Display device and method of manufacturing the same

By using a second laser beam to form a mixing area between the glass frit and the base material in the crack starting area during the display device manufacturing process, the crack problem caused by laser sealing is solved, and the mechanical strength and sealing performance of the display device are improved.

CN111697164BActive Publication Date: 2024-11-26SAMSUNG DISPLAY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010149716.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-03-13
Filing Date
2020-03-06
Publication Date
2024-11-26
Estimated Expiration
2040-03-06

AI Technical Summary

Technical Problem

When manufacturing organic light emitting display equipment, when using laser sealing glass frit, it may deteriorate the thickness and bonding surface uniformity of the glass frit, leading to crack problems, affecting mechanical strength and sealing performance.

Method used

By radiating the first laser beam in the first sealing region to melt the glass frit, the first mother substrate is combined with the second mother substrate, and radiating the second laser beam at the crack starting point region to form the second sealing region, so that the glass frit and the substrate are mixed with the glass frit and the substrate. Mix the materials to enhance bonding properties.

Benefits of technology

The mechanical strength and bonding characteristics of the display device are improved, the external impact propagation speed is reduced, the sealing performance is enhanced, and the bonding strength is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111697164B_ABST
    Figure CN111697164B_ABST
Patent Text Reader

Abstract

A display device and a method for manufacturing the display device are provided. The method for manufacturing the display device includes: forming a plurality of displays each including a light emitting diode on a surface of a first mother substrate; preparing a second mother substrate; forming a first sealing area on a surface of at least one of the first mother substrate and the second mother substrate, wherein the first sealing area surrounds each of the plurality of displays and includes glass frit; first bonding the first mother substrate to the second mother substrate by irradiating a first laser beam to melt the glass frit in the first sealing area; and second bonding the first mother substrate to the second mother substrate by partially irradiating a second laser beam to the first sealing area to form a second sealing area, in which the glass frit and the first mother substrate and / or the glass frit and the second mother substrate are melted and mixed with each other.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application claims priority to and the benefit of Korean Patent Application No. 10-2019-0028859 filed on March 13, 2019, in the Korean Intellectual Property Office, the disclosure of which is incorporated herein in its entirety by reference. Technical Field

[0002] Aspects of one or more embodiments are directed to a display apparatus and a method of manufacturing the display apparatus. Background Art

[0003] The organic light emitting display device has a characteristic that it is degraded due to moisture penetration. Therefore, when a sealing process for isolating the organic light emitting diode from the outside is performed during the manufacture of the display device, a glass frit having a high internal pressure characteristic and an excellent sealing characteristic is used.

[0004] In order to seal using glass frit, laser may be used to greatly reduce the thermal effect on the organic light emitting diode and melt the glass frit. However, when sealing is performed by using laser, the thickness of the glass frit and the uniformity of the bonding surface between the glass frit and the substrate may be deteriorated. Therefore, problems such as cracks in the bonding surface may occur. Summary of the invention

[0005] According to an aspect of one or more embodiments, there is provided a display device whose mechanical strength is enhanced by improving the bonding characteristics of a region where cracks are generated. However, the embodiments described herein are merely examples, and the scope of the present invention is not limited thereto.

[0006] Additional aspects will be set forth in part in the description which follows and, in part, will be apparent from the description, or may be learned by practice of the presented embodiments.

[0007] According to one or more embodiments, a method for manufacturing a display device includes the following steps: forming a plurality of displays each including a light-emitting diode on a surface of a first mother substrate; preparing a second mother substrate; forming a first sealing area on a surface of at least one of the first mother substrate and the second mother substrate, wherein the first sealing area surrounds each of the plurality of displays and includes glass frit; bonding the first mother substrate to the second mother substrate for the first time by irradiating a first laser beam to melt the glass frit in the first sealing area; and bonding the first mother substrate to the second mother substrate for the second time by forming a second sealing area by partially irradiating a second laser beam into the interior of the first sealing area, wherein the glass frit and the first mother substrate and / or the glass frit and the second mother substrate are melted and mixed with each other.

[0008] The first sealing area may include a first end arranged near or close to each of the multiple displays and a second end arranged away from or far from each of the multiple displays, and the center of the second laser beam may move from a position closer to the first end than the second end along a path traveled by the second laser beam.

[0009] The second laser beam may be centered between a point corresponding to ¼ of the width of the first sealing area from the first end and a point corresponding to ½ of the width of the first sealing area from the first end and move along a path along which the second laser beam travels.

[0010] The width of the second laser beam may be smaller than the width of the first laser beam.

[0011] The frequency of the second laser beam may be higher than the frequency of the first laser beam.

[0012] The first laser beam may be a continuous wave laser beam.

[0013] The second laser beam may be a femtosecond laser beam.

[0014] The first sealing area may have a closed loop shape surrounding a periphery of each of the plurality of displays.

[0015] The second sealing area may be formed continuously in the first sealing area.

[0016] The second sealing area may be formed discontinuously in the first sealing area.

