Self-Aligned Double Patterning

By forming core layers and spacer layers of different widths in photolithography, and adjusting the thickness of the spacers and the etching method, the problem of feature short circuits caused by optical proximity effect is solved, enabling more flexible feature design and capacitance control.

CN112750760BActive Publication Date: 2024-11-05TAIWAN SEMICONDUCTOR MANUFACTURING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011177021.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-09-11
Filing Date
2020-10-28
Publication Date
2024-11-05
Estimated Expiration
2040-10-28

AI Technical Summary

Technical Problem

In existing photolithography technologies, as integrated circuit features shrink, the optical proximity effect causes short circuits in the features, a problem that dual patterning techniques struggle to effectively solve.

Method used

By forming mandrel layers of different widths on the target layer and depositing spacer layers, controlling the thickness and etching method of the spacer layers, spacer etching masks of different widths are formed, and the spacing between metal lines is adjusted.

Benefits of technology

It effectively reduces or eliminates optical proximity effects, improves the flexibility of feature formation and the control of capacitance effects, and optimizes integrated circuit design.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112750760B_ABST
    Figure CN112750760B_ABST
Patent Text Reader

Abstract

The present application relates to self-aligned double patterning. A method includes patterning a mandrel layer above a target layer to form a first mandrel and a second mandrel, the width of the first mandrel being greater than the width of the second mandrel. A spacer layer is formed above the first mandrel and the second mandrel and is modified so that the thickness of the spacer layer above the first mandrel is greater than the thickness of the spacer layer above the second mandrel. Spacers are formed from the spacer layer, the width of the spacers adjacent to the first mandrel being greater than the width of the spacers adjacent to the second mandrel. The target layer is etched using the spacers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure generally relates to self-aligned dual patterning. Background Technology

[0002] Dual patterning is a technique developed for photolithography to enhance feature density. Typically, to form features of integrated circuits on a wafer, photolithography is used, which involves applying a photoresist and defining features on the photoresist. The features in the patterned photoresist are first defined in a photomask, and are realized through transparent or opaque portions of the photomask. The features in the patterned photoresist are then transferred to the fabricated features.

[0003] As integrated circuits continue to shrink, the optical proximity effect has become an increasingly significant problem. When two individual features are too close to each other, the optical proximity effect can cause these features to short-circuit. To address this issue, dual-patterning techniques have been introduced. In dual-patterning, features that are geographically close are separated into two lithographic masks within the same dual-patterning mask set, and both masks are used to expose the same photoresist or to pattern the same hard mask. Within each mask, the distance between features increases relative to the distance between features in a single mask, thus reducing or essentially eliminating the optical proximity effect in dual-patterning. Summary of the Invention

[0004] According to a first aspect of this disclosure, a method for forming a semiconductor device is provided, comprising: patterning a first mandrel layer over a target layer to form a first mandrel and a second mandrel, the width of the first mandrel being greater than the width of the second mandrel; depositing a spacer layer over the first mandrel and the second mandrel; forming a mask layer over the spacer layer and the first mandrel; thinning the spacer layer over the second mandrel; removing the mask layer; etching the spacer layer to form a spacer etching mask, the spacer etching mask including a first spacer contacting a sidewall of the first mandrel and a second spacer contacting a sidewall of the second mandrel, the width of the first spacer being greater than the width of the second spacer; and etching the target layer based on the spacer etching mask.

[0005] According to a second aspect of this disclosure, a method for forming a semiconductor device is provided, comprising: patterning a first mandrel layer over a target layer to form a first mandrel and a second mandrel, the width of the first mandrel being greater than the width of the second mandrel; depositing a spacer layer over the first mandrel and the second mandrel; forming a mask layer over the spacer layer and the second mandrel, a portion of the spacer layer over the first mandrel being exposed from the mask layer; depositing a pad layer over the mask layer and the exposed spacer layer; removing the mask layer; etching the spacer layer and the pad layer over the first mandrel to form a first spacer etch mask including first spacers, and etching the spacer layer over the second mandrel to form a second spacer mask including second spacers, each of the first spacers being wider than the second spacers; and etching the target layer based on the first spacer etch mask and the second spacer etch mask.

