Preparation method of aluminum using hydrate

Through the combination of perfluoroalkylsulfonimide ionic liquid and aluminum halide hydrate, nitrile solvents and ligands are used to remove water molecules, achieving low-cost, low-energy consumption aluminum electrodeposition, solving the problem of Hall The problems of high cost and high energy consumption of the Herault method have improved the efficiency of aluminum preparation.

CN111101156BActive Publication Date: 2024-10-25UACJ CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201911012686.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-10-25
Filing Date
2019-10-23
Publication Date
2024-10-25
Estimated Expiration
2039-10-23

AI Technical Summary

Technical Problem

Among the existing aluminum preparation methods, the Holger Lauter method requires a large amount of electricity, resulting in high costs and large energy consumption. Moreover, aluminum halide hydrate is difficult to dissolve in non-aqueous solvents, resulting in low aluminum electrodeposition efficiency.

Method used

The perfluoroalkylsulfonimide or perfluoroalkylsulfonamide ionic liquid is mixed with the aluminum halide hydrate to synthesize the aluminum compound, dissolve it in a nitrile organic solvent, and add the phosphorus compound and amide ligand , remove water molecules, and deposit aluminum on the cathode through electrolysis.

Benefits of technology

It achieves high-efficiency electrodeposition of aluminum from aluminum halide hydrate at low cost and low energy consumption, reduces electrodeposition obstacles, and improves the production efficiency of aluminum.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0004999651580000011
    Figure FDA0004999651580000011
  • Figure GDA0004999651590000021
    Figure GDA0004999651590000021
  • Figure GDA0004999651590000041
    Figure GDA0004999651590000041
Patent Text Reader

Abstract

The present invention provides a method for preparing aluminum using hydrates, which is a novel preparation method. By utilizing an ionic liquid method, aluminum can be efficiently electrodeposited from an aluminum halide hydrate at a low cost and with less energy consumption than before. The aluminum preparation method comprises the following steps: a step of synthesizing an aluminum compound from a mixture of an ionic liquid represented by the general formula (1) and an aluminum halide hydrate; a step of dissolving the aluminum compound in a nitrile organic solvent to prepare an aluminum electrolyte; a step of adding a ligand to remove water molecules from the hydrate contained in the aluminum electrolyte; and a step of electrodepositing aluminum on the cathode by passing electricity between the anode and the cathode in the aluminum electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing aluminum using a hydrate, and more particularly to a novel method for producing aluminum by efficiently electrodepositing aluminum from an aluminum halide hydrate using an ionic liquid method. Background Art

[0002] Aluminum is generally produced by the Hall-Heroult process, which involves refining alumina from bauxite (Bayer process), and then dissolving the alumina for electrolysis. However, in the Hall-Heroult process, alumina is electrolyzed at a very high temperature, so a large amount of electricity is required for electrolysis, resulting in high production costs. Therefore, energy-saving aluminum production is desired.

[0003] As a technology for producing aluminum at low temperatures, especially near room temperature, electroplating using an electrolyte is well known. However, the standard electrode potential of aluminum is significantly lower than that of hydrogen, so an aqueous solution cannot be used as an electrolyte under normal circumstances. Therefore, aluminum electrodeposition is performed by an ionic liquid method using a non-aqueous solution such as a molten salt or an organic solvent as an electrolyte.

[0004] For example, Patent Document 1 describes an aluminum electroplating method using a molten salt bath of anhydrous aluminum halide (anhydrous AlCl3, etc.) and a dialkylimidazolium halide. In addition, Non-Patent Document 1 describes a rechargeable aluminum battery that synthesizes aluminum bistrifluoromethanesulfonyl imide (Al(TFSI)3) from anhydrous AlCl3 and bistrifluoromethanesulfonyl imide (H-TFSI), and uses an electrolyte containing acetonitrile and the synthesized Al(TFSI)3.

[0005] However, anhydrous AlCl3 as a raw material is usually prepared by reacting aluminum obtained by the Hall-Heroult method with chlorine. Therefore, in the method of preparing aluminum using anhydrous AlCl3 as a raw material by an ionic liquid method, the preparation cost is still high and a large amount of energy (electricity) is required.

[0006] As an alternative to anhydrous AlCl3, AlCl3·6H2O has attracted attention. Hydrate AlCl3·6H2O can be prepared by reacting aluminum hydroxide obtained as an intermediate product of the previous stage of the Hall-Heroult process (i.e., the Bayer process) with hydrochloric acid. That is, it can be obtained without going through the Hall-Heroult process that consumes a lot of electricity. Therefore, in the ionic liquid method, it is expected that using AlCl3·6H2O as a raw material can be used to perform aluminum electrodeposition with less energy consumption and low cost.

[0007] However, AlCl3·6H2O is difficult to dissolve in existing non-aqueous solvents such as molten salts and organic solvents. Moreover, even if AlCl3·6H2O can be dissolved, as mentioned above, since the standard electrode potential of aluminum is very low, when water from hydrates exists in the electrolyte, aluminum is not electrodeposited, but water is electrolyzed preferentially.

[0008] In addition, aluminum halide hydrates such as AlCl3·6H2O have the following structure: H2O is bonded to Al in a manner that surrounds Al, and Cl is bonded around it. On the other hand, water molecules surrounding Al may hinder electrodeposition, so electrodeposition can be performed more efficiently by removing water molecules from the hydrate as much as possible. However, even if aluminum compounds having water molecules such as aluminum halide hydrates are heated in order to remove the water molecules, the bond between H2O and Al cannot be cut off, thereby forming aluminum oxide. Therefore, it is desired to develop a technology that can remove water molecules from hydrates from the electrolyte and efficiently deposit aluminum.

[0009] [Prior art literature]

[0010] [Patent document]

[0011] [Patent Document 1] Japanese Patent Application Laid-Open No. 1-272790

[0012] [Non-patent document]

[0013] [Non-patent document 1] Masanobu Chiku et al., "Journal of the electrochemical society", 164(9)A1841-1844 (2017) Summary of the invention

[0014] [Technical Problems to be Solved by the Invention]

[0015] In view of the above facts, an object of the present invention is to provide a novel method for preparing aluminum, which can utilize an ionic liquid method to efficiently electrodeposit aluminum from aluminum halide hydrate with less energy consumption and at a lower cost than before.

[0016] [Solution to the problem]

[0017] The present invention is a method for preparing aluminum, characterized in that it comprises the following steps:

[0018] A step of synthesizing an aluminum compound derived from perfluoroalkylsulfonyl imide aluminum or perfluoroalkylsulfonamide aluminum from a mixture containing a perfluoroalkylsulfonyl imide type or perfluoroalkylsulfonamide type ionic liquid represented by the following general formula (1) and an aluminum halide hydrate;

[0019]

[0020] (In formula (1), Rf 1 and Rf 2 are independently CF3 or C4F9, M is H, alkali metal, quaternary ammonium or imidazolium)

[0021] A step of dissolving the aluminum compound in a nitrile organic solvent to prepare an aluminum electrolyte;

[0022] A step of adding at least one ligand selected from a phosphorus compound and an organic compound having an amide group to the aluminum electrolyte to remove water molecules from the hydrate contained in the aluminum electrolyte;

[0023] After the dehydration step, a step is performed in which electricity is passed between the anode and the cathode in the aluminum electrolyte to electrodeposit aluminum on the cathode.

[0024] An aspect of the present invention is a method for producing aluminum, wherein in the dehydration step, the aluminum electrolyte to which the at least one ligand is added is stirred at 0° C. or higher and 100° C. or lower.

[0025] The present invention is a method for producing aluminum, wherein in the electrodeposition step, constant potential electrolysis is performed at an electrode potential of not less than -6.0 V and less than 0 V relative to aluminum used as a reference electrode, or a current density of 1 μA cm -2 Above 10000μAcm -2 The following constant current electrolysis.

[0026] An aspect of the present invention is a method for producing aluminum, wherein in the electrodeposition step, a temperature of the electrolytic bath is 20° C. or higher and 100° C. or lower.

[0027] The present invention is a method for preparing aluminum, wherein in the general formula (1), Rf 1 and Rf 2 It is CF3.

[0028] An embodiment of the present invention is a method for producing aluminum, wherein the aluminum halide hydrate is aluminum (III) chloride hexahydrate.

[0029] An aspect of the present invention is a method for producing aluminum, wherein the phosphorus compound is selected from the group consisting of phosphonic acid, phosphinic acid, phosphine oxide, and tributyl phosphate.

[0030] An aspect of the present invention is a method for producing aluminum, wherein the organic compound having an amide group is selected from the group consisting of N-phenylacetamide, dimethylformamide and dimethylacetamide.

[0031] [Effects of the Invention]

[0032] According to the present invention, aluminum can be electrodeposited from aluminum halide hydrate using an ionic liquid method. Therefore, a novel method for producing aluminum that can electrodeposit aluminum at a lower cost and with less energy consumption than before can be provided. Furthermore, since water molecules from hydrates that are an obstacle to electrodeposition are removed from the electrolyte, aluminum can be electrodeposited efficiently. DETAILED DESCRIPTION

[0033] Hereinafter, embodiments of the present invention will be described. In addition, the present invention is not limited to the following embodiments, and can be implemented in various forms within the scope not departing from the gist of the present invention.

[0034] The method for preparing aluminum of the present invention comprises the following steps: comprising the following general formula (1):

[0035]

[0036] (In formula (1), Rf 1 and Rf 2 A mixture of an ionic liquid of the perfluoroalkylsulfonyl imide type or perfluoroalkylsulfonamide type represented by CF3 or C4F9 independently of each other, M being H, an alkali metal, a quaternary ammonium or an imidazolium and an aluminum halide hydrate to synthesize an aluminum compound, i.e., perfluoroalkylsulfonyl imide aluminum or perfluoroalkylsulfonamide aluminum;

[0037] dissolving the aluminum compound in a nitrile organic solvent to prepare an aluminum electrolyte;

[0038] Adding at least one ligand selected from a phosphorus compound and an organic compound having an amide group to an aluminum electrolyte to remove water molecules from a hydrate contained in the aluminum electrolyte;

[0039] After the dehydration step, aluminum is electrodeposited on the cathode by passing electricity between the anode and the cathode in the aluminum electrolyte.

[0040] That is, in the method for producing aluminum of the present invention, from the viewpoints of production cost, energy consumption, etc., aluminum halide hydrate is used instead of anhydrous aluminum halide which is not preferred as a raw material. Furthermore, a specific aluminum compound is synthesized from aluminum halide hydrate and a predetermined ionic liquid, and an aluminum electrolyte is prepared using an organic solvent that can dissolve the aluminum compound. Thus, aluminum can be electrodeposited at room temperature by an ionic liquid method, that is, an electrolytic reaction using an electrolyte prepared from aluminum halide hydrate, so that aluminum (hereinafter also referred to as "Al") can be produced at a lower cost and with less energy consumption than before. Furthermore, by adding a predetermined ligand to the aluminum electrolyte, water molecules (H2O ligands) contained in hydrates contained in the aluminum electrolyte, such as hydrates of synthesized aluminum compounds, and unreacted aluminum halide hydrates remaining in the aluminum electrolyte are replaced by the predetermined ligand. Thus, water molecules that become obstacles to electrodeposition are removed from the hydrates contained in the aluminum electrolyte, so that aluminum can be efficiently electrodeposited.

[0041] <Synthesis of Aluminum Compounds>

[0042] First, the synthesis of the aluminum compound carried out in the aluminum preparation method of the present invention is described. The aluminum compound derived from perfluoroalkylsulfonyl imide aluminum or perfluoroalkylsulfonamide aluminum (hereinafter, also referred to as "Al compound") is synthesized by mixing the specified ionic liquid represented by formula (1) with aluminum halide hydrate, heating the mixture, and evaporating the water and hydrogen chloride from the aluminum halide as by-products. The mixing ratio of the ionic liquid and the aluminum halide hydrate is not particularly limited, and the molar ratio of the ionic liquid: aluminum halide hydrate is preferably 0.1:1 to 10:1, and more preferably 0.5:1 to 5:1. In addition, the heating temperature of the mixture is not particularly limited, and is preferably 80°C or more and 200°C or less, and more preferably 100°C or more and 150°C or less. In addition, in order to further remove impurities from the heated mixture, distillation can be performed as needed. The desired Al compound is synthesized through such a process. Such Al compounds are, for example, aluminum perfluoroalkylsulfonyl imide (amide) and hydrates thereof such as aluminum bistrifluoromethanesulfonyl imide.

[0043] (Ionic Liquids)

[0044] In the present invention, the so-called ionic liquid is a general term for a liquid ionic compound (salt) containing a combination of a cationic species and an anionic species, and refers to a compound that forms a liquid phase at a relatively low temperature below 100°C. Such ionic liquids have a very low vapor pressure and can sometimes be used even in a vacuum such as SEM. The ionic liquid can also be made hydrophobic by appropriately selecting anionic species.

[0045] As the ionic liquid, a compound which can be dissolved in the nitrile organic solvent described later and used as an aluminum electrolyte is selected. Specifically, the following general formula (1) is used:

[0046]

[0047] (In formula (1), Rf 1 and Rf 2 Each of the ionic liquids is independently CF3 or C4F9, and M is H, an alkali metal, a quaternary ammonium or an imidazolium. Such ionic liquids can be exemplified by the following general formula (1): 1 and Rf 2 Bis(trifluoromethanesulfonyl)imides of CF3, Rf 1 and Rf 2 Bis(nonafluorobutanesulfonyl)imides of C4F9, Rf 1 is CF3 and Rf 2 The ionic liquids of the nonafluoro-N-[(trifluoromethane)sulfonyl]butanesulfonamide type are preferably C4F9. Among these ionic liquids, in the general formula (1), Rf 1 and Rf 2 The ionic liquids are preferably CF3, i.e., ionic liquids containing anions of bis(trifluoromethanesulfonyl)imide (hereinafter also referred to as "TFSI"), and particularly preferably, ionic liquids in which M as a cation is H, K (potassium), Li (lithium) or Na (sodium), i.e., HTFSI, KTFSI, LiTFSI or NaTFSI. In addition, the "imide" in the ionic liquid used in the present invention means Rf 1 and Rf 2 For the case of the same structure, "amide" means Rf 1 and Rf 2 For situations where the structures are different from each other.

[0048] (Aluminum Halide Hydrate)

[0049] Aluminum halide hydrates include, for example, aluminum fluoride (III) hexahydrate (AlF3·6H2O), aluminum chloride (III) hexahydrate (AlCl3·6H2O), aluminum bromide (III) hexahydrate (AlBr3·6H2O), aluminum iodide (III) hexahydrate (AlI3·6H2O), etc. The Al compound synthesized from a mixture of such an aluminum halide hydrate and the above-mentioned perfluoroalkylsulfonyl imide (amide) type ionic liquid can be an Al source in the aluminum electrolyte described later. Among aluminum halide hydrates, aluminum chloride (III) hexahydrate is preferred from the perspective of low cost and easy availability.

[0050] <Production of Aluminum Electrolyte>

[0051] After the Al compound is synthesized, the obtained Al compound is dissolved in a nitrile organic solvent to prepare an aluminum electrolyte (hereinafter, also referred to as "electrolyte"). The amount of the Al compound contained in the electrolyte is not particularly limited as long as it can be fully dissolved in the nitrile organic solvent and a sufficient amount of Al can be precipitated by electrodeposition described later. It is preferably 0.1 g or more and 100 g or less relative to 100 ml of the electrolyte, and more preferably 0.5 g or more and 50 g or less. In addition, although the Al compound can be dissolved by stirring at room temperature, in order to dissolve the Al compound quickly and reliably, a heating treatment of, for example, 40°C to 80°C may be performed.

[0052] (Organic Solvent)

[0053] As for the organic solvent, a nitrile compound is used from the viewpoint that it can dissolve the Al compound synthesized from the aluminum halide hydrate and the above-mentioned specific perfluoroalkylsulfonyl imide (amide) type ionic liquid and be used as a solution of the electrolyte. As such a nitrile compound, for example, acetonitrile, acrylonitrile, benzonitrile are preferred, and acetonitrile is particularly preferred.