[0017] When the second sealing region is viewed from a surface perpendicular to a main surface of the first mother substrate, the second sealing region may be formed to include a portion protruding toward the first mother substrate from a surface where the frit contacts the first mother substrate.

[0018] When the second sealing region is viewed from a surface perpendicular to a main surface of the second mother substrate, the second sealing region may be formed to include a portion protruding toward the second mother substrate from a surface where the frit contacts the second mother substrate.

[0019] When the second sealing area is viewed from a surface perpendicular to the main surface of the first mother substrate, the second sealing area can be formed to include a portion protruding toward the first mother substrate from the surface where the glass material contacts the first mother substrate, and when the second sealing area is viewed from a surface perpendicular to the main surface of the second mother substrate, the second sealing area can be formed to include a portion protruding toward the second mother substrate from the surface where the glass material contacts the second mother substrate.

[0020] The method may further include cutting the first mother substrate and the second mother substrate for each of the plurality of displays after second bonding the first mother substrate to the second mother substrate.

[0021] The method may further include cutting the first mother substrate and the second mother substrate for each of the plurality of displays, wherein the step of second bonding the first mother substrate to the second mother substrate is performed for each of the plurality of cut and separated displays.

[0022] According to one or more embodiments, a display device includes: a first substrate; a display arranged on the first substrate and including a light emitting diode; a second substrate facing the first substrate; a first sealing area arranged between the first substrate and the second substrate, surrounding the display, and including glass material; and a second sealing area arranged in the first sealing area and including at least one portion protruding toward the first substrate and / or the second substrate.

[0023] The first substrate and / or the second substrate may include a glass material.

[0024] The first sealing area may have a closed loop shape surrounding a periphery of the display.

[0025] The first sealing area may include a first end disposed near or close to the display and a second end disposed away from or distal to the display, and a center of the second sealing area may be closer to the first end than the second end.

[0026] The center of the second sealing area may be located between a point corresponding to ¼ of the width of the first sealing area from the first end and a point corresponding to ½ of the width of the first sealing area from the first end.

[0027] The width of the second sealing area may be smaller than the width of the first sealing area.

[0028] The second sealing region may include a region where the glass frit and the material of the first substrate and / or the glass frit and the material of the second substrate are melted and mixed with each other.

[0029] The second sealing area may be formed continuously in the first sealing area.

[0030] The second sealing area may be formed discontinuously in the first sealing area. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] These and / or other aspects will become clear and more readily understood through the following description of some example embodiments in conjunction with the accompanying drawings, in which:

[0032] Figure 1 is a schematic flow chart showing a method of manufacturing a display device according to an embodiment;

[0033] Figure 2 is a schematic plan view showing a method of manufacturing a display device according to an embodiment;

[0034] Figure 3A yes Figure 2 An enlarged schematic cross-sectional view of a region III of FIG. 1 , wherein a process of irradiating a first laser beam is shown;

[0035] Figure 3B yes Figure 2 An enlarged schematic plan view of a region III of FIG. 1 , wherein a process of irradiating a first laser beam is shown;

[0036] Figure 4 is a cross-sectional view of an active matrix organic light emitting device as an example of a display;

[0037] Figure 5 yes Figure 3B An enlarged view of region V;

[0038] Fig. 6A is a schematic cross-sectional view showing a process of irradiating a second laser beam;

[0039] Figure 6B is a schematic plan view showing a process of irradiating a second laser beam;

[0040] Figure 7 It is along Figure 6B A cross-sectional view of the display device taken along line VII-VII;

[0041] Figure 8 is a cross-sectional view showing a second sealing area according to an embodiment;

[0042] Fig. 9 is a cross-sectional view showing a second sealing area according to an embodiment;

[0043] Fig.10 is a plan view showing a second sealing area according to an embodiment;

[0044] Fig.11 is a cross-sectional view showing a second sealing area according to an embodiment;

[0045] Fig.12 is a graph for comparing the bonding strength between a first sample and a second sample; and

[0046] Fig.13 is a diagram illustrating an operation in which a plurality of displays are divided into unit cells by cutting a first mother substrate and a second mother substrate. DETAILED DESCRIPTION

[0047] Now will be more detailed with reference to the embodiment of its example shown in the accompanying drawings, wherein the same reference numerals always represent the same elements. In this respect, the present embodiment can have different forms and should not be construed as being limited to the description set forth herein. Therefore, the following only describes the embodiments with reference to the accompanying drawings to explain the various aspects of this description. As used herein, the term "and / or" includes any combination and all combinations of one or more related listed items. When an expression such as "at least one (kind / person) of ... " is after a column of elements, the entire column of elements is modified without modifying the individual elements in the column.

[0048] Since the present disclosure allows various changes and many embodiments, some example embodiments will be shown in the figures and further described in detail in the written description. Through the detailed description of various embodiments disclosed below in conjunction with the accompanying drawings, the effects and features of the present disclosure and the methods for achieving them will become clear to those skilled in the art. However, the present disclosure can be implemented in many different forms and should not be construed as being limited to the example embodiments set forth herein.