[0006] According to a third aspect of this disclosure, a method for forming a semiconductor device is provided, comprising: forming a first set of mandrels in a first region of a wafer; forming a second set of mandrels in a second region of the wafer, wherein the spacing of the first set of mandrels is wider than the spacing of the second set of mandrels; depositing a first spacer layer over the first set of mandrels and the second set of mandrels; depositing a second spacer layer over the first set of mandrels and the second set of mandrels; forming a mask over the first region; removing the second spacer layer over the second set of mandrels in the second region; removing the mask; etching the first spacer layer in the second region and etching the first spacer layer and the second spacer layer in the first region to form a spacer mask including a first spacer in the first region and a second spacer in the second region, wherein the first spacer is wider than the second spacer; removing the first set of mandrels and the second set of mandrels; and etching a target layer beneath the spacer mask. Attached Figure Description

[0007] The various aspects of this disclosure can be best understood from the following detailed description when read in conjunction with the accompanying drawings. Note that, according to industry standard practice, the various features are not drawn to scale. In fact, for clarity of discussion, the dimensions of the various features may be arbitrarily increased or decreased.

[0008] Figure 1A , Figure 1B and Figure 1C ,to Figure 24A and Figure 24B These are cross-sectional and top views of an intermediate stage in the formation of a metal wire according to some embodiments.

[0009] Figure 25-27Various process flows for forming metal wires according to some embodiments are shown.

[0010] Figure 28A and Figure 28B ,to Figure 35A and Figure 35B These are cross-sectional and top views of an intermediate stage in the formation of a metal wire according to some embodiments.

[0011] Figure 36 A process flow for forming a metal wire according to some embodiments is shown.

[0012] Figure 37A and Figure 37B ,to Figure 47A and Figure 47B These are cross-sectional and top views of an intermediate stage in the formation of a metal wire according to some embodiments.

[0013] Figure 48 A process flow for forming a metal wire according to some embodiments is shown.

[0014] Figure 49A and Figure 49B ,to Figure 54A and Figure 54B These are cross-sectional and top views of an intermediate stage of forming a column of sacrificial material according to some embodiments.

[0015] Figure 55 A process flow for forming a metal wire according to some embodiments is shown. Detailed Implementation

[0016] The following disclosure provides various embodiments or examples for implementing different features of the invention. Specific examples of components and arrangements, etc., are described below to simplify this disclosure. Of course, these are merely examples and not limiting. For example, in the following description, forming a first feature above or on a second feature can include embodiments where the first and second features are formed in direct contact, and can also include embodiments where an additional feature can be formed between the first and second features such that the first and second features do not need to be in direct contact. Furthermore, reference numerals and / or letters may be repeated in various examples throughout this disclosure. Such repetition is for simplicity and clarity and does not in itself indicate a relationship between the various embodiments and / or configurations discussed.

[0017] In addition, spatially related terms (e.g., "below," "below," "lower than," "above," "upper") may be used herein to facilitate the description of the relationship of one element or feature shown in the figure relative to another element(s) or feature(s). These spatially related terms are intended to cover different orientations of the device in use or operation other than those shown in the figure. The device may be oriented in other ways (rotated 90 degrees or in other orientations), and the spatially related descriptors used herein may be interpreted accordingly.

[0018] Features such as metal wires and methods for forming them are provided according to various exemplary embodiments. Intermediate stages for forming features are illustrated according to some embodiments. Variations of some embodiments are discussed. Throughout the various views and illustrative embodiments, the same reference numerals are used to indicate the same elements.

[0019] Typically, self-aligned double patterning (SADP) works by using a base pattern (sometimes called a mandrel layer) that is patterned using available photolithography processes. A spacer layer is then conformally deposited over the mandrel layer base pattern and etched to remove the horizontal portions of the spacer layer. After the mandrel layer base pattern is removed, the remaining vertical portions of the spacer layer then become a mask for patterning the underlying layers. The width of these vertical portions of the spacer layer is determined by the deposition thickness of the spacer layer.

[0020] Examples are provided that enable different thicknesses of spacer layers deposited on the core layer. When the spacer layer is etched to remove horizontal portions, the resulting mask can have different widths in different regions of a single die or wafer. Masks with larger widths provide larger spacing between subsequently formed metal lines, while masks with smaller widths provide smaller spacing between subsequently formed metal lines. These differences can be advantageously used in die design to achieve smaller die regions where metal lines require smaller spacing, while maintaining larger spacing in other regions of the die. As a result, the total die area can be advantageously reduced. For example, by controlling the width of the spacing between metal lines, the capacitance effect between lines can be controlled. Regions of the device that are sensitive to capacitance effects can use thicker spacers to provide more spacing, while less sensitive regions of the device can use thinner spacers to provide less spacing. Examples provide ways to have thicker or thinner spacers in the same device die and patterning process.

