Lithium secondary battery

By using a hydrophilic surface-modified porous polyolefin film protective layer and a high-concentration lithium salt electrolyte in lithium metal secondary batteries, the problems of life characteristics degradation and electrolyte side reactions caused by the growth of lithium dendrites are solved, significantly Improved battery stability and performance.

CN112368860BActive Publication Date: 2024-10-18LG ENERGY SOLUTION LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202080003632.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-05-11
Publication Date
2024-10-18
Estimated Expiration
2040-05-11

AI Technical Summary

Technical Problem

The uneven growth of lithium dendrites in lithium metal secondary batteries leads to the degradation of life characteristics and cell short circuit, and the side reactions of the electrolyte are difficult to control.

Method used

Using a hydrophilic surface-modified porous polyolefin membrane protective layer, combined with a high-concentration lithium salt electrolyte, plasma treatment improves the hydrophilicity and air permeability of the membrane, inhibits the uneven growth of lithium dendrites, and reduces electrolysis Liquid side reactions.

Benefits of technology

It significantly improves the stability and life characteristics of lithium secondary batteries, prevents battery short circuits caused by uneven growth of lithium dendrites, minimizes side reactions of the electrolyte, and improves the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112368860B_ABST
    Figure CN112368860B_ABST
Patent Text Reader

Abstract

The present invention relates to a lithium secondary battery which exhibits excellent lifespan characteristics and stability, wherein side reactions of an electrolyte are minimized and uneven growth of lithium dendrites is effectively suppressed.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of Korean Patent Application No. 10-2019-0056447 filed in the Korean Intellectual Property Office on May 14, 2019, and Korean Patent Application No. 10-2020-0055448 filed in the Korean Intellectual Property Office on May 8, 2020, the disclosures of which are incorporated herein by reference in their entirety.

[0003] The present invention relates to a lithium secondary battery having improved lifespan characteristics. [Background Technology]

[0004] With the rapid development of the electrical, electronic, communication and computer industries, the demand for high-capacity batteries is increasing. In order to meet this demand, lithium metal secondary batteries using lithium metal or lithium alloy as the negative electrode with high energy density have attracted much attention.

[0005] Lithium metal secondary batteries are secondary batteries that use lithium metal or lithium alloy as the negative electrode. Lithium metal has a mass of 0.54 g / cm 3 Due to its low density and extremely low standard reduction potential of -3.045 V (based on SHE: standard hydrogen electrode), it has attracted the most attention as an electrode material for high energy density batteries.

[0006] In the case of such a lithium metal secondary battery, unlike the existing lithium ion secondary battery, lithium metal is plated on the negative electrode and charged, stripped and discharged, wherein lithium dendrites may grow in the negative electrode. If lithium dendrites grow unevenly on the surface of the negative electrode, the separator placed between the positive electrode and the negative electrode may be damaged, and an internal short circuit may be caused, which may lead to fire. Therefore, a technology for preventing the growth of lithium dendrites should be ensured. [Summary of the invention]

[0007] Technical issues

[0008] An object of the present invention is to provide a lithium secondary battery capable of preventing degradation of life characteristics and cell short circuit caused by growth of lithium dendrites, wherein side reactions of an electrolyte are minimized.

[0009] Technical Solution

[0010] To achieve this object, a lithium secondary battery is provided, which includes a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte.

[0011] The negative electrode comprises a current collector, a porous polyolefin film protective layer with a hydrophilic surface modification, and an optional lithium metal layer disposed between the current collector and the protective layer.

[0012] The porous polyolefin film protective layer has a contact angle of 40° or less to an electrolyte prepared by dissolving LiFSI at a concentration of 3.5 M in a solvent mixture of polycarbonate and dimethyl carbonate in a volume ratio of 3:7, and

[0013] The electrolyte includes an organic solvent and a lithium salt, and includes the lithium salt at a concentration of 2M to 7M.

[0014] The porous polyolefin membrane protective layer can be hydrophilic surface modified by plasma treatment.

[0015] The porous polyolefin may be a polymer of an olefin monomer or a copolymer of an olefin monomer and a polar monomer.

[0016] The olefin monomer may be one or more selected from the group consisting of ethylene, propylene, 1-butene, 1,3-butadiene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene and 1-eicosene.

[0017] Furthermore, the polar monomer may be one or more selected from the group consisting of unsaturated carboxylic acids and derivatives thereof, styrene derivatives, (meth)acrylamide and derivatives thereof, acrylonitrile and derivatives thereof, and C1-6 alkyl vinyl ketone.

[0018] Preferably, the polar monomer may be one or more selected from the group consisting of (meth)acrylic acid, vinyl acetate, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, styrene, α-methylstyrene, acrylonitrile and methyl vinyl ketone.

[0019] The air permeability of the porous polyolefin film may be 300 sec / 100 cc or less.

[0020] The thickness of the porous polyolefin film protective layer may be 1 to 30 μm.

[0021] The pore size of the porous polyolefin membrane protective layer may be 10 to 1000 nm and the porosity may be 20 to 80%.

[0022] In the electrolyte, the organic solvent may be a carbonate solvent, an ether solvent, a phosphate solvent or a combination thereof. Specifically, the carbonate solvent may be one or more selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC) and butylene carbonate (BC), and

[0023] The ether solvent may be one or more selected from the group consisting of dibutyl ether, tetraglyme, diglyme, dimethoxyethane, 2-methyltetrahydrofuran and tetrahydrofuran.

[0024] In the electrolyte, the lithium salt can be LiPF6, LiBF4, LiSbF6, LiAsF6, LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (wherein x and y are natural numbers), LiCl, LiI, LiB(C2O4)2, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(perfluoroethylsulfonyl)imide, lithium (fluorosulfonyl)(nonafluorobutanesulfonyl)imide, lithium (fluorosulfonyl)(trifluoromethanesulfonyl)imide or a combination thereof.

[0025] The positive electrode may include one or more positive electrode active materials selected from the group consisting of lithium-manganese oxide, lithium-cobalt oxide, lithium-nickel oxide, lithium-nickel-manganese oxide, lithium-nickel-cobalt oxide, lithium-manganese-cobalt oxide, and lithium-nickel-manganese-cobalt oxide.

[0026] According to one embodiment, the positive electrode may include a nickel-cobalt-manganese positive electrode active material.

[0027] Effects of the Invention

[0028] The lithium secondary battery of the present invention exhibits excellent lifespan characteristics and stability because the side reaction of the electrolyte is minimized and the uneven growth of lithium dendrites is effectively suppressed. [Drawings]

[0029] Figure 1 The photographs of the negative electrode protective layer surfaces of the batteries of Comparative Example 2 and Example 1 after they were charged once and then disassembled are shown. [Specific implementation method]

[0030] The terms used herein are only used to illustrate specific embodiments and are not intended to limit the present invention. Unless explicitly stated or it is obvious from the context that this is not the case, singular expressions include their plural expressions. As used herein, the terms "including" or "having" and the like are intended to specify the presence of implemented features, steps, constituent elements, or combinations thereof, and they are not intended to exclude the possibility of the presence or addition of one or more other features, steps, constituent elements, or combinations thereof.

[0031] Although various modifications can be made to the present invention and the present invention can have various forms, specific embodiments will be illustrated and described in detail below. However, it should be understood that these are not intended to limit the present invention to specific disclosures, and the present invention includes all modifications, equivalents or replacements thereof without departing from the spirit and technical scope of the present invention.

[0032] Hereinafter, the present invention will be described in detail.

[0033] According to one embodiment of the present invention, there is provided a lithium secondary battery, which includes a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte.

[0034] The negative electrode comprises a current collector, a porous polyolefin film protective layer with a hydrophilic surface modification, and an optional lithium metal layer disposed between the current collector and the protective layer.

[0035] The porous polyolefin film protective layer has a contact angle of 40° or less to an electrolyte prepared by dissolving LiFSI at a concentration of 3.5 M in a solvent mixture of polycarbonate and dimethyl carbonate in a volume ratio of 3:7, and

[0036] The electrolyte includes an organic solvent and a lithium salt, and includes the lithium salt at a concentration of 2M to 7M.

[0037] In order to improve the stability and life characteristics of lithium metal secondary batteries using lithium metal as negative electrode active materials, a hydrophilic surface modified porous polyolefin film protective layer is included in the negative electrode. The protective layer has a uniform nanoscale pore structure, thereby inducing uniform growth of lithium dendrites during charge / discharge of the battery, and is hydrophilic and has excellent wettability, thereby showing high compatibility (affinity) with high-concentration electrolytes. Therefore, a lithium secondary battery including a negative electrode to which the protective layer is applied can show excellent battery performance, because the battery short circuit caused by the uneven growth of lithium dendrites and the degradation of life characteristics caused by the side reactions of the electrolyte are improved.

[0038] The negative electrode includes a current collector, a porous polyolefin film protective layer, and optionally a lithium metal layer disposed between the current collector and the protective layer.

[0039] The current collector is not particularly limited as long as it does not cause chemical changes in the battery and has conductivity, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium and silver, etc., and aluminum-cadmium alloy, etc. can be used. Also, it can have various shapes, such as a film, sheet, foil, net, porous material, foam, non-woven fabric, etc., with / without fine irregularities on the surface.

[0040] The thickness of the current collector is not particularly limited, but may be preferably 3 to 30 μm, more preferably 10 to 20 μm. If the thickness of the current collector is greater than 30 μm, the unit volume capacity of the electrode may decrease, and if less than 3 μm, folding may occur during the manufacture of the electrode.

[0041] An electrode active material layer may be optionally included. That is, the electrode of the present invention may include a current collector and a protective layer without an electrode active material layer, or may include a current collector, an electrode active material layer and a protective layer. Among them, the electrode active material layer may be placed between the current collector and the protective layer, and the electrode may have a structure in which the current collector, the electrode active material layer and the protective layer are stacked in sequence. In the case of an electrode without an electrode active material layer, during the charge / discharge process after the battery is assembled, lithium metal is plated between the current collector and the protective layer, and therefore, an electrode active material layer may be generated during the use of the battery.

[0042] The electrode active material layer includes lithium metal as an active material, and may further include one or more selected from the group consisting of lithium alloys, lithium metal composite oxides, lithium-containing titanium composite oxides (LTO), and combinations thereof. Among them, the lithium alloy includes elements capable of alloying with lithium, and as elements capable of alloying with lithium, Si, Sn, C, Pt, Ir, Ni, Cu, Ti, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, or a combination thereof may be mentioned.

[0043] Preferably, the electrode active material layer may be lithium metal or lithium alloy, more preferably lithium metal.

[0044] The thickness of the electrode active material layer may be 0 to 40 μm, preferably 5 to 40 μm, and more preferably 5 to 20 μm.

[0045] The method for forming the electrode active material layer on the current collector is not particularly limited, and methods known in the art can be used. For example, the electrode active material layer can be formed by depositing or coating lithium metal or lithium alloy on the current collector by dry or wet methods, or by stacking a prepared lithium metal sheet or foil on the current collector.

[0046] The porous polyolefin used as the negative electrode protective layer may be a polymer of an olefin monomer or a copolymer of an olefin monomer and a polar monomer.

[0047] As specific examples of the olefin monomer, there may be mentioned one or more selected from the group consisting of ethylene, propylene, 1-butene, 1,3-butadiene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene and 1-eicosene.

[0048] Polar monomers are compounds with a larger dipole moment than olefin monomers, and refer to olefins having one or more polar functional groups. Since the porous polyolefin membrane prepared using such polar monomers as comonomers has high hydrophilicity, it can show excellent affinity with an electrolyte in which a high concentration of lithium salt is dissolved, thereby reducing battery resistance and improving output characteristics.

[0049] As the polar monomer, unsaturated carboxylic acids and their derivatives such as vinyl acetate, (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate, etc., styrene and styrene derivatives such as α-methylstyrene, (meth)acrylamide and its derivatives such as acrylamide and methacrylamide, acrylonitrile and its derivatives, and C1-6 alkyl vinyl ketones such as methyl vinyl ketone, etc., can be mentioned, and they can be used in combination. Among them, "(meth)acrylic acid" is used to represent acrylic acid and methacrylic acid, "(meth)acrylate" is used to represent acrylic acid and methacrylate, and "(meth)acrylamide" is used to represent acrylamide and methacrylamide.

[0050] More specifically, the polar monomer may be one or more selected from the group consisting of (meth)acrylic acid, vinyl acetate, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, styrene, α-methylstyrene, acrylonitrile, and methyl vinyl ketone.

[0051] According to one embodiment, the porous polyolefin membrane may be polyethylene (PE), polypropylene (PP), a copolymer of ethylene and vinyl acetate (ethylene-vinyl acetate, EVA), a copolymer of ethylene and acrylic acid (ethylene-acrylic acid, EAA), or a copolymer of ethylene and ethyl acrylate (ethylene-ethyl acrylate, EEA), but is not limited thereto.

[0052] Generally, since the polyolefin film is a polymer of olefin monomers and exhibits hydrophobicity, when an electrolyte containing a high concentration of lithium salt is used, the wettability is reduced, and the desired electrochemical characteristics cannot be achieved. Therefore, the porous polyolefin film protective layer is hydrophilic surface modified by plasma treatment to improve the affinity with the high concentration electrolyte. As described above, compared with the polyolefin prepared using only the olefin monomer, the polyolefin prepared using the polar monomer together exhibits improved hydrophilicity, but can have further improved hydrophilicity by plasma treatment.

[0053] The active gas used for plasma treatment may be nitrogen, oxygen, air, argon, helium, carbon dioxide, carbon monoxide, ozone, silane, alkane and fluoroalkane, etc., preferably nitrogen, oxygen, air, argon or a mixture thereof.

[0054] The plasma treatment may be performed using radio frequency plasma, cyclotron resonance frequency plasma, microwave plasma, or corona discharge, and specifically, corona discharge may be used. The corona discharge may be performed without providing an inert gas as described above.

[0055] The corona discharge may be performed at atmospheric pressure using a plasma output of 1 to 10 kW, more preferably 100 to 3000 W, most preferably 100 to 500 W.

[0056] During the plasma treatment, the distance between the nozzle and the porous polyolefin membrane (exposure distance) may be 0.1 to 300 mm, more preferably 1 to 200 mm, even more preferably 1 to 50 mm, most preferably 1 to 10 mm.

[0057] By the above-mentioned plasma treatment, the surface of the porous polyolefin film protective layer is modified to be hydrophilic, thereby showing excellent wettability even with a high-concentration electrolyte having a high viscosity.

