Photosensitive resin composition, dry film, cured film, printed circuit board and method for producing the same

By using a photosensitive resin composition of a specific composition and controlling the crosslinking structure, the problem of heat resistance and softness of the cured film is solved, and a cured film with high heat resistance and softness is achieved.

CN111936931BActive Publication Date: 2024-12-03KANEKA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980023779.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-03-29
Filing Date
2019-03-19
Publication Date
2024-12-03
Estimated Expiration
2039-03-19

AI Technical Summary

Technical Problem

When the existing cured film improves heat resistance, its softness is easily reduced, and it is difficult to take into account both.

Method used

The photosensitive resin composition containing a specific composition includes a polymer having a carboxyl group, a (meth)acryloyl monomer with a molecular weight of less than 1000, a polycyclic aromatic epoxy resin and a photopolymerization initiator, and is photocured and Thermal curing forms a crosslinked structure, and the ratio of carboxyl groups to epoxy groups is controlled to improve the stability of the dry film.

Benefits of technology

It achieves the combination of heat resistance and softness of the cured film, and is suitable for applications such as protective films of flexible wiring boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002709450630000241
    Figure BDA0002709450630000241
Patent Text Reader

Abstract

The photosensitive resin composition contains: (A) a polymer having a carboxyl group and not having a (meth)acryloyl group; (C) a monomer having a molecular weight of less than 1000 and having a (meth)acryloyl group and not having a carboxyl group; (D) a compound having a molecular weight of 1000 or more and not having a carboxyl group and having a (meth)acryloyl group; (E) a polycyclic aromatic epoxy resin; and (F) a photopolymerization initiator. The photosensitive resin composition may optionally contain (B) a compound having a carboxyl group and a (meth)acryloyl group, but the content thereof is 10% by weight or less relative to the total solid content.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a photosensitive resin composition, a dry film, a cured film, a printed circuit board with the cured film, and a method for producing the same. Background Art

[0002] Surface protective materials for flexible printed circuit boards (FPCs) require high heat resistance, and therefore use cured films obtained by curing resin compositions by photocuring or thermal curing. In recent years, photosensitive surface protective materials for FPCs have been required to have flexibility in addition to heat resistance.

[0003] As a method for improving the softness of the cured film, a method of adding a soft filler is known (for example, Patent Document 1). As a method for improving the heat resistance of the cured film, it is known to increase the crosslinking density of the resin composition, increase the amount of aromatic rings, etc. (for example, Patent Documents 2 and 3). Patent Document 2 describes the use of a pigment as an inorganic filler.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2016-194669

[0007] Patent Document 2: Japanese Patent Application Publication No. 2016-008267

[0008] Patent Document 3: Japanese Patent Application Publication No. 2001-249450 Summary of the invention

[0009] Problem that the invention aims to solve

[0010] The heat resistance of the cured film increases with the increase of rigid structures such as cross-linked structures and aromatic rings, but the flexibility tends to decrease. That is, heat resistance and flexibility are usually in a trade-off relationship. In the compositions disclosed in the above-mentioned Patent Documents 1 to 3, it is difficult to achieve both flexibility and heat resistance of the cured film.

[0011] Solutions for solving problems

[0012] The photosensitive resin composition of the present invention contains: (A) a polymer having a carboxyl group and not having a (meth)acryloyl group; (C) a monomer having a molecular weight of less than 1000 and not having a carboxyl group and having a (meth)acryloyl group; (D) a compound having a molecular weight of 1000 or more and not having a carboxyl group and having a (meth)acryloyl group; (E) a polycyclic aromatic epoxy resin; and (F) a photopolymerization initiator. The photosensitive resin composition may further contain a colorant as a component (G).

[0013] The photosensitive resin composition may further contain (B) a compound having a carboxyl group and a (meth)acryloyl group, but the content thereof is preferably 10% by weight or less relative to the total solid content. That is, the content of the compound having (B) a carboxyl group and a (meth)acryloyl group in the photosensitive resin composition is preferably 0 to 10% by weight of the total solid content.

[0014] The acid value of the component (A) is preferably 5 to 200 mgKOH / g, and the weight average molecular weight is preferably 1000 to 1000000. As the component (D), a compound having a urethane skeleton such as urethane (meth)acrylate is preferred.

[0015] The content of component (A) in the photosensitive resin composition is preferably 20 to 70 parts by weight relative to a total of 100 parts by weight of solid content. The content of component (C) is preferably 1 to 30 parts by weight, the content of component (D) is preferably 3 to 50 parts by weight, and the content of component (E) is preferably 5 to 30 parts by weight. The content of component (D) is preferably 1.1 to 5.0 times the content of component (C) by weight ratio.

[0016] The number of moles of carboxyl groups in the photosensitive resin composition is preferably 0.9 to 1.5 times the number of moles of epoxy groups. When the ratio of carboxyl groups to epoxy groups is within this range, the stability of a dry film obtained by forming the photosensitive resin composition into a layer tends to be improved.

[0017] By photocuring and thermosetting the above-mentioned photosensitive resin composition, a cured film can be obtained. For example, the above-mentioned photosensitive resin composition is applied to the surface of a printed circuit board to form a coating film, and at least a portion of the surface of the coating film is irradiated with active light to perform photocuring, and after developing with an alkali or the like as needed, the photocured coating film is heated to perform thermocuring, and a printed circuit board with a cured film can be formed. The printed circuit board can also be a flexible printed circuit board using a flexible film substrate such as a polyimide film.

[0018] The photosensitive resin composition may be formed into a layer on a carrier film and used in the form of a dry film. For example, a printed circuit board with a cured film may be obtained by laminating the dry film on a metal wiring of a printed circuit board, irradiating at least a portion of the surface of the dry film with active light to perform photocuring, and heating the photocured dry film to perform thermal curing.

[0019] Effects of the Invention

[0020] The cured film obtained by curing the photosensitive resin composition of the present invention can achieve both heat resistance and flexibility, and is suitable for a protective film of a flexible wiring board and the like. DETAILED DESCRIPTION

[0021] The photosensitive resin composition of the present invention contains (A): a carboxyl group-containing polymer, (C) (D): a (meth)acryloyl group-containing component, (E): a polycyclic aromatic epoxy resin, and (F): a photopolymerization initiator. Component (A) is a polymer that does not contain a (meth)acryloyl group. Components (C) and (D) are compounds that contain a (meth)acryloyl group and do not contain a carboxyl group, and those with a molecular weight of less than 1000 are defined as (C): a (meth)acryloyl group-containing monomer, and those with a molecular weight of 1000 or more are defined as (D): a (meth)acryloyl group-containing compound.

[0022] In addition to the above, the photosensitive resin composition may optionally contain a compound having a carboxyl group and a (meth)acryloyl group as the (B) component. When the photosensitive resin composition contains the (B) component, its content is 10% by weight or less relative to the total solid content of the photosensitive resin composition. That is, the content of the (B) component in the photosensitive resin composition is 0 to 10% by weight.

[0023] The photosensitive resin composition is applied on a substrate, and after the solvent is removed, it is irradiated with active light to perform photocuring, and then heat-cured to obtain a cured film. A B-stage photosensitive resin layer (dry film) can also be formed, and the dry film can be laminated on the substrate and then photocured and heat-cured. The B-stage photosensitive resin layer (dry film) is obtained by applying the photosensitive resin composition on a carrier film and drying it.

[0024] Component (A) has a carboxyl group, so the photosensitive resin composition is alkali-soluble. Component (F) of the photosensitive resin composition is activated by exposure (irradiation with active light), and a photoradical polymerization reaction of the (meth)acryloyl groups of components (C) and (D) is carried out. When the photosensitive resin composition contains component (B), the (meth)acryloyl group of component (B) also participates in the photoradical polymerization reaction. By photocuring, the resin composition becomes insoluble in alkali. When the resin composition is heated, component (E) is thermally cured. During thermal curing, the carboxyl group of component (A) reacts with the epoxy group of component (E) to form a crosslinked structure. When component (B) is contained, component (B) also participates in the formation of thermal crosslinks.