[0021] Figure 1A , Figure 1B and Figure 1C ,to Figure 24A and Figure 24B Top and cross-sectional views of an intermediate stage in forming features in a target layer, according to some example embodiments, are shown. Figure 28A and Figure 28B ,to Figure 35A and Figure 35B Top and cross-sectional views of an intermediate stage in forming features in a target layer, according to other example embodiments, are shown. Figure 37A and Figure 37B ,to Figure 47A and Figure 47B Top and cross-sectional views of an intermediate stage of forming features in a target layer according to other example embodiments are shown. Figure 49A and Figure 49B ,to Figure 54A and Figure 54B Top and cross-sectional views of an intermediate stage in forming features in a target layer, according to some example embodiments, are shown.

[0022] exist Figure 1A and Figures 1B to 24A and Figure 24B , Figure 28A and Figures 28B to 35A and Figure 35B , Figure 37A and Figures 37B to 47A and Figure 47B ,as well as Figure 49A and Figures 49B to 54A and Figure 54B In this context, drawing numbers may include the letters "A", "B", or "C". The letter "A" indicates that the corresponding drawing shows a vertical cross-sectional view. The letter "B" indicates that the corresponding drawing shows a top view or horizontal cross-sectional view through the upper layer. The letter "C" indicates that the corresponding drawing shows a vertical cross-sectional view. Drawings with the same numbers but different letters "A", "B", and "C" indicate that they are different views of the same process step. Furthermore, the cross-sectional view in drawing "A" is obtained from the plane containing line AA in the corresponding drawing "B", (if applicable) the cross-sectional view in drawing "B" is obtained from the plane containing line BB in the corresponding drawing "A", and the cross-sectional view in drawing "C" is obtained from the plane containing line CC in the corresponding drawing "B".

[0023] Figure 1A The line AA of wafer 100 is shown (see Figure 1B A cross-sectional view of the substrate 10 and the overlay. Figure 1B yes Figure 1A and Figure 1C A top view of wafer 100. Figure 1C The CC along wafer 100 is shown (see Figure 1B Cross-sectional view of ). Figure 1BThe wafer includes a first region 100A, a second region 100B, and a third region 100C. The first region 100A will have metallic features including metal lines and vias formed at a first spacing, and the second region 100B will have metallic features including metal lines and vias formed at a second spacing. In other words, the spacing between lines and / or the width of the lines will be different in the first region 100A and the second region 100B. An optional third region 100C is a region in which no metal lines are formed. The wafer may have multiple regions of each of the first region 100A, the second region 100B, and the third region 100C.

[0024] The substrate 10 may be formed of a semiconductor material such as silicon or silicon-germanium. According to some embodiments of this disclosure, the substrate 10 is a crystalline semiconductor substrate, such as a crystalline silicon substrate, a crystalline silicon-carbon substrate, a crystalline silicon-germanium substrate, a III-V compound semiconductor substrate, etc. An active device 12 is formed on the top surface of the substrate 10, and the active device 12 may include a transistor.

[0025] A dielectric layer 14 is formed on the substrate 10. According to some embodiments of this disclosure, the dielectric layer 14 is an intermetallic dielectric (IMD) or an interlayer dielectric (ILD), which may be formed of a dielectric material, for example, with a dielectric constant (k value) less than 3.8, less than about 3.0, or less than about 2.5. The dielectric layer 14 may include a silicon oxide layer, such as silicon oxide formed from tetraethyl orthosilicate (TEOS). According to some embodiments of this disclosure, conductive features 16 are formed in the dielectric layer 14, which may be metallic features such as copper wires or tungsten contact plugs. In some embodiments, an etch stop layer 26 is formed on the dielectric layer 14. The etch stop layer 26 may be formed of a dielectric material such as silicon carbide, silicon nitride, silicon carbide, silicon oxynitride, etc. In some embodiments, the etch stop layer 26 may be omitted.

[0026] A dielectric layer 28 is further formed over the etch stop layer 26. The dielectric layer 28 may be an IMD layer formed of a dielectric material, for example, with a dielectric constant (k value) less than 3.8, less than about 3.0, or less than about 2.5. The dielectric layer 14 may include a silicon oxide layer, such as silicon oxide formed from TEOS. The dielectric layer 28 may be a carbon-containing compound and may have pores therein. According to an alternative embodiment of this disclosure, the dielectric layer 28 is a non-low-k dielectric layer with a k value equal to or greater than 3.8. Throughout this specification, layer 28 is also referred to as target layer 28. According to some embodiments of this disclosure, a plurality of patterned features are formