Non-aqueous electrolyte secondary battery

By using the negative electrode material of lithium silicate phase and silicon particles in a nonaqueous electrolyte secondary battery, and adding an appropriate amount of halogenated benzene to the electrolyte solution, the initial charge of the existing battery was solved by forming a sparse coating to inhibit the irreversible reaction. The problem of low discharge efficiency improves the energy density and cycle stability of the battery.

CN112313826BActive Publication Date: 2024-11-01PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980040729.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-06-29
Filing Date
2019-02-20
Publication Date
2024-11-01
Estimated Expiration
2039-02-20

AI Technical Summary

Technical Problem

The existing nonaqueous electrolyte secondary batteries have low initial charge and discharge efficiency during charging and discharging, especially due to the irreversible reaction in the lithium silicate phase, the lithium ion storage efficiency is reduced, which affects the high energy density and cycle stability of the battery. .

Method used

Using a negative electrode material containing a lithium silicate phase and silicon particles dispersed therein, a sparse coating film is formed by adding an appropriate amount of halogenated benzene to the electrolyte to inhibit irreversible reactions, and combining appropriate combinations of lithium salts and nonaqueous solvents. , optimize the composition of the electrolyte to improve lithium ion conductivity and battery stability.

Benefits of technology

The initial charging and discharging efficiency and circulation capacity maintenance rate of the nonaqueous electrolyte secondary battery are significantly improved, the service life of the battery is extended, and the structural stability and circulation characteristics of the battery are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112313826B_ABST
    Figure CN112313826B_ABST
Patent Text Reader

Abstract

The non-aqueous electrolyte secondary battery comprises a positive electrode, a negative electrode and an electrolyte. The negative electrode comprises a negative electrode active material capable of electrochemically absorbing and releasing lithium, and the negative electrode active material comprises a lithium silicate phase and silicon particles dispersed in the lithium silicate phase. The lithium silicate phase is an oxide phase comprising lithium, silicon and oxygen, and the atomic ratio of oxygen to silicon in the lithium silicate phase: O / Si is greater than 2 and less than 4. The electrolyte comprises a halogenated benzene, and the content of the halogenated benzene in the electrolyte is greater than 1 ppm and less than 500 ppm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a non-aqueous electrolyte secondary battery obtained using a negative electrode active material containing a lithium silicate phase in which silicon particles are dispersed. Background Art

[0002] In recent years, non-aqueous electrolyte secondary batteries, particularly lithium ion secondary batteries, have been highly anticipated as power sources for small consumer applications, energy storage devices, and electric vehicles because of their high voltage and high energy density. In today's search for higher energy density batteries, materials containing silicon that alloy with lithium are expected as negative electrode active materials with high theoretical capacity density.

[0003] Compared with graphite, the amount of lithium ions occluded per unit volume of SiO x is large, but the irreversible capacity during charge and discharge is large. The initial charge-discharge efficiency of a non-aqueous electrolyte secondary battery using SiO (x = 1) may be as low as, for example, about 70%.

[0004] SiO x contains a matrix of SiO2 and fine Si particles dispersed in the matrix. During charging, the Si particles undergo the reaction of the following formula (i), and the SiO2 matrix undergoes the reaction of the following formula (ii).

[0005] (i) Si + 4Li + + 4e - → Li4Si

[0006] (ii) 2SiO2 + 8Li + + 8e - → Li4Si + Li4SiO4

[0007] The reaction of the above formula (ii) is an irreversible reaction. That is, the lithium ions occluded in the SiO2 matrix during charging are difficult to be released during discharging. The formation of Li4SiO4 is the main cause of the reduction in the initial charge-discharge efficiency.

[0008] On the other hand, Patent Document 1 proposes a non-aqueous electrolyte secondary battery in which a composite material containing a lithium silicate phase represented by Li 2z SiO 2+z (0 < z < 2) and silicon particles dispersed in the lithium silicate phase is used as the negative electrode active material. The above composite material has a smaller irreversible capacity compared with SiO x , and thus, the initial charge-discharge efficiency is improved.

[0009] Prior Art Documents

[0010] Patent Documents

[0011] Patent Document 1: International Publication No. 2016 / 035290 Summary of the invention

[0012] Problem that the invention aims to solve

[0013] As electronic devices and the like become more advanced in performance, further improvement in charge and discharge efficiency (increase in capacity) is sought for nonaqueous electrolyte secondary batteries using the above-mentioned composite materials, which are expected to be power sources thereof.

[0014] Solutions for solving problems

[0015] In view of the above, one aspect of the present invention relates to a non-aqueous electrolyte secondary battery, which comprises a positive electrode, a negative electrode and an electrolyte, wherein the negative electrode comprises a negative electrode active material capable of electrochemically absorbing and releasing lithium, the negative electrode active material comprises a lithium silicate phase and silicon particles dispersed in the lithium silicate phase, the lithium silicate phase is an oxide phase comprising lithium, silicon and oxygen, the atomic ratio of the oxygen in the lithium silicate phase to the silicon: O / Si is greater than 2 and less than 4, and the electrolyte comprises halogenated benzene, and the content of the halogenated benzene in the electrolyte is greater than 1 ppm and less than 500 ppm.

[0016] Effects of the Invention

[0017] According to the present invention, the initial charge and discharge efficiency of a nonaqueous electrolyte secondary battery can be improved.

