Non-aqueous electrolyte secondary battery

Through the layer structure design of the first negative electrode mixture layer with a high content of Si-based active material and the second negative electrode mixture layer with a low-content Si-based active material in the wound electrode body of the non-aqueous electrolyte secondary battery, the Si problem is solved It is a problem of reduced cycle characteristics caused by changes in the volume of active materials, which improves the cycle characteristics and capacity retention rate of the battery.

CN112204767BActive Publication Date: 2024-10-11PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980035813.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-05-30
Filing Date
2019-04-26
Publication Date
2024-10-11
Estimated Expiration
2039-04-26

AI Technical Summary

Technical Problem

Si and Si-containing materials have a large volume change in non-aqueous electrolyte secondary batteries, resulting in reduced cycle characteristics, especially in the part with a small curvature radius in the wound electrode body.

Method used

In the negative electrode of the wound electrode body, the Si standard of the Si-based active material is controlled by layer structure design such that the first negative electrode mixture layer contains a high content of Si-based active material and the second negative electrode mixture layer contains a low-content Si-based active material. The content ratio is such that the content ratio of the Si-based active material in the negative electrode mixture layer is higher in the first layer than in the second layer, thereby reducing the negative impact of volume changes on battery cycle characteristics during charge and discharge.

Benefits of technology

It effectively improves the cycle characteristics of non-aqueous electrolyte secondary batteries, prevents the Si-based active material particles from weakening the contact and isolating the conductive paths, and achieves high capacity while suppressing the degradation of cycle characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112204767B_ABST
    Figure CN112204767B_ABST
Patent Text Reader

Abstract

The object of the present invention is to improve the cycle characteristics in a non-aqueous electrolyte secondary battery having a wound electrode body using a Si-based active material in a negative electrode active material. As an example of an embodiment, a non-aqueous electrolyte secondary battery has a wound electrode body in which a positive electrode and a negative electrode are wound with a separator. The negative electrode has a negative electrode collector, a first negative electrode mixture layer formed on the first surface of the negative electrode collector facing the outside of the electrode body, and a second negative electrode mixture layer formed on the second surface of the negative electrode collector facing the inside of the electrode body. At least the first negative electrode mixture layer contains a Si-based active material, and the Si-based content ratio of the Si-based active material in the second negative electrode mixture layer is lower than the Si-based content ratio of the Si-based active material in the first negative electrode mixture layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a nonaqueous electrolyte secondary battery, and more specifically to a nonaqueous electrolyte secondary battery including a wound electrode body. Background Art

[0002] It is known that Si and Si-containing materials can absorb more lithium ions per unit volume compared to carbon materials such as graphite. Therefore, by using Si-containing materials in the negative electrode active material, it is possible to achieve a high capacity of the battery. For example, Patent Document 1 discloses a non-aqueous electrolyte secondary battery using graphite and Si-containing materials in the negative electrode active material. In addition, Patent Document 1 discloses a structure in which the mass ratio of graphite to Si-containing material in the negative electrode mixture layer (mass of graphite / mass of Si-containing material) increases continuously or intermittently as it moves away from the surface of the negative electrode collector.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2013-178913 Summary of the invention

[0006] Problem that the invention aims to solve

[0007] However, Si and Si-containing materials undergo large volume changes with charge and discharge, so there is a problem that the cycle characteristics are easily reduced in non-aqueous electrolyte secondary batteries using Si-based active materials composed of at least one of Si and Si-containing materials as negative electrode active materials. In particular, in the case of a wound electrode body, the volume change of the Si-based active material has a large impact on the part with a small radius of curvature of the negative electrode such as the end portion at the start of winding. The purpose of the present invention is to improve the cycle characteristics in a non-aqueous electrolyte secondary battery having a wound electrode body using a Si-based active material as a negative electrode active material.

[0008] Means used to solve problems

[0009] A nonaqueous electrolyte secondary battery as one embodiment of the present invention is a nonaqueous electrolyte secondary battery having a wound electrode body in which a positive electrode and a negative electrode are wound with a separator interposed therebetween, wherein the negative electrode comprises a negative electrode current collector, a first negative electrode mixture layer formed on a first surface of the negative electrode current collector facing the outside of the electrode body, and a second negative electrode mixture layer formed on a second surface of the negative electrode current collector facing the inside of the electrode body. The first negative electrode mixture layer contains a Si-based active material composed of at least one of Si and a Si-containing material, and the Si-based content ratio of the Si-based active material in the second negative electrode mixture layer is lower than the Si-based content ratio of the Si-based active material in the first negative electrode mixture layer.

[0010] Effects of the Invention

[0011] According to one aspect of the present invention, the cycle characteristics can be improved in a non-aqueous electrolyte secondary battery including a wound electrode body using a Si-based active material as a negative electrode active material. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 It is a cross-sectional view of a nonaqueous electrolyte secondary battery as an example of an embodiment.

[0013] Figure 2 It is a cross-sectional view of a negative electrode as an example of an embodiment. DETAILED DESCRIPTION

[0014] As described above, for a non-aqueous electrolyte secondary battery having a wound electrode body using a Si-based active material as a negative electrode active material, there is a problem that the cycle characteristics are easily reduced. The reduction in the cycle characteristics occurs due to the large volume change of the Si-based active material during charging and discharging. Specifically, it is believed that the main reason is that due to the large volume change of the Si-based active material, the degree of contact between the active material particles becomes weaker, or the contact state is lost, and the number of active material particles isolated from the conductive path in the negative electrode mixture layer increases. In a wound electrode body, especially in the part where the curvature radius of the negative electrode is small, such as the end of the winding start side, the volume change of the Si-based active material has a great impact.

[0015] As a result of in-depth research by the inventors to solve the above-mentioned problems, it was found that by making the Si-based content ratio of the Si-based active material in the second negative electrode mixture layer lower than the Si-based content ratio of the Si-based active material in the first negative electrode mixture layer, the cycle characteristics of the battery are particularly improved. According to the non-aqueous electrolyte secondary battery of the present invention, it is possible to efficiently add Si-based active materials to the negative electrode mixture layer to achieve high capacity while suppressing the reduction of cycle characteristics.

[0016] Hereinafter, an example of an embodiment of the present invention will be described in detail. Hereinafter, a cylindrical battery in which a wound electrode body 14 is contained in a cylindrical battery case 15 is exemplified, but the battery case is not limited to a cylindrical shape, and may be, for example, a square shape, or may be a battery case composed of a laminated sheet including a metal layer and a resin layer. The electrode body may have a wound structure and may be formed into a flat shape. The configuration of the negative electrode according to the present invention is particularly effective when the electrode body has a cylindrical wound structure.

[0017] Figure 1 FIG. 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery 10 as an example of an embodiment. Figure 1As shown, the nonaqueous electrolyte secondary battery 10 includes a wound electrode body 14, a nonaqueous electrolyte (not shown), and a battery case 15 that accommodates the electrode body 14 and the nonaqueous electrolyte. The electrode body 14 has a wound structure in which the positive electrode 11 and the negative electrode 12 are wound with a separator 13 interposed therebetween. The battery case 15 is composed of a bottomed cylindrical outer can 16 and a sealing body 17 that seals the opening of the outer can 16. In addition, the nonaqueous electrolyte secondary battery 10 includes a resin gasket 28 disposed between the outer can 16 and the sealing body 17.

[0018] The non-aqueous electrolyte comprises a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Among the non-aqueous solvents, for example, esters, ethers, nitriles, amides, and mixed solvents of two or more thereof can be used. The non-aqueous solvent may contain a halogen-substituted substance in which at least a portion of the hydrogen of these solvents is replaced by a halogen atom such as fluorine. It should be noted that the non-aqueous electrolyte is not limited to a liquid electrolyte, and may be a solid electrolyte using a gel-like polymer or the like. Among the electrolyte salts, for example, lithium salts such as LiPF6 are used.

[0019] The electrode body 14 is composed of a long positive electrode 11, a long negative electrode 12, two long separators 13, a positive electrode tab 20 joined to the positive electrode 11, and a negative electrode tab 21 joined to the negative electrode 12. In order to prevent lithium precipitation, the negative electrode 12 is formed to be one size larger than the positive electrode 11. That is, the negative electrode 12 is formed longer than the positive electrode 11 in the length direction and the width direction (short side direction). The two separators 13 are formed to be at least one size larger than the positive electrode 11, and are arranged in a manner to sandwich the positive electrode 11, for example.

[0020] Insulating plates 18 and 19 are disposed above and below the electrode body 14 , respectively. Figure 1 In the example shown, the positive electrode tab 20 attached to the positive electrode 11 extends to the sealing body 17 side through the through hole of the insulating plate 18, and the negative electrode tab 21 attached to the negative electrode 12 extends to the bottom side of the outer can 16 through the outer side of the insulating plate 19. The positive electrode tab 20 is connected to the lower surface of the bottom plate 23 of the sealing body 17 by welding or the like, and the top plate of the sealing body 17, that is, the cap 27 electrically connected to the bottom plate 23 serves as the positive terminal. The negative electrode tab 21 is connected to the bottom inner surface of the outer can 16 by welding or the like, and the outer can 16 serves as the negative terminal.

[0021] The outer can 16 is, for example, a metal container in a cylindrical shape with a bottom. As described above, a gasket 28 is provided between the outer can 16 and the sealing body 17, and the internal space of the battery case 15 is sealed. The outer can 16 has a groove 22 for supporting the sealing body 17, for example, formed by squeezing the side surface from the outside. The groove 22 is preferably formed in an annular shape along the circumference of the outer can 16, and the sealing body 17 is supported on its upper surface. In addition, the upper end of the outer can 16 is bent inwardly and riveted to the peripheral portion of the sealing body 17.

[0022] The sealing body 17 has a structure in which a bottom plate 23, a lower valve body 24, an insulating component 25, an upper valve body 26 and a cap 27 are stacked in order from the electrode body 14 side. The components constituting the sealing body 17 have, for example, a disc shape or a ring shape, and the components except the insulating component 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected at their respective central portions, and an insulating component 25 is present between their respective peripheral portions. If the internal pressure of the battery rises due to abnormal heat generation, the lower valve body 24 deforms and breaks in such a way that the upper valve body 26 is pushed up to the cap 27 side, thereby blocking the current path between the lower valve body 24 and the upper valve body 26. If the internal pressure rises further, the upper valve body 26 breaks, and the gas is discharged from the opening of the cap 27.

[0023] [positive electrode]

[0024] The positive electrode 11 has a positive electrode collector 30 and a positive electrode mixture layer 31 formed on both sides of the positive electrode collector 30. For the positive electrode collector 30, a foil of a metal such as aluminum or aluminum alloy that is stable within the potential range of the positive electrode 11, a film that arranges the metal on the surface, etc. can be used. The positive electrode mixture layer 31 contains a positive electrode active material, a conductive material, and a binder. The positive electrode 11 can be made in the following manner: for example, a positive electrode mixture slurry containing a positive electrode active material, a conductive material, and a binder is applied to the positive electrode collector 30, and the coating is dried and then compressed to form a positive electrode mixture layer 31 on both sides of the positive electrode collector 30.

[0025] The positive electrode active material is composed of a lithium-containing metal composite oxide as a main component. As the metal elements contained in the lithium-containing metal composite oxide, Ni, Co, Mn, Al, B, Mg, Ti, V, Cr, Fe, Cu, Zn, Ga, Sr, Zr, Nb, In, Sn, Ta, W, etc. can be cited. An example of a suitable lithium-containing metal composite oxide is a composite oxide containing at least one of Ni, Co, Mn, and Al. It should be noted that inorganic compound particles such as aluminum oxide and compounds containing lanthanide elements may be fixed on the surface of the particles of the lithium-containing metal composite oxide.

[0026] As the conductive material included in the positive electrode mixture layer 31, carbon materials such as carbon black, acetylene black, Ketjen black, and graphite can be exemplified. As the binder included in the positive electrode mixture layer 31, fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide, acrylic resin, polyolefin, etc. can be exemplified. These resins can be used in combination with cellulose derivatives such as carboxymethyl cellulose (CMC) or its salt, polyethylene oxide (PEO), etc.

[0027] [negative electrode]

[0028] Figure 2 is a diagram showing a cross section of the negative electrode 12. Figure 1 He Ru Figure 2 For example, the negative electrode 12 includes a negative electrode current collector 40, a negative electrode mixture layer 41 (first negative electrode mixture layer) formed on the first surface 40a of the negative electrode current collector 40 facing the outside of the electrode body 14, and a negative electrode mixture layer 42 (second negative electrode mixture layer) formed on the second surface 40b of the negative electrode current collector 40 facing the inside of the electrode body 14. The positive electrode 11 has a layer structure in which the same positive electrode mixture layer 31 is formed on both sides of the positive electrode current collector 30, while the negative electrode 12 has a layer structure in which different negative electrode mixture layers 41 and 42 are formed on the first surface 40a and the second surface 40b of the negative electrode current collector 40. As will be described in detail later, the composition of the mixture contained in the negative electrode mixture layer 41 and the composition of the mixture contained in the negative electrode mixture layer 42 are different from each other.

[0029] For the negative electrode collector 40, a foil of a metal such as copper or copper alloy that is stable within the potential range of the negative electrode 12, a film in which the metal is arranged on the surface, etc. can be used. The negative electrode mixture layer 41 contains a negative electrode active material and a binder. The negative electrode 12 can be manufactured in the following manner: for example, a negative electrode mixture slurry containing a negative electrode active material and a binder is applied to the negative electrode collector 40, and the coating is dried and then compressed to form a negative electrode mixture layer 41 on the first surface 40a of the negative electrode collector 40, and a negative electrode mixture layer 42 is formed on the second surface 40b of the negative electrode collector 40. In the manufacture of the negative electrode 12, for example, two kinds of negative electrode mixture slurries are used.

[0030] like Figure 2 For example, the negative electrode 12 constituting the wound electrode body 14 is bent over the entire length in the longitudinal direction. The negative electrode 12 is manufactured in a flat plate state, and is wound together with the positive electrode 11 and the separator 13 when manufacturing the electrode body 14, so as to be bent. The negative electrode 12 generally has a curvature radius of about 1 mm to 10 mm, and the curvature radius is different at the winding start side and the winding end side of the electrode body 14. The curvature radius of the negative electrode 12 is such that the end of the winding start side is less than the end of the winding end side. The minimum value of the curvature radius of the negative electrode 12 is, for example, 1 mm to 5 mm, or 1 mm to 2 mm.

[0031] The negative electrode 12 is manufactured in a flat state, so the convex side is stretched and the concave side is compressed in a bent state. That is, the negative electrode mixture layer 41 formed on the first surface 40a of the negative electrode collector 40 facing the outside of the electrode body 14 is stretched, and the negative electrode mixture layer 42 formed on the second surface 40b of the negative electrode collector 40 facing the inside of the electrode body 14 is compressed. It should be noted that the inventors of the present invention have focused on this point and successfully improved the cycle characteristics of the battery by improving the layer structure of the negative electrode 12.

[0032] The negative electrode mixture layers 41 and 42 have in common that they contain a Si-based active material composed of at least one of Si and a Si-containing material. On the other hand, the Si-based content ratio of the Si-based active material in the negative electrode mixture layer 42 is lower than the Si-based content ratio of the Si-based active material in the negative electrode mixture layer 41. As described above, since the negative electrode mixture layer 42 is compressed, there is less room for allowing a large volume change of the Si-based active material compared to the negative electrode mixture layer 41. Therefore, from the viewpoint of improving the cycle characteristics, it is preferable to set the Si-based content ratio of the Si-based active material in the negative electrode mixture layer 41> the Si-based content ratio of the Si-based active material in the negative electrode mixture layer 42. The Si-based content ratio of the Si-based active material is calculated as a ratio of the Si-based mass of the Si-based active material in each of the negative electrode mixture layers 41 and 42 to the mass of the negative electrode active material. The Si-based mass of the Si-based active material is calculated by multiplying the mass of the Si-based active material by the mass ratio of Si to the Si-based active material.

[0033] In other words, the Si-based content ratio of the Si-based active material in the negative electrode mixture layer 41 is made higher than the Si-based content ratio of the Si-based active material in the negative electrode mixture layer 42. As described above, since the negative electrode mixture layer 41 is elongated, the negative electrode mixture layer 41 has a space margin that allows a large volume change of the Si-based active material compared to the negative electrode mixture layer 42, so even if the amount of the Si-based active material is increased, it is not easy to cause a decrease in the cycle characteristics. By controlling the Si-based content ratio of the Si-based active material in the negative electrode mixture layers 41 and 42 in the above manner, it is possible to efficiently add the Si-based active material to achieve high capacity while suppressing the decrease in cycle characteristics.

[0034] The negative electrode mixture layers 41 and 42 preferably also contain a carbon-based active material. That is, as the negative electrode active material, it is preferred to use a Si-based active material and a carbon-based active material in combination. It should be noted that the Si-based active material may not be added to the negative electrode mixture layer 42, but only added to the negative electrode mixture layer 41. In the present embodiment, it is added to both the negative electrode mixture layers 41 and 42. If the cycle characteristics are considered, it is preferred that the content of the Si-based active material in the negative electrode mixture layers 41 and 42 is less than the content of the carbon-based active material. Suitable carbon-based active materials are graphites such as natural graphites such as flaky graphite, blocky graphite, and amorphous graphite, blocky artificial graphite (MAG), and artificial graphite such as graphitized mesophase carbon microbeads (MCMB).

[0035] The Si-based active material is composed of at least one of Si and a Si-containing material, and is preferably composed of a Si-containing material whose volume change during charge and discharge is smaller than that of Si. Examples of the Si-containing material include SiO x (0.5≤x≤1.6) represented by the material. SiO xIt has a structure in which Si particles are dispersed in a SiO2 matrix. The Si-containing material can be a lithium silicate (Li 2y SiO (2+y) (0<y<2)) A material (LSi) in which Si fine particles are dispersed in the phase. The negative electrode mixture layers 41 and 42 may contain SiO x and LSi.

[0036] On the surface of the particles of the Si-containing material, a conductive coating composed of a material having a higher conductivity than that of the Si-containing material is preferably formed. As the constituent material of the conductive coating, at least one selected from carbon materials, metals, and metal compounds can be exemplified. Among them, carbon materials such as amorphous carbon are preferred. The carbon coating can be formed by, for example, a CVD method using acetylene, methane, etc.; a method of mixing coal tar, petroleum asphalt, phenolic resin, etc. with Si-containing material particles and heat treating them, etc. In addition, a conductive coating can be formed by fixing a conductive filler such as carbon black to the surface of the particles of the Si-containing material using a binder. The conductive coating is formed, for example, at 0.5% to 10% by mass relative to the mass of the Si-containing material particles.

[0037] As described above, the Si-based content ratio of the Si-based active material in the negative electrode mixture layers 41 and 42 is negative electrode mixture layer 41>negative electrode mixture layer 42. The difference in the Si-based content ratio of the Si-based active material in the negative electrode mixture layers 41 and 42 is preferably 1% or more, more preferably 1.5% or more, and further preferably 2% or more. In this case, the effect of improving the cycle characteristics becomes more significant. The Si-based content ratio of the Si-based active material and the carbon-based active material can be measured by ICP (Inducticely Coupled Plasma: plasma emission analysis).

[0038] When a Si-based active material and a carbon-based active material are used in combination as the negative electrode active material, the mass-based content ratio of the Si-based active material (Si-containing material) in the negative electrode mixture layers 41 and 42 is also preferably negative electrode mixture layer 41> negative electrode mixture layer 42. The content ratio of the Si-based active material in the negative electrode mixture layer 41 is preferably 5% by mass to 25% by mass, and more preferably 10% by mass to 15% by mass. The content ratio of the Si-based active material in the negative electrode mixture layer 42 is a value lower than the content ratio of the negative electrode mixture layer 41, preferably lower than 15% by mass, and more preferably 5% by mass to 10% by mass. It should be noted that different Si-based active materials can be added to the negative electrode mixture layers 41 and 42.

[0039] The content ratio of the Si-based active material in the negative electrode active material in the negative electrode mixture layer 41 is preferably 5% by mass to 25% by mass, and more preferably 10% by mass to 15% by mass. The content ratio of the Si-based active material in the negative electrode active material in the negative electrode mixture layer 42 is preferably less than 15% by mass, and more preferably 5% by mass to 10% by mass. In other words, the content ratio of the carbon-based active material in the negative electrode active material in the negative electrode mixture layer 41 is preferably 75% by mass to 95% by mass, and the content ratio of the carbon-based active material in the negative electrode active material in the negative electrode mixture layer 42 is preferably 85% by mass or more.

[0040] As for the binder contained in the negative electrode mixture layers 41 and 42, as in the case of the positive electrode 11, fluororesins, PAN, polyimide, acrylic resins, polyolefins, etc. can be used, preferably styrene-butadiene rubber (SBR) or its modified body. In the negative electrode mixture layers 41 and 42, for example, on the basis of SBR, CMC or its salt, polyacrylic acid (PAA) or its salt, polyvinyl alcohol, etc. can also be included. The type and content of the binder in the negative electrode mixture layers 41 and 42 can be different from each other or the same.

[0041] The negative electrode mixture layers 41 and 42 may have different thicknesses, but are preferably formed with approximately the same thickness. The thickness of the negative electrode mixture layers 41 and 42 is, for example, 30 μm to 80 μm, preferably 40 μm to 60 μm. Other negative electrode active materials other than Si-based active materials and carbon-based active materials may be further added to the negative electrode mixture layers 41 and 42. Examples of other negative electrode active materials include metals other than Si that alloy with lithium, compounds containing the metals, lithium titanate, and the like.

[0042] [Spacer]

[0043] The spacer 13 may be a porous sheet having ion permeability and insulation. Specific examples of the porous sheet include microporous films, woven fabrics, nonwoven fabrics, etc. The material of the spacer 13 is preferably olefin resins such as polyethylene and polypropylene, cellulose, etc. The spacer 13 may be a single-layer structure or a laminated structure. A heat-resistant layer may be formed on the surface of the spacer 13.

[0044] Example

[0045] Hereinafter, the present invention will be further described by way of examples, but the present invention is not limited to these examples.

[0046] <Example 1>

[0047] [Production of positive electrode]

[0048] Will be made of LiNi 0.88 Co 0.09 Al0.03 A lithium-containing metal composite oxide represented by O2, carbon black, and polyvinylidene fluoride were mixed in a mass ratio of 100:0.8:0.7, and after adding an appropriate amount of N-methyl-2-pyrrolidone, they were kneaded to prepare a positive electrode mixture slurry. The positive electrode mixture slurry was coated on both sides of a positive electrode collector formed of aluminum foil with a thickness of 15 μm, and after the coating film was dried, the coating film was rolled with a roller and cut into a specified electrode size, thereby producing a positive electrode having a positive electrode mixture layer formed on both sides of the positive electrode collector.

[0049] [Preparation of the first negative electrode mixture slurry]

[0050] Graphite powder and SiO x The Si-containing material represented by (x=1) was mixed in a mass ratio of 88:12 to prepare a negative electrode active material. The negative electrode active material, sodium salt of CMC, and polyacrylic acid were mixed in a mass ratio of 100:1:1, and pure water was added to knead for 30 minutes so that the solid content was 60% by mass. Thereafter, pure water was added so that the solid content was 50% by mass, and a dispersion of SBR was added so that it was 1% by mass relative to the negative electrode active material, thereby preparing a first negative electrode mixture slurry.

[0051] [Preparation of Second Negative Electrode Mixture Slurry]

[0052] A second negative electrode mixture slurry was prepared in the same manner as in the first negative electrode mixture slurry except that graphite and the Si-containing material were mixed at a mass ratio of 92:8.

[0053] [Production of negative electrode]

[0054] The first negative electrode mixture slurry is applied to one side of a negative electrode collector formed of copper foil with a thickness of 8 μm, and the coating is dried to form the first negative electrode mixture layer on one side of the negative electrode collector. Then, the second negative electrode mixture slurry is applied to the other side of the negative electrode collector with the same coating amount as the first negative electrode mixture slurry, and the coating is dried to form the second negative electrode mixture layer on the other side of the negative electrode collector. Next, the coating (mixture layer) is rolled with a roller and cut into a specified electrode size to produce a negative electrode. It should be noted that the wound electrode body described later is produced in such a way that one side of the collector becomes the first side facing the outside of the electrode body and the other side becomes the second side facing the inside of the electrode body. Table 1 shows the content ratio of the Si-containing material in each negative electrode mixture layer relative to the total mass of the negative electrode active material. In addition, the Si-based content ratio of the Si-containing material in each negative electrode mixture layer is shown in the brackets of Table 1.

[0055] [Production of electrode body]

[0056] The positive electrode and the negative electrode were wound around a winding core with a curvature radius of 1.5 mm through a separator having a thickness of 20 μm and made of a polyethylene microporous film, and a tape was attached to the outermost surface to prepare a cylindrical wound electrode body. It should be noted that an aluminum positive electrode lead was welded to the exposed portion of the positive electrode collector, and a nickel negative electrode lead was welded to the exposed portion of the negative electrode collector.

[0057] [Preparation of non-aqueous electrolyte]

[0058] In a mixed solvent of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate at a volume ratio of 20:60:20, vinylene carbonate was dissolved at a concentration of 2 mass %. Thereafter, LiPF6 was dissolved at a concentration of 1.3 mol / L to prepare a non-aqueous electrolyte.

