytes, a high coulombic efficiency of 73% was obtained when 1 M NaBF4 in tetraglyme was used as the electrolyte, in contrast to a coulombic efficiency of 33% when 1 M NaClO4 in EC-PC was used as the electrolyte. Similar to the case of the deep discharge pathway using these two electrolyte solutions, swapping the electrolyte from the conventional carbonate-based state-of-the-art electrolyte to 1 M NaBF4 in tetraglyme electrolyte could potentially be used to improve the deep discharge performance of the electrochemically active carbonic acid esters. The pathway saves up to 114 mAh / g of irreversible capacity, which is a significant advantage.

[0151] From the perspective of cycle performance, Figure 3 b and Figure 3 c, this pathway can respond even at an ultrafast 40C rate (90 s), similar to previous reports on EC-PC electrolytes using conventional 1 M NaClO4 (A. Rudola, et al., Electrochem. Commun., 2015, 61, 10-13). More importantly, from Figure 3 d As can be seen, this pathway shows negligible capacity loss over 100 cycles with a stable Coulombic efficiency greater than 99%. These results demonstrate the potential of this electrolyte for low-voltage transition metal-based anodes such as Effectiveness of sodium storage pathways.

[0152] Example 4

[0153] Performance of graphite anode in 1M NaBF4 tetraglyme

[0154] An important advantage of tetraglyme of NaBF4 is that it is based on glyme, which allows sodium storage in graphite in the form of co-intercalation of sodium with solvent molecules, which is not possible with conventional NIB electrolytes based on alkyl carbonates (B. Jache, et al., Angew. Chem. Int. Ed., 2014, 53, 10169–10173). Graphite is very cheap and shows a medium-high sodium storage capacity close to 100 mAh / g, with all capacity contributions being essentially at 0.4 V vs Na / Na + To 1.3Vvs Na / Na + The safe voltage range of Na / Na (B. Jache, et al., Angew. Chem. Int. Ed., 2014, 53, 10169–10173). Due to its advantageously low but not too low voltage activity (1.3–0.4 V vs Na / Na + ), it is probably safe to use graphite in NIBs at low voltages, as this would appear to avoid sodium plating on the graphite anode (which is typically possible at 0.0 V vs Na / Na + It should be noted that graphite cannot be used as the NIB anode with conventional carbonate-based prior art NIB electrolytes, because graphite cannot store Na (it can only store sodium via a co-intercalation mechanism in glyme-based electrolytes, which requires simultaneous storage of Na and a solvent for the electrolyte).

[0155] Figure 4 The sodium storage performance of graphite electrode in 1M NaBF4 tetraglyme electrolyte is shown. Figure 4 , which shows the cycling curves of graphite in 1M NaBF4 tetraglyme electrolyte versus sodium metal, it can be seen that the cycling curves of graphite are identical to those reported in the literature using other glyme-based electrolytes and are below 0.4 V vs Na / Na + There is a very small capacity contribution. The graphite electrode exhibits impressive rate performance characteristics with essentially no drop in charge capacity. The charge capacity is about 91 mAh / g at C / 5 rate and 89 mAh / g at 5C rate, indicating that the material can retain almost 100% of its capacity when the operating conditions switch from requiring a 5 h response from the battery to requiring a fast 12 min response.

[0156] from Figure 4 As can be seen in b, the graphite electrode is also stable at these different rates. More importantly, the graphite electrode shows no observable capacity loss over 200 cycles at C / 2 rate, with a high Coulombic efficiency of approximately 99% over the entire cycle ( Figure 4 c). Therefore, graphite, as in Example 3 The sodium storage pathway is similar, and it also has good compatibility and stability with 1M NaBF4 tetraethylene glycol dimethyl ether electrolyte.