[0025] Components (A) and (E) participate only in thermal curing, components (C) and (D) participate in photocuring and do not substantially contribute to thermal curing, and component (B) participates in both photocuring and thermal curing.

[0026] In the conventional photosensitive resin composition for FPC, the content of resin components having both functional groups participating in photocuring and functional groups participating in thermal curing, such as the above-mentioned component (B), is high, and during curing, the photocuring network and the thermal curing network are developed around the component (B). These photocuring networks and thermal curing networks are chemically bonded by the component (B) to form a complex and intertwined three-dimensional network, thereby improving the heat resistance of the cured film.

[0027] On the other hand, the resin composition of the present invention includes a component that contributes to the formation of a photo-crosslinked network and is substantially not conducive to the formation of a thermal crosslinked network, and a component that contributes to the formation of a thermal crosslinked network and is substantially not conducive to the formation of a photo-crosslinked network, and does not include component (B) or even if it includes component (B), its content is small. The cured film obtained by curing the photosensitive resin composition can take into account both heat resistance and flexibility. It can be considered that the heat resistance brought about by the coexistence of the photo-crosslinked network and the thermal crosslinked network is maintained, and the mobility of the molecular chain is ensured in the cured film, which helps to take into account both heat resistance and flexibility.

[0028] The preferred embodiments of the components constituting the photosensitive resin composition are described in sequence below. It should be noted that, unless otherwise specified, the following components can be used alone or in combination of two or more. In this specification, "(meth)acrylic acid" means acrylic acid or methacrylic acid, and "(meth)acryloyl" means acryloyl or methacryloyl.

[0029] <Component (A): Carboxyl Group-Containing Polymer>

[0030] The component (A) is a polymer containing a carboxyl group and not containing a (meth)acryloyl group. The component (A) is a main component for forming a coating film based on a resin composition. The component (A) contributes to the formation of a thermal crosslinking network by reacting the carboxyl group with the epoxy group of the component (E) described later. The component (A) does not contain a (meth)acryloyl group and therefore does not contribute to the formation of a photocrosslinking network.

[0031] The polyethylene glycol-equivalent weight average molecular weight of the component (A) is preferably 1,000 to 100,000, more preferably 2,000 to 80,000, further preferably 3,000 to 60,000, particularly preferably 4,000 to 50,000. When the weight average molecular weight of the carboxyl group-containing polymer is within the above range, a cured film having excellent heat resistance and flexibility can be easily obtained.

[0032] Since the photosensitive resin composition contains a carboxyl group-containing polymer as the component (A), the photosensitive resin composition before curing is alkali-soluble. The carboxyl group of the component (A) contained in the photosensitive resin composition may be a carboxylic anhydride obtained by dehydrating two carboxyl groups.

[0033] The acid value of component (A) is preferably 5 to 200 mgKOH / g, more preferably 10 to 150 mgKOH / g, and further preferably 15 to 100 mgKOH / g. By setting the acid value of component (A) to the above range, the photosensitive resin composition before curing exhibits moderate alkali solubility. In addition, by setting the acid value to the above range, the heat resistance, insulation reliability and chemical resistance of the cured film can be improved, and flexibility can be imparted.

[0034] Specific examples of the component (A) include carboxyl group-containing (meth) acrylic polymers, carboxyl group-containing vinyl polymers, acid-modified polyurethanes, acid-modified polyesters, acid-modified polycarbonates, acid-modified polyamides, acid-modified polyimides, acid-modified polyurethane amides, acid-modified polyurethane imides, etc. From the viewpoints of flexibility and chemical resistance of the cured film, carboxyl group-containing (meth) acrylic copolymers, acid-modified polyurethanes, acid-modified polyamides, and acid-modified polyimides are preferred.

[0035] (A) component can be obtained by various known methods. The polymerization can be solution polymerization or solvent-free polymerization. In order to control the reaction, solution polymerization is preferred. As an organic solvent for solution polymerization, any organic solvent can be used without particular limitation as long as it can dissolve both the monomer components and the polymer after polymerization. The amount of solvent in the solution polymerization can be adjusted so that the solution concentration becomes 5 to 90% by weight, preferably 20 to 70% by weight.

[0036] The carboxyl group-containing (meth)acrylic polymer is a copolymer containing (meth)acrylic acid ester and a compound having a carboxyl group and a polymerizable double bond in one molecule as monomer components. Examples of the carboxyl group-containing monomer include (meth)acrylic acid, crotonic acid, isocrotonic acid, myristic acid, palmitoleic acid, oleic acid, elaidic acid, vaccenic acid, gadoleic acid, eicosenoic acid, erucic acid, nervonic acid, ω-carboxy-polycaprolactone mono(meth)acrylate, phthalic acid monohydroxyethyl (meth)acrylate, (meth)acrylic acid dimer, 2-(meth)acryloyloxypropyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl succinic acid, maleic acid, fumaric acid, citraconic acid, mesaconic acid, atropic acid, and cinnamic acid. Acid, linoleic acid, eicosadienoic acid, docosadienoic acid, linolenic acid, pinolenic acid, eleostearic acid, mead acid, dihomo-γ-linolenic acid, eicosatrienoic acid, octadecatetraenoic acid, arachidonic acid, eicosatetraenoic acid, docosatetraenoic acid, octadecatoneic acid, eicosapentaenoic acid, docosapentaenoic acid, herringic acid, tetracosapentaenoic acid, docosahexaenoic acid, tetracosahexaenoic acid, 2,2,2-tri(meth)acryloyloxymethylsuccinic acid, 2-tri(meth)acryloyloxymethylethylphthalic acid, etc. As the (meth)acrylate, an alkyl (meth)acrylate is preferred.

[0037] In addition to the carboxyl-containing monomer and (meth)acrylate, the carboxyl-containing (meth)acrylic polymer may optionally contain (meth)acrylamide such as diacetone (meth)acrylamide, esters of vinyl alcohol such as acrylonitrile and vinyl n-butyl ether, styrene, vinyl toluene, etc. as copolymerization components. The carboxyl-containing (meth)acrylic polymer can be obtained, for example, by free radical polymerization of the above-mentioned monomer components. The free radical polymerization can be thermal polymerization or photopolymerization. A polymerization initiator can also be used in the free radical polymerization. The carboxyl-containing (meth)acrylic polymer is preferably obtained by solution polymerization using an azo compound, an organic peroxide, a persulfate, hydrogen peroxide, etc. as a thermal polymerization initiator.

[0038] The acid-modified polyurethane can be obtained, for example, by reacting a diol compound having two hydroxyl groups and one carboxyl group with a diisocyanate compound.

[0039] The acid-modified polyester can be obtained, for example, by reacting a diol compound having two hydroxyl groups and one carboxyl group with a dicarboxylic acid.

[0040] The acid-modified polyamide is a compound having an amic acid structure, and can be obtained, for example, by the reaction of a diamino compound and tetracarboxylic dianhydride.

[0041] Acid-modified polyimide can be obtained, for example, by the reaction of a diisocyanate compound and tetracarboxylic dianhydride. By adding tetracarboxylic dianhydride in excess of the equivalent of the diisocyanate compound, an imide compound having a carboxylic anhydride group at the end can be obtained. By reacting an imide compound having a carboxylic anhydride group at the end with water and / or a primary alcohol such as methanol, ethanol, propanol, butanol, an imide compound having a carboxyl group at the end can be obtained.

