A method for testing high temperature attenuation of back-passivated solar cells
By adjusting the irradiation intensity and temperature, combined with the testing method of multiple monitoring, the problem of long and inaccurate testing of high-temperature attenuation of back-passivated solar cells in the existing technology is solved, and fast and accurate high-temperature attenuation value testing is achieved to ensure Provide timely monitoring and accurate reflection of production line quality.
Patent Information
- Application Number
- CN202010836277.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-08-19
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-08-19
AI Technical Summary
The existing method of testing high-temperature attenuation of back-passivated solar cells is time-consuming and lacks real-time monitoring, resulting in inaccurate attenuation values and the inability to accurately judge the quality of back-passivated solar cells.
By adjusting the irradiation intensity and table temperature, the test time is shortened. The adjustable test device is used to increase the light intensity from 1SUN to 2-5SUN and the temperature from 75℃ to 90-110℃. The battery is monitored multiple times during the test. The attenuation value of the chip can be quickly determined at high temperature.
The original test time of 168 hours is shortened to 24-48 hours, which improves the accuracy and timeliness of the test, ensures a true reflection of the quality of the back passivation solar cell, and avoids the problem of the attenuation value not reaching the maximum or recovering.
Smart Images

Figure CN112017984B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar cells and relates to a method for testing the high-temperature attenuation of a back-side passivated solar cell. Background Art
[0002] Back-passivated solar cells can effectively passivate the back of the cell, reduce the recombination of minority carriers on the back surface, and thus greatly improve the photoelectric conversion efficiency of the cell. The outermost layer on the back is usually a silicon nitride dielectric layer, which is used to achieve passivation and protection. The silicon nitride dielectric layer contains a large amount of hydrogen. During the sintering process of the cell, part of this hydrogen will diffuse to the surface of the silicon wafer and leave the cell, and part will diffuse into the body of the silicon wafer to form passivation defects. The hydrogen elements in this passivation defect are easily damaged by high temperature and light. Excessive hydrogen can induce the formation of recombination centers, so the power of the component will be attenuated during subsequent use, and the attenuation is particularly severe at high temperatures. Therefore, testing the high-temperature attenuation value of back-passivated solar cells is an effective means to judge the quality of back-passivated solar cells.
[0003] The current method for testing high temperature attenuation of back-passivated solar cells is as follows:
[0004] 1) Test the initial efficiency of the cell and record it as P0;
[0005] 2) Place the cell on a platform with an irradiance of a standard sunlight intensity and a temperature of 75°C for 168 hours;
[0006] 3) Test the efficiency value of the cell after attenuation and record it as P1;
[0007] 4) Calculate the high temperature attenuation value of the battery cell. The specific formula is: P0-P1 / P0*100%.
[0008] This test scheme takes a long time, there is no monitoring during the process, and only the decay value is tested once. The high temperature decay of the back passivated battery is a process of rapid decay first, slow decay, and finally slow recovery (such as Figure 3 As shown, as the test time of the back-passivated battery increases, the AB segment is a rapid decay period, the BC segment is a slow decay period, and the CD segment is a slow recovery period). It is unknown whether the battery has decayed completely in 168 hours or whether it has decayed and then recovered. Therefore, this test scheme is likely to lead to inaccurate values of high-temperature decay of the battery cell, which interferes with the judgment of the actual results. Summary of the invention
[0009] The present invention relates to a method for testing the high-temperature attenuation of a back-passivated solar cell. By means of a device capable of adjusting the irradiation intensity and the table temperature, the irradiance is increased from one standard solar intensity (1SUN) to between 2 and 5 standard solar intensities (2-5SUN), and the table temperature is increased from 75°C to between 90 and 110°C, thereby quickly testing the high-temperature attenuation value of the back-passivated solar cell, shortening the original test time of 168 hours to 24 to 48 hours, and monitoring the attenuation value of the cell during the process, thereby improving the test accuracy.