[0157] Example 5

[0158] Performance of M-Na2Fe2(CN)6.2H2O cathode in 1M NaBF4 tetraglyme

[0159] 1M NaBF4 tetraethylene glycol dimethyl ether electrolyte also showed similar excellent performance for the cathode. M-Na2Fe2(CN)6.2H2O cathode (monoclinic phase of Na2Fe2(CN)6) was used in this study because it can be used at up to 3.9 V vs Na / Na + The invention operates at a relatively high voltage (see International Patent Application No. PCT / SG2017 / 050203 and J. Electochem. Soc. 2017, 164, A1098-A1109). Figure 5 The cycling performance of the M-Na2Fe2(CN)6.2H2O cathode at different rates from C / 5 to 10C is shown. Figure 5 As can be seen in a, there is little increase in polarization of this cathode until a fast 10C rate is used. Figure 5 In b, it is clear that the cathode material is very stable at all rates, even with 1M NaBF4 in tetraethylene glycol dimethyl ether. Considering the similarity in rate performance between the novel electrolyte and conventional carbonate-based electrolytes, this suggests that the electrolyte does not affect the performance of the cell and can also improve safety. The long-term cycling performance of the M-Na2Fe2(CN)6.2H2O cathode in the novel electrolyte also reveals essentially no capacity loss, with a high coulombic efficiency (>99.5%) that is stable. Figure 5 c). This high coulombic efficiency of the cathode is very consistent with the high anode stability index of the electrolyte revealed by CV experiments (see Examples 1 and Figure 1 ).

[0160] Example 6

[0161] Performance of R-Na2Fe2(CN)6 cathode in 1M NaBF4 tetraglyme

[0162] To illustrate the stability of another high voltage cathode using 1M NaBF4 tetraglyme electrolyte, a hexagonal phase Na2Fe2(CN)6 (hereinafter referred to as R-Na2Fe2(CN)6) cathode because it outputs high capacity (theoretical capacity is 170.85 mAh / g) and has a high charge / discharge rate of 3.1 and 3.3 V vs Na / Na +Two charging and discharging platforms centered on the battery (see International Patent Application No. PCT / SG2017 / 050203 and J. Electochem. Soc. 2017, 164, A1098-A1109).

[0163] Figure 6 a shows the first galvanostatic cycle of R-Na2Fe2(CN) between 3.9-3.0V. In the first charge cycle, two charge plateaus were obtained, the lower charge plateau at 3.1V and the upper charge plateau at 3.35V, resulting in a capacity slightly higher than the theoretical capacity of 170.85mAh / g. During discharge, the R-Na2Fe2(CN)6 cathode was intentionally cycled to 3.0V so that the cycle was truncated just before the onset of the lower discharge plateau, resulting in a capacity of 79mAh / g with a discharge plateau at 3.25V. This was done because the theoretical capacity of the R-Na2Fe2(CN)6 cathode is 170.85mAh / g, which is much higher than graphite (100mAh / g) and Theoretical capacity of the sodium storage pathway (88.9 mAh / g). If a full cell is prepared with R-Na2Fe2(CN)6 as the cathode and either of these two anodes, there will be a large capacity mismatch. Therefore, to circumvent this, and also to withstand the Coulombic inefficiencies of the anode(s) and cathode in the initial cycles of the full cell, the lower charging platform of R-Na2Fe2(CN)6 can be used to compensate for these inefficiencies (such as Figure 6 a), then in the full cell, the R-Na2Fe2(CN)6 cathode can be cycled practically only within its upper charge-discharge plateau (3.9-3.0 V vs Na / Na + between).

[0164] As a representative example of the 3.9-3.0 V cycling curve of R-Na2Fe2(CN)6, Figure 6 b depicts the 1C rate at 3.9–3.0 V vs Na / Na + The tenth galvanostatic cycle of R-Na2Fe2(CN)6 can be seen at a flat charge and discharge platform at an average voltage of 3.3 V, with a discharge capacity of 78 mAh / g, which is comparable to the graphite anode (89 mAh / g) and The charge capacity of the R-Na2Fe2(CN)6 cathode is very close to that of the R-Na2Fe2(CN)6 cathode (74 mAh / g). This ensures that the full cell is well balanced. Most importantly, we found that the 3.9-3.0 V cycling of the R-Na2Fe2(CN)6 cathode is also quite stable, with 87% capacity retention after 200 cycles and a high stable Coulombic efficiency of greater than 99% ( Figure 6 c).