[0018] The novel features of the present invention are described in the appended claims, and both the configuration and content of the present invention, together with other objects and features of the present invention, will be more easily understood from the following detailed description with accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a partially cutaway perspective schematic diagram of a nonaqueous electrolyte secondary battery according to one embodiment of the present invention. DETAILED DESCRIPTION

[0020] The non-aqueous electrolyte secondary battery described in the embodiment of the present invention comprises a positive electrode, a negative electrode and an electrolyte, and the negative electrode comprises a negative electrode active material capable of electrochemically absorbing and releasing lithium. The negative electrode active material is a negative electrode material (hereinafter also referred to as "negative electrode material LSX" or simply "LSX") comprising a lithium silicate phase and silicon particles dispersed in the lithium silicate phase. The lithium silicate phase is an oxide phase comprising lithium (Li), silicon (Si) and oxygen (O). The atomic ratio of O to Si in the lithium silicate phase: O / Si is greater than 2 and less than 4. The electrolyte comprises halogenated benzene. The content of halogenated benzene in the electrolyte is greater than 1 ppm and less than 500 ppm by mass ratio.

[0021] When the O / Si is more than 2 and less than 4 (z in the formula described later is 0 < z < 2), it is advantageous in terms of stability and lithium ion conductivity. The atomic ratio of Li to Si in the lithium silicate phase: Li / Si is, for example, more than 0 and less than 4. In the lithium silicate phase, in addition to containing Li, Si, and O, it may also contain trace amounts of other elements such as iron (Fe), chromium (Cr), nickel (Ni), manganese (Mn), copper (Cu), molybdenum (Mo), zinc (Zn), and aluminum (Al).

[0022] The above-mentioned lithium silicate phase may have the formula: Li 2z SiO 2+z (0 < z < 2) as shown in the composition.

[0023] For example, when the composition of the lithium silicate phase of LSX is Li2Si2O5 (z = 1 / 2), during charging, the silicon particles undergo the reaction of formula (1), and a part of the lithium silicate phase undergoes the reaction of formula (2). Formula (2) is an irreversible reaction.

[0024] (1) Si + 4Li + + 4e - → Li4Si

[0025] (2) 0.8Li2Si2O5 + 4.8Li + + 4.8e - → 0.6Li4Si + Li4SiO4

[0026] Compared with SiOx, LSX consumes a smaller proportion of lithium when generating Li4SiO4 and has a smaller irreversible capacity. If the electrolyte of the non-aqueous electrolyte secondary battery using this LSX contains halogenated benzene, mainly during the first charging, a film derived from halogenated benzene is moderately formed on the surface of LSX. By moderately covering the surface of LSX with the above-mentioned film, the irreversible reaction (formation of Li4SiO4) of formula (2) is suppressed, and the reaction of formula (1) proceeds efficiently. That is, by adding halogenated benzene, the proportion of lithium consumed by the irreversible reaction is reduced. Therefore, the initial charge-discharge efficiency of the non-aqueous electrolyte secondary battery using LSX is improved. Since the above-mentioned film is a moderately sparse film, it can be considered that its reaction resistance is small and it has good lithium ion conductivity.

[0027] Among them, when the content of halogenated benzene in the electrolyte is less than 1 ppm, the effect brought by adding halogenated benzene becomes small. Therefore, it is difficult to suppress the irreversible capacity of the negative electrode, and the effect of improving the initial charge-discharge efficiency cannot be obtained.

[0028] In addition, when the content of halogenated benzene in the electrolyte exceeds 500 ppm, an excessive film is formed on the surface of LSX, and thus the reaction resistance of the film increases. As a result, not only the reaction of the above formula (2) but also the reaction of the above formula (1) is inhibited, and the initial charge and discharge efficiency and initial capacity are reduced.

[0029] From the viewpoint of improving the initial charge and discharge efficiency, the content of the halogenated benzene in the electrolyte solution is preferably 1 ppm or more and 400 ppm or less.

[0030] Halogenated benzene is a compound having at least one halogen atom bonded to a benzene ring. The type of the halogen atom bonded to the benzene ring is not particularly limited, but is preferably at least one of a fluorine atom and a chlorine atom from the viewpoint of facilitating the formation of a moderately sparse film.

[0031] When a plurality of halogen atoms are bonded to the benzene ring, the relative positional relationship of the plurality of halogen atoms is not particularly limited. Regardless of the relative positional relationship of the halogen atoms bonded to the benzene ring, as long as the halogen atoms are bonded to the benzene ring, the film is formed into a sparse film with appropriateness, and the effect of improving the charge and discharge efficiency can be obtained. In addition, the types of the plurality of halogen atoms bonded to the benzene ring may be the same or different.

[0032] Specific examples of halogenated benzenes include, for example, at least one selected from the group consisting of chlorobenzene, dichlorobenzene, fluorobenzene, difluorobenzene, and hexafluorobenzene. Among them, chlorobenzene is preferred. Dichlorobenzene may be any one of 1,2-dichlorobenzene, 1,3-dichlorobenzene, and 1,4-dichlorobenzene, and difluorobenzene may be any one of 1,2-difluorobenzene, 1,3-difluorobenzene, and 1,4-difluorobenzene.

[0033] The content of halogenated benzene in the electrolyte solution can be determined by using gas chromatography-mass spectrometry (GCMS) for the electrolyte solution contained in the battery.

[0034] The electrolyte solution contains a non-aqueous solvent, a lithium salt dissolved in the non-aqueous solvent, and a specific amount of halogenated benzene as an additive.

[0035] From the perspective of wide potential window and high conductivity, the lithium salt preferably includes at least one of LiN(SO2F)2 (hereinafter referred to as LFSI) and LiPF6. LiPF6 will form a passive film on the positive electrode collector, etc., so the corrosion of the positive electrode collector, etc. is suppressed and the battery reliability is improved. LFSI easily forms a high-quality film (SEI: Solid Electrolyte Interface) on the surface of LSX.

[0036] The concentration of LFSI in the electrolyte is preferably 0.1 mol / L or more and 1.0 mol / L or less. The concentration of LiPF6 in the electrolyte is preferably 0.5 mol / L or more and 1.5 mol / L or less. The total concentration of LFSI and LiPF6 in the electrolyte is preferably 1 mol / L or more and 2 mol / L or less. When LFSI and LiPF6 with concentrations in the above ranges are used in combination, the effects brought by the above LFSI and LiPF6 can be obtained with a good balance, and the initial charge-discharge efficiency of the battery is further improved.

[0037] [Negative electrode material LSX]

[0038] The above lithium silicate phase may have a composition represented by Li 2z SiO 2+z (0 < z < 2). The smaller z is, the more sites for occluding lithium in the lithium silicate phase will increase. Therefore, the effect of suppressing lithium occlusion in the lithium silicate phase by halogenated benzene is significantly obtained. From the viewpoints of stability, ease of production, lithium ion conductivity, etc., z preferably satisfies the relationship of 0 < z < 1, and more preferably z = 1 / 2.

[0039] Compared with the SiO2 matrix in SiO x , the lithium silicate phase has fewer sites capable of reacting with lithium. Therefore, compared with SiO x , LSX is less likely to have an irreversible capacity associated with charge and discharge. When silicon particles are dispersed in the lithium silicate phase, excellent charge-discharge efficiency can be obtained at the initial stage of charge and discharge. In addition, the content of silicon particles can be arbitrarily changed, so a high-capacity negative electrode can be designed.

[0040] The crystallite size of the silicon particles dispersed in the lithium silicate phase is, for example, 10 nm or more. The silicon particles have a particulate phase of silicon (Si)单质. When the crystallite size of the silicon particles is 10 nm or more, the surface area of the silicon particles can be suppressed to be small, so that the deterioration of the silicon particles accompanied by the generation of irreversible capacity is not likely to occur. The crystallite size of the silicon particles is calculated from the half-value width of the diffraction peak attributed to the Si(111) plane in the X-ray diffraction (XRD) pattern of the silicon particles by the Scherrer formula.

[0041] The negative electrode material LSX also has excellent structural stability. This is because: the silicon particles are dispersed in the lithium silicate phase, and therefore, the expansion and contraction of the negative electrode material LSX associated with charging and discharging is suppressed. From the viewpoint of suppressing cracking of the silicon particles themselves, the average particle size of the silicon particles is preferably 500nm or less, more preferably 200nm or less, and further preferably 50nm or less before the initial charge. After the initial charge, the average particle size of the silicon particles is preferably 400nm or less, and more preferably 100nm or less. By miniaturizing the silicon particles, the volume change during charging and discharging becomes smaller, and the structural stability of the negative electrode material LSX is further improved.

[0042] The average particle size of the silicon particles is measured by observing a cross-sectional SEM (scanning electron microscope) photograph of the negative electrode material LSX. Specifically, the average particle size of the silicon particles is obtained by averaging the maximum diameters of any 100 silicon particles. The silicon particles are formed by the aggregation of a plurality of microcrystals.

[0043] From the viewpoint of high capacity, the content of silicon particles in the negative electrode material LSX can be, for example, 30% by mass or more, preferably 35% by mass or more, and more preferably 55% by mass or more. At this time, the diffusibility of lithium ions is good, and excellent load characteristics are easily obtained. On the other hand, from the viewpoint of improving cycle characteristics, the content of silicon particles in the negative electrode material LSX is preferably 95% by mass or less, and more preferably 75% by mass or less. This is because: the surface of the silicon particles that are not covered by the lithium silicate phase and exposed is reduced, and the reaction between the electrolyte and the silicon particles is easily suppressed.

[0044] The content of silicon particles can be measured by Si-NMR. Preferred measurement conditions of Si-NMR are shown below.

[0045] Measuring device: Varian, solid-state nuclear magnetic resonance spectrometer (INOVA-400)

[0046] Probe: Varian 7mm CPMAS-2

[0047] MAS: 4.2kHz

[0048] MAS speed: 4kHz

[0049] Pulse: DD (45° pulse + signal reading time 1H decoupling)

[0050] Repeat time: 1200 seconds

[0051] Observation amplitude: 100kHz

[0052] Observation center: around -100ppm

[0053] Signal reading time: 0.05 seconds

[0054] Cumulative number of times: 560

[0055] Sample volume: 207.6 mg

[0056] Lithium silicate phase Li 2z SiO 2+z The composition of can be analyzed by, for example, the following method.

[0057] First, the mass of the negative electrode material LSX sample is measured. Then, the contents of carbon, lithium, and oxygen contained in the sample are calculated as follows. Next, the carbon content is subtracted from the mass of the sample to calculate the contents of lithium and oxygen occupying the remainder, and the ratio of 2z to (2+z) is obtained from the molar ratio of lithium (Li) to oxygen (O).

[0058] The carbon content is measured using a carbon / sulfur analyzer (e.g., EMIA-520 manufactured by Horiba, Ltd.). The sample is weighed on a magnetic plate, a combustion aid is added, and the sample is inserted into a combustion furnace (carrier gas: oxygen) heated to 1350°C, and the amount of carbon dioxide gas generated during combustion is detected by infrared absorption. The standard curve is prepared using, for example, carbon steel (carbon content 0.49%) manufactured by Bureau of Analyzed Sampe. Ltd., and the carbon content of the sample is calculated (high-frequency induction heating furnace combustion-infrared absorption method).

[0059] The oxygen content is measured using an oxygen / nitrogen / hydrogen analyzer (e.g., EGMA-830 manufactured by Horiba, Ltd.). The sample is placed in a Ni capsule, and the sample is placed in a carbon crucible heated with 5.75 kW of electricity together with Sn pellets and Ni pellets that become flux, and the released carbon monoxide gas is detected. The standard curve is prepared using the standard sample Y2O3, and the oxygen content of the sample is calculated (inactive gas melting-non-dispersive infrared absorption method).