[0054] <Dehydration of Water Molecules>

[0055] After preparing the electrolyte, at least one ligand selected from a phosphorus compound and an organic compound having an amide group is added to the obtained electrolyte to remove water molecules from the hydrate contained in the electrolyte. The amount of the ligand added is not particularly limited as long as it can replace the water molecules in the hydrate contained in the electrolyte and does not affect the electrodeposition described later. It is preferably 0.01 mol / L or more and 10 mol / L or less, and more preferably 0.05 mol / L or more and 5 mol / L or less relative to 100 ml of the electrolyte. Moreover, the added ligand may be a single type or two or more types.

[0056] When removing water molecules from the hydrate contained in the electrolyte, the aluminum electrolyte to which at least one ligand is added is preferably stirred at a temperature of 0° C. to 100° C. In addition, in order to perform the dehydration process under more appropriate conditions and to perform the subsequent electrodeposition more efficiently, the temperature of the aluminum electrolyte containing the ligand is more preferably 20° C. to 90° C., and further preferably 30° C. to 70° C.

[0057] (ligand)

[0058] The ligand is a compound that can replace water molecules from hydrates contained in the electrolyte and is dissolved in a nitrile organic solvent, and is selected from a phosphorus compound and an organic compound having an amide group. These compounds have a stronger bonding force to Al than water molecules, and therefore can replace water molecules existing around Al and coordinate in a manner of surrounding Al. It replaces water molecules contained in hydrates contained in the electrolyte, such as hydrates of synthesized Al compounds, and unreacted aluminum halide hydrates remaining in the electrolyte. That is, the ligand has a function as a dehydrating agent that removes water molecules (H2O ligands) surrounding Al.

[0059] Phosphorus compounds are a general term for compounds containing phosphorus atoms (P), such as phosphates, phosphonic acid, phosphinic acid, phosphinates, phosphine oxides, etc. Phosphoric acid esters may be any of monoesters, diesters, and triesters, preferably triesters. Phosphoric acid esters may include, for example, alkyl phosphates such as trimethyl phosphate, triethyl phosphate, tripropyl phosphate, tributyl phosphate, and trioctyl phosphate, phosphates (alkyl) aryl esters such as triphenyl phosphate, tricresyl phosphate, and tri(xylene) phosphate, tributoxyethyl phosphate, etc., and tributyl phosphate is particularly preferred. Phosphonic acid, phosphinic acid, phosphinates, and phosphine oxides may be derivatives formed by replacing at least one of the H atoms bonded to the phosphorus atom with an organic group such as an alkyl group, an aryl group, an alkyl group, an alkoxy group, etc. Among these compounds, the phosphorus compound is preferably selected from the group consisting of phosphonic acid, phosphinic acid, phosphine oxide, and tributyl phosphate, and is particularly preferably selected from the group consisting of phosphinic acid, phosphine oxide, and tributyl phosphate.

[0060] Examples of organic compounds having an amide group include aliphatic amides and aromatic amides. These amides may be any of primary amides, secondary amides, and tertiary amides, preferably secondary or tertiary amides. Examples of primary amides include formamide, acetamide, propionamide, butyramide, benzamide, etc. Examples of secondary amides include N-methylformamide, N-ethylformamide, N-methylacetamide, N-ethylacetamide, N-phenylformamide, N-phenylacetamide, etc. Examples of tertiary amides include dimethylformamide, diethylformamide, dimethylacetamide, diethylacetamide, N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, etc. Among these compounds, the organic compound having an amide group is preferably selected from the group consisting of N-phenylacetamide, dimethylformamide, and dimethylacetamide, and is particularly preferably selected from dimethylformamide and dimethylacetamide.

[0061] <Electrodeposition of Aluminum>

[0062] After preparing the electrolyte, electricity is passed between the anode and the cathode in the electrolyte, that is, aluminum is electrodeposited on the cathode by electrolysis. The electrolysis is as follows: an electrolytic cell filled with an electrolyte is prepared, the cathode and the anode are arranged opposite to each other in the electrolyte, and a voltage or current or both are applied between the two electrodes to conduct electricity, thereby electrodepositing Al on the cathode surface. In addition, during the electrodeposition, water from the aluminum halide hydrate reacts with the electrodeposited product, and aluminum oxide or hydroxide is electrodeposited simultaneously with the electrodeposited Al, but the electrodeposited amount of these byproducts is very small, and Al is mainly electrodeposited.

