A method for preparing a current collector, a current collector, and a secondary battery

By compounding and thinning the foil with the release film or viscosity-reducing film, combined with the base material, a composite current collector with high density and strength is prepared, which solves the problems of high investment and low production efficiency in the existing technology, and achieves high Safety performance and stable continuous production.

CN112436152BActive Publication Date: 2024-10-11JIANGSU ADVANCED MATERIAL TECH CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202011344239.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-26
Publication Date
2024-10-11
Estimated Expiration
2040-11-26

AI Technical Summary

Technical Problem

When preparing current collectors for lithium-ion batteries, the existing technology requires high investment, low production efficiency, and difficulty in controlling the density of the electrodeposited layer or electroplated layer, which can easily lead to problems such as electrolyte immersion and falling off.

Method used

The foil is compounded with a release film or viscosity-reducing film, thinned to the required thickness to avoid damage to the foil, and compounded with the base material to prepare a composite current collector with high density and strength, which is verified by the electrolyte immersion test Safety performance, using low-cost equipment to achieve stable and continuous production.

Benefits of technology

It reduces the difficulty of current collector preparation, improves safety performance, reduces investment, achieves stable and continuous production, and rapidly expands production through low-cost equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112436152B_ABST
    Figure CN112436152B_ABST
Patent Text Reader

Abstract

The present application discloses a method for preparing a current collector, a current collector, and a secondary battery, and relates to the technical field of secondary batteries. The present application first composites the foil with a release film or a viscosity-reducing film, and then thins the foil to the required thickness, which can ensure the density and strength of the foil, avoid damage to the foil during the composite process of the foil and the substrate, and reduce the difficulty of preparing the composite current collector. The composite current collector prepared in this way can pass the electrolyte immersion test and has high safety performance. At the same time, the technical solution of the present application has a small investment, the process flow is similar to that of a cleaning machine, the equipment is lower in cost than a vacuum coating machine, and it can be rapidly expanded by relying on domestic equipment manufacturers, which is easier to achieve stable and continuous production than the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of secondary batteries, and in particular to a method for preparing a current collector, a current collector, and a secondary battery. Background Art

[0002] The current collector is the main component of lithium-ion secondary batteries, used to carry positive and negative active materials, collect and conduct electrons. The common configuration is that the negative electrode uses copper foil material and the positive electrode uses aluminum foil material. Due to the use of metal materials, the positive and negative current collectors account for a large proportion of the total weight of the battery cell (about 8%), so reducing the weight of the current collector is an effective way to increase the energy density (kWh / kg) of lithium-ion batteries. At present, the minimum thickness of aluminum foil products is 9μm, and the minimum thickness of copper foil is 6μm. Due to process limitations, their thickness has approached the limit.

[0003] In this regard, the Chinese invention patent application with publication number CN106960960A discloses a "flexible current collector for improving the cycle performance of negative electrode materials for lithium-ion batteries", which is a nodular negative electrode current collector material prepared by a simple two-step method of electrodeposition and high-temperature annealing; the current collector uses carbon fiber cloth as the substrate material for electrodeposition. Secondly, the Chinese invention patent with publication number CN109599563A discloses "a lithium-ion battery current collector", including a flexible substrate and a conductive coating coated on the surface of the flexible substrate, and the conductive coating includes a chemical coating and an electroplating layer from the inside to the outside.

[0004] The disadvantages of the above technical solution are: 1) large investment and low production efficiency, especially difficult to achieve stable and continuous production; 2) the density of the electrodeposited layer or electroplated layer is difficult to control and it is easy to fall off when immersed in the electrolyte. Summary of the invention

[0005] The purpose of this application is to provide a method for preparing a current collector to solve the problems in the prior art.

[0006] To achieve the above objectives, the present application embodiment adopts the following technical solution: A method for preparing a current collector, comprising the following steps:

[0007] Compounding the foil with the release film or the viscosity-reducing film;

[0008] Soak the foil in an alkaline solution;

[0009] Compounding the foil material with the substrate to obtain a composite film;

[0010] Peel off the release film or the viscosity-reducing film in the composite film.

[0011] In the above technical scheme, the embodiment of the present application first composites the foil with a release film or a viscosity-reducing film, and then thins the foil to the required thickness, which can ensure the density and strength of the foil, avoid damage to the foil during the composite process of the foil and the substrate, and reduce the difficulty of preparing the composite current collector. Then the foil is composited with the substrate, and the composite current collector obtained in this way can pass the electrolyte immersion test and has a high safety performance. At the same time, the technical solution of the present application has a small investment, the process flow is similar to that of a cleaning machine, the equipment is lower in cost than a vacuum coating machine, and it can be rapidly expanded by relying on domestic equipment manufacturers, which is easier to achieve stable and continuous production than the prior art.

[0012] Further, according to an embodiment of the present application, the foil is made of aluminum, copper, nickel, silver, gold, carbon, stainless steel or an alloy thereof.

[0013] Further, according to an embodiment of the present application, the peeling force of the release film or the viscosity-reducing film is less than 10 g.

[0014] Further, according to an embodiment of the present application, the composite pressure of the foil and the release film or the viscosity-reducing film is 0.4-0.6 MPa.

[0015] Further, according to an embodiment of the present application, the thickness of the foil after immersion is 0.75-5 μm.

[0016] Further, according to an embodiment of the present application, the foil material is composited on both side surfaces of the substrate.

[0017] Further, according to an embodiment of the present application, the composite pressure of the foil and the substrate is greater than or equal to 0.4 MPa, and the composite temperature is greater than or equal to 90° C.

[0018] Further, according to an embodiment of the present application, the prepared composite membrane is placed at 50° C. for 72 hours.

[0019] Further, according to an embodiment of the present application, the substrate is made of one or more materials selected from the group consisting of PET, PP, PE, PI, and polyarylsulfone.

[0020] In order to achieve the above-mentioned purpose, the embodiment of the present application further discloses a current collector, which is made by the preparation method as described above.

[0021] In order to achieve the above-mentioned purpose, an embodiment of the present application further discloses a battery, which includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet and / or the negative electrode sheet has a current collector as described above.

[0022] In order to achieve the above-mentioned purpose, an embodiment of the present application further discloses an object, and the object has a battery as described above.

[0023] Further, according to an embodiment of the present application, the object is an electronic product or an electric vehicle.

[0024] Compared with the prior art, the present application has the following beneficial effects: the present application first composites the foil with a release film or a viscosity-reducing film, and then thins the foil to the desired thickness, which can ensure the density and strength of the foil, avoid damage to the foil during the composite process of the foil and the substrate, and reduce the difficulty of preparing the composite current collector. The composite current collector prepared in this way can pass the electrolyte immersion test and has high safety performance. At the same time, the technical solution of the present application requires a small investment, the process flow is similar to that of a cleaning machine, the equipment is lower in cost than a vacuum coating machine, and production can be rapidly expanded with the support of domestic equipment manufacturers. Compared with the prior art, it is easier to achieve stable and continuous production. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The present application is further described below in conjunction with the accompanying drawings and embodiments.

[0026] Figure 1 It is a flow chart of a method for preparing a current collector in the present application.

[0027] Figure 2 This is the surface morphology of the aluminum foil before thinning in this application.

[0028] Figure 3 This is a surface morphology diagram of the aluminum foil after thinning in this application. DETAILED DESCRIPTION

[0029] In order to make the purpose and technical solution of the present invention clearly and completely described, and the advantages more clearly understood, the embodiments of the present invention are further described in detail with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are part of the embodiments of the present invention, rather than all of the embodiments, and are only used to explain the embodiments of the present invention, and are not used to limit the embodiments of the present invention. All other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] In the description of the present invention, it should be noted that the terms "center", "middle", "upper", "lower", "left", "right", "inner", "outer", "top", "bottom", "side", "vertical", "horizontal" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "one", "first", "second", "third", "fourth", "fifth", "sixth" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.

[0031] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0032] For the purpose of simplicity and illustration, the principles of the embodiments are mainly described by reference to examples. In the following description, many specific details are proposed to provide a thorough understanding of the embodiments. However, it is obvious that for those of ordinary skill in the art, these embodiments may not be limited to these specific details in practice. In some instances, known methods and structures are not described in detail to avoid making these embodiments unnecessarily difficult to understand. In addition, all embodiments can be used in combination with each other.

[0033] Figure 1 A method for preparing a current collector in this application is shown. Figure 1 As shown, the current collector preparation method comprises the following steps:

[0034] S10, compounding the foil material with the release film or the viscosity-reducing film;

[0035] S20, soaking the composite foil in S10 in an alkaline solution;

[0036] S30, compounding the foil material soaked in S20 with a substrate to obtain a composite film, wherein the metal surface of the foil material is bonded to one side surface of the substrate;

[0037] S40, peeling off the release film or the viscosity-reducing film in the composite film obtained in S30.

[0038] In the above technical solution, the present application first composites the foil with a release film or a viscosity-reducing film, and then thins the foil to the required thickness, which can ensure the density and strength of the foil, avoid damage to the foil during the composite process of the foil and the substrate, and reduce the difficulty of preparing the composite current collector. The composite current collector prepared in this way can pass the electrolyte immersion test and has high safety performance. At the same time, the technical solution of the present application has a small investment, the process flow is similar to that of a cleaning machine, the equipment is lower in cost than a vacuum coating machine, and it can be rapidly expanded by relying on domestic equipment manufacturers, which is easier to achieve stable and continuous production than the prior art.

[0039] To ensure the safety performance of the battery with the above composite film, it is necessary to limit the thickness of the foil after immersion etching. Let the thickness of the foil after immersion etching be H. Preferably, H satisfies the following relationship: 0.75μm < H < 5μm. In this regard, if the thickness of the foil is less than 1μm, especially below 0.75μm, it is not conducive to the current collector generating sufficient current; if the thickness of the foil is greater than 5μm, it will lead to deterioration of the safety performance of the battery cell.

[0040] In addition, in step S10, the composite pressure between the foil and the release film or the anti-adhesive film is 0.4 - 0.6MPa, and the peeling force of the release film or the anti-adhesive film is below 10g. On the one hand, there should be sufficient composite strength between the release film or the anti-adhesive film and the foil to ensure that the release film or the anti-adhesive film and the foil do not separate during the preparation process; on the other hand, it is necessary to ensure that the release film or the anti-adhesive film is easy to peel off, otherwise it will be easy to damage the composite film in step S40.

[0041] In step S20, the immersion temperature is 40 - 50°C, the immersion time is 0.5 - 2min, and the pH of the alkaline solution is 9 - 10. In this regard, the thinning amount of the foil can be controlled by controlling the immersion temperature, immersion time, and the concentration of the alkaline solution respectively. Specifically, the alkaline solution preferably uses a NaOH solution, and the concentration is controlled within the range of 10 - 15%.

[0042] Taking aluminum foil as an example, the surface of the aluminum foil before immersion etching is as Figure 2 shown, and the aluminum foil after immersion etching is as Figure 3 shown. The processed aluminum surface has obvious microtopography changes compared with ordinary aluminum foil. Specifically, there are pit structures with a size of 1μm - 10μm on the surface.

[0043] In addition, in step S30, the foil is laminated on both side surfaces of the substrate. The composite pressure between the foil and the substrate is greater than or equal to 0.4MPa, and the composite temperature is greater than or equal to 90°C. That is, under the allowable conditions, the higher the composite temperature and composite pressure, the better, to ensure the firmness of the composite between the first foil, the second foil and the substrate. Specifically, step S30 includes the following sub-steps:

[0044] S31: Coat the adhesive (gravure) on the first surface of the substrate, and laminate the metal surface of a piece of foil with the substrate;

[0045] S32: Coat the adhesive (gravure) on the second surface of the substrate, and laminate the metal film of another piece of foil with the substrate;

[0046] S33: Place the product of step S32 at a temperature of 50°C for 72h; then cure it at 85°C for 72h to obtain the composite film.

[0047] Furthermore, the substrate is made of one or more materials selected from PET, PP, PE, PI, and polysulfone, or other light-weight, high-strength insulating materials may be used as substitutes to provide support and reduce the mass of the current collector. Preferably, the thickness of the substrate is 1.5-8 μm. A too thin substrate is easily corroded by the alkaline solution in step S30, which weakens its support capacity and affects the safety performance of the lithium-ion battery.

[0048] Furthermore, the foil is made of aluminum, copper, nickel, silver, gold, carbon, stainless steel or their alloys. Conventionally, the foil used as the positive electrode current collector is generally pressed from aluminum or aluminum alloy, and the foil used as the negative electrode current collector is generally pressed from copper or copper alloy.

[0049] Furthermore, the thickness of the adhesive is 0.5-2 μm. Within this thickness range, the adhesive can provide sufficient bonding force to ensure the firmness of the composite between the substrate and the foil, while not excessively increasing the thickness of the current collector to affect the performance of the battery. The adhesive uses CY-C612 glue produced by Dongguan Jujie New Energy Factory.

[0050] The technical solution of the present application is further illustrated below by using Examples 1-8, but the present application is not limited to these Examples.

[0051] The details of the current collectors in Examples 1-8 are shown in Table 1.

[0052] Table 1

[0053]

[0054] The above current collectors were used to make lithium batteries to obtain Examples 9-14, and the specific details are shown in Table 2.

[0055] Table 2

[0056] Positive current collector Negative current collector Example 9 Example 1 Example 5 Example 10 Example 2 Example 8 Embodiment 11 Example 3 Example 7 Example 12 Example 4 Example 8 Embodiment 13 Example 1 Example 5 Embodiment 14 Example 3 Example 7

[0057] In order to demonstrate the effect of the present application, the current collectors in the following comparative examples 1-6 are introduced for comparison with the embodiments 1-8 of the present application. The specific conditions of comparative examples 1-6 are shown in Table 3.

[0058] Table 3

[0059]

[0060] The current collector in the above comparative example was made into a secondary battery, and the specific conditions are shown in Table 4

[0061] Table 4

[0062]

[0063]

[0064] The secondary batteries in Examples 9-14 and Comparative Examples 7-12 were subjected to nail penetration test (Nail), impact test (Impact), crush test (Crush) and battery cycle test (Cycle), all in accordance with the UN38.3 lithium battery test standard. The test results are shown in Table 5.

[0065] Table 5

[0066] Nail Impact Crush Cycle Example 9 Pass Pass Pass Pass Example 10 Pass Pass Pass Pass Embodiment 11 Pass Pass Pass Pass Example 12 Pass Pass Pass Pass Embodiment 13 Pass Pass Pass Pass Embodiment 14 Pass Pass Pass Pass Comparative Example 7 NG NG NG Pass Comparative Example 8 Pass Pass Pass NG Comparative Example 9 Pass Pass Pass Pass Comparative Example 10 Pass Pass Pass NG Comparative Example 11 NG NG NG Pass Comparative Example 12 Pass Pass Pass Pass

[0067] Although the above describes the illustrative specific implementation methods of the present application so that technicians in this technical field can understand the present application, the present application is not limited to the scope of the specific implementation methods. For ordinary technicians in this technical field, as long as various changes are within the spirit and scope of the present application defined and determined by the attached claims, all application creations using the concept of the present application are protected.

Claims

1. A method for preparing a current collector, characterized in that: The following steps are involved: S10: Compounding the foil material with the release film or the viscosity-reducing film; S20: soaking the foil in an alkaline solution; the thickness of the foil after soaking is 0.75-5 μm; the soaking temperature is 40-50° C., the soaking time is 0.5-2 min, the Ph of the alkaline solution is 9-10; the alkaline solution is a NaOH solution with a concentration of 10-15%; S30: Compounding the foil material with the substrate to obtain a composite film; wherein the metal surface of the foil material is bonded to one side surface of the substrate; S40: peeling off the release film or the viscosity-reducing film in the composite film.

2. A method for preparing a current collector according to claim 1, characterized in that: The foil material is made of aluminum, copper, nickel, silver, gold or stainless steel.

3. The method for preparing a current collector according to claim 1, characterized in that: The release film or the viscosity-reducing film has a peeling force of less than 10 g.

4. The method for preparing a current collector according to claim 1, characterized in that: The composite pressure of the foil material and the release film or the viscosity-reducing film is 0.4-0.6 MPa.

5. The method for preparing a current collector according to claim 1, characterized in that: The foil material is laminated on both side surfaces of the substrate.

6. The method for preparing a current collector according to claim 1, characterized in that: The composite pressure of the foil and the substrate is greater than or equal to 0.4 MPa, and the composite temperature is greater than or equal to 90° C.

7. The method for preparing a current collector according to claim 1, characterized in that: The prepared composite film was placed at 50° C. for 72 hours.

8. The method for preparing a current collector according to claim 1, characterized in that: The substrate is made of one or more materials selected from the group consisting of PET, PP, PE, PI and polyarylsulfone.

9. A current collector, characterized in that: The current collector is made by the preparation method according to any one of claims 1 to 8.

10. A battery, characterized in that: The battery comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet and / or the negative electrode sheet has a current collector as claimed in claim 9.

11. An electronic product, characterized in that: The electronic product comprises a battery as claimed in claim 10.

12. An electronic product according to claim 11, characterized in that: The electronic product is an electric car.

Citation Information

Patent Citations

  • Preparation method for flexible current collector and capable of improving cycling performance of negative electrode material of lithium ion battery

    CN106960960A

  • Lithium ion battery current collector and preparation method thereof

    CN109599563A

  • Composite current collector material and preparation method thereof

    CN104716328A

  • Battery packaging material, flexibly packaged battery and battery heat control device

    CN107154471A

  • Current collector and preparation method and application thereof

    CN111900413A