[0049] It will be understood that although the terms "first", "second", etc. may be used herein to describe various components, these components should not be limited by these terms. These terms are used to distinguish one component from another.

[0050] As used herein, the singular forms "a", "an" and "the" are intended to include the plural forms as well, unless the context clearly indicates otherwise.

[0051] It will also be understood that the terms “comprises,” “comprising,” and variations thereof used herein specify the presence of stated features or components, but do not preclude the presence or addition of one or more other features or components.

[0052] It will be understood that when a layer, region, or component is referred to as being "formed on" another layer, region, or component, the layer, region, or component may be directly or indirectly formed on the other layer, region, or component. That is, for example, there may be one or more intermediate layers, regions, or components. Also, for example, when a layer, region, or component is referred to as being electrically "connected to" or electrically "coupled to" another layer, region, or component, the layer, region, or component may be directly electrically connected to or directly electrically coupled to the other layer, region, or component, or indirectly electrically connected to or indirectly electrically coupled to the other layer, region, or component with one or more intermediate elements located therebetween.

[0053] When a certain embodiment can be implemented differently, the specific process order may be different from the described order. For example, two processes described in succession may be performed substantially simultaneously or in an order opposite to the described order.

[0054] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the exemplary embodiments of the inventive concepts belong. It will also be understood that terms (such as those defined in general dictionaries) should be interpreted as having a meaning consistent with their meaning in the context of the relevant art, and will not be interpreted in an idealized or overly formal sense unless expressly so defined herein.

[0055] Figure 1 is a schematic flowchart illustrating a method of manufacturing a display device according to an embodiment.

[0056] Reference Figure 1 According to an embodiment, the method for manufacturing a display device includes: forming a plurality of displays each including a light emitting diode on a surface of a first mother substrate (S10); preparing a second mother substrate (S20); forming a first sealing area surrounding the displays and including glass material on a surface of the first mother substrate or the second mother substrate (S30); first bonding the first mother substrate to the second mother substrate by irradiating a first laser beam to melt the glass material in the first sealing area (S40); bonding the first mother substrate to the second mother substrate for a second time by forming a second sealing area by partially irradiating a second laser beam to the inside of the first sealing area (S50), in which the glass material and the first mother substrate and / or the glass material and the second mother substrate are melted and mixed.

[0057] Figure 2 is a schematic plan view showing a method of manufacturing a display device according to an embodiment; Figure 3A yes Figure 2 An enlarged schematic cross-sectional view of a region III of FIG. 1 , showing a process of irradiating a first laser beam; and Figure 3B yes Figure 2 An enlarged schematic plan view of region III of FIG. 1 , wherein a process of irradiating a first laser beam is shown.

[0058] Reference Figure 2 , prepare the first mother substrate 1 and the second mother substrate 2 facing each other. Then, a plurality of displays 3 are formed on the surface of the first mother substrate 1 as one of the first mother substrate 1 and the second mother substrate 2. The first sealing area 51 has a closed loop shape surrounding the periphery of each display 3.

[0059] In an embodiment, the first mother substrate 1 and the second mother substrate 2 may include a transparent glass material, but are not limited thereto.

[0060] In an embodiment, each display 3 comprises a plurality of light emitting diodes. According to an embodiment, the display 3 may comprise a plurality of organic light emitting diodes.

[0061] Figure 4 An active matrix organic light emitting device is shown as an example of the display 3 .

[0062] like Figure 4 As shown in the figure, an insulating layer 11 such as a barrier layer and / or a buffer layer can be formed on the upper surface of the first mother substrate 1, wherein the insulating layer 11 is constructed to prevent or substantially prevent impurity ions from diffusing into the first mother substrate 1, is constructed to prevent or substantially prevent moisture or external air from penetrating into the first mother substrate 1, and is constructed to planarize the surface of the first mother substrate 1.

[0063] On the insulating layer 11, an active layer 12 of a thin film transistor (TFT) is formed of a semiconductor material, and a gate insulating layer 13 is formed to cover the insulating layer 11 and the active layer 12. The active layer 12 may include an inorganic material semiconductor such as amorphous silicon or polycrystalline silicon or an organic semiconductor. The active layer 12 includes a source region 12b, a drain region 12c, and a channel region 12a located between the source region 12b and the drain region 12c.

[0064] The gate electrode 14 is arranged on the gate insulating layer 13, and the interlayer insulating layer 15 is formed to cover the gate insulating layer 13 and the gate electrode 14. In addition, the source electrode 16a and the drain electrode 16b are arranged on the interlayer insulating layer 15. Then, the planarization layer 17 and the pixel defining layer 18 are sequentially arranged to cover the interlayer insulating layer 15, the source electrode 16a, and the drain electrode 16b.

[0065] The gate insulating layer 13 , the interlayer insulating layer 15 , the planarizing layer 17 , and the pixel defining layer 18 may include an insulator and be formed to have a single-layer or multi-layer structure including an organic material, an inorganic material, or an organic / inorganic composite material.