[0063] (Electrodeposition Conditions)

[0064] The electrodeposition temperature, i.e., the temperature of the electrolytic bath during electrodeposition, is preferably 20°C or more and 100°C or less, more preferably 20°C or more and 80°C or less, and further preferably 30°C or more and 70°C or less. The lower limit of 20°C is set to a temperature near room temperature. On the other hand, if the electrodeposition temperature exceeds 100°C, volatilization of the nitrile organic solvent in the electrolyte is likely to occur, causing the composition of the electrolyte to become unstable. As a result, if poor electrodeposition occurs, it becomes difficult to precipitate Al.

[0065] The electrodeposition is preferably carried out by constant potential electrolysis at an electrode potential of -6.0 V or more and less than 0 V relative to aluminum used as a reference electrode, or by a current density of 1 μA cm -2 Above and 10000μAcm -2 The following constant current electrolysis is carried out. The so-called constant potential electrolysis is a method of performing electrolysis while keeping the electrode potential of one side of the anode or cathode immersed in the electrolyte constant relative to the reference electrode. During constant potential electrolysis, the electrode potential is set as follows: relative to the Al line as the reference electrode, the potential region lower than 0V vs Al / Al(III) where the reduction current is observed, preferably an electrode potential of -4.0V or more and less than 0V, more preferably -2.0V or more and -0.7V or less. If the electrode potential is less than -6.0, the electrodeposition rate is too slow, resulting in a decrease in the electrodeposition efficiency, resulting in difficulty in depositing Al. Moreover, the so-called constant current electrolysis is a method of performing electrolysis while keeping the current value constant. The current density during constant current electrolysis is preferably 10μAcm -2 Above and 10000μAcm -2 Below, more preferably 20μAcm -2 Above and 1000μAcm -2 Below, more preferably 30 μAcm -2 Above and 500μAcm -2 Below, particularly preferably 50 μAcm -2 Above and 300μAcm -2 If the current density is less than 1μAcm-2 , the electrodeposition rate is too slow, resulting in a decrease in electrodeposition efficiency, thus making it difficult to precipitate Al. On the other hand, if the current density exceeds 10000 μA / cm -2 , the electrolytic bath is likely to decompose, and as a result, it becomes difficult to precipitate Al.

[0066] (Cathode)

[0067] In the method for preparing aluminum of the present invention, the cathode is not particularly limited. For example, a cathode made of a metal material such as platinum, gold, or copper can be used to precipitate Al on the metal material for recovery. Alternatively, a cathode made of a metal material with a passivation film (oxide film) such as titanium, nickel, or stainless steel can be used to precipitate Al on the passivation film, and the precipitated Al can be continuously peeled off and recovered by utilizing the property of low adhesion between the passivation film and Al. Moreover, the material of the cathode is not limited to metal materials, and a cathode made of carbon, a conductive plastic material, etc. can also be used.

[0068] (Anode)

[0069] Moreover, the anode is not particularly limited. By using soluble aluminum, the aluminum source consumed in the electrolyte during electrodeposition can be replenished from the anode. As an insoluble anode, a pure metal electrode such as platinum or titanium, or a titanium electrode coated with an insoluble metal such as platinum, iridium oxide, ruthenium oxide, or lead dioxide can be used.

[0070] [Examples]

[0071] Next, the present invention will be described in more detail based on examples, but the present invention is not limited to these examples.

[0072] [Examples 1 - 40, Comparative Examples 1 - 8]

[0073] Aluminum was prepared in the following order.

[0074] <Synthesis of Al Compound>

[0075] The ionic liquid and aluminum halide compound shown in Table 1 were used and mixed so that the ionic liquid:aluminum halide compound = 3:1 (molar ratio). Then, the obtained mixture was heated at 120 °C to prepare an aluminum compound as the desired Al source. As an example, the synthesis reaction formulas of Example 1 are shown in Formulas (2) and (3).