[0059] [Battery production]

[0060] The electrode body was placed in a bottomed cylindrical outer can, the positive electrode lead was welded to the sealing body, and the negative electrode lead was welded to the inner bottom surface of the outer can. After the non-aqueous electrolyte was injected into the outer can, the opening of the outer can was sealed with the sealing body, thereby manufacturing a non-aqueous electrolyte secondary battery (height 65mm, diameter 18mm, design capacity 3500mAh).

[0061] [Evaluation of Cycle Characteristics (Capacity Retention Ratio)]

[0062] The battery was charged and discharged at 25° C. under the following conditions to determine the capacity retention rate. The evaluation results shown in Table 1 are relative values ​​when the capacity retention rate of the battery of Comparative Example 1 is set to 100.

[0063] <Charge and discharge conditions>

[0064] Charging: Constant current charging at 1050 mA until the battery voltage reaches 4.2 V. Then constant voltage charging at 4.2 V until the current value reaches 70 mA.

[0065] Discharge: Discharge at a constant current of 1750 mA until the voltage reaches 2.5 V.

[0066] This charge and discharge cycle was repeated 100 times, and the capacity retention rate was calculated by the following formula.

[0067] Capacity retention rate (%) = 100th cycle discharge capacity ÷ 1st cycle discharge capacity × 100

[0068] <Example 2>

[0069] A negative electrode and a nonaqueous electrolyte secondary battery were prepared in the same manner as in Example 1 except that the content ratio of the Si-containing material to the total mass of the negative electrode active material was set to the amounts shown in Table 1, and the cycle characteristics were evaluated.

[0070] <Comparative Example 1>

[0071] As the negative electrode mixture slurry for forming the above-mentioned first negative electrode mixture layer and the above-mentioned second negative electrode mixture layer, the same slurry (mass ratio of graphite to Si-containing material = 90:10) was used as shown in Table 1. Except for this, the negative electrode and non-aqueous electrolyte secondary battery were prepared in the same manner as in Example 1, and the cycle characteristics were evaluated.

[0072] [Table 1]

[0073]

[0074] As shown in Table 1, the batteries of the embodiment in which the Si-based content ratio of the Si-based active material was set to 1st negative electrode mixture layer>2nd negative electrode mixture layer had higher capacity retention and better cycle characteristics than the batteries of Comparative Example 1. The battery of Example 2 in which the difference in the content ratio of the Si-based active material in each negative electrode mixture layer was 2% also clearly confirmed the improvement in cycle characteristics.

[0075] Description of Reference Numerals

[0076] 10 non-aqueous electrolyte secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 15 battery case, 16 outer can, 17 sealing body, 18, 19 insulating plate, 20 positive electrode terminal, 21 negative electrode terminal, 22 groove, 23 bottom plate, 24 lower valve body, 25 insulating member, 26 upper valve body, 27 cap, 28 gasket, 30 positive electrode collector, 31 positive electrode mixture layer, 40 negative electrode collector, 40a first surface, 40b second surface, 41, 42 negative electrode mixture layer

Claims

1. A non-aqueous electrolyte secondary battery comprising a wound electrode body in which a positive electrode and a negative electrode are wound with a separator interposed therebetween, wherein: The negative electrode comprises: a negative electrode current collector, a first negative electrode mixture layer formed on a first surface of the negative electrode current collector facing the outside of the electrode body, and a second negative electrode mixture layer formed on a second surface of the negative electrode current collector facing the inside of the electrode body. The first negative electrode mixture layer includes a Si-based active material composed of at least one of Si and a Si-containing material. The content ratio of the Si-based active material in the second negative electrode mixture layer based on Si is lower than the content ratio of the Si-based active material in the first negative electrode mixture layer based on Si. The second negative electrode mixture layer contains the Si-based active material, the content ratio of the Si-based active material in the first negative electrode mixture layer is 10 mass % to 15 mass %, and the content ratio of the Si-based active material in the second negative electrode mixture layer is 5 mass % to 10 mass %, A difference between a content ratio of the Si-based active material in the first negative electrode mixture layer and a content ratio of the Si-based active material in the second negative electrode mixture layer based on Si is 1% or more and 2.5% or less.

2. The nonaqueous electrolyte secondary battery according to claim 1, wherein The minimum value of the curvature radius of the negative electrode is 1 mm to 5 mm.

3. The nonaqueous electrolyte secondary battery according to claim 1 or 2, wherein: The first negative electrode mixture layer and the second negative electrode mixture layer contain a carbon-based active material.