[0060] The lithium content is determined as follows: the sample is completely dissolved in hot hydrofluoric acid-nitric acid (a mixture of heated hydrofluoric acid and nitric acid), the carbon in the dissolved residue is filtered out, and the resulting filtrate is analyzed and determined by inductively coupled plasma emission spectrometry (ICP-AES). A standard curve is prepared using a commercially available lithium standard solution to calculate the lithium content of the sample.

[0061] The amount obtained by subtracting the carbon content, oxygen content, and lithium content from the sample mass of the negative electrode material LSX is the silicon content. The silicon content includes contributions from both silicon in the form of silicon particles and silicon in the form of lithium silicate. The content of silicon particles is determined by Si-NMR measurement, and the content of silicon in the form of lithium silicate in the negative electrode material LSX is determined.

[0062] The negative electrode material LSX is preferably formed into a granular material (hereinafter referred to as LSX particles) with an average particle size of 1 to 25 μm, and further 4 to 15 μm. Within the above particle size range, it is easy to relax the stress caused by the volume change of the negative electrode material LSX accompanying charge and discharge, and it is easy to obtain good cycle characteristics. The surface area of ​​the LSX particles also becomes moderate, and the capacity reduction caused by the side reaction with the non-aqueous electrolyte is also suppressed.

[0063] The average particle size of LSX particles refers to the particle size (volume average particle size) at which the volume cumulative value reaches 50% in the particle size distribution measured by the laser diffraction scattering method. For example, the measuring device that can be used is "LA-750" manufactured by HORIBA.

[0064] The LSX particles preferably have a conductive material covering at least a portion of their surface. The lithium silicate phase lacks electronic conductivity, so the conductivity of the LSX particles is also likely to be low. By covering the surface with a conductive material, the conductivity can be greatly improved. The conductive layer is preferably substantially thin to the extent that it does not affect the average particle size of the LSX particles.

[0065] Next, the nonaqueous electrolyte secondary battery according to the embodiment of the present invention will be described in detail. The nonaqueous electrolyte secondary battery includes, for example, the following negative electrode, positive electrode, and nonaqueous electrolyte.

[0066] [negative electrode]

[0067] The negative electrode includes, for example, a negative electrode current collector and a negative electrode mixture layer formed on the surface of the negative electrode current collector and containing a negative electrode active material. The negative electrode mixture layer can be formed by applying a negative electrode slurry obtained by dispersing a negative electrode mixture in a dispersion medium to the surface of the negative electrode current collector and drying it. The dried coating film can be rolled as needed. The negative electrode mixture layer can be formed on one surface of the negative electrode current collector or on both surfaces.

[0068] The negative electrode mixture may contain negative electrode material LSX (or LSX particles) as an essential component as a negative electrode active material, and may contain a binder, a conductive agent, a thickener, etc. as optional components. The silicon particles in the negative electrode material LSX can absorb a plurality of lithium ions, thus contributing to the high capacity of the negative electrode.

[0069] The negative electrode active material preferably also includes a carbon material that electrochemically absorbs and releases lithium ions. The volume of the negative electrode material LSX expands and contracts with charging and discharging. Therefore, when the ratio of the negative electrode material LSX in the negative electrode active material increases, poor contact between the negative electrode active material and the negative electrode collector may occur with charging and discharging. On the other hand, by combining the negative electrode material LSX and the carbon material, it is possible to give the negative electrode both a high capacity of silicon particles and excellent cycle characteristics. The proportion of the negative electrode material LSX in the sum of the negative electrode material LSX and the carbon material is preferably, for example, 3 to 30% by mass. This makes it easy to take into account both high capacity and improved cycle characteristics.

[0070] As carbon materials, for example, graphite, easily graphitized carbon (soft carbon), and difficultly graphitized carbon (hard carbon) can be exemplified. Among them, graphite having excellent charge and discharge stability and small irreversible capacity is preferred. Graphite refers to a material having a graphite-type crystal structure, including, for example, natural graphite, artificial graphite, and graphitized mesophase carbon particles. One carbon material can be used alone, or two or more can be used in combination.

[0071] As the negative electrode current collector, a non-porous conductive substrate (metal foil, etc.), a porous conductive substrate (mesh, grid, punched metal sheet, etc.) can be used. As the material of the negative electrode current collector, stainless steel, nickel, nickel alloy, copper, copper alloy, etc. can be exemplified. The thickness of the negative electrode current collector is not particularly limited, and from the viewpoint of the balance between the negative electrode strength and lightness, it is preferably 1 to 50 μm, and more preferably 5 to 20 μm.

[0072] As the binder, resin materials such as fluororesins such as polytetrafluoroethylene and polyvinylidene fluoride (PVDF); polyolefin resins such as polyethylene and polypropylene; polyamide resins such as aramid resins; polyimide resins such as polyimide and polyamideimide; acrylic resins such as polyacrylic acid, polymethyl acrylate, and ethylene-acrylic acid copolymers; vinyl resins such as polyacrylonitrile and polyvinyl acetate; polyvinyl pyrrolidone; polyether sulfone; rubber-like materials such as styrene-butadiene copolymer rubber (SBR), etc. These can be used alone or in combination of two or more.

[0073] Examples of the conductive agent include carbons such as acetylene black and carbon nanotubes; conductive fibers such as carbon fibers and metal fibers; carbon fluoride; metal powders such as aluminum; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; organic conductive materials such as phenylene derivatives, etc. These may be used alone or in combination of two or more.

[0074] Examples of thickeners include carboxymethyl cellulose (CMC) and modified products thereof (including salts such as Na salts), cellulose derivatives such as methyl cellulose (cellulose ethers, etc.), saponified products of polymers having vinyl acetate units such as polyvinyl alcohol, polyethers (polyalkylene oxides such as polyethylene oxide), etc. These may be used alone or in combination of two or more.