[0076] AlCl3·6H2O + 3HTFSI → Al(TFSI)3 + 3HCl + 6H2O (2)

[0077] AlCl3·6H2O + 3HTFSI → Al(TFSI)3·6(H2O) + 3HCl (3)

[0078] In addition, in Table 1, regarding the ionic liquids used in Comparative Examples 2 to 4, EMIC represents "1-ethyl-3-methylimidazolium chloride", EMIFSI represents "1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide", and LiBETI represents "lithium bis(pentafluoroethylsulfonyl)imide".

[0079] <Preparation of electrolyte>

[0080] Dissolve 2 g of the synthesized Al compound in 20 ml of the nitrile organic solvent shown in Table 1 to prepare an electrolyte.

[0081] <Dehydration of water molecules>

[0082] Add a specified amount of each ligand shown in Table 1 dropwise to the electrolyte, and keep it for two days or more under the state of heating and stirring at the temperature (dehydration temperature) shown in Table 1 using a heating stirrer, thereby removing water molecules.

[0083] <Electrodeposition of Al>

[0084] Use a Cu plate as the cathode and glassy carbon as the anode, and perform potentiostatic electrolysis and galvanostatic electrolysis under the electrodeposition conditions shown in Table 1. After electrolysis, wash the cathode with water and dry it, and electrodeposit Al on the cathode.

[0085] In each example and comparative example, the electrodeposits obtained on the cathode were evaluated as follows. The electrodeposition conditions and evaluation results are shown in Table 1.

[0086] [Table 1]

[0087]

[0088] <Appearance observation>

[0089] Visually confirm the electrodeposit on the cathode. Evaluate the case where Al is electrodeposited evenly without electrodeposition unevenness as "◎", the case where electrodeposition unevenness is observed but the electrodeposit can be visually confirmed as "○", the case where the current or voltage can be confirmed during electrolysis although the electrodeposit cannot be visually confirmed as "△", and the case where neither the current nor the voltage is confirmed during electrolysis and Al is not electrodeposited as "×". That is, if the evaluation is "△" or above, it is evaluated that Al can be electrodeposited.

[0090] <sem-eds>

[0091] In order to analyze the obtained electrodeposition in more detail, a scanning electron microscope (SEM: Scanning Electron Microscope) (manufactured by JEOL Ltd., trade name: JSM-6010PLUS) and an energy dispersive X-ray spectrometer (EDS: Energy Dispersive X-ray Spectroscope) built into the SEM were used for SEM-EDS analysis. The case where Al was clearly detected was evaluated as "◎", the case where Al was detected was evaluated as "○", the case where Al was detected in small amounts was evaluated as "△", and the case where Al was not detected was evaluated as "×".

[0092] <xrd>

[0093] In order to analyze the obtained electrodeposited product in more detail, X-ray diffraction (XRD) was performed using an X-ray diffraction device (manufactured by BRUKER, trade name: D2 PHASER). The case where a strong peak of Al could be confirmed was evaluated as "◎", the case where a peak of Al could be confirmed was evaluated as "○", the case where a weak peak of Al could be confirmed was evaluated as "△", and the case where no peak of Al could be confirmed was evaluated as "×".

[0094] <Electrodeposition Efficiency>

[0095] The weight of the obtained electrodeposited product (recovery amount) was measured, and the electrodeposition efficiency (recovery rate) was calculated based on the ratio of the recovery amount to the theoretical yield. According to Faraday's law, the theoretical yield was calculated by the following formula (4). When the recovery rate was 50% or more, the electrodeposition efficiency was determined to be high and recorded as "0", and when the recovery rate was less than 50%, the electrodeposition efficiency was determined to be low and recorded as "×".

[0096] Theoretical yield = (current density × film forming area × film forming time × atomic weight of Al) / (valence of Al ions × Faraday constant) (4)

[0097] · Atomic weight of Al = 26.98,

[0098] Ion valence = 3,

[0099] Faraday constant = 96500 [C·mol -1 ]

[0100] <Overall Evaluation>

[0101] The case where the electrodeposition efficiency is "○" and all the other three items of appearance observation, SEM-EDS and XRD are "◎" is evaluated as "◎◎"; the case where there is 1 or 2 evaluation items of "◎" and the remaining items are ○ is evaluated as "◎"; the case where there is 1 evaluation item of "△" and the remaining items are "○" or "◎", or the case where all items are "0" is evaluated as "○"; the case where there are more than 2 evaluation items of "△" and the remaining items are "○" or "△" is evaluated as "△", and the case where there is more than 1 evaluation item of "×" is evaluated as "×".