[0058] The contact angle of the hydrophilic surface modified porous polyolefin film protective layer to the electrolyte prepared by dissolving LiFSI at a concentration of 3.5M in a solvent mixture of polycarbonate and dimethyl carbonate in a volume ratio of 3:7 can be 40° or less, 30° or less, or 20° or less. The closer the contact angle is to 0°, the better the hydrophilicity is, so the lower limit of the water contact angle is not limited and can be 0°. The contact angle can be measured by a static drop method, in which a drop of the electrolyte is dropped on the surface of the protective layer and left for 30 minutes, and then the contact angle is measured using a microscope.

[0059] Since the porous polyolefin film protective layer has uniform nanoscale pores, lithium dendrites can be uniformly grown on the electrode surface during the charge / discharge of the battery. Therefore, damage to the protective layer and the separator caused by the uneven growth of lithium dendrites and the resulting battery short circuit can be prevented, and thus the stability and life characteristics of the battery can be significantly improved.

[0060] In order to ensure the above effect, the pore size of the porous polyolefin membrane protective layer can be 10 to 1000nm, or 10 to 100nm, preferably 20 to 50nm. If the pore size of the protective layer is less than 10nm, the impedance may increase when transferring lithium ions, and if it is greater than 1000nm, the elasticity of the porous polyolefin membrane protective layer may decrease. Among them, the pore size can be measured using a commercially available pore size distribution measurement device, for example, it can be measured by N2 adsorption method using the BELSORP-miniX device of SOLETEX.

[0061] The air permeability of the porous polyolefin film protective layer can be less than 300sec / 100cc, or less than 250sec / 100cc, or less than 220sec / 100cc, and more than 50sec / 100cc, more than 100sec / 100cc, or more than 120sec / 100cc. If the air permeability of the protective layer exceeds 300sec / 100cc, elasticity may be reduced, thereby causing problems in mechanical properties, and if less than 50sec / 100cc, impedance may increase. Air permeability can be measured using Gurley air permeability tester according to JIS P-8117, and the measurement method of air permeability will be described in detail in the following embodiments.

[0062] And, the porosity of the porous polyolefin membrane protective layer is preferably 20 to 80%, more preferably 30 to 70%, or 40 to 50%. The porosity is a value calculated by measuring the true density, thickness and mass of the porous polyolefin membrane protective layer, and specifically, can be derived from the following equation.

[0063] [Equation 1]

[0064] Porosity (%) = (1-(measured density of porous polyolefin film protective layer / theoretical density of polyolefin)) × 100

[0065] If the porosity of the protective layer is less than 20%, impedance may increase when lithium ions are transferred, and if it exceeds 80%, mechanical properties (such as elasticity) of the protective layer may decrease. Therefore, it is preferable to satisfy the above range.

[0066] The thickness of the porous polyolefin film protective layer can be appropriately controlled according to the configuration of the electrode and the battery, for example, it can be in the range of 1 to 30 μm, or 3 to 10 μm. Within the above thickness range, the growth and uneven growth of lithium dendrites can be effectively suppressed.

[0067] Meanwhile, the electrolyte includes an organic solvent and a lithium salt, and includes the lithium salt at a concentration of 2M to 7M, or 3M to 5M.

[0068] If the lithium salt molar concentration of the electrolyte is high, the battery life degradation caused by the side reactions of the electrolyte can be minimized. Specifically, the free solvent that does not dissolve lithium ions present in the electrolyte preferentially causes side reactions during the charge / discharge of the battery, and if a high-concentration electrolyte is used, the amount of free solvent is reduced, thereby reducing the side reactions of the electrolyte. In particular, lithium metal secondary batteries using lithium metal as negative electrode active materials produce more serious side reactions of the electrolyte during charging, which has the most adverse effect on battery life. However, by applying a high-concentration electrolyte, the above problems can be solved to significantly improve the battery life characteristics. Among them, a high-concentration electrolyte refers to an electrolyte with a molar concentration of lithium salt of more than 2M.

[0069] However, if the molar concentration of the lithium salt is greater than 7 M, the viscosity of the electrolyte may become too high and the lithium salt may not be completely dissociated, and therefore, it is preferable to satisfy the above range.

[0070] The organic solvent contained in the electrolyte is a non-aqueous organic solvent, and carbonate, ester, ether, ketone, alcohol and phosphate solvents commonly used in the art can be used without limitation. According to one embodiment, as the organic solvent, a carbonate solvent, an ether solvent, a phosphate solvent or a combination thereof can be used. In the case of using a carbonate solvent and / or an ether solvent, it can appropriately dissociate the lithium salt and has a low viscosity, and therefore has a relatively excellent ionic conductivity.

[0071] As the carbonate solvent, one or more selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC) and fluoroethylene carbonate (FEC) can be used. According to one embodiment, as the carbonate solvent, a solvent mixture having a volume ratio of DMC to PC of 10:1 to 1:1 or 7:3 to 1:1 can be used, or a solvent mixture having a volume ratio of EMC to FEC of 10:1 to 7:3 or 9:1 to 7:3 can be used.

[0072] As the ether solvent, one or more selected from the group consisting of dimethyl ether (DME), diethyl ether (DEE), dibutyl ether (DBE), tetraglyme, diglyme, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) can be used. Among them, DME, DEE, TTE, etc. can be more appropriately used.

[0073] When a carbonate solvent and an ether solvent are used in combination, the mixing ratio is not particularly limited and can be appropriately controlled according to the target battery performance. For example, a solvent mixture having a volume ratio of DMC to TTE of 10:1 to 1:1 or 7:3 to 1:2 can be used.

[0074] As the phosphate solvent, one or more selected from the group consisting of trimethyl phosphate, triethyl phosphate, triphenyl phosphate, tricresyl phosphate, cresyl diphenyl phosphate, octyl diphenyl phosphate, biphenyl diphenyl phosphate, trioctyl phosphate and tributyl phosphate may be used, but is not limited thereto.

[0075] As lithium salts used in the electrolyte, there can be mentioned LiPF6, LiBF4, LiFSI, LiTFSI, LiSbF6, LiAsF6, LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (wherein x and y are natural numbers), LiCl, LiI, LiB(C2O4)2, lithium bis(oxalato)borate (LiBOB), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(perfluoroethylsulfonyl)imide (LiBETI), lithium (fluorosulfonyl)(nonafluorobutanesulfonyl)imide (LiNFSI), lithium (fluorosulfonyl)(trifluoromethanesulfonyl)imide (LiFTI or LiFTA), or a combination thereof.

[0076] In addition to the organic solvent and the lithium salt, the electrolyte may also include additives generally included in the electrolyte for lithium secondary batteries. For example, the electrolyte may further include vinylene carbonate or ethylene carbonate compounds as additives, such as difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate and fluoroethylene carbonate, etc., to improve battery life.

[0077] Meanwhile, the positive electrode includes a positive electrode active material layer formed on a positive electrode collector.

[0078] The positive electrode current collector is not particularly limited as long as it does not cause chemical changes in the battery and has high conductivity, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. can be used. The current collector may have various forms, such as a film, a sheet, a foil, a net, a porous body, a foam, and a non-woven fabric. The thickness of the current collector may be in the range of 3 to 500 μm, but is not limited thereto.

[0079] The positive electrode active material layer may be prepared by coating a positive electrode active material slurry prepared by mixing a positive electrode active material, a conductive agent, and a binder in the presence of an organic solvent on a current collector, drying, and roll-pressing.

[0080] As the positive electrode active material, a compound capable of reversibly inserting and deinserting lithium known in the art may be used without limitation. Specifically, the positive electrode active material may be a lithium composite metal oxide including one or more metals (eg, cobalt, manganese, nickel or aluminum) and lithium.

[0081] As the lithium composite metal oxide, mention may be made of lithium-manganese oxides (e.g., LiMnO2, LiMn2O4), lithium-cobalt oxides (e.g., LiCoO2), lithium-nickel oxides (e.g., LiNiO2), lithium-nickel-manganese oxides (e.g., LiNi 1-Y Mn Y O2 (where 0 < Y < 1), LiMn 2-z Ni z O4 (where 0 < Z < 2)), lithium-nickel-cobalt oxides (e.g., LiNi 1-Y1 Co Y1 O2 (where 0 < Y1 < 1)), lithium-manganese-cobalt oxides (e.g., LiCo 1-Y2 Mn Y2 O2 (where 0 < Y2 < 1), LiMn 2-Z1 Co Z1 O4 (where 0 < Z1 < 2)), lithium-nickel-manganese-cobalt oxides (e.g., Li(Ni p Co q Mn r1 )O2 (where 0 < p < 1, 0 < q < 1, 0 < r1 < 1, p + q + r1 = 1) or Li(Ni p1 Co q1 Mn r2 )O4 (where 0 < p1 < 2, 0 < q1 < 2, 0 < r2 < 2, p1 + q1 + r2 = 2)), or lithium-nickel-cobalt-transition metal (M) oxides (e.g., Li(Ni p2 Co q2 Mn r3 M S2 )O2 (where M is one or more selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg, and Mo, p2, q2, r3, and s2 are the atomic fractions of the respective elements, and 0 < p2 < 1, 0 < q2 < 1, 0 < r3 < 1, 0 < s2 < 1, p2 + q2 + r3 + s2 = 1)), etc., and among them, one or two or more mixtures may be included.

[0082] Among them, the lithium metal composite oxide may be LiCoO2, LiMnO2, LiNiO2, lithium-nickel-manganese-cobalt oxide (e.g., Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2 or Li(Ni 0.8 Mn 0.1 Co 0.1)O2) or lithium-nickel-cobalt-aluminum oxide (e.g., Li(Ni 0.8 Co 0.15 Al 0.05 )O2), etc., because they can improve battery capacity characteristics and stability.

[0083] According to one embodiment, the positive electrode active material may be lithium-nickel-manganese-cobalt oxide. Lithium-nickel-manganese-cobalt oxide, also known as NCM active material, has excellent economical properties (due to a portion of the expensive cobalt component being replaced by manganese), high capacity and stability, and therefore may be preferably used. Specifically, the positive electrode active material may be Li(Ni 0.6 Mn 0.2 Co 0.2 )O2、Li(Ni 0.5 Mn 0.3 Co 0.2 )O2 or Li(Ni 0.8 Mn 0.1 Co 0.1 )O2.