[0075] The dispersion medium is not particularly limited, and examples thereof include water, alcohols such as ethanol; ethers such as tetrahydrofuran; amides such as dimethylformamide; N-methyl-2-pyrrolidone (NMP), and mixed solvents thereof.

[0076] [positive electrode]

[0077] The positive electrode includes, for example, a positive electrode current collector and a positive electrode mixture layer formed on the surface of the positive electrode current collector. The positive electrode mixture layer can be formed by applying a positive electrode slurry obtained by dispersing a positive electrode mixture in a dispersion medium to the surface of the positive electrode current collector and drying it. The dried coating film can be rolled as needed. The positive electrode mixture layer can be formed on one surface of the positive electrode current collector or on both surfaces.

[0078] As the positive electrode active material, a lithium composite metal oxide can be used. Examples thereof include Li a CoO2、Li a NiO2、Li a MnO2、Li a Co b Ni 1-b O2、Li a Co b M 1-b O c , Li a Ni 1-b M b O c , Li a Mn2O4、Li a Mn 2-b M b O4, LiMPO4, Li2MPO4F (M is at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, B). Here, a = 0 to 1.2, b = 0 to 0.9, c = 2.0 to 2.3. It should be noted that the value a representing the lithium molar ratio is equivalent to the value immediately after the active material is produced, and increases or decreases due to charge and discharge.

[0079] Among them, Li is preferred a Ni b M 1-bA lithium nickel composite oxide represented by O2 (where M is at least one selected from the group consisting of Mn, Co, and Al, 0 < a ≤ 1.2, 0.3 ≤ b ≤ 1). From the viewpoint of high capacity, it is more preferably satisfied that 0.85 ≤ b ≤ 1. From the viewpoint of crystal structure stability, it is further preferably Li containing Co and Al as M a Ni b Co c Al d O2 (0 < a ≤ 1.2, 0.85 ≤ b < 1, 0 < c < 0.15, 0 < d ≤ 0.1, b + c + d = 1).

[0080] As the binder and the conductive agent, the same substances as those exemplified for the negative electrode can be used. As the conductive agent, graphite such as natural graphite and artificial graphite can be used.

[0081] The shape and thickness of the positive electrode current collector can be selected respectively from those conforming to the shape and range of the negative electrode current collector. As the material of the positive electrode current collector, for example, stainless steel, aluminum, aluminum alloy, titanium, etc. can be exemplified.

[0082] [Electrolyte solution]

[0083] The electrolyte solution contains a non-aqueous solvent, a lithium salt dissolved in the non-aqueous solvent, and a specific amount of halogenated benzene as an additive.

[0084] The lithium salt concentration in the electrolyte solution is preferably, for example, 0.5 mol / L or more and 2 mol / L or less. By controlling the lithium salt concentration within the above range, an electrolyte solution with excellent ion conductivity and moderate viscosity can be obtained. However, the lithium salt concentration is not limited to the above.

[0085] As the non-aqueous solvent, for example, cyclic carbonates (excluding the unsaturated cyclic carbonates described later), chain carbonates, cyclic carboxylic acid esters, chain carboxylic acid esters, etc. can be used. As the cyclic carbonate, propylene carbonate (PC), ethylene carbonate (EC), etc. can be cited. As the chain carbonate, diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), etc. can be cited. As the cyclic carboxylic acid ester, γ-butyrolactone (GBL), γ-valerolactone (GVL), etc. can be cited. As the chain carboxylic acid ester, methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, etc. can be cited. The non-aqueous solvent can be used alone or in combination of two or more.

[0086] As the lithium salt, known lithium salts can be used. As the preferred lithium salt, for example, LiClO4, LiBF4, LiPF6, LiAlCl4, LiSbF6, LiSCN, LiCF3SO3, LiCF3CO2, LiAsF6, LiB 10 Cl10 , lower aliphatic carboxylic acid lithium, LiCl, LiBr, LiI, borates, imide salts, etc. Examples of borates include bis(1,2-benzenediolate (2-)-O,O') lithium borate, bis(2,3-naphthalenediolate (2-)-O,O') lithium borate, bis(2,2'-biphenylediolate (2-)-O,O') lithium borate, and bis(5-fluoro-2-oleate-1-benzenesulfonic acid-O,O') lithium borate. Examples of imide salts include LFSI, bistrifluoromethanesulfonyl imide lithium (LiN(CF3SO2)2), trifluoromethanesulfonyl nonafluorobutanesulfonyl imide lithium (LiN(CF3SO2)(C4F9SO2)), and bispentafluoroethanesulfonyl imide lithium (LiN(C2F5SO2)2). Among these, at least one of LiPF6 and LFSI is preferred. The lithium salt may be used alone or in combination of two or more.

[0087] The electrolyte may further include other additives except halogenated benzene. As other additives, a cyclic carbonate (hereinafter referred to as unsaturated cyclic carbonate) having at least one carbon-carbon unsaturated bond in the molecule may be included. By decomposing the unsaturated cyclic carbonate on the negative electrode and forming a high coating with lithium ion conductivity on the negative electrode surface, the charge and discharge efficiency is further improved.

[0088] As unsaturated cyclic carbonate, known compounds can be used. As preferred unsaturated cyclic carbonate, for example, vinylene carbonate, 4-methyl vinylene carbonate, 4,5-dimethyl vinylene carbonate, 4-ethyl vinylene carbonate, 4,5-diethyl vinylene carbonate, 4-propyl vinylene carbonate, 4,5-dipropyl vinylene carbonate, 4-phenyl vinylene carbonate, 4,5-diphenyl vinylene carbonate, vinyl ethylene carbonate, divinyl ethylene carbonate etc. can be listed. Among these, preferably at least one selected from the group consisting of vinylene carbonate, vinyl ethylene carbonate and divinyl ethylene carbonate. Unsaturated cyclic carbonate can be used alone or in combination with more than two kinds. A part of hydrogen atoms in the unsaturated cyclic carbonate is optionally substituted by fluorine atoms.