[0165] Example 7

[0166] The cathode (M-Na2Fe2(CN)6.2H2O or R-Na2Fe2(CN)6) and anode (graphite) combination of non-flammable NIBs in full cells using 1M NaBF4 tetraglyme electrolyte

[0167] To demonstrate the advantages of this electrolyte in practically relevant NIBs, two different types of full cell combinations were investigated. In both combinations, a graphite anode and a 1M NaBF4 tetraglyme electrolyte were used, while the cathode consisted of M-Na2Fe2(CN)6.2H2O( Figure 7 a) or when at 3.9-3.0V vs Na / Na + When circulating between R-Na2Fe2(CN)6( Figure 7 b). For the R-Na2Fe2(CN)6 / / graphite full cell, the cathode is cycled only within its upper voltage charge-discharge platform, so that the lower charge platform is used to compensate for the low Coulombic efficiency of the full cell (e.g. Figure 6 described in a).

[0168] For both full cells, no prior cycling of the anode or cathode in the half-cell was performed, and all irreversibilities of the cathode and anode were calculated by using a relatively heavy cathode. Nevertheless, both types of full cells were able to achieve moderately high energy densities between 67 and 71 Wh / kg (taking into account the weight of the active materials in the cathode and anode), as well as stable cycling for 300 cycles, as shown in Figure 2. Figure 7 c. With further optimization, the energy density of R-Na2Fe2(CN)6 / / graphite and M-Na2Fe2(CN)6.2H2O / / graphite full cells is expected to approach 87-89Wh / kg and 75Wh / kg, respectively. Considering the low cost of cathode, anode and electrolyte, these are very attractive for gate storage battery applications.

[0169] Example 8

[0170] Using 1M NaBF4 in tetraglyme electrolyte, the cathode (R-Na2Fe2(CN)6) and anode ( Pathway) combination

[0171] As another example of a viable nonflammable NIB, the + The R-Na2Fe2(CN)6 circulating in the cathode is used as the The anode was used as the anode, and 1 M NaBF4 in tetraethylene glycol dimethyl ether was used as the electrolyte. A representative C / 2 galvanostatic cycle of such a full cell is shown in FIG. Figure 8As shown in a. Similar to the case of R-Na2Fe2(CN)6 / / graphite full cell, the lower charging platform of R-Na2Fe2(CN)6 is again used to compensate for the low Coulombic efficiency in this full cell. The full cell shows a flat discharge platform between 3.1-3 V and delivers a very attractive energy density of 89 Wh / kg (based on the weight of both cathode and anode) at an average voltage of 2.53 V without any pre-cycling step, comparing the 0.2 V charge platform of the R-Na2Fe2(CN)6 pathway and the 3.3 V upper discharge platform of R-Na2Fe2(CN)6. The full cell also showed fairly stable cycling over 40 cycles, as Figure 8 b. With further optimization, the full cell could potentially deliver energy densities exceeding 100 Wh / kg as well as stable cycling, as demonstrated by the cathode and anode in their respective half-cells.

[0172] Example 9

[0173] Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2 cathode performance in 1M NaBF4 tetraethylene glycol dimethyl ether

[0174] The performance of metal oxide cathodes according to the above formula was studied in 1M NaBF4 in tetraethylene glycol dimethyl ether. The metal oxide has the general formula Na a [Cu b Fe c Mn d Ni e Ti f M g ]O2, where:

[0175] 0≤a≤1; 0≤b≤0.3; 0≤c≤0.5; 0≤d≤0.6; 0≤e≤0.3; 0≤f≤0.2; 0≤g≤0.4;

[0176] M may be selected from the group consisting of Mo, Zn, Mg, Cr, Co, Zr, Al, Ca, K, Sr, Li, H, Sn, Te, Sb, Nb, Sc, Rb, Cs, Na; and

[0177] • The values ​​are chosen in such a way and with such a stoichiometry that the charge balance is maintained.