[0010] To solve the deficiencies of the prior art, the present invention adopts the following technical solution: A method for testing the high temperature attenuation of a back-passivated solar cell, comprising the following steps:
[0011] (1) Test the initial efficiency of the cell, recorded as P0;
[0012] (2) Adjust the light intensity and table temperature of the test device, and place the cell on the test platform for attenuation after the light intensity and table temperature are stable;
[0013] (3) After 4-8 hours, remove the battery cell, wait for the battery to return to normal temperature, test and record the battery efficiency P1, and place the battery cell on the test platform again to continue attenuation;
[0014] (4) Repeat step (3) and record the battery efficiency P2, P3, P4, ..., P n When the efficiency difference between two consecutive times is less than 0.1%, proceed to the next test step;
[0015] (5) After 1-2 hours, remove the battery cells and test and record the battery efficiency P after the battery returns to normal temperature. n+1 , place the cell on the test platform again to continue attenuation;
[0016] (6) Repeat step (5) and record the battery efficiency P n+2 , P n+3 , P n+4 , P n+m , the power of the next test is higher than the efficiency of the previous test, the test is over, and the efficiency of the penultimate test is P n+m-1 Determine the final efficiency after the battery cell decays and calculate the high temperature decay value of the battery cell.
[0017] The high temperature attenuation value of the battery cell is calculated as follows: High temperature attenuation value = (P0-P n+m-1 / P0)*100%.
[0018] The light intensity of the test device in step (2) is 2-5 standard sun intensities, and the table temperature is 90-110°C.
[0019] In the step (6), the values of n and m are equal or unequal.
[0020] Compared with the prior art, the present invention has the following advantages:
[0021] (1) The present invention increases the irradiance from one standard solar intensity (1SUN) to 2-5 standard solar intensities (2-5SUN), and the table temperature from 75°C to between 90-110°C, which can quickly test the high-temperature attenuation value of the back-passivated solar cell, shortening the original 168-hour test time to 24-48 hours. The quality of the back-passivated solar cells on the production line can be monitored timely and accurately. The present invention has been put into use, and there are no defects such as oxidation and pollution on the surface of the cell, with ideal results.
[0022] (2) The present invention monitors the attenuation value of the back-side passivated solar cell multiple times during the entire test process to avoid the attenuation value of the back-side passivated solar cell failing to reach the maximum or recovering after reaching the maximum value, thereby improving the test accuracy and more truly reflecting the quality of the back-side passivated solar cells on the production line. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Attached Figure 1 It is a schematic diagram of the process of high temperature attenuation test of back-passivated solar cells.
[0024] Attached Figure 2 It is a schematic diagram of the high temperature attenuation test device for back-passivated solar cells.
[0025] Attached Figure 3 This is a graph showing the efficiency of back-passivated solar cells changing with test time.
[0026] Attached Figure 4 This is the attenuation trend diagram of battery samples #1-5 in Example 1.
[0027] Attached Figure 5 This is the attenuation trend diagram of 6-10# battery samples in Example 2.
[0028] Attached Figure 6 This is the attenuation trend diagram of 11-15# battery samples in Example 3.
[0029] Attached Figure 7 This is the attenuation trend diagram of the 16-20# battery samples in Example 4.
[0030] Attached Figure 8 This is the attenuation trend diagram of 21-25# battery samples in Example 5.
[0031] Explanation of reference numerals: 1 - test light source; 2 - battery cell; 3 - temperature control platform. DETAILED DESCRIPTION
[0032] The specific implementation of the present invention is described in detail below in conjunction with the technical scheme and the accompanying drawings.
[0033] Example 1
[0034] A method for testing high temperature attenuation of a back-passivated solar cell comprises the following steps:
[0035] (1) Test the initial efficiency of the cell, recorded as P0;
[0036] (2) Adjust the light intensity of the test device to 2SUN and the table temperature to 90°C. After the light intensity and table temperature are stable, place the cell on the test platform for attenuation.
[0037] (3) After 8 hours, remove the battery cell, wait for the battery to return to normal temperature, test and record the battery efficiency P1, and place the battery cell on the test platform again for decay;
[0038] (4) Repeat step (3) and record the battery efficiencies P2, P3, P4, and P5 at the same time. It is found that the efficiency difference between P5 and P4 is less than 0.1%, and the next test step is entered;
[0039] (5) After 2 hours, remove the battery cell, wait for the battery to return to normal temperature, test and record the battery efficiency P6, and place the battery cell on the test platform again for decay;
[0040] (6) Repeat step (5) and record the battery efficiencies P7, P8, and P9 at the same time. It is found that the value of P9 is higher than that of P8. The test is completed and the efficiency P8 is determined as the final efficiency after the battery cell decays. The high temperature decay value of the battery cell is calculated: high temperature decay value = (P0-P8 / P0)*100%.
[0041] In this embodiment, five battery samples 1#-5# are tested simultaneously. The values of battery efficiency are shown in Table 1. The attenuation trend diagram of battery samples 1#-5# is shown in Figure 4 .
[0042] Table 1 Battery efficiency and battery attenuation values under different test conditions in Example 1
[0043]
[0044] From Table 1 and Figure 4 It can be seen that the battery decays to the lowest point at 46h, and the battery efficiency increases to a certain extent at 48h. Therefore, P8 corresponding to 46h is determined as the final efficiency of the battery after attenuation, and the attenuation values of 1-5# batteries are calculated, which are 2.96%, 3.36%, 3.16%, 3.21%, and 3.74% respectively.
[0045] Example 2
[0046] A method for testing high temperature attenuation of a back-passivated solar cell comprises the following steps:
[0047] (1) Test the initial efficiency of the cell, recorded as P0;
[0048] (2) Adjust the light intensity of the test device to 2SUN and the table temperature to 110°C. After the light intensity and table temperature are stable, place the cell on the test platform for attenuation.
[0049] (3) After 8 hours, remove the battery cell, wait for the battery to return to normal temperature, test and record the battery efficiency P1, and place the battery cell on the test platform again for decay;
[0050] (4) Repeat step (3) and record the battery efficiencies P2 and P3 at the same time. It is found that the efficiency difference between P3 and P2 is less than 0.1%, and the next test step is entered;
[0051] (5) After 2 hours, remove the battery cell, wait for the battery to return to normal temperature, test and record the battery efficiency P4, and place the battery cell on the test platform again for decay;
[0052] (6) Repeat step (5) and record the battery efficiencies P5 and P6 at the same time. It is found that the value of P6 is higher than that of P5. The test is completed and the efficiency P5 is determined as the final efficiency after the battery cell decays. The high temperature decay value of the battery cell is calculated: high temperature decay value = (P0-P5 / P0)*100%.
[0053] In this embodiment, five battery test samples 6#-10# are used. The values of battery efficiency are shown in Table 2. The attenuation trend diagram of battery samples 5-10# is shown in Figure 5 .
[0054] Table 2 Battery efficiency and battery attenuation values under different test conditions in Example 2
[0055]
[0056] From Table 2 and Figure 5 It can be seen that the battery decays to the lowest point at 28 hours, and the battery efficiency increases to a certain extent at 30 hours. Therefore, P5 corresponding to 28 hours is determined as the final efficiency of the battery cell after decay, and the attenuation values of 6-10# batteries are calculated, which are 2.94%, 3.23%, 3.18%, 3.57%, and 3.04% respectively.
[0057] Example 3
[0058] A method for testing high temperature attenuation of a back-passivated solar cell comprises the following steps:
[0059] (1) Test the initial efficiency of the cell, recorded as P0;
[0060] (2) Adjust the light intensity of the test device to 5SUN and the table temperature to 90°C. After the light intensity and table temperature are stable, place the cell on the test platform for attenuation.