[0089] [Separator]

[0090] Usually, it is preferred to sandwich a separator between the positive electrode and the negative electrode. The separator has high ion permeability and has appropriate mechanical strength and insulation. As the separator, a microporous film, a woven fabric, a non-woven fabric, etc. can be used. As the material of the separator, polyolefins such as polypropylene and polyethylene are preferred.

[0091] As an example of the structure of a non-aqueous electrolyte secondary battery, an electrode group formed by winding a positive electrode and a negative electrode across a separator and a structure obtained by containing a non-aqueous electrolyte in an outer package can be listed. Alternatively, an electrode group of other forms such as a stacked electrode group formed by stacking a positive electrode and a negative electrode across a separator can also be used to replace the wound electrode group. The non-aqueous electrolyte secondary battery can be any form such as a cylindrical type, a square type, a coin type, a button type, a laminated type, etc.

[0092] Figure 1 It is a partially cutaway perspective schematic diagram of a prismatic nonaqueous electrolyte secondary battery according to one embodiment of the present invention.

[0093] The battery comprises a square-bottomed battery case 4, an electrode group 1 and a non-aqueous electrolyte (not shown) contained in the battery case 4. The electrode group 1 comprises a long strip-shaped negative electrode, a long strip-shaped positive electrode, and a separator sandwiched therebetween to prevent direct contact. The electrode group 1 is formed by winding the negative electrode, the positive electrode and the separator around a flat winding core as the center and pulling out the winding core.

[0094] One end of the negative electrode lead 3 is mounted on the negative electrode collector of the negative electrode by welding or the like. The other end of the negative electrode lead 3 is electrically connected to the negative terminal 6 provided on the sealing plate 5 by means of a resin insulating plate (not shown). The negative terminal 6 is insulated relative to the sealing plate 5 by means of a resin gasket 7. One end of the positive electrode lead 2 is mounted on the positive electrode collector of the positive electrode by welding or the like. The other end of the positive electrode lead 2 is connected to the back of the sealing plate 5 by means of an insulating plate. That is, the positive electrode lead 2 is electrically connected to the battery case 4 which also serves as the positive terminal. The insulating plate separates the electrode group 1 from the sealing plate 5 and separates the negative electrode lead 3 from the battery case 4. The outer edge of the sealing plate 5 is fitted into the open end of the battery case 4, and the fitting portion is laser welded. In this way, the opening of the battery case 4 is sealed by the sealing plate 5. The injection hole for the non-aqueous electrolyte provided in the sealing plate 5 is blocked by the sealing plug 8.

[0095] Hereinafter, the present invention will be specifically described based on Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0096] <Example 1>

[0097] [Preparation of negative electrode material LSX]

[0098] Silicon dioxide and lithium carbonate were mixed in an atomic ratio of Si / Li of 1.05, and the mixture was calcined in air at 950°C for 10 hours to obtain lithium silicate represented by the formula: Li2Si2O5 (z=0.5). The obtained lithium silicate was pulverized in an average particle size of 10 μm.

[0099] Lithium silicate (Li2Si2O5) with an average particle size of 10 μm and raw silicon (3N, average particle size of 10 μm) were mixed at a mass ratio of 45:55. The mixture was filled into a pot (SUS, volume: 500 mL) of a planetary ball mill (FRITSCH, P-5), 24 SUS balls (diameter 20 mm) were put into the pot and sealed, and the mixture was pulverized at 200 rpm in an inert atmosphere for 50 hours.

[0100] Next, the powdered mixture was taken out in an inert atmosphere, and calcined at 800° C. for 4 hours in the inert atmosphere under pressure with a hot press, thereby obtaining a sintered body of the mixture (negative electrode material LSX).

[0101] Thereafter, the negative electrode material LSX was crushed and passed through a 40 μm sieve, and the obtained LSX particles were mixed with coal tar (MCP250 manufactured by JFE Chemical Co., Ltd.), and the mixture was calcined at 800° C. in an inert atmosphere, and the surface of the LSX particles was covered with conductive carbon to form a conductive layer. The covering amount of the conductive layer was set to 5% by mass relative to the total mass of the LSX particles and the conductive layer. Thereafter, a sieve was used to obtain LSX particles having an average particle size of 5 μm having a conductive layer.

[0102] The crystallite size of the silicon particles calculated from the diffraction peak attributed to the Si (111) plane using the Scherrer equation through XRD analysis of the LSX particles was 15 nm.

[0103] The composition of the lithium silicate phase was analyzed using the above-mentioned methods (high-frequency induction heating furnace combustion-infrared absorption method, inert gas melting-non-dispersive infrared absorption method, inductively coupled plasma emission spectrometry (ICP-AES)). The Si / Li ratio was 1.0, and the Li2Si2O5 content measured by Si-NMR was 45 mass% (the content of silicon particles was 55 mass%).

[0104] [Production of negative electrode]

[0105] The LSX particles with a conductive layer were mixed with graphite and used as negative electrode active materials. The ratio of graphite to the sum of the LSX particles with a conductive layer and graphite was 94% by mass. The negative electrode active material, sodium carboxymethyl cellulose (CMC-Na) and styrene-butadiene rubber (SBR) were mixed at a mass ratio of 97.5:1:1.5, and after adding water, a mixer (manufactured by PRIMIX, TKHIVIS MIX) was used for stirring to prepare a negative electrode slurry.