[0042] Examples of the diol compound containing two hydroxyl groups and one carboxyl group include aliphatic diols such as 2,2-bis(hydroxymethyl)propionic acid, 2,2-bis(2-hydroxyethyl)propionic acid, 2,2-bis(3-hydroxypropyl)propionic acid, 2,3-dihydroxy-2-methylpropionic acid, 2,2-bis(hydroxymethyl)butyric acid, 2,2-bis(2-hydroxyethyl)butyric acid, 2,2-bis(3-hydroxypropyl)butyric acid, 2,3-dihydroxybutyric acid, 2,4-dihydroxy-3,3-dimethylbutyric acid, and 2,3-dihydroxyhexadecanoic acid; and aromatic diols such as 2,3-dihydroxybenzoic acid, 2,4-dihydroxybenzoic acid, 2,5-dihydroxybenzoic acid, 2,6-dihydroxybenzoic acid, 3,4-dihydroxybenzoic acid, and 3,5-dihydroxybenzoic acid. In particular, when an aliphatic diol is used, the photosensitive resin composition tends to have excellent photosensitivity.

[0043] The diisocyanate compound may be an alicyclic diisocyanate compound or an aliphatic diisocyanate compound. The diisocyanate compound may also be a reaction product of a diisocyanate compound and a compound having two or more functional groups that can react with the isocyanate group of the diisocyanate compound, for example, a carbamate compound having an isocyanate group at the end.

[0044] The tetracarboxylic dianhydride may be either an aromatic tetracarboxylic dianhydride or an aliphatic tetracarboxylic dianhydride, preferably an aromatic tetracarboxylic dianhydride in which an aromatic ring is directly bonded to a carboxylic anhydride group. Among them, aromatic tetracarboxylic dianhydride is preferred, preferably a carboxylic anhydride group is directly bonded to an aromatic ring. The diamino compound may be either an aromatic diamine or an aliphatic diamine, preferably an aromatic diamine.

[0045] The content of component (A) is preferably 20 to 70 parts by weight, more preferably 30 to 65 parts by weight, and further preferably 40 to 60 parts by weight relative to the total solid content of 100 parts by weight of the photosensitive resin composition. The content of component (A) may be 55 parts by weight or less or 50 parts by weight or less. As the content of component (A) increases, the softness of the cured film tends to increase. If the content of component (A) is within the above range, it is easy to form a cured film having both softness and heat resistance.

[0046] <Component (C) and component (D): (meth)acryloyl group-containing component>

[0047] Components (C) and (D) are compounds having at least one (meth)acryloyl group and no carboxyl group. Components (C) and (D) form a photo-crosslinked network. Components (C) and (D) do not have a carboxyl group and therefore do not substantially contribute to the formation of a thermally crosslinked network.

[0048] The component (C) is a compound (monomer) having a molecular weight of less than 1000. Specific examples of the (meth)acryloyl group-containing monomer having a molecular weight of 1000 or less include stearyl (meth)acrylate, lauryl (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, methoxydipropylene glycol (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, nonylphenoxyethylene glycol (meth)acrylate, β-(meth)acryloyloxyethyl hydrogen phthalate, β- -(meth)acryloyloxyethyl hydrogen succinate, 3-chloro-2-hydroxypropyl (meth)acrylate, 1-(meth)acryloyloxypropyl-2-phthalate and other monofunctional (meth)acrylic compounds; ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, 2-hydroxy-1-(meth)propylene 1,4-Butanediol di(meth)acrylate, 1,3-Butanediol di(meth)acrylate, 1,6-Hexanediol di(meth)acrylate, Neopentyl glycol di(meth)acrylate, Pentaerythritol di(meth)acrylate, Tricyclodecane dimethanol di(meth)acrylate, 2,4-Diethyl-1,5-pentanediol di(meth)acrylate, 2-Hydroxy-1,3-di(meth)acryloyloxypropane, 3-Methyl-1,5 -pentanediol di(meth)acrylate, 2,4-diethyl-1,5-pentanediol di(meth)acrylate, 1,4-cyclohexanedimethanol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 4,4'-isopropylidene diphenol di(meth)acrylate, 2,2-bis[4-((meth)acryloyloxyethoxy)phenyl]propane, 2,2-bis[4-((meth)acryloyloxy / diethoxy)phenyl]propane and other multifunctional (meth)acrylic compounds.

[0049] The multifunctional (meth)acrylic compound may also be a compound having three or more (meth)acryloyl groups in one molecule. Examples of the trifunctional or higher (meth)acrylic compound include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, isocyanuric acid tri(ethane (meth)acrylate), 1,3,5-tri(meth)acryloyl hexahydro-s-triazine, tetramethylolmethane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and dipentaerythritol poly(meth)acrylate.

[0050] (C) Component may be a (meth)acrylic compound containing a long-chain alkylene group or a polyoxyalkylene structure as long as the molecular weight is less than 1,000. Examples of the (meth)acrylic compound containing a polyoxyalkylene structure include methoxy polyethylene glycol (meth)acrylate, phenoxy polyethylene glycol (meth)acrylate, nonylphenoxy polyethylene glycol (meth)acrylate, nonylphenoxy polypropylene glycol (meth)acrylate, polyoxyethylene alkyl ether (meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, propoxylated pentaerythritol tetra(meth)acrylate, 2,2-bis[4-((meth)acryloyloxy / polyethoxy)phenyl]propane, 2,2-hydrogenated bis[4-((meth)acryloyloxy / polyethoxy)phenyl]propane, 2,2-bis[4-((meth)acryloyloxy / polypropoxy)phenyl]propane, bisphenol F EO-modified di(meth)acrylate, bisphenol A EO-modified di(meth)acrylate, bisphenol S EO modified di(meth)acrylate, etc.

[0051] From the viewpoint of heat resistance of the cured film, it is preferred to use a polyfunctional (meth)acrylic monomer containing two or more (meth)acryloyl groups in one molecule as the (C) component. By using a polyfunctional monomer as the (C) component, a cross-linked structure having a relatively short distance between cross-linking points is formed, and therefore, the heat resistance of the cured film tends to be improved.

[0052] The functional group equivalent of the (meth)acryloyl group of the (C) component (the mass (g) of the compound containing 1 equivalent of the (meth)acryloyl group) is preferably 480 or less, and more preferably 450 or less. The smaller the functional group equivalent of the (meth)acryloyl group of the (C) component, the more the heat resistance of the cured film tends to be improved, but the flexibility may be reduced. Therefore, the functional group equivalent of the (meth)acryloyl group of the (C) component is preferably 100 or more, more preferably 150 or more, and further preferably 200 or more. From the viewpoint of appropriately maintaining the distance between crosslinking points based on the (C) component, as the (C) component, a (meth)acrylic compound containing a modified structure (polyoxyalkylene structure) based on an alkylene oxide such as ethylene oxide and propylene oxide is preferred.

[0053] The component (D) is a compound having a molecular weight of 1000 or more. From the viewpoint of achieving both heat resistance and flexibility of the cured film, the molecular weight of the component (D) is preferably 20000 or less, more preferably 10000 or less, and further preferably 5000 or less. The molecular weight of the component (D) is obtained as a weight average molecular weight converted to polyethylene glycol.

[0054] From the viewpoint of improving the heat resistance of the cured film, the component (D) is preferably a polyfunctional (meth)acrylic compound, and particularly preferably a polymer (oligomer) having a (meth)acryloyl group at both ends of the polymer chain.

[0055] Specific examples of component (D) include polymers (oligomers) such as urethane (meth) acrylate resins, epoxy (meth) acrylate resins, polyester (meth) acrylate resins, and acrylic (meth) acrylate resins. From the viewpoint of being easy to form a cured film with excellent flexibility, urethane (meth) acrylates are preferred, and urethane di(meth) acrylates are particularly preferred.

[0056] By using a (meth)acryloyl group-containing component having a curable molecular weight of less than 1000 and a (D) component having a molecular weight of 1000 or more as a (meth)acryloyl group-containing component that contributes to the formation of a photo-crosslinked network, a short-distance crosslinked structure and a long-distance crosslinked structure coexist, thereby making it easy to form a cured film having improved heat resistance and flexibility.

[0057] The (meth)acryloyl group of the components (C) and (D) may be either acrylic acid or methacryloyl. From the viewpoint of improving photocurability, in photosensitive resin compositions, compounds having an acryloyl group are often used. On the other hand, when one or both of the components (C) and (D) are methacrylic compounds, the reactivity of photoradical polymerization is low compared to the case of using acrylic compounds, so unreacted (uncured) methacrylic compounds are likely to remain after photocuring. Unreacted methacrylic compounds act as plasticizers in the cured film, so it is believed that they contribute to improving the flexibility of the cured film.

[0058] The content of component (C) is preferably 1 to 30 parts by weight, more preferably 3 to 20 parts by weight, and further preferably 5 to 15 parts by weight, relative to 100 parts by weight of the total solid content of the photosensitive resin composition. The content of component (D) is preferably 3 to 50 parts by weight, more preferably 5 to 40 parts by weight, and further preferably 10 to 30 parts by weight, relative to 100 parts by weight of the total solid content of the photosensitive resin composition.

[0059] When the content of component (C) increases, it is easy to form a rigid structure based on a photocrosslinking network, and the heat resistance of the cured film tends to be improved. When the content of component (D) increases, the distance between the crosslinking points of the photocrosslinking network increases, and the softness of the cured film tends to be improved. In terms of weight ratio, the content of component (D) is preferably 1.1 to 5.0 times, more preferably 1.5 to 4.0 times, and further preferably 1.7 to 3.0 times relative to the content of component (C). If the contents of components (C) and (D) are within the above range, it is easy to form a cured film having both softness and heat resistance.

[0060] <Component (E): Polycyclic aromatic epoxy resin>

[0061] The (E) component is a compound having at least one epoxy group in the molecule and a condensed polycyclic aromatic group in the molecule. The epoxy group of the (E) component reacts with the carboxyl group of the (A) component to form a cross-linked structure (thermal cross-linked network). When the photosensitive resin composition contains the (B) component described later, the carboxyl group of the (B) component will also react with the epoxy group of the (E) component. The (E) component has a rigid structure based on condensed polycyclic aromatics, and the heat resistance of the cured film tends to be improved. The polycyclic aromatic epoxy resin preferably has two or more epoxy groups in the molecule.

[0062] From the viewpoint of heat resistance and chemical resistance of the cured film, the epoxy equivalent (mass (g) of the compound containing 1 equivalent of epoxy group) of the component (E) is preferably 2000 or less, and more preferably 1500 or less. The weight average molecular weight of the epoxy resin is preferably about 150 to 2000, and more preferably about 200 to 1500.

[0063] Specific examples of the component (E) include naphthalene-type epoxy resins and fluorene-type epoxy resins. Commercially available products of naphthalene-type epoxy resins include EPICLON series "HP-4700", "HP-4710", "HP-4770", "HP-4032D", "HP-5000", "HP-6000", etc. manufactured by DIC Corporation. Commercially available products of fluorene-type epoxy resins include OGSOL series "PG-100", "CG-500", "EG-200", "EG-280", etc. manufactured by Osaka Gas Chemicals Co., Ltd. From the viewpoint of the flexibility of the cured film, fluorene-type epoxy resins are particularly preferred as the component (E).

[0064] The content of the component (E) is preferably 3 to 40 parts by weight, more preferably 5 to 30 parts by weight, and further preferably 7 to 25 parts by weight relative to 100 parts by weight of the total solid content of the photosensitive resin composition. If the content of the component (E) is within the above range, the cured film has excellent heat resistance and flexibility, and a photosensitive resin layer (e.g., dry film) of high stability in the B stage is easily formed.

[0065] For the photosensitive resin composition, the ratio of the number of moles of carboxyl groups to the number of moles of epoxy groups ([the number of moles of carboxyl groups in all components] / [the number of moles of epoxy groups in all components]) is preferably 0.9 to 1.5, and more preferably 1.0 to 1.2. The carboxyl groups in the photosensitive resin composition are derived from the component (A) and the component (B) described later, and the epoxy groups in the photosensitive resin composition are derived from the component (E).

[0066] When the content of component (E) is too small and the amount of epoxy group is small, the heat resistance of the cured film may be reduced. If the molar ratio of carboxyl group / epoxy group is 0.9 or more, the cured film tends to show high heat resistance. If the molar ratio of carboxyl group / epoxy group is 1.5 or less, even if the photosensitive resin layer (e.g., dry film) is stored for a long time in the state of B stage, the photosensitivity can be maintained and the stability is excellent.

[0067] The number of moles of the epoxy group and the number of moles of the carboxyl group were calculated by the following formula.

[0068] The number of moles of epoxy groups = the reciprocal of epoxy equivalent × the content of epoxy resin (g)

[0069] The number of moles of carboxyl groups = (acid value / 56.11 / 1000) × the content of carboxyl-containing components (g)

[0070] It should be noted that the above 56.11 is the formula weight of potassium hydroxide.

[0071] <Component (B): Carboxyl-containing compound containing a (meth)acryloyl group>

[0072] The photocurable resin composition may contain a compound having a carboxyl group and a (meth)acryloyl group as the component (B) in addition to the above-mentioned components (A), (C), (D) and (E).

[0073] Examples of the component (B) include acid-modified epoxy (meth)acrylates obtained by adding a saturated or unsaturated polycarboxylic acid anhydride to an ester obtained by reacting an epoxy resin with an unsaturated monocarboxylic acid; urethane (meth)acrylates which are polymers of a diol compound having a carboxyl group and a diisocyanate compound; (meth)acrylated (meth)acrylates obtained by reacting a portion of the carboxyl groups in the side chains of a copolymer of (meth)acrylic acid and (meth)acrylate having a carboxyl group and a polymerizable double bond with an epoxy group of a compound having a (meth)acrylic group and an epoxy group, such as glycidyl (meth)acrylate; and the like.

[0074] Component (B) participates in both photocuring and thermal curing, thus increasing the crosslinking density of the cured film, which can contribute to the improvement of heat resistance and chemical resistance. On the other hand, when the content of component (B) increases, the softness of the cured film tends to decrease. The content of component (B) is less than 10 parts by weight, preferably less than 5 parts by weight, more preferably less than 3 parts by weight, and further preferably less than 1 part by weight relative to 100 parts by weight of the total solid content of the photosensitive resin composition. The photosensitive resin composition optionally contains component (B). By reducing the content of component (B) or excluding component (B), a cured film with excellent softness can be formed.

[0075] <(G) Coloring agent>

[0076] The photosensitive resin composition optionally contains a colorant. The colorant is added to make the cured film into a desired color. The colorant can be a dye or a pigment, preferably an organic substance. As the colorant, blue colorants, red colorants, yellow colorants, orange colorants, purple colorants, etc. can be mentioned. By combining a variety of colorants, cured films of various colors can be formed. Specific examples of colorants are shown below by color index numbers.

[0077] Examples of blue colorants include CI Pigment Blue 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, and 60, which are phthalocyanine-based, anthraquinone-based, or dioxazine-based pigments; and Solvent Blue 35, 63, 68, 70, 83, 87, 94, 97, 122, 136, 67, and 70, which are dye-based. In addition to the above, metal-substituted or unsubstituted phthalocyanine compounds can also be used as blue colorants. In particular, copper phthalocyanine-based colorants are preferred from the viewpoint of coloring power.

[0078] Examples of the red colorant include CI Pigment Red 122, 149, 166, 177, 179, 242, 224, 254, 264, and 272.

[0079] Examples of the yellow colorant include CI Pigment Yellow 83, 110, 128, 138, 139, 150, 151, 154, 155, 180, and 181.

[0080] Examples of the orange colorant include CI Pigment Orange 5, 13, 14, 16, 17, 24, 34, 36, 38, 40, 43, 46, 49, 51, 55, 59, 61, 63, 64, 71, and 73.

[0081] Examples of the violet colorant include CI Pigment Violet 19, 23, 29, 30, 32, 36, 37, 38, 39, 40, and 50; and Solvent Violet 13 and 36.

[0082] The above colorants may be combined to form a black colorant. Specific examples of combinations of colorants for forming a black cured film are shown below. The following ratios are expressed by weight ratio.

[0083] The orange colorant is combined at a ratio of 1.5 to 3.0 with respect to 1.0 of the blue colorant.

[0084] The red colorant is combined at a ratio of 1.2 to 3.0 with respect to 1.0 of the blue colorant.

[0085] The violet colorant is combined at a ratio of 1.2 to 3.0 with respect to 1.0 of the blue colorant.

[0086] The yellow colorant is combined at a ratio of 1.5 to 4, and the orange colorant is combined at a ratio of 1.0 to 2.5, relative to 1.0 of the blue colorant.

[0087] The red colorant is combined at a ratio of 1.0 to 2.0, and the yellow colorant is combined at a ratio of 1.5 to 3.0, relative to 1.0 of the blue colorant.

[0088] The yellow colorant is combined at a ratio of 1.0 to 3.0, and the violet colorant is combined at a ratio of 1.0 to 2.0, relative to 1.0 of the blue colorant.

[0089] The orange colorant is combined at a ratio of 0.5 to 2.0, and the violet colorant is combined at a ratio of 0.5 to 2.0, relative to 1.0 of the blue colorant.

[0090] Among the above, a combination of a blue colorant, an orange colorant, and a violet colorant is preferred because of excellent blackness and easy adjustment of the amount of the colorant.

[0091] The content of component (G) can be appropriately set according to the type of colorant and the color of the cured film. For example, in order to obtain a black cured film, the content of component (G) is preferably 3 parts by weight or more, more preferably 4 parts by weight or more, relative to 100 parts by weight of the total solid content of the photosensitive resin composition. From the viewpoint of colorability, there is no particular problem with the amount of colorant, but as the amount of colorant increases, the photocurability is easily reduced. In addition, when the amount of colorant is large, the thixotropic index will increase, and there are concerns about clogging during ink filtering, deterioration of printability, and reduction of resolution. Therefore, relative to 100 parts by weight of the total solid content of the photosensitive resin composition, the content of component (G) is preferably 10 parts by weight or less, more preferably 7 parts by weight or less.

[0092] <Component (F): Photopolymerization Initiator>

[0093] The photopolymerization initiator as the component (F) is a compound (photoradical polymerization initiator) that absorbs light energy such as UV (ultraviolet light) to become activated, thereby initiating / promoting the formation of a photocrosslinked network based on the photoradical polymerization reaction of the (meth)acryloyl groups of the components (C) and (D).

[0094] Examples of photoradical polymerization initiators include self-cleavage type photoradical polymerization initiators such as benzoin compounds, acetophenones, aminoketones, oxime esters, acylphosphine oxide compounds, and azo compounds; and hydrogen-abstracting type photoradical polymerization initiators such as benzophenones, benzoin ethers, benzyl ketals, dibenzosuberones, anthraquinones, xanthones, thioxanthones, halogenated acetophenones, dialkoxyacetophenones, hydroxyacetophenones, halogenated diimidazoles, and halogenated triazines.

[0095] As a photoradical polymerization initiator, a photoradical polymerization initiator having an absorption band at a wavelength of 405 nm can also be used. By using a photopolymerization initiator having an absorption band at a wavelength of 405 nm, the heat resistance of the cured film tends to be further improved, and this tendency becomes significant when the photosensitive resin composition contains a colorant. As a photoradical polymerization initiator having an absorption band at a wavelength of 405 nm, acylphosphine oxide compounds, acetophenones, aminoketones, oxime esters, etc. can be cited. Among them, oxime esters are preferred due to their high sensitivity. As commercially available products of oxime esters having an absorption band at a wavelength of 405 nm, "ADEKA ARKLS NCI-831", "ADEKA ARKLS N-1717" and "ADEKA ARKLS N-1919" manufactured by ADEKA, "Irgacure OXE03" manufactured by BASF, etc. can be cited.

[0096] When the coating film of the photosensitive resin composition is irradiated with active light such as ultraviolet rays and short-wavelength visible light, the photopolymerization initiator near the irradiated surface absorbs the light and becomes activated, and the light that is not absorbed near the irradiated surface reaches the bottom. Therefore, generally, photocuring is easier to proceed on the irradiated surface side than on the bottom. In particular, when the photosensitive resin composition contains a colorant, the colorant absorbs active light in addition to the photopolymerization initiator, so the amount of active light reaching the bottom is small, and the photocuring of the bottom is likely to become insufficient compared to the light irradiated surface.

[0097] Short-wavelength light is relatively high energy, so in the photocuring based on the irradiation of active light, short-wavelength light is preferentially used near the light irradiation surface, and long-wavelength light that is not absorbed near the light irradiation surface is easy to reach the bottom. By using a photo-radical polymerization initiator having an absorption band at a long wavelength (405nm) as component (F), photocuring based on long-wavelength light reaching the bottom is easy to carry out. Therefore, it is believed that even when the composition has a colorant, the photocuring reaction at the bottom can be maintained, and the heat resistance of the cured film is improved.

[0098] The photo-radical polymerization initiator preferably has an absorbance of 0.001 wt % methanol solution at a wavelength of 405 nm of 0.02 or more, measured by a visible-ultraviolet spectrophotometer using a quartz cuvette with an optical path length of 1 cm. In other words, it is preferred to use an absorbance coefficient of 20[% at a wavelength of 405 nm. -1 / cm -1 ] or above photoradical polymerization initiator.

[0099] The content of component (F) is preferably 0.1 to 20 parts by weight, more preferably 0.3 to 10 parts by weight, and even more preferably 0.5 to 5 parts by weight, relative to 100 parts by weight of the total solid content of component (B), component (C), and component (D). By setting the above blending ratio, the photosensitivity of the photosensitive resin composition can be improved to increase the efficiency of the photocuring reaction, and overexposure can be prevented.

[0100] <Other ingredients>

[0101] In addition to the above-mentioned (A) to (G) components, the photosensitive resin composition may optionally contain various additives such as fillers, adhesive aids, defoamers, leveling agents, polymerization inhibitors, flame retardants, etc. as needed. As fillers, inorganic fillers such as silica, mica, talc, barium sulfate, wollastonite, calcium carbonate, and organic polymer fillers can be mentioned. As defoamers and leveling agents, silicone compounds, acrylic compounds, etc. can be mentioned. As adhesive aids (also called adhesion-imparting agents), silane coupling agents, triazole compounds, tetrazole compounds, triazine compounds, etc. can be mentioned. As polymerization inhibitors, for example, hydroquinone, hydroquinone monomethyl ether, etc. can be mentioned.

[0102] As the flame retardant, phosphate compounds, halogen-containing compounds, metal hydroxides, organic phosphorus compounds, organic silicon compounds, etc. From the viewpoint of preventing environmental pollution, non-halogen flame retardants such as metal hydroxides and phosphorus compounds are preferred.

[0103] <Preparation of Photosensitive Resin Composition>

[0104] The photosensitive resin composition can be obtained by mixing the above-mentioned components and a suitable solvent as required. The above-mentioned components can be crushed / dispersed, deaerated, etc. as required before and / or after mixing. The crushing / dispersion can be carried out using a mixing device such as a bead mill, a ball mill, a three-roll mill, etc.

[0105] <Formation of Cured Film>

[0106] The photosensitive resin composition is applied in a layered form, heated as necessary to remove the solvent, and then photocured and thermally cured to form a cured film. When the photosensitive resin composition contains a colorant, a colored cured film colored in black or the like can be obtained.

[0107] The cured film obtained by curing the above-mentioned photosensitive resin composition can achieve both heat resistance and flexibility. It is believed that a small content of the component (B) in the photosensitive resin composition or the absence of the component (B) in the photosensitive resin composition contributes to achieving both heat resistance and flexibility, which are usually in a compromise.