[0061] (3) After 8 hours, remove the battery cell, wait for the battery to return to normal temperature, test and record the battery efficiency P1, and place the battery cell on the test platform again for decay;
[0062] (4) Repeat step (3) and record the battery efficiencies P2 and P3 at the same time. It is found that the efficiency difference between P3 and P2 is less than 0.1%, and the next test step is entered;
[0063] (5) After 2 hours, remove the battery cell, wait for the battery to return to normal temperature, test and record the battery efficiency P4, and place the battery cell on the test platform again for decay;
[0064] (6) Repeat step (5) and record the battery efficiencies P5, P6, and P7 at the same time. It is found that the value of P7 is higher than that of P6. The test is completed and the efficiency P6 is determined as the final efficiency after the battery cell decays. The high temperature decay value of the battery cell is calculated: high temperature decay value = (P0-P6 / P0)*100%.
[0065] In this embodiment, five battery test samples 11#-15# are used. The values of battery efficiency are shown in Table 3. The attenuation trend diagram of battery samples 11#-15# is shown in Figure 6 .
[0066] Table 3 Battery efficiency and battery attenuation values under different test conditions in Example 3
[0067]
[0068] From Table 3 and Figure 6 It can be seen that the battery decays to the lowest point at 30h, and the battery efficiency increases to a certain extent at 32h. Therefore, P6 corresponding to 30h is determined as the final efficiency of the battery cell after decay, and the decay values of 11-15# batteries are calculated, which are 2.82%, 3.46%, 2.87%, 3.14%, and 2.92% respectively.
[0069] Example 4
[0070] A method for testing high temperature attenuation of a back-passivated solar cell comprises the following steps:
[0071] (1) Test the initial efficiency of the cell, recorded as P0;
[0072] (2) Adjust the light intensity of the test device to 5SUN and the table temperature to 110°C. After the light intensity and table temperature are stable, place the cell on the test platform for attenuation.
[0073] (3) After 8 hours, remove the battery cell, wait for the battery to return to normal temperature, test and record the battery efficiency P1, and place the battery cell on the test platform again for decay;
[0074] (4) Repeat step (3) and record the battery efficiency P2 at the same time. It is found that the efficiency difference between P2 and P1 is less than 0.1%, and then proceed to the next test step;
[0075] (5) After 2 hours, remove the battery cell, wait for the battery to return to normal temperature, test and record the battery efficiency P3, and place the battery cell on the test platform again for decay;
[0076] (6) Repeat step (5) and record the battery efficiencies P4, P5, and P6 at the same time. It is found that the value of P6 is higher than that of P5. The test is completed and the efficiency P5 is determined as the final efficiency after the battery cell decays. The high temperature decay value of the battery cell is calculated: high temperature decay value = (P0-P5 / P0)*100%.
[0077] In this embodiment, five battery test samples 16#-20# are used. The values of battery efficiency are shown in Table 4. The attenuation trend diagram of battery samples 16#-20# is shown in Figure 7 .
[0078] Table 4 Battery efficiency and battery attenuation values under different test conditions in Example 4
[0079]
[0080] From Table 4 and Figure 7 It can be seen that the battery decays to the lowest point at 22h, and the battery efficiency increases to a certain extent at 24h. Therefore, P5 corresponding to 22h is determined as the final efficiency of the battery cell after decay, and the decay values of 16-20# batteries are calculated, which are 3.82%, 2.73%, 3.73%, 3.23%, and 2.83% respectively.
[0081] Example 5
[0082] A method for testing high temperature attenuation of a back-passivated solar cell comprises the following steps:
[0083] (1) Test the initial efficiency of the cell, recorded as P0;
[0084] (2) Adjust the light intensity of the test device to 3SUN and the table temperature to 100°C. After the light intensity and table temperature are stable, place the cell on the test platform for attenuation.