[0106] Next, the negative electrode slurry was mixed with an average of 1 m 2The negative electrode mixture was coated on the surface of the copper foil in such a manner that the mass of the negative electrode mixture reached 190 g, and after the coating was dried, it was rolled to form a layer with a density of 1.5 g / cm on both sides of the copper foil. 3 The negative electrode of the negative electrode mixture layer.

[0107] [Production of positive electrode]

[0108] Lithium nickel composite oxide (LiNi 0.8 Co 0.18 Al 0.02 O2), acetylene black and polyvinylidene fluoride were mixed in a mass ratio of 95:2.5:2.5, N-methyl-2-pyrrolidone (NMP) was added, and a mixer (manufactured by PRIMIX, TKHIVIS MIX) was used to stir to prepare a positive electrode slurry. Next, the positive electrode slurry was applied to the surface of the aluminum foil, and after the coating was dried, it was rolled to form a 3.6 g / cm2 film on both sides of the aluminum foil. 3 The positive electrode of the positive electrode mixture layer.

[0109] [Preparation of electrolyte]

[0110] The electrolyte is prepared by dissolving a lithium salt in a non-aqueous solvent. The non-aqueous solvent is a mixed solvent containing ethylene carbonate (EC), dimethyl carbonate (DMC) and methyl acetate (MA) in a volume ratio of 20:40:40. The electrolyte contains 500 ppm (dosage amount) of fluorobenzene as a halogenated benzene. LiPF6 is used as the lithium salt. The concentration of LiPF6 in the electrolyte is 1.2 mol / L.

[0111] [Fabrication of non-aqueous electrolyte secondary battery]

[0112] The electrode group was prepared by installing a tab on each electrode, and winding the positive electrode and the negative electrode in a spiral shape with the tab located at the outermost periphery through a separator. The electrode group was inserted into an outer package made of an aluminum laminate film, vacuum dried at 105° C. for 2 hours, and then injected with an electrolyte solution, and the opening of the outer package was sealed to obtain a battery A1.

[0113] <Examples 2 to 4>

[0114] In the preparation of the electrolyte, the compounds shown in Table 1 were used as halogenated benzenes, and the content (feed amount) of halogenated benzenes in the electrolyte was set to the values ​​shown in Table 1. LiPF6 or LiPF6 and LFSI were used as lithium salts. The concentrations of LiPF6 in the electrolyte and LFSI in the electrolyte were set to the values ​​shown in Table 1, respectively. Except for the above, the same operation as in Example 1 was performed to produce batteries A2 to A4.

[0115] <Comparative Example 1>

[0116] Battery B1 was produced in the same manner as in Example 1 except that the electrolyte did not contain halogenated benzene in the preparation of the electrolyte.

[0117] <Comparative Examples 2 to 4>

[0118] In the preparation of the electrolyte, the compounds shown in Table 1 were used as halogenated benzenes, and the content (feed amount) of halogenated benzenes in the electrolyte was set to the values ​​shown in Table 1. LiPF6 and LFSI were used as lithium salts. The concentrations of LiPF6 in the electrolyte and LFSI in the electrolyte were set to the values ​​shown in Table 1, respectively. Except for the above, the same operation as in Example 1 was performed to produce batteries B2 to B4.

[0119] <Comparative Example 5>

[0120] In the preparation of the negative electrode, only graphite was used as the negative electrode active material. In the preparation of the electrolyte, the electrolyte did not contain halogenated benzene. Except for the above, the same operation as in Example 1 was performed to prepare Battery B5.

[0121] <Comparative Example 6>

[0122] In the preparation of the negative electrode, only graphite was used as the negative electrode active material. In the preparation of the electrolyte, the compounds shown in Table 1 were used as halogenated benzenes, and the content (dosage) of halogenated benzenes in the electrolyte was set to the values ​​shown in Table 1. LiPF6 and LFSI were used as lithium salts. The concentrations of LiPF6 in the electrolyte and LFSI in the electrolyte were set to the values ​​shown in Table 1, respectively. Except for the above, the battery B6 was prepared in the same manner as in Example 1.

[0123] Each of the batteries produced above was evaluated by the following methods.

[0124] [Evaluation 1: Initial charge and discharge efficiency and initial capacity]

[0125] For each battery after production, a constant current charge is performed at a current of 0.3It at 25°C until the voltage reaches 4.2V, and then a constant voltage charge is performed at a constant voltage of 4.2V until the current reaches 0.015It. Thereafter, a constant current discharge is performed at a current of 0.3It until the voltage reaches 2.75V. It should be noted that (1 / X)It represents the current, (1 / X)It(A) = rated capacity (Ah) / X(h), and X represents the time used to charge or discharge the rated capacity of electricity. For example, 0.5It means X = 2, and the current value is the rated capacity (Ah) / 2(h).

[0126] The rest period between charging and discharging was set to 10 minutes. Charging and discharging were performed in an environment of 25°C.

[0127] The ratio (percentage) of the discharge capacity to the charge capacity at this time was determined as the initial charge and discharge efficiency. In addition, the discharge capacity at this time was determined as the initial capacity.

[0128] Table 1 shows the evaluation results.

[0129] [Evaluation 2: Analysis of electrolyte in battery]

[0130] The charge and discharge were repeated 5 times under the charge and discharge conditions of the above Evaluation 1. Thereafter, the battery was taken out and disassembled, and the components of the electrolyte were analyzed by gas chromatography-mass spectrometry (GCMS).

[0131] The measurement conditions of GCMS used for the analysis of the electrolyte solution are as follows.