[0066] However, the stack structure of the above-mentioned TFT is not limited thereto, and any one of various structures of the TFT may be adopted.

[0067] A pixel electrode 31 as an electrode of an organic light emitting diode is disposed on the planarization layer 17. A pixel defining layer 18 is disposed on the planarization layer 17. An opening is formed in the pixel defining layer 18 to expose the pixel electrode 31. Then, an organic light emitting layer 32 of the organic light emitting diode is formed.

[0068] In an embodiment, the organic light emitting diode displays image information by emitting red light, green light, blue light or white light according to the flow of current. The organic light emitting diode includes a pixel electrode 31 contacting the drain electrode 16b of the TFT via a contact hole, a counter electrode 33 arranged to cover all pixels, and an organic light emitting layer 32 arranged between the pixel electrode 31 and the counter electrode 33 and configured to emit light.

[0069] The pixel electrode 31 is insulated from the counter electrode 33 by the organic light emitting layer 32. The pixel electrode 31 and the counter electrode 33 apply voltages of different polarities to the organic light emitting layer 32, so that the organic light emitting layer 32 emits light.

[0070] In an embodiment, the organic light emitting layer 32 may include a low molecular weight organic film or a polymer organic film. When a low molecular weight organic film is used, the organic light emitting layer 32 may include a single layer or multilayer structure in which a hole injection layer (HIL), a hole transport layer (HTL), an emission layer (EML), an electron transport layer (ETL), an electron injection layer (EIL), etc. are stacked. The organic light emitting layer 32 may include a material such as copper phthalocyanine (CuPc), N,N'-di(naphthalene-1-yl)-N,N'-diphenyl-benzidine (NPB), tri-8-hydroxyquinoline aluminum (Alq 3 ) and the like. Such a low molecular weight organic film can be formed by using a vacuum deposition method. HIL, HTL, ETL, EIL, etc. are common layers and can be commonly applied to pixels of red light, green light, blue light or white light. In an embodiment, like the counter electrode 33, the common layer can be formed to cover all pixels.

[0071] In the embodiment, the pixel electrode 31 is used as an anode electrode, and the counter electrode 33 is used as a cathode electrode. However, the polarities of the pixel electrode 31 and the counter electrode 33 may be opposite to those described above.

[0072] When the display device is a bottom emission type display device in which an image is presented in a direction toward the first mother substrate 1, the pixel electrode 31 may be a transparent electrode, and the counter electrode 33 may be a reflective electrode. In this case, the pixel electrode 31 may be made of indium tin oxide (ITO), indium zinc oxide (IZO), zinc oxide (ZnO), or indium oxide (In 2 O 3 ), the counter electrode 33 can be formed of a metal with a low work function such as silver (Ag), magnesium (Mg), aluminum (Al), platinum (Pt), palladium (Pd), gold (Au), nickel (Ni), neodymium (Nd), iridium (Ir), chromium (Cr), lithium (Li), calcium (Ca), etc.

[0073] When the display device is a top emission type display device in which an image is presented in a direction toward the counter electrode 33, the pixel electrode 31 may include a reflective electrode, and the counter electrode 33 may include a transparent electrode. In this case, the reflective electrode as the pixel electrode 31 may be arranged to include a reflective layer formed of Ag, Mg, Al, Pt, Pd, Au, Ni, Nd, Ir, Cr, Li, Ca, or a mixture thereof, and ITO, IZO, ZnO, InO, etc., each having a high work function. 2 O 3In addition, the transparent electrode as the counter electrode 33 can be formed by depositing a metal having a low work function (i.e., Ag, Mg, Al, Pt, Pd, Au, Ni, Nd, Ir, Cr, Li, Ca, or a mixture thereof) and then forming a transparent electrode by using a metal such as ITO, IZO, ZnO, In 2 O 3 Auxiliary electrodes or bus electrode lines are formed by transparent conductive materials such as the above.

[0074] In the case of a dual emission type display device, both the pixel electrode 31 and the counter electrode 33 may include transparent electrodes.

[0075] However, the pixel electrode 31 and the counter electrode 33 are not limited to the above materials. In an embodiment, the pixel electrode 31 and the counter electrode 33 may be formed of a conductive organic material, a conductive paste including conductive particles such as Ag, Mg, Cu, etc. When such a conductive paste is used, the conductive paste may be printed by using an inkjet printing method, and after printing, the conductive paste may be sintered to form it into an electrode.

[0076] On the upper surface of the counter electrode 33 of the display 3 manufactured as described above, a passivation layer 34 may be further included to cover the display 3 .

[0077] The passivation layer 34 may include at least one organic layer and / or at least one inorganic layer.

[0078] The inorganic layer may include one or more inorganic insulating materials selected from aluminum oxide, titanium oxide, tantalum oxide, hafnium oxide, zinc oxide, silicon oxide, silicon nitride, and silicon oxynitride. The inorganic layer may be formed using a chemical vapor deposition (CVD) method or the like.