[0085] (3) After 8 hours, remove the battery cell, wait for the battery to return to normal temperature, test and record the battery efficiency P1, and place the battery cell on the test platform again for decay;
[0086] (4) Repeat step (3) and record the battery efficiencies P2 and P3 at the same time. It is found that the efficiency difference between P3 and P2 is less than 0.1%, and the next test step is entered;
[0087] (5) After 2 hours, remove the battery cell, wait for the battery to return to normal temperature, test and record the battery efficiency P4, and place the battery cell on the test platform again for decay;
[0088] (6) Repeat step (5) and record the battery efficiencies P5 and P6 at the same time. It is found that the value of P6 is higher than that of P5. The test is completed and the efficiency P5 is determined as the final efficiency after the battery cell decays. The high temperature decay value of the battery cell is calculated: high temperature decay value = (P0-P5 / P0)*100%.
[0089] In this embodiment, five battery test samples 21#-25# are used. The values of battery efficiency are shown in Table 5. The attenuation trend diagram of battery samples 21#-25# is shown in Figure 8 .
[0090] Table 5 Battery efficiency and battery attenuation values under different test conditions in Example 5
[0091]
[0092] From Table 5 and Figure 8 It can be seen that the battery decays to the lowest point at 28h, and the battery efficiency increases to a certain extent at 30h. Therefore, P5 corresponding to 28h is determined as the final efficiency of the battery cell after decay, and the decay values of 21-25# batteries are calculated, which are 2.82%, 3.61%, 2.55%, 2.72%, and 3.16% respectively.
[0093] Figure 2 This is a schematic diagram of the high temperature attenuation test device for back-passivated solar cells. Figure 2 The high temperature attenuation test of the back passivated solar cell in Examples 1-5 is performed on the test device shown. The present invention increases the irradiance from 1SUN to 2-5SUN, and the table temperature from 75°C to between 90-110°C, and can quickly test the high temperature attenuation value of the back passivated solar cell, shortening the original 168-hour test time to 24-48 hours, and can timely and accurately monitor the quality of the back passivated solar cells on the production line. It has been put into use, and there are no defects such as oxidation and pollution on the surface of the cell, and the effect is ideal.
[0094] The present invention monitors the attenuation value of the back-side passivated solar cell multiple times during the entire test process to avoid the attenuation value of the back-side passivated solar cell failing to reach the maximum or recovering after reaching the maximum value, thereby improving the test accuracy and more truly reflecting the quality of the back-side passivated solar cells on the production line.
[0095] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for testing high temperature attenuation of a back-passivated solar cell, characterized in that: The following steps are involved: (1) Test the initial efficiency of the cell, recorded as P0; (2) Adjust the light intensity and table temperature of the test device. After the light intensity and table temperature are stable, place the cell on the test platform for attenuation. (3) After 4-8 hours, remove the battery cell, wait for the battery to return to normal temperature, test and record the battery efficiency P1, and place the battery cell on the test platform again to continue attenuation; (4) Repeat step (3) and record the battery efficiency P2, P3, P4, ..., P n When the efficiency difference between two consecutive times is less than 0.1%, proceed to the next test step; (5) After 1-2 hours, remove the battery cells and test and record the battery efficiency P after the battery returns to normal temperature. n+1 , place the cell on the test platform again to continue attenuation; (6) Repeat step (5) and record the battery efficiency P n+2 , P n+3 , P n+4 , P n+m , the power of the next test is higher than the efficiency of the previous test, the test is over, and the efficiency of the penultimate test is P n+m-1 Determine the final efficiency after the battery cell decays and calculate the high temperature decay value of the battery cell; The light intensity of the test device in step (2) is 2-5 standard suns, and the table temperature is 90-110°C; In step (6), the values of n and m are equal or unequal; The calculation formula of the high temperature attenuation value of the battery cell is: high temperature attenuation value = (P0-P n+m-1 / P0)*100%.
Citation Information
Patent Citations
Monitoring testing method of long-time photo induced deterioration property of solar battery
CN103336236A
Method and device for eliminating light-induced degradation of B-doped crystal silicon solar cell
CN105552173A