[0108] As described above, component (B) participates in the formation of both the photo-crosslinked network and the thermal-crosslinked network, so the cured film obtained by curing the photosensitive resin composition containing a large amount of component (B) has a complex three-dimensional network formed by the photo-crosslinked network and the thermal-crosslinked network intertwined with each other. Therefore, the heat resistance is excellent, but on the other hand, the flexibility tends to be poor.

[0109] The photosensitive resin composition of the present invention has a small content of component (B) or does not contain component (B), so it is believed that the flexibility is improved. When a cured film is formed from the photosensitive resin composition of the present invention, components (C) and (D) are initially photocured to form a photocrosslinked network. At this time, components (A) and (E) are unreacted (uncured), so it is believed that a sea-island structure in which components (A) and (E) exist in the matrix of the photocrosslinked network is formed.

[0110] It is believed that during thermal curing, the components (A) and (E) present in the photo-crosslinked network in an island shape react and form a chemical bond, thereby forming a structure formed by the photo-crosslinked network and the thermal crosslinked network interlaced. In this structure, the photo-crosslinked network and the thermal crosslinked network exist without the aid of chemical bonding, so it is speculated that compared with the crosslinked network formed with the component (B) as the center, the movement of the molecular chain is less restricted, which helps to improve flexibility. In addition, it is believed that the component (E) as the center of the thermal crosslinked network has a rigid structure derived from a condensed polycyclic aromatic group, which helps to improve heat resistance.

[0111] (Formation of B-stage film)

[0112] The formation of a cured film using a photosensitive resin composition can be implemented by various known methods. The photosensitive resin composition (solution) can be applied by screen printing, curtain roller, reverse roller, spraying, spin coating using a spinner, etc. The thickness of the coating film can be adjusted so that the thickness after drying is about 5 to 100 μm, preferably about 10 to 50 μm. When drying by heating, from the viewpoint of suppressing the thermal curing reaction, the drying temperature is preferably below 120°C, more preferably 40 to 100°C.

[0113] By removing the solvent from the coating film, a B-stage photosensitive resin layer (B-stage film) is formed. When the photosensitive resin composition is applied in a layer on a substrate (object to form a cured film) such as a printed circuit board, the B-stage film can be cured on the substrate. Alternatively, the photosensitive resin composition can be applied in a layer on a carrier film to form a B-stage film, and then cured after being laminated on the substrate as a dry film.

[0114] The case where the dry film is laminated and cured on the substrate is the same as the case where the B-stage film is formed and cured by coating the photosensitive resin composition on the substrate, and a cured film that takes into account both heat resistance and flexibility can also be formed. In the case of using a B-stage film (dry film) formed on a carrier film, the period from the formation of the B-stage film (coating and drying of the photosensitive resin composition) to the implementation of exposure and development is longer than the case of forming the B-stage film directly on the substrate. Therefore, when the photosensitive resin composition is made into a dry film and used, stability in the state of the B-stage film is required. As mentioned above, by setting the ratio of the carboxyl group to the epoxy group of the photosensitive resin composition to a specified range, the storage stability in the state of the B-stage film tends to be improved, and even when lamination, exposure and development are performed with the substrate after storage in the state of the B-stage film (dry film), a fine photosensitive pattern can be formed.

[0115] As the carrier film when forming the dry film, a plastic film such as a polyester film such as polyethylene terephthalate (PET), a polyimide film, a polyamide-imide film, a polypropylene film, a polystyrene film, etc. can be used. The thickness of the carrier film is not particularly limited, and is usually about 10 to 150 μm. The film thickness of the dry film formed on the carrier film is, for example, 10 to 150 μm, preferably 20 to 60 μm.

[0116] Preferably, a peelable cover film is laminated on the dry film. When peeling off the cover film, the adhesion between the dry film and the cover film is smaller than the adhesion between the dry film and the carrier film. Polyethylene film, polytetrafluoroethylene film, polypropylene film, surface-treated paper, etc. can be used.

[0117] (exposure)

[0118] Photocuring is performed by exposing a B-stage film disposed on a substrate. During exposure, a photomask may be arranged on the B-stage film, and after selectively exposing a portion of the surface of the coating film, a relief pattern is formed by development. During exposure, active light such as ultraviolet rays and visible light is irradiated. When a photopolymerization initiator having an absorption band at a long wavelength is used as the (F) component, exposure is preferably performed by a light source containing light of a short wavelength of visible light (for example, 400 to 450 nm). When an LED is used for exposure, a long-wavelength LED having a peak emission wavelength greater than 385 nm is preferably used.

[0119] (development)

[0120] As a developer, an aqueous alkali solution is generally used, and an organic alkali aqueous solution and an inorganic alkali aqueous solution can be used without particular limitation. The developer optionally contains an organic solvent miscible with water, such as methanol, ethanol, n-propanol, isopropanol, N-methyl-2-pyrrolidone, etc. The alkali concentration of the developer is generally 0.01 to 20% by weight, preferably 0.02 to 10% by weight, and the temperature of the developer is generally 0 to 80° C., preferably 10 to 60° C. The relief pattern after development is preferably rinsed with a rinse solution such as water or an acidic aqueous solution.

[0121] By performing heat treatment after development to perform heat curing, a heat crosslinking network based on the above-mentioned (A) component and (E) component is formed, so that a cured film with high heat resistance can be obtained. From the viewpoint of allowing the heat curing to proceed sufficiently and suppressing the oxidation of the metal wiring caused by heat, the curing temperature (the maximum temperature during heat curing) is preferably 100 to 250°C, more preferably 120 to 200°C, and further preferably 130 to 180°C.

[0122] (Application of Cured Film)

[0123] The cured film obtained from the photosensitive resin composition has a resolution of about 10 to 1000 μm, for example, and can therefore be suitably used as a surface protective material for a printed circuit board. In addition, the cured film has excellent flexibility, and can therefore also be suitably used as a cured film for a flexible printed circuit board having metal wiring on a flexible film such as a polyimide film. The photosensitive resin composition can also be used to form various wiring cover protective materials, photosensitive heat-resistant adhesives, wire / cable insulation coatings, and the like.

[0124] Example

[0125] The present invention will be specifically described below with reference to Examples, but the present invention is not limited to these Examples.

[0126] [Synthesis example]

[0127] In the following synthesis examples, (A) a polymer having a carboxyl group and having no (meth)acryloyl group was polymerized. The properties of the solutions and polymers obtained in Synthesis Examples 1 to 3 were evaluated by the following methods.

[0128] <Solid content concentration>

[0129] The measurement was performed in accordance with JIS K 5601-1-2. The drying conditions were set to 170° C.×1 hour.

[0130] <Weight Average Molecular Weight>

[0131] The measurement was carried out by gel permeation chromatography (GPC) under the following conditions.

[0132] Device used: Tosoh Corporation HLC-8220GPC equivalent

[0133] Column: Tosoh Corporation TSK gel Super AWM-H (6.0mm ID × 15cm) × 2 pieces

[0134] Guard column: TSK guard column Super AW-H manufactured by Tosoh Corporation

[0135] Eluent: 30 mM LiBr + 20 mM H 3 PO 4 in DMF

[0136] Flow rate: 0.6mL / min

[0137] Column temperature: 40°C

[0138] Detection conditions: RI: Polarity (+), response (0.5 seconds)

[0139] Sample concentration: about 5 mg / mL

[0140] Molecular weight standard: PEG (polyethylene glycol)

[0141] <Acid value>

[0142] The measurement was conducted in accordance with JIS K 5601-2-1.