[0178] Two examples of such cathodes are shown (Na0.9 [Cu 0.22 Fe 0.30 Mn 0.48 ]O2 and Na 0.9 [Cu 0.12 Ni 0.10 Fe 0.30 Mn 0.43 Ti 0.05 ]O2). Fig. 9 a shows the C / 5 rate in 1 M NaBF4 tetraglyme electrolyte from 4.1–2.5 V vs Na / Na + Na in the mesocycle 0.9 [Cu 0.22 Fe 0.30 Mn 0.48 ] Cycling curve of O2 half-cell; and Fig. 9 b shows the high Coulombic efficiency (≈99%) and stable discharge capacity of this half-cell over 150 cycles.

[0179] Fig. 9 c shows the C / 5 rate in 1 M NaBF4 tetraglyme electrolyte from 4.2–2.5 V vs Na / Na + Na in the mesocycle 0.9 [Cu 0.12 Ni 0.10 Fe 0.30 Mn 0.43 Ti 0.05 ] Cycling curve of O2 half-cell; and Fig. 9 b shows the high Coulombic efficiency (≈98–99%) and stable discharge capacity of the half-cell over 50 cycles.

[0180] Example 10

[0181] Comparison of the performance of hard carbon anodes in 1M NaBF4 in tetraglyme and 1M NaClO4 in EC-PC (1:1, v / v)

[0182] like Fig.10 As shown in a, the hard carbon anode in 1M NaBF4 tetraethylene glycol dimethyl ether obtained a higher charge capacity (268 mAh / g) compared to the hard carbon anode in 1M NaClO4 EC-PC (197 mAh / g). In addition, Fig.10 b shows that the same anode in 1M NaBF4 in tetraethylene glycol dimethyl ether achieves a higher first cycle Coulombic efficiency (85.9%) compared to the anode in 1M NaClO4 in EC-PC (74.5%), as well as higher cycling stability and higher average Coulombic efficiency (99.9% vs. 98.9%) in cycles 2-30.

[0183] Based on the above half-cell results, NIB full cells using hard carbon anodes in 1M NaBF4 tetraglyme electrolyte will require less cathode, thereby increasing the specific energy density of the full cell. This was demonstrated in Examples 11 and 12 using several different cathodes.

[0184] Embodiment 11

[0185] Cathode (R-Na2Fe2(CN)6) and anode (hard carbon) combinations for nonflammable NIBs in full cells using 1 M NaBF4 in tetraglyme electrolyte

[0186] like Fig.11 As shown, the R-Na2Fe2(CN)6 / / hard carbon full cell outputs a high specific energy density of 137Wh / kg with no capacity drop over 100 cycles. Therefore, this R-Na2Fe2(CN)6 / / hard carbon full cell combination may be another attractive candidate for commercial NIBs.

[0187] Example 12

[0188] The cathode of non-flammable NIBs (Na 0.9 [Cu 0.12 Ni 0.10 Fe 0.30 Mn 0.43 Ti 0.05 ]O2) and anode (hard carbon) combination

[0189] Na 0.9 [Cu 0.12 Ni 0.10 Fe 0.30 Mn 0.43 Ti 0.05 ]O2 / / Hard carbon full cells can deliver very high specific energy density approaching 187Wh / kg in 10 cycles with a stable Coulombic efficiency of 100% ( Fig.12 b) Such a full cell combination will be attractive for many commercial applications due to its very high specific energy density. The high Coulombic efficiency of the anode and cathode in 1M NaBF4 tetraglyme electrolyte greatly contributes to the high specific energy density and Coulombic efficiency.

[0190] Embodiment 13

[0191] Non-flammability and thermal stability of the electrolyte

[0192] To demonstrate the non-flammability and thermal stability of tetraglyme electrolytes, various electrolytes were continuously exposed to open flames for the entire exposure time under ambient conditions. The tetraglyme electrolyte in 1M NaBF4 did not ignite even after continuous exposure to open flames for a full 1 min (60 s) ( Fig.13 a). In contrast, conventional electrolytes, such as EC-DMC based on the flammable DMC solvent 1 M NaPF6, easily ignite within 2 s of exposure to an open flame ( Fig.13 b). In addition, other glyme-based electrolytes were found to be flammable. For example, the highly flammable diethylene glycol dimethyl ether (DGE)-based electrolyte, which is currently the most commonly used Glyme-based NIB electrolyte, ignites within 5 seconds of exposure to flame ( Fig.13 c shows the flammability test of 0.6M NaPF6 in diglyme electrolyte solution).

[0193] These flammability test results are supported by differential scanning calorimetry (DSC) results for various conventionally used electrolytes. Fig.13 The corresponding DSC temperature rise curves in an inert argon atmosphere (simulating the sealing conditions of NIB) are shown in d. It can be seen that the 1M NaBF4 tetraethylene glycol dimethyl ether electrolyte is the most thermally stable electrolyte, with no major thermal events occurring at high temperatures up to 273°C. In contrast, 1M NaPF6 EC-DMC at 135°C and 0.6M NaPF6 diethylene glycol dimethyl ether at a much lower temperature of 116°C experienced significant thermal events. These DSC and flammability test results provide direct evidence for the 1M NaBF4 tetraethylene glycol dimethyl ether electrolyte and its safe use as an electrolyte incorporated into NIBs.

[0194] in conclusion

[0195] The above results, using 1 M NaBF4 in tetraglyme as the electrolyte, highlight that this non-flammable electrolyte can work well with both the high voltage cathode as well as the low voltage anode of NIBs.

[0196] Therefore, other known NIB cathodes and anodes are expected to function when cycled with this electrolyte (e.g., by Figure 1 The CV results shown have shown that the electrochemical stability window of this electrolyte is from 0.0 V to at least 4-4.5 V vs Na / Na + In particular, Na3V2(PO4)3 (NVP) is another cathode that works well with 1M NaBF4 in tetraglyme electrolyte, as NVP also typically cycles between 3.9-2.0 V, and its charge / discharge plateau is at 3.4 V vs Na / Na +In addition, the related mixed phosphate phase Na4Mn3(PO4)2(P2O7) may be another potential cathode that works well with this electrolyte, as it shows a 4 V vs Na / Na + The charge / discharge plateau is centered around φ, which is within the electrochemical stability limit of the electrolyte.

Claims

1. A non-flammable sodium-ion battery, include: cathode for sodium-ion batteries; Anodes for sodium-ion batteries; Diaphragm; and An electrolyte comprising a salt and a glycol ether solvent, wherein: The salt includes NaBF 4 ; NaBF provided 4 The concentration of is from 0.5M to 2.0M in the glycol ether solvent; The glycol ether solvent is selected from one or more of the group consisting of tetraglyme and the like; The battery has an average voltage of from 1.5V to 6.0V; as well as A Coulombic efficiency of at least 95% after 5 charge / discharge cycles; and The cathode and anode include an active material pair selected from the group consisting of: Zn-doped Na 3 V 2 (PO 4 ) 3 (NVP) / / Hard Carbon; Na 0.9 [Cu 0.12 Ni 0.10 Fe 0.30 Mn 0.43 Ti 0.05 ]O 2 / / Hard carbon, and Na 0.9 [Cu 0.12 Ni 0.10 Fe 0.30 Mn 0.43 Ti 0.05 ]O 2 / / Graphite.

2. The battery according to claim 1, in, The average voltage is from 1.75 to 5.5V.

3. The battery according to claim 2, in, The average voltage is from 2.0 to 5.0V.

4. The battery according to claim 3, in, The average voltage is from 2.5 to 5.0V.

5. The battery according to claim 1, in, The battery has a cycle life of from 50 cycles to 50,000 charge / discharge cycles.

6. The battery according to claim 5, in, The battery has a cycle life of from 100 to 25,000 charge / discharge cycles.

7. The battery according to claim 6, in, The battery has a cycle life of from 300 to 10,000 charge / discharge cycles.

8. The battery according to claim 1, in, The battery has a coulombic efficiency of at least 97% after 5 charge / discharge cycles.

9. The battery according to claim 1, in, Supplied NaBF 4 The concentration of is 1 M in the glycol ether solvent.

10. The battery according to claim 1, in, The glycol ether solvent further comprises one or more solvents selected from the group consisting of cyclic carbonates, linear carbonates, cyclic esters, linear esters, cyclic ethers or linear ethers other than glycol ethers, nitriles, dioxolanes or their derivatives, ethylene sulfide, sulfolanes, sultones or their derivatives.

11. The battery according to claim 10, in, The glycol ether solvent further includes one or more selected from the group consisting of propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, tetrahydrofuran, sulfolane and acetonitrile.

12. The battery according to claim 1, in, The salt also includes NaCN, NaClO 4 、NaAsF 6 、NaPF 6 、NaPF 6-x (C n F 2n+1 ) x , where 1 < x < 6, n = 1 or 2, NaSCN, NaBr, NaI, Na 2 SO 4 、Na 2 B 10 Cl 10 、NaCl, NaF, NaPF 4 、NaOCN, Na(CF 3 SO 3 )、NaN(CF 3 SO 2 ) 2 、NaN(FSO 2 )、NaN(C 2 F 5 SO 2 ) 2 、NaN(CF 3 SO 2 )(C 4 F 9 SO 2 )、NaC(CF 3 SO 2 ) 3 、NaC(C 2 F 5 SO 2 ) 3 、(CH 3 ) 4 NBF 4 、(CH 3 ) 4 NBr、(C 2 H 5 ) 4 NClO 4 、(C 2 H 5 ) 4 NI、(C 3 H 7 ) 4 NBr、(n-C 4 H 9 ) 4 NClO 4 、(n-C 4 H 9 ) 4 NI、(C 2 H 5 ) 4 N - maleate, (C 2 H 5 ) 4 N - benzoate, (C 2 H 5 ) 4 One or more salts from the group consisting of N-phthalate, sodium stearyl sulfonate, sodium octyl sulfonate and sodium dodecylbenzene sulfonate.

13. The battery according to claim 12, in, Each of the one or more salts according to claim 12, when present, is provided at a concentration of greater than 0 to 2.5M.

14. The battery according to claim 1, in, The cathode and anode include active material pair Zn-doped NVP / / hard carbon.

15. The battery according to claim 1, in, The cathode and the anode include active materials Na 0.9 [Cu 0.12 Ni 0.10 Fe 0.30 Mn 0.43 Ti 0.05 ]O 2 / / Graphite.

16. The battery according to claim 1, in, The cathode and the anode include active materials So 0.9 [Cu 0.12 Ni 0.10 Feb 0.30 Mr 0.43 Tea 0.05 ]O 2 / / hard carbon.

17. The battery according to claim 1, in, The electrolyte further includes one or more additives selected from the group consisting of fluoroethylene carbonate, vinylene carbonate, vinylethylene carbonate, and adiponitrile.

Citation Information

Patent Citations

  • Sodium-ion battery anode

    WO2016137401A1

  • Monoclinic sodium iron hexacyanoferrate

    WO2017180059A1

  • Sodium ion battery negative electrode sheet and sodium ion battery

    CN104966813A

  • Method for producing nonaqueous electrolyte secondary cell

    CN105900275A

  • Secondary battery

    EP0317351A2