[0102] In Examples 1 to 40, the ionic liquid, the aluminum halide compound and the organic solvent are within the range specified in the present invention, so Al can be prepared by electrodeposition. That is, in Examples 1 to 40, aluminum can be electrodeposited from aluminum halide hydrate by the ionic liquid method, instead of the raw material anhydrous aluminum halide which is not preferred from the viewpoint of preparation cost, energy consumption, etc. As a result, aluminum can be prepared at a lower cost and with less energy consumption than in the past. Moreover, in any of Examples 1 to 40, the recovery rate of aluminum as an electrodeposited product is high, and aluminum can be efficiently electrodeposited. In addition, in Examples 1 to 4, 12, 17 to 19, 24, 25, 28 to 33, and 35 to 39, the comprehensive evaluation is "◎" or above, so aluminum can be electrodeposited more efficiently as a whole, especially in Examples 1 to 4, 29 to 30, 32 to 33, and 36 to 37, which are comprehensively evaluated as "◎◎", aluminum can be further efficiently electrodeposited.

[0103] In Comparative Example 1, no ligand was used, so although Al electrodeposition was confirmed, the electrodeposition efficiency was inferior to that of the examples. In Comparative Examples 2 to 4, the ionic liquid was not suitable, in Comparative Example 5, the aluminum halide hydrate was not used, in Comparative Examples 6 to 7, the organic solvent was not suitable, and in Comparative Example 8, the ligand was not suitable, so the desired electrolyte could not be prepared. As a result, Al electrodeposition could not be performed, and Al was not prepared.< / xrd>

Claims

1. A method for preparing aluminum, characterized in that: Including the following processes: A step of synthesizing an aluminum compound derived from perfluoroalkylsulfonyl imide aluminum or perfluoroalkylsulfonamide aluminum from a mixture containing a perfluoroalkylsulfonyl imide type or perfluoroalkylsulfonamide type ionic liquid represented by the following general formula (1) and an aluminum halide hydrate, In formula (1), Rf 1 and Rf 2 Independently of each other, they are CF3 or C4F9, and M is H, an alkali metal, a quaternary ammonium or an imidazolium; A step of dissolving the aluminum compound in a nitrile organic solvent to prepare an aluminum electrolyte; A step of adding a phosphorus compound or an organic compound having an amide group as a ligand to the aluminum electrolyte to remove water molecules from the hydrate contained in the aluminum electrolyte; After the dehydration step, a current is passed between the anode and the cathode in the aluminum electrolyte to electrodeposit aluminum on the cathode.

2. The method for preparing aluminum according to claim 1, wherein: In the dehydration step, the aluminum electrolyte to which the at least one ligand is added is stirred at a temperature of 0° C. to 100° C.

3. The method for preparing aluminum according to claim 1 or 2, wherein: In the electrodeposition step, constant potential electrolysis is performed at an electrode potential of -6.0 V or more and less than 0 V relative to aluminum used as a reference electrode or at a current density of 1 μA cm -2 Above and 10000μAcm -2 The following constant current electrolysis.

4. The method for preparing aluminum according to claim 1 or 2, wherein: In the electrodeposition step, the temperature of the electrolytic bath is 20° C. or higher and 100° C. or lower.

5. The method for preparing aluminum according to claim 1 or 2, wherein: In the general formula (1), Rf 1 and Rf 2 It is CF3.

6. The method for preparing aluminum according to claim 1 or 2, wherein: The aluminum halide hydrate is aluminum (III) chloride hexahydrate.

7. The method for preparing aluminum according to claim 1 or 2, wherein: The phosphorus compound is selected from the group consisting of phosphonic acid, phosphinic acid, phosphine oxide and tributyl phosphate.

8. The method for preparing aluminum according to claim 1 or 2, wherein: The organic compound having an amide group is selected from the group consisting of N-phenylacetamide, dimethylformamide and dimethylacetamide.