[0143] (Synthesis example 1)

[0144] In a reaction container equipped with a stirrer, a thermometer, a dropping funnel, and a nitrogen inlet tube, 100.0 g of methyl triglyme (1,2-bis(2-methoxyethoxy)ethane) as a polymerization solvent was placed, and the temperature was raised to 80°C while stirring under a nitrogen stream. While maintaining the temperature at 80°C, 12.0 g (0.14 mol) of methacrylic acid, 28.0 g (0.16 mol) of benzyl methacrylate, 60.0 g (0.42 mol) of butyl methacrylate, and 0.5 g of azobisisobutyronitrile as a radical polymerization initiator were dropped from the dropping funnel over 3 hours. After the dropwise addition was completed, the reaction solution was heated to 90°C while stirring, and the reaction solution was further stirred for 2 hours while the temperature was maintained at 90°C, thereby obtaining a solution of an acrylic polymer (A-1) having a carboxyl group in the molecule. The solid content concentration of the solution was 50%, the weight average molecular weight of the polymer was 48,000, and the acid value was 78 mgKOH / g.

[0145] (Synthesis example 2)

[0146] In a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, and a nitrogen inlet tube, 30.00 g of methyl triglyme and 10.31 g (0.050 mol) of norbornene diisocyanate as a polymerization solvent were placed, and heated to 80°C under a nitrogen stream while stirring to dissolve them. To the solution, 50.00 g (0.025 mol) of polycarbonate diol (manufactured by Asahi Kasei Corporation, trade name: PCDL T5652, weight average molecular weight 2000) and 3.70 g (0.025 mol) of 2,2-bis(hydroxymethyl)butyric acid dissolved in 30.00 g of methyl triglyme were added dropwise from the dropping funnel over 1 hour. The solution was heated and stirred at 80°C for 5 hours to obtain a solution of a carboxyl group-containing urethane polymer (A-2) in the molecule. The solid content concentration of the solution was 52%, the weight average molecular weight of the polymer was 5600, and the acid value was 22 mgKOH / g.

[0147] (Synthesis example 3)

[0148] In a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, and a nitrogen inlet tube, 35.00 g of methyl triglyme and 10.31 g (0.050 mol) of norbornene diisocyanate as a polymerization solvent were placed, and heated to 80° C. under a nitrogen stream while stirring to dissolve. A solution prepared by dissolving 50.00 g (0.025 mol) of polycarbonate diol in 35.00 g of methyl triglyme was added dropwise from the dropping funnel over 1 hour, and after heating and stirring at 80° C. for 2 hours, 15.51 g (0.050 mol) of 3,3',4,4'-oxydiphthalic dianhydride was added, and the temperature was raised to 190° C. and heated and stirred for 1 hour. After that, the mixture was cooled to 80°C, 3.60 g (0.200 mol) of pure water was added, the temperature was raised to 110°C and heated under reflux for 5 hours to obtain a solution of a carboxyl-containing urethane imide polymer (A-3) in the molecule. The solid content concentration of the solution was 53%, the weight average molecular weight of the polymer was 9200, and the acid value was 86 mgKOH / g.

[0149] [Preparation of resin compositions of Examples and Comparative Examples]

[0150] The composition of the proportion shown in Table 1 was dissolved in methyl triglyme, stirred by a stirring device, and passed through a three-roll mill twice. After that, degassing was performed with a degassing device to prepare a uniform solution. The amount of methyl triglyme as a solvent (including the total amount of solvents contained in the polymer solution of the above synthesis example) was 30 parts by weight. In addition, in addition to the components shown in Table 1, 0.1 parts by weight of a butadiene-based defoamer ("FLOWLEN AC-2000" manufactured by Kyoeisha Chemical Co., Ltd.) was added to each resin composition.

[0151] [Formation and evaluation of cured film]

[0152] <Photosensitivity>

[0153] On a polyimide film with a thickness of 25 μm (manufactured by Kaneka Corporation, "APICAL 25NPI"), using a Baker applicator, a photosensitive resin composition was cast / coated to an area of 100 mm × 100 mm such that the final dry thickness became 30 μm, and dried at 80°C for 20 minutes. A negative photomask with a line width / line pitch = 100 μm / 100 μm was placed, and ultraviolet light with a cumulative exposure dose of 300 mJ / cm 2 was irradiated, and after exposure, a 1.0 wt% aqueous sodium carbonate solution (30°C) was sprayed for 90 seconds at a spraying pressure of 1.0 kgf / mm 2 for development. After washing with pure water, it was heat-cured in an oven at 150°C for 30 minutes to produce a pattern-cured film (embossed pattern) of the photosensitive resin composition.

[0154] The embossed patterns formed using the compositions of the examples and comparative examples were observed under an optical microscope. In any case of using the compositions, no significant thick lines or development residues of the patterns were confirmed, and photosensitive patterns with a line width / line pitch = 100 / 100 μm were all drawn.

[0155] <Stability of B-stage film>

[0156] Similar to the above evaluation of photosensitivity, the photosensitive resin composition was cast / coated on the polyimide film and dried at 80°C for 20 minutes to form a photosensitive resin layer (B-stage film) with a thickness of 30 μm. After storing this specimen at room temperature for 5 days, development / exposure was carried out in the same manner as the above evaluation of photosensitivity to produce a cured film (embossed pattern). The embossed pattern was observed under an optical microscope, and the stability was evaluated according to the following criteria.

[0157] 〇: No significant thick lines or development residues were confirmed on the surface of the polyimide film, and a photosensitive pattern with a line width / line pitch = 100 / 100 μm was drawn

[0158] △: No development residues were seen on the surface of the polyimide film, but thick lines were generated

[0159] ×: Development residues and thick lines were confirmed on the surface of the polyimide film, and a photosensitive pattern with a line width / line pitch = 100 / 100 μm was not drawn

[0160] <Heat resistance>

[0161] On a flexible copper-clad laminated board formed by laminating a 25 μm thick polyimide film ("APICAL25NPI" manufactured by Kaneka Co., Ltd.) and a 12 μm thick electrolytic copper foil with a polyimide-based adhesive, the photosensitive resin composition was cast / coated, dried, exposed, developed and cured by heating in the same manner as above to form a cured film on the copper foil of the flexible printed circuit board. It should be noted that a photomask was not used during exposure, but ultraviolet rays were irradiated to the entire surface.

[0162] The sample was immersed in a solder bath (320° C., 300° C., and 288° C.) for 5 seconds, then pulled out, and the appearance was observed and evaluated based on the following criteria.

[0163] ◎: No appearance change (expansion or peeling of the insulating film) before and after the test at any temperature

[0164] ○: Appearance change was observed before and after the test at 320°C, but no appearance change was observed before and after the test at 288°C and 300°C

[0165] △: Appearance changes were observed before and after the test at 300°C and 320°C, but no appearance changes were observed before and after the test at 288°C.

[0166] ×: Appearance changes were observed before and after the test at any temperature

[0167] <Softness>

[0168] The photosensitive resin composition was cast / coated on a 25 μm thick polyimide film ("APICAL 25NPI" manufactured by Kaneka Co., Ltd.) to an area of ​​100 mm×100 mm using a Baker-type applicator so that the final dry thickness was 20 μm, and dried at 80° C. for 20 minutes. The test piece was cut into a size of 15 mm×100 mm, and exposed, developed, and heat-cured in the same manner as above to form a cured film on the polyimide film, thereby preparing a sample for evaluating flexibility.

[0169] The evaluation sample was bent 180° with the cured film as the outside, and a load of 200 g was applied to the bent position for 3 seconds. After the load was removed, the bent position was visually observed to evaluate the presence or absence of cracks. This operation was performed until the cured film cracked, and the number of times that no cracking occurred was taken as the folding endurance number. For example, when cracking occurred in the second test, the folding endurance number was 1.

[0170] The compounding ratios and evaluation results of the photosensitive resin compositions of Examples and Comparative Examples are listed in Table 1. The numerical values ​​of the compounding ratios in Table 1 are parts by weight of the solid content (non-volatile content), and the details of each component are as follows.