[0132] Equipment: Shimadzu Corporation, GC17A, GCMS-QP5050A

[0133] Column: HP-1 (film thickness 1.0 μm×length 60 m) manufactured by Agilent Technologies

[0134] Column temperature: 50°C → 110°C (5°C / min, hold for 12 minutes) → 250°C (5°C / min, hold for 7 minutes) → 300°C (10°C / min, hold for 20 minutes)

[0135] Split ratio: 1 / 50

[0136] Line speed: 29.2cm / s

[0137] Inlet temperature: 270℃

[0138] Injection volume: 0.5 μL

[0139] Interface temperature: 230℃

[0140] Mass spectrum range: m / z = 30 ~ 400 (SCAN mode), m / z = 29, 31, 32, 43, 45, 60 (SIM mode)

[0141] Table 1 shows the content of halogenated benzene obtained by analysis (mass ratio relative to the entire electrolytic solution).

[0142] [Evaluation 3: Cycle capacity maintenance rate]

[0143] The battery was charged at a constant current of 0.3 It until the voltage reached 4.2 V, and then charged at a constant voltage of 4.2 V until the current reached 0.015 It. Thereafter, the battery was discharged at a constant current of 0.3 It until the voltage reached 2.75 V. The rest period between charging and discharging was 10 minutes. Charging and discharging were performed at 25°C.

[0144] The charge and discharge were repeated under the above-mentioned charge and discharge conditions, and the ratio (percentage) of the discharge capacity at the 500th cycle to the discharge capacity at the 1st cycle was calculated as the cycle capacity retention rate.

[0145] Table 1 shows the evaluation results.

[0146] [Table 1]

[0147]

[0148] In Examples 1 to 4 (batteries A1 to A4) and Comparative Examples 2 to 4 (batteries B2 to B4), the analyzed values ​​of the halogenated benzene content were less than the charged amount. This is considered to be because the halogenated benzene was used to form a film on the surface of LSX.

[0149] In batteries A1 to A4 in which the halogenated benzene content (analyzed value) was 1 ppm or more and 500 ppm or less, the initial charge and discharge efficiency, the initial capacity, and the cycle capacity retention rate were improved.

[0150] Compared with battery A1, the content of halogenated benzene in the electrolyte of batteries A3 and A4 is less, and LiPF6 and LFSI are used simultaneously as lithium salts of the electrolyte, so the initial charge and discharge efficiency and initial capacity are further improved. The concentration of LFSI in the electrolyte of batteries A3 and A4 is 0.1 mol / L or more and 1.0 mol / L or less, and the concentration of LiPF6 in the electrolyte is 0.5 mol / L or more and 1.5 mol / L or less.

[0151] In the battery B1 in which the electrolyte solution did not contain halogenated benzene, the initial charge and discharge efficiency, the initial capacity, and the cycle capacity retention rate decreased.

[0152] It is considered that in batteries B2 and B3 where the halogenated benzene content (analyzed value) in the electrolyte solution exceeded 500 ppm, a film derived from halogenated benzene was excessively formed on the surface of LSX, and the initial charge and discharge efficiency, initial capacity, and cycle capacity retention rate decreased.

[0153] In the battery B4 in which the content (analyzed value) of halogenated benzene in the electrolyte solution was less than 1 ppm, the effect of adding halogenated benzene was small, and therefore the initial charge and discharge efficiency, initial capacity, and cycle capacity retention rate were not improved.

[0154] In batteries B5 and B6, only graphite was used as the negative electrode active material without using LSX, so the initial capacity was reduced. On the other hand, no effect was observed by adding halogenated benzene.

[0155] Industrial Applicability

[0156] The nonaqueous electrolyte secondary battery of the present invention is useful as a main power source for mobile communication devices, portable electronic devices, and the like.

[0157] The preferred embodiments of the present invention are described, but are not subject to the restrictive interpretation of this disclosure. By reading the above disclosure, a person skilled in the art of the present invention can clearly understand various modifications and changes without doubt. Therefore, it should be interpreted that the attached claims include all modifications and changes that do not exceed the true spirit and scope of the present invention.

[0158] Description of Reference Numerals

[0159] 1: Electrode group, 2: Positive lead, 3: Negative lead, 4: Battery case, 5: Sealing plate, 6: Negative terminal, 7: Gasket, 8: Sealing plug

Claims

1. A non-aqueous electrolyte secondary battery comprising a positive electrode, a negative electrode, and an electrolyte solution, wherein the negative electrode contains a negative electrode active material capable of electrochemically occluding and releasing lithium, the negative electrode active material contains a lithium silicate phase and silicon particles dispersed in the lithium silicate phase, the lithium silicate phase is an oxide phase containing lithium, silicon, and oxygen, the atomic ratio of oxygen to silicon in the lithium silicate phase: O / Si is more than 2 and less than 4, the electrolyte solution contains a halogenated benzene, the content of the halogenated benzene in the electrolyte solution is 1 ppm or more and 500 ppm or less, the halogenated benzene contains at least one selected from the group consisting of chlorobenzene, dichlorobenzene, fluorobenzene, difluorobenzene, and hexafluorobenzene.

2. The nonaqueous electrolyte secondary battery according to claim 1, wherein The composition of the lithium silicate phase is expressed as: Li 2z SiO 2+z express, z in the formula satisfies the relationship 0 < z < 2.

3. The nonaqueous electrolyte secondary battery according to claim 2, wherein: z in the formula satisfies the relationship 0 < z < 1.

4. The nonaqueous electrolyte secondary battery according to any one of claims 1 to 3, wherein the electrolyte solution contains a non-aqueous solvent and a lithium salt dissolved in the non-aqueous solvent, the lithium salt contains at least one of LiN(SO2F)2 and LiPF6.

5. The nonaqueous electrolyte secondary battery according to claim 4, wherein the concentration of LiN(SO2F)2 in the electrolyte solution is 0.1 mol / L or more and 1.0 mol / L or less.