[0079] The organic layer may include polyethylene terephthalate, polyethylene naphthalate, polycarbonate, polyimide, polyvinyl sulfonate, polyoxymethylene, polyarylate, hexamethyldisiloxane, acrylic resin (eg, polymethyl methacrylate, polyacrylic acid, etc.), or a combination thereof.

[0080] like Figure 2 As shown in FIG. 1 , m displays 3 in a first direction (eg, X direction) and n displays 3 in a second direction (eg, Y direction) are arranged. Figure 2 , but a pad (or "pad") unit for connecting each display 3 to an external device may also be arranged in the periphery of each display 3. In this case, the display 3 and the pad unit (not shown) may constitute one unit cell. The respective unit cells are arranged adjacent to each other.

[0081] In addition, a first sealing region 51 is formed around each display 3. In an embodiment, glass frit in a paste state is applied to the surface of the second mother substrate 2 facing the first mother substrate 1, and then pre-sintered to harden the glass frit. However, the first sealing region 51 including glass frit may be formed on the surface of the first mother substrate 1 facing the second mother substrate 2. In an embodiment, the first sealing region 51 including glass frit may be formed on both the surface of the second mother substrate 2 facing the first mother substrate 1 and the surface of the first mother substrate 1 facing the second mother substrate 2. The glass frit in a paste state may be sequentially applied to each unit cell by using a dispenser, or the glass frit in a paste state may be applied to each unit cell together by using a screen printing method.

[0082] Reference Figure 3A and Figure 3B After aligning the second mother substrate 2 and the first mother substrate 1 (in which a first sealing area 51 including glass material is formed on the second mother substrate 2 and the first mother substrate 1), a first laser beam L1 having a first width WL1 is radiated toward the first sealing area 51 by a first laser irradiator 61, thereby bonding the first mother substrate 1 to the second mother substrate 2.

[0083] The first width WL1 of the first laser beam L1 may be substantially the same as the first width WS1 of the first sealing area 51. Figure 3A and Figure 3B , but a mask having an opening formed therein may be disposed between the first laser irradiator 61 and the first sealing area 51, and the first laser beam L1 may be irradiated through the opening of the mask toward the first sealing area 51. The first width WL1 of the first laser beam L1 may be the width of the laser beam having passed through the opening.

[0084] exist Figure 3A , the first laser beam L1 is shown as radiating from above the second mother substrate 2. However, the irradiation of the first laser beam L1 is not limited thereto. In an embodiment, the first laser beam L1 may be radiated from below the first mother substrate 1, or (e.g., simultaneously) from above the second mother substrate 2 and below the first mother substrate 1.

[0085] Laser that can melt the glass frit may be used as the first laser beam L1. For example, the first laser beam L1 may be a continuous wave (CW) laser beam that has a Gaussian distribution characteristic and can be continuously oscillated at a constant output.

[0086] However, when the substrate is sealed by melting the frit using a CW laser beam having a Gaussian distribution characteristic, uniformity of both thickness of the frit and a bonding surface may be deteriorated, and thus, problems such as cracks generated in the bonding surface between the frit and the substrate may occur.

[0087] Figure 5 yes Figure 3B Magnified view of region V.

[0088] Reference Figure 5 , it can be understood that a plurality of first cracks CR1 and a plurality of second cracks CR2 may appear in the first sealing area 51. The first sealing area 51 includes a first end 511 disposed near or close to the display 3 and a second end 512 disposed away from or far from the display 3. It can be understood that the starting points S1 and S2 of the first crack CR1 and the second crack CR2 start from the inside of the first sealing area 51 and extend to the second end 512 of the first sealing area 51. When the starting points S1 and S2 of the first crack CR1 and the second crack CR2 are viewed from the virtual center line 510 of the first sealing area 51, the starting points S1 and S2 of the first crack CR1 and the second crack CR2 may be formed closer to the first end 511 than the second end 512.

[0089] In this way, since a plurality of first cracks CR1 and a plurality of second cracks CR2 appear in the first sealing region 51, when an external impact is applied, the mechanical strength may be deteriorated, and defects in the display device may be caused by moisture penetration into the display device. In the present embodiment, in order to solve such a problem, by irradiating a second laser beam L2 toward the inside of the first sealing region 51 where the starting points S1 and S2 of the first cracks CR1 and the second cracks CR2 are concentratedly distributed, the glass frit and the first mother substrate 1 and the second mother substrate 2 are melted in the region where the starting points S1 and S2 of the first cracks CR1 and the second cracks CR2 are formed, thereby bonding the glass frit to the first mother substrate 1 and the second mother substrate 2 for the second time.

[0090] Fig. 6A is a schematic cross-sectional view showing a process of irradiating the second laser beam L2; and Figure 6B 2 is a schematic plan view showing a process of irradiating the second laser beam L2.

[0091] Reference Fig. 6A and Figure 6B A second laser beam L2 having a second width WL2 is radiated toward the interior of the first sealing area 51 by a second laser radiator 62, thereby forming a second sealing area 52, in which the glass material and the first mother substrate 1 and / or the glass material and the second mother substrate 2 are melted and mixed with each other.