[0084] The conductive material is used to impart conductivity to the electrode, and any electronically conductive material can be used as long as it does not cause chemical changes in the battery and is electronically conductive, and for example, carbonaceous materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black and carbon fiber, etc.; metallic materials such as metal powders such as copper, nickel, aluminum and silver, or metal fibers; conductive polymers such as polyphenylene derivatives; or mixtures thereof can be used.

[0085] The role of the binder is to make the active material particles adhere properly to each other and to make the active material adhere properly to the current collector, and as representative examples, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin and nylon, etc. can be mentioned, but the binder is not limited to these.

[0086] The diaphragm separates the negative electrode from the positive electrode and provides a path for the movement of lithium ions, and a diaphragm commonly used in lithium batteries can be used. That is, a diaphragm with low impedance to the movement of electrolyte ions and excellent wettability of the electrolyte can be used. For example, it can be selected from glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene (PTFE) or a combination thereof, and it can be in the form of a non-woven fabric or a woven fabric. For example, in lithium-ion batteries, polyolefin polymer diaphragms such as polyethylene and polypropylene are mainly used, and a coated diaphragm including a ceramic component or a polymer material can be used to ensure heat resistance or mechanical strength, and optionally, it can be used in a single layer or multiple layers. According to one embodiment, a diaphragm prepared by coating a ceramic coating material including ceramic particles and an ionic adhesive polymer on both sides of a polyolefin polymer substrate can be used.

[0087] The lithium secondary battery of the present invention can use lithium metal as the negative electrode active material to achieve high energy density, and the porous polyolefin film protective layer formed on the negative electrode induces uniform growth of lithium dendrites, thereby showing excellent stability and life characteristics. In addition, the lithium secondary battery of the present invention can use an electrolyte containing a high concentration of lithium salt to minimize electrolyte side reactions during battery charging / discharging.

[0088] In the following, preferred embodiments are provided for a better understanding of the present invention, but these embodiments are provided only as examples of the present invention, and it is obvious to a person skilled in the art that various modifications and changes can be made within the scope and technical idea of ​​the present invention, and these modifications and changes are within the scope of the appended claims.

[0089] Example

[0090] Preparation Example 1: Preparation of porous polypropylene (PP) membrane

[0091] Polypropylene (PP) resin (Toray Industries, Inc.) was fed to a single screw extruder (discharge rate 10 kg / hour) and melt-extruded at 230° C. A sintered filter (filtration area: 65000 mm2) with 5 pieces cut to 10 μm was used. 2 ) leaf disc filter to remove foreign matter from the extruded PP resin, and then the resin is passed through a wire mesh filter cut into 30μm (filtration area: 20000mm 2). Thereafter, it was discharged from the T die to a casting drum whose surface temperature was controlled to 120°C, and cast so as to be in contact with the drum for 20 seconds, thereby obtaining an unstretched sheet. Subsequently, it was preheated using a ceramic roller heated to 120°C, thereby stretching it at a 2-fold stretching ratio in the longitudinal direction of the sheet. Subsequently, the end was clamped with a clip and introduced into a tenter stretching machine, and stretched at a 4-fold stretching ratio and a stretching speed of 50% / min at 150°C. While applying 10% relaxation in the transverse direction, heat treatment was performed at 140°C for 7 seconds, thereby obtaining a porous PP film having a thickness of 10 μm.

[0092] Preparation Example 2: Preparation of porous polyethylene (PE) membrane

[0093] A porous PE film was obtained by the same method as Preparation Example 1, except that polyethylene (PE) resin (Toray Industries, Inc.) was used instead of polypropylene resin.

[0094] Preparation Example 3: Preparation of porous ethylene vinyl acetate (EVA) membrane

[0095] EVA resin (LG Chem.) was fed to a single screw extruder (discharge rate 5 kg / hour) and melt-extruded at 160° C. A sintered filter (filtration area: 65000 mm2) with 5 pieces cut to 10 μm was used. 2 ) leaf disk filter to remove foreign matter, and then the extruded resin is passed through a wire mesh filter cut into 30μm (filtration area: 20000mm 2 ). Thereafter, it was discharged from the T die to a casting drum whose surface temperature was controlled to 120°C, and cast so as to be in contact with the drum for 20 seconds, thereby obtaining an unstretched sheet. Subsequently, it was preheated using a ceramic roller heated to 100°C, thereby stretching it at a 2-fold stretching ratio in the longitudinal direction. Subsequently, the end was clamped with a clip and introduced into a tenter stretching machine, and stretched at 120°C at a 4-fold stretching ratio and a stretching speed of 20% / min. While applying 10% relaxation in the transverse direction, a heat treatment was performed at 100°C for 7 seconds, thereby obtaining a porous EVA film having a thickness of 10 μm.

[0096] Preparation Example 4: Preparation of plasma treated porous polypropylene (PP) membrane

[0097] On both sides of the porous PP film prepared in Preparation Example 1, plasma treatment was performed using a spottec device of Tentec Corporation under the following conditions, thereby preparing a plasma-treated porous PP film.