[0171] (1) "KAYARAD UXE-3000" manufactured by Nippon Kayaku Co., Ltd.; a dilution of carbitol acetate of an acid-modified epoxy acrylate having a urethane skeleton (weight average molecular weight 10,000, acid value 98 mgKOH / g)

[0172] (2) “FANCRYL FA-321M” manufactured by Hitachi Chemical Co., Ltd.: EO-modified bisphenol A dimethacrylate, average molecular weight 804

[0173] (3) “EBECRYL 3708” manufactured by Daicel-Allnex Ltd.: modified epoxy acrylate, weight average molecular weight 1500

[0174] (4) “GENOMER 4256” manufactured by Rahn: aliphatic urethane methacrylate, weight average molecular weight 6500

[0175] (5) EPICLON HP-4032D manufactured by DIC Corporation: naphthalene-based epoxy resin, epoxy equivalent weight 140

[0176] (6) OGSOL EG-200 manufactured by Osaka Gas Chemicals Co., Ltd.: fluorene-based epoxy resin, epoxy equivalent weight 290

[0177] (7) “jER828” manufactured by Mitsubishi Chemical Corporation; bisphenol A type epoxy resin, epoxy equivalent weight 190)

[0178] (8) ADEKA ARKLS NCI-831 manufactured by ADEKA Corporation; nitro-substituted carbazole type oxime ester photoradical polymerization initiator; absorbance of 0.001% methanol solution at a wavelength of 405 nm: 0.03

[0179] (9) Black colorant: A colorant obtained by mixing the following blue colorant, orange colorant, and purple colorant in a weight ratio of 1:1:1

[0180] Blue colorant: BASF "GLVO"; Pigment Blue 15:3

[0181] Orange colorant: Clariant Specialty Chemicals "GRL"; Pigment Orange 43

[0182] Purple colorant: Clariant Specialty Chemicals "ER-02"; Pigment Violet 19

[0183] [Table 1]

[0184]

[0185] In Examples 1 to 9, which do not contain component (B) and use a condensed polycyclic aromatic epoxy resin as a thermosetting resin, any cured film has a soldering heat resistance of 288°C or more, and the number of folding resistance is 5 or more, and has both heat resistance and flexibility. Example 10, in which a part of component (A) of Example 7 is replaced with component (B) (the content of component (B) is 10% by weight relative to the total solid content), also has both heat resistance and flexibility like Examples 1 to 9. Compared with Example 7, Example 10 has improved heat resistance, but slightly reduced flexibility.

[0186] In Comparative Example 1, which does not contain component (A) and contains component (B) at 46% by weight relative to the total solid content, the cured film exhibits high heat resistance, but the number of folding resistance is 0, and the flexibility is poor. Comparative Example 2, in which the content of component (B) is 28% by weight relative to the total solid content, also exhibits high heat resistance as in Comparative Example 1, but has poor flexibility. In Comparative Example 3, in which bisphenol A epoxy resin is used as the epoxy resin, no improvement in flexibility compared to Comparative Example 2 is confirmed, and the soldering heat resistance is also reduced compared to Comparative Example 2.

[0187] From the above results, it can be seen that the cured film of the resin composition that does not contain the (B) component (a compound having both a carboxyl group and a (meth)acryloyl group) or contains a small content thereof and contains the (E) component (thermosetting resin component) as a polycyclic aromatic epoxy resin can achieve both excellent heat resistance and flexibility.

[0188] From the comparison between Example 3 and Example 6, it is understood that the use of a compound having a urethane skeleton and a molecular weight of 1,000 or more as the component (D) can improve flexibility without reducing the heat resistance of the cured film.

[0189] In Example 8, in which the amount of component (E) was increased compared to Examples 6 and 7, although the heat resistance was improved, the accuracy of the photosensitive pattern decreased when the film was stored in the form of a dry film and exposed / developed. In other examples, even when stored in the form of a dry film, a high-precision photosensitive pattern was formed, showing excellent stability.

[0190] From the above results, it is understood that the photosensitive resin composition of the present invention has excellent heat resistance and flexibility of the cured film and is also suitable for use in the form of a dry film.

Claims

1. A photosensitive resin composition comprising: (A) a polymer having a carboxyl group and having no (meth)acryloyl group, (C) a monomer having no carboxyl group and having a (meth)acryloyl group and having a molecular weight of less than 1000, (D) a compound having no carboxyl group and having a (meth)acryloyl group and having a molecular weight of 1000 or more, (E) a polycyclic aromatic epoxy resin, and (F) a photopolymerization initiator, The photosensitive resin composition does not contain (B) a compound having a carboxyl group and a (meth)acryloyl group, or contains 10 wt % or less of (B) a compound having a carboxyl group and a (meth)acryloyl group based on the total solid content, The number of moles of carboxyl groups in the composition is 0.9 to 1.5 times the number of moles of epoxy groups. The acid value of (A) is 5 to 200 mgKOH / g, and the weight average molecular weight is 1000 to 100000. With respect to a total of 100 parts by weight of the solid content, the content of (A) is 20 to 70 parts by weight, the content of (C) is 1 to 30 parts by weight, the content of (D) is 3 to 50 parts by weight, and the content of (E) is 5 to 30 parts by weight, The content of the (D) is 1.1 to 5.0 times the content of the (C) by weight.

2. The photosensitive resin composition according to claim 1, wherein The compound (D) having no carboxyl group and having a (meth)acryloyl group and having a molecular weight of 1,000 or more has a urethane skeleton.

3. The photosensitive resin composition according to claim 2, wherein The molecular weight of (A) is 4,000 to 50,000. 4 . The photosensitive resin composition according to claim 1 , further comprising (G) a colorant.

5. The photosensitive resin composition according to claim 4, wherein The (G) colorant is a black colorant.

6. The photosensitive resin composition according to claim 4, wherein The (G) colorant comprises an organic pigment, The organic pigment includes at least one selected from the group consisting of a blue organic pigment, an orange organic pigment, a yellow organic pigment, a red organic pigment, and a violet organic pigment.

7. The photosensitive resin composition according to claim 1, wherein The content of (A) is 40 to 60 parts by weight based on 100 parts by weight of the total solid content.

8. The photosensitive resin composition according to claim 1, wherein The content of (A) is 50 parts by weight or less based on 100 parts by weight of the total solid content.

9. The photosensitive resin composition according to claim 1, wherein The content of (C) is 5 to 15 parts by weight based on 100 parts by weight of the total solid content.

10. The photosensitive resin composition according to claim 1, wherein The content of (D) is 10 to 30 parts by weight based on 100 parts by weight of the total solid content.

11. The photosensitive resin composition according to claim 1, wherein The content of (E) is 7 to 25 parts by weight based on 100 parts by weight of the total solid content.

12. The photosensitive resin composition according to claim 1 or 2, wherein The number of moles of the carboxyl group in the composition is 1.0 to 1.2 times the number of moles of the epoxy group.

13. The photosensitive resin composition according to claim 1 or 2, wherein The content of (D) is 1.7 to 3.0 times the content of (C) by weight.

14. The photosensitive resin composition according to claim 1 or 2, wherein The (C) contains two or more (meth)acryloyl groups in one molecule, and the functional group equivalent of the (meth)acryloyl group is 100-480.

15. The photosensitive resin composition according to claim 1 or 2, wherein The (C) contains two or more (meth)acryloyl groups in one molecule, and the functional group equivalent of the (meth)acryloyl group is 200-450.

16. The photosensitive resin composition according to claim 1 or 2, wherein The (C) contains a polyoxyalkylene structure. 17 . A dry film obtained by forming the photosensitive resin composition according to claim 1 into a layer. 18 . A cured film formed from a cured product of the photosensitive resin composition according to claim 1 .

19. A printed circuit board with a cured film, comprising the cured film according to claim 18 on and in contact with metal wiring of the printed circuit board.

20. The printed circuit board with a cured film according to claim 19, wherein The printed circuit board has flexibility.

21. A method for manufacturing a printed circuit board with a cured film, wherein: The dry film according to claim 17 is laminated on metal wiring of a printed circuit board, irradiating at least a portion of the surface of the dry film with active light to perform photocuring, The dry film after light curing is heated to perform thermal curing.