[0092] The second width WL2 of the second laser beam L2 may be substantially the same as the second width WS2 of the second sealing area 52. Fig. 6A and Figure 6B, but a mask having an opening formed therein may be arranged between the second laser irradiator 62 and the second sealing area 52, and the second laser beam L2 may be irradiated toward the second sealing area 52 through the opening of the mask. The second width WL2 of the second laser beam L2 may be the width of the laser beam that has passed through the opening.

[0093] exist Fig. 6A , the second laser beam L2 is shown as radiating from above the second mother substrate 2. However, the radiation of the second laser beam L2 is not limited thereto. In an embodiment, the second laser beam L2 may be radiated from below the first mother substrate 1, or (e.g., simultaneously) from above the second mother substrate 2 and below the first mother substrate 1.

[0094] The second laser beam L2 may have high energy so that the heat generated in the glass frit is greatly reduced while the glass frit and the first mother substrate 1 and / or the glass frit and the second mother substrate 2 are melted together. For example, the second laser beam L2 may be a femtosecond laser beam. The frequency of the second laser beam L2 may be higher than that of the first laser beam L1.

[0095] The second sealing region 52 includes a region where the glass frit is mixed with a material of at least one of the first mother substrate 1 and the second mother substrate 2 by melting at least one of the first mother substrate 1 and the second mother substrate 2 using the second laser beam L2 .

[0096] On the bonding surface where the first sealing region 51 is bonded to the first mother substrate 1 and the second mother substrate 2, the boundary between the first sealing region 51 and the first mother substrate 1 and the second mother substrate 2 may be shown as a flat surface to distinguish the first sealing region 51 from the first mother substrate 1 and the second mother substrate 2. However, on the bonding surface where the glass frit of the second sealing region 52 is bonded to the first mother substrate 1 and the second mother substrate 2, the boundary between the glass frit and the first mother substrate 1 and the second mother substrate 2 may not be clear. For example, on the bonding surface where the glass frit of the second sealing region 52 is bonded to the first mother substrate 1 and the second mother substrate 2, two materials of at least one of the first mother substrate 1 and the second mother substrate 2 and the glass frit may be melted and mixed with each other, respectively, so that a protruding shape instead of a flat shape may be formed at the boundary between at least one of the first mother substrate 1 and the second mother substrate 2 and the glass frit.

[0097] Figure 7 It is along Figure 6B A cross-sectional view of the display device taken along line VII-VII.

[0098] Reference Figure 7 The second sealing region 52 includes a first portion 524 in the first sealing region 51 and a protruding portion 525 protruding in a direction toward the second mother substrate 2 .

[0099] The first sealed area 51 includes a first end 511 disposed near the display 3 and a second end 512 disposed away from the display 3. The first portion 524 of the second sealed area 52 is disposed between the first end 511 and the second end 512 of the first sealed area 51. The second width WS2 of the second sealed area 52 is smaller than the first width WS1 of the first sealed area 51.

[0100] As mentioned above Figure 5 As described, since the second laser beam L2 is radiated toward the area in which the starting points S1 and S2 of the first crack CR1 and the second crack CR2 are concentratedly distributed, the center 520 of the second sealing area 52 can be formed to be closer to the first end 511 than the second end 512. In an embodiment, the center 520 of the second sealing area 52 can be arranged between a point corresponding to 1 / 4 of the first width WS1 of the first sealing area 51 from the first end 511 and a point corresponding to 1 / 2 of the first width WS1 of the first sealing area 51 from the first end 511. However, the present disclosure is not limited thereto. For example, when the starting points S1 and S2 of the first crack CR1 and the second crack CR2 are arranged near the second end 512 of the first sealing area 51, the center 520 of the second sealing area 52 can be arranged to be closer to the second end 512 than the first end 511. In this way, the center 520 of the second sealing area 52 is not limited to a specific point in the first sealing area 51.

[0101] exist Figure 7 In the embodiment, the first sealing region 51 is bonded to the bonding surface where the first mother substrate 1 and the second mother substrate 2 are located, and the boundary between the first sealing region 51 and the first mother substrate 1 and the second mother substrate 2 can be shown as a flat surface. However, at the bonding surface where the glass frit of the second sealing region 52 is bonded to the second mother substrate 2, the two materials of the glass frit and the second mother substrate 2 can be melted and mixed with each other. Therefore, the protrusion 525 can be formed at the boundary between the glass frit and the second mother substrate 2. That is, when the second sealing region 52 is viewed from a surface perpendicular to the main surface of the second mother substrate 2, the second sealing region 52 is arranged to include a protrusion 525 protruding from the surface where the glass frit contacts the second mother substrate 2 toward the second mother substrate 2.