[0098] Output frequency: 25KHz

[0099] Output power: 300 watts

[0100] Exposure distance: 10mm

[0101] Exposure time: 90 seconds per side

[0102] Preparation Example 5: Preparation of plasma treated porous ethylene vinyl acetate (EVA) membrane

[0103] The porous EVA prepared in Preparation Example 3 was plasma-treated by the same method as Preparation Example 4, thereby preparing a plasma-treated porous EVA membrane.

[0104] Experimental Example 1: Measuring the properties of porous polyolefin (PO) membrane

[0105] The properties of the porous polyolefin membranes of Preparation Examples 1, 2, 4 and 5 were measured as follows, and the results are shown in Table 1.

[0106] (1) Pore size: The pore size was measured by N2 adsorption using the BELSORP-miniX instrument from SOLETEX.

[0107] (2) Porosity: The true density, thickness, and mass of each PO membrane were measured, and the porosity was calculated according to the following Equation 1.

[0108] [Equation 1]

[0109] Porosity (%) = (1-(measured density of porous polyolefin film protective layer / theoretical density of polyolefin)) × 100

[0110] (3) Air permeability: The air permeability was measured using a Gurley air permeability tester according to JIS P-8117. The air permeability was measured by measuring the air permeability of 100cc of air through a 28.6mm diameter and 645mm area. 2 time.

[0111] (4) Contact angle: A drop of an electrolyte solution prepared by dissolving LiFSI at a concentration of 3.5 M in a solvent mixture of polycarbonate (PC) and dimethyl carbonate (DMC) in a volume ratio of 3:7 was dripped on the surface of each PO film and left for 30 minutes. The contact angle was then measured using a microscope by a sessile drop method.

[0112] [Table 1]

[0113]

[0114] Examples 1 to 2 and Comparative Examples 1 to 4

[0115] (1) Preparation of positive electrode

[0116] 96g Li(Ni 0.6 Mn 0.2 Co 0.2)O2, 2 g of PVDF and 2 g of carbon black were added to 150 ml of N-methylpyrrolidone to prepare a slurry, and then the slurry was coated on an aluminum foil having a thickness of 15 μm and dried at about 130° C. for 2 hours to prepare a positive electrode.

[0117] (2) Preparation of negative electrode

[0118] The metal was deposited on a copper foil having a thickness of 15 μm to a thickness of 5 μm to prepare a lithium metal electrode, and each protective layer of the following Table 2 was stacked thereon to prepare a negative electrode. However, in Comparative Example 1, a lithium metal electrode prepared by depositing lithium metal on a copper foil without a separate protective layer was used as a negative electrode.

[0119] [Table 2]

[0120] Protective layer Example 1 Preparation Example 4 Example 2 Preparation Example 5 Comparative Example 1 none Comparative Example 2 BN / PVDF Comparative Example 3 Preparation Example 1 Comparative Example 4 Preparation Example 2

[0121] The BN / PVDF protective layer of Comparative Example 2 was prepared as follows.

[0122] 500 ml of PVDF (polyvinylidene fluoride) and NMP (N-methylpyrrolidone) solution was mixed with 500 ml of BN (boron nitride) and NMP solution to prepare a BN / PVDF / NMP solution (composition for forming a protective layer). The composition was prepared so that the mass ratio of BN:PVDF in the composition for forming a protective layer was 9:1.

[0123] The protective layer-forming composition was applied on the lithium metal electrode using a doctor blade and dried to form a protective layer (BN 90 wt %, PVDF 10 wt %) having a thickness of 2 μm.

[0124] (3) Preparation of electrolyte

[0125] LiFSI was dissolved at a concentration of 3.5 M in a solvent mixture of polycarbonate (PC): dimethyl carbonate (DMC) = 3:7 in volume ratio to prepare an electrolyte.

[0126] (4) Preparation of lithium secondary batteries

[0127] A ceramic-coated polyolefin separator (Asahi kasei, ND307B15) with a thickness of 15 μm was inserted between the positive electrode and the negative electrode to prepare an electrode assembly with a structure in which the positive electrode / separator / negative electrode protective layer / negative electrode was stacked in sequence, and it was placed inside a battery casing, and then an electrolyte was injected to prepare a lithium secondary battery.

[0128] Experimental Example 2: Evaluation of initial discharge capacity and life characteristics

[0129] The initial discharge capacity and life characteristics of each battery prepared in Examples and Comparative Examples were evaluated. The battery was operated at 25° C. under the following conditions.

[0130] [Initial discharge capacity]

[0131] Charging: rate 0.1C, voltage 4.25V, CC / CV (1C cutoff current 5%)

[0132] Discharge: rate 0.1C, voltage 3V, CC

[0133] [Life characteristics]

[0134] Charging: rate 0.3C, voltage 4.25V, CC / CV (1C cutoff current 5%)

[0135] Discharge: rate 0.5C, voltage 3V, CC

[0136] [Table 3]

[0137] Initial discharge capacity (mAh) The number of cycles when the discharge capacity retention rate is 80% Example 1 125 92 Example 2 126 110 Comparative Example 1 128 30 Comparative Example 2 126 54 Comparative Example 3 122 82 Comparative Example 4 121 71

[0138] Referring to Table 3, it was confirmed that when the porous polyolefin protective layer was introduced into the negative electrode, significantly improved life characteristics were exhibited compared to Comparative Example 1 without a protective layer and Comparative Example 2 introducing a BN / PVDF protective layer. However, it was confirmed that the porous polyolefin protective layer that was not treated with plasma acted as an impedance, thereby reducing the initial discharge capacity.

[0139] Experimental Example 3: Evaluation of the durability of the protective layer

[0140] The battery of Example 1 and the battery of Comparative Example 2 were charged once, and then the batteries were disassembled to confirm the state of the protective layer. Figure 1 Photo showing the surface of the protective layer.

[0141] refer to Figure 1 , it was confirmed that the surface of the protective layer of Example 1 was not damaged even after the battery was operated, while the surface of the protective layer of Comparative Example 2 was penetrated by lithium dendrites.

Claims

1. A lithium secondary battery comprising a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte, in, The negative electrode comprises a current collector, a porous polyolefin film protective layer with a hydrophilic surface modification, and a lithium metal layer disposed between the current collector and the protective layer. The porous polyolefin film protective layer has a contact angle of 40° or less to an electrolyte prepared by dissolving LiFSI at a concentration of 3.5 M in a solvent mixture of polycarbonate and dimethyl carbonate in a volume ratio of 3:7, and the pore size of the porous polyolefin film protective layer is 10 nm to 1000 nm, and The electrolyte includes an organic solvent and a lithium salt, and includes the lithium salt at a concentration of 2M to 7M.

2. The lithium secondary battery according to claim 1, in, The porous polyolefin membrane protective layer is hydrophilically surface-modified by plasma treatment.

3. The lithium secondary battery according to claim 1, in, The porous polyolefin is a polymer of an olefin monomer or a copolymer of an olefin monomer and a polar monomer.

4. The lithium secondary battery according to claim 3, in, The olefin monomer is one or more selected from the group consisting of ethylene, propylene, 1-butene, 1,3-butadiene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene and 1-eicosene.

5. The lithium secondary battery according to claim 3, in, The polar monomer is one or more selected from the group consisting of unsaturated carboxylic acids and derivatives thereof, styrene derivatives, (meth)acrylamide and derivatives thereof, acrylonitrile and derivatives thereof, and C1-6 alkyl vinyl ketone.

6. The lithium secondary battery according to claim 3, in, The polar monomer is one or more selected from the group consisting of (meth)acrylic acid, vinyl acetate, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, styrene, α-methylstyrene, acrylonitrile and methyl vinyl ketone.

7. The lithium secondary battery according to claim 1, in, The air permeability of the porous polyolefin film protective layer is 300 sec / 100 cc or less.

8. The lithium secondary battery according to claim 1, in, The thickness of the porous polyolefin membrane protective layer is 1 μm to 30 μm.

9. The lithium secondary battery according to claim 1, in, The porosity of the porous polyolefin membrane protective layer is 20% to 80%.

10. The lithium secondary battery according to claim 1, in, The organic solvent is a carbonate solvent, an ether solvent, a phosphate solvent or a combination thereof.

11. The lithium secondary battery according to claim 1, in, The lithium salt is LiPF 6 , LiBF 4 、LiSbF 6 、LiAsF 6 ,LiC 4 F 9 SO 3 、LiClO 4 、LiAlO 2 、LiAlCl 4 、LiN(C x F 2x+1 SO 2 )(C y F 2y+1 SO 2 )、LiCl、LiI、LiB(C 2 O 4 ) 2 , lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(perfluoroethylsulfonyl)imide, lithium (fluorosulfonyl)(nonafluorobutanesulfonyl)imide, lithium (fluorosulfonyl)(trifluoromethanesulfonyl)imide or a combination thereof, wherein x and y are natural numbers.

12. The lithium secondary battery according to claim 1, in, The positive electrode includes one or more positive electrode active materials selected from the group consisting of lithium-manganese oxide, lithium-cobalt oxide, lithium-nickel oxide, lithium-nickel-manganese oxide, lithium-nickel-cobalt oxide, lithium-manganese-cobalt oxide and lithium-nickel-manganese-cobalt oxide.

13. The lithium secondary battery according to claim 1, in, The positive electrode includes a nickel-cobalt-manganese positive electrode active material.

Citation Information

Patent Citations

  • Rotational torsion tester

    KR1020190056447A

  • Multi-layered Anode Comprising Silicon-based Compound and Lithium Secondary Battery Comprising the Same

    KR1020200055448A

  • Negative electrode for lithium metal battery and lithium metal battery comprising the same

    CN107359309A

  • Polyolefin microporous membrane surface-modified by hydrophilic polymer, surface modification method thereof and lithium-ion polymer battery using the same

    KR1020110003131A