[0102] The protruding portion 525 is Figure 7 525 is shown as having a curved shape. However, this is only an example. Here, unlike the boundary surface between the first sealing area 51 and the second mother substrate 2, which is considered to be a flat surface, the protruding portion 525 may represent a bend caused when the boundary surface between materials with different melting points collapses. This indicates that the curved portion may protrude toward the second mother substrate 2. Compared with the flat portion, the protruding portion 525 can significantly reduce the speed at which the external impact propagates.

[0103] Figure 8 and Fig. 9 is a cross-sectional view showing an example of the second sealing area 52 .

[0104] Reference Figure 8 , the first portion 524 of the second sealing region 52 is located in the first sealing region 51 and is arranged closer to the first end 511 than the second end 512 of the first sealing region 51. When the second sealing region 52 is viewed from a surface perpendicular to the main surface of the first mother substrate 1, the second sealing region 52 is arranged to include a portion 526 protruding toward the first mother substrate 1 from the surface where the glass frit contacts the first mother substrate 1.

[0105] Reference Fig. 9 The first portion 524 of the second sealing region 52 is located in the first sealing region 51 and is arranged closer to the first end 511 than the second end 512 of the first sealing region 51 .

[0106] When the second sealing area 52 is viewed from a surface perpendicular to the main surface of the first mother substrate 1, the second sealing area 52 is arranged to include a portion 526 protruding from the surface where the glass material contacts the first mother substrate 1 toward the first mother substrate 1, and when the second sealing area 52 is viewed from a surface perpendicular to the main surface of the second mother substrate 2, the second sealing area 52 is arranged to include a protruding portion 525 protruding from the surface where the glass material contacts the second mother substrate 2 toward the second mother substrate 2.

[0107] Fig.10 is a plan view showing another embodiment of the second sealing area 52 .

[0108] The display 3 is disposed between the first mother substrate 1 and the second mother substrate 2. The first sealing region 51 is disposed to surround the display 3 and includes frit glass. Figure 6B The second sealing area 52 shown in FIG. 5 is formed continuously in the first sealing area 51 in a closed loop shape. On the other hand, Fig.10 The second sealing area 52 shown in FIG. 5 may be formed discontinuously in the first sealing area 51 .

[0109] Fig.11 is a cross-sectional view showing another embodiment of the second sealing area 52 .

[0110] Reference Fig.11 The first portion 524 of the second sealing region 52 is located in the first sealing region 51 and is arranged closer to the first end 511 than the second end 512 of the first sealing region 51 .

[0111] The second sealing region 52 includes a protruding portion 525 protruding toward the second mother substrate 2. The metal layer 70 is disposed between the second sealing region 52 and the first mother substrate 1 and between the first sealing region 51 and the first mother substrate 1.

[0112] In an embodiment, metal layer 70 may include the same material as that used for wirings, electrodes, etc. of display 3. Metal layer 70 may serve to quickly increase the temperature of first mother substrate 1 by converting energy received from the first laser beam into heat.

[0113] In an embodiment, the metal layer 70 may be melted with the glass frit by using the energy received from the second laser beam. Fig.11 Although not shown in FIG. 5 , the second sealing region 52 may also include a portion protruding toward the metal layer 70 .

[0114] As described above, according to various embodiments, the starting point of the crack can be removed by irradiating the second laser beam L2 toward an area in the first sealing region where the starting points of the cracks are concentratedly distributed so that the glass material and the substrate are melted and mixed with each other, and a protrusion can be formed at the boundary between the glass material and the substrate by melting the glass material and the substrate and mixing with each other, thereby reducing the speed at which the external impact spreads.

[0115] Fig.12 It is a graph for comparing the bonding strength between the first sample D1 and the second sample D2.

[0116] Reference Fig.12 The peel strength of the first sample D1 not including the second sealing area 52 is 4.94 kgf, while the peel strength of the second sample D2 including the second sealing area 52 is 5.78 kgf, which is about 17% higher than the peel strength of the first sample D1. That is, it can be understood that the bonding strength of the second sample D2 is increased.

[0117] Fig.13 1 is a diagram showing an operation in which a plurality of displays 3 are divided into unit cells by cutting the first mother substrate 1 and the second mother substrate 2 .

[0118] Reference Fig.13 By cutting the first mother substrate 1 and the second mother substrate 2 along a plurality of first scribe lines SLX1, SLX2 and SLX3 and a plurality of second scribe lines SLY1, SLY2 and SLY3 using a cutter, a laser, etc., a plurality of displays 3 can be divided into unit cells, wherein the first scribe lines SLX1, SLX2 and SLX3 extend in a first direction (e.g., X direction) and the second scribe lines SLY1, SLY2 and SLY3 extend in a second direction (e.g., Y direction).

[0119] In the above embodiment, if Fig.13As shown in , after the display 3 is divided into unit cells, a process of forming a second sealing region by irradiating a second laser beam may be performed on each unit cell.

[0120] According to the embodiment, the starting point of the crack can be removed by irradiating the second laser beam toward the area in the first sealing area where the starting point of the crack is concentratedly distributed so that the glass frit and the substrate are melted and mixed with each other, and a protrusion can be formed at the boundary between the glass frit and the substrate by melting the glass frit and the substrate and mixing with each other, thereby reducing the speed at which the external impact spreads. However, the above aspects and effects are only examples.

[0121] It will be understood that the embodiments described herein should be considered in a descriptive sense only and not for purposes of limitation. Descriptions of features or aspects within each embodiment should typically be considered as available for other similar features or aspects in other embodiments.

[0122] Although one or more embodiments have been described with reference to the drawings, it will be understood by those of ordinary skill in the art that various changes in form and details may be made therein without departing from the spirit and scope as set forth in the claims.

Claims

1. A method for manufacturing a display device, the method The following steps are involved: forming a plurality of displays each including a light emitting diode on a surface of the first mother substrate; preparing a second mother substrate; forming a first sealing region on a surface of at least one of the first mother substrate and the second mother substrate, wherein the first sealing region surrounds each of the plurality of displays and includes glass frit; bonding the first mother substrate to the second mother substrate for the first time by irradiating a first laser beam to melt the glass frit in the first sealing region; as well as A second sealing area is formed by partially irradiating a second laser beam into the interior of the first sealing area, and the first mother substrate is bonded to the second mother substrate for a second time. In the second sealing area, the glass material and the first mother substrate and / or the glass material and the second mother substrate are melted and mixed with each other.

2. The method according to claim 1, in, The first sealing area includes a first end disposed proximal to each of the plurality of displays and a second end disposed distal to each of the plurality of displays, and The center of the second laser beam moves from a position closer to the first end than the second end along a path along which the second laser beam travels.

3. The method according to claim 2, in, The center of the second laser beam is located between a point corresponding to 1 / 4 of the width of the first sealing area from the first end and a point corresponding to 1 / 2 of the width of the first sealing area from the first end, and moves along the path traveled by the second laser beam.

4. The method according to claim 1, in, The width of the second laser beam is smaller than the width of the first laser beam.

5. The method according to claim 1, in, The frequency of the second laser beam is higher than the frequency of the first laser beam.

6. The method according to claim 1, in, The first laser beam is a continuous wave laser beam.

7. The method according to claim 1, in, The second laser beam is a femtosecond laser beam.

8. The method according to claim 1, in, The first sealing area has a closed loop shape surrounding a periphery of each of the plurality of displays.

9. The method according to claim 1, in, The second sealing area is formed continuously in the first sealing area.

10. The method according to claim 1, in, The second sealing area is formed discontinuously in the first sealing area.

11. The method according to claim 1, in, The second sealing region is formed to include a portion protruding toward the first mother substrate from a surface where the frit contacts the first mother substrate when the second sealing region is viewed from a surface perpendicular to a major surface of the first mother substrate.

12. The method according to claim 1, in, The second sealing region is formed to include a portion protruding toward the second mother substrate from a surface where the frit contacts the second mother substrate when the second sealing region is viewed from a surface perpendicular to a main surface of the second mother substrate.

13. The method according to claim 1, in, When the second sealing region is viewed from a surface perpendicular to a main surface of the first mother substrate, the second sealing region is formed to include a portion protruding toward the first mother substrate from a surface where the glass frit contacts the first mother substrate, and The second sealing region is formed to include a portion protruding toward the second mother substrate from a surface where the frit contacts the second mother substrate when the second sealing region is viewed from a surface perpendicular to a main surface of the second mother substrate. 14 . The method of claim 1 , further comprising cutting the first mother substrate and the second mother substrate for each of the plurality of displays after bonding the first mother substrate to the second mother substrate for a second time.

15. The method according to claim 1, further comprising cutting the first mother substrate and the second mother substrate for each of the plurality of displays, in, The step of second-bonding the first mother substrate to the second mother substrate is performed for each of the plurality of cut and separated displays.

16. A display device, the display device include: first base; a display, arranged on the first substrate and comprising light emitting diodes; a second substrate, facing the first substrate; a first sealing region disposed between the first substrate and the second substrate, surrounding the display, and comprising glass frit; and a second sealing region, arranged in the first sealing region and comprising at least one portion protruding toward the first substrate and / or the second substrate, The second sealing region includes a region where the glass frit and the material of the first substrate and / or the glass frit and the material of the second substrate are melted and mixed with each other.

17. The display device according to claim 16, in, The first substrate and / or the second substrate includes a glass material.

18. The display device according to claim 16, in, The first sealing area has a closed loop shape surrounding a periphery of the display.

19. The display device according to claim 16, in, The first sealing area includes a first end arranged close to the display and a second end arranged away from the display, and The center of the second sealing area is closer to the first end than the second end.

20. The display device according to claim 19, in, The center of the second sealed area is located between a point corresponding to ¼ of the width of the first sealed area from the first end and a point corresponding to ½ of the width of the first sealed area from the first end.

21. The display device according to claim 16, in, The second sealing area has a width smaller than that of the first sealing area.

22. The display device according to claim 16, in, The second sealing area is formed continuously in the first sealing area.

23. The display device according to claim 16, in, The second sealing area is formed discontinuously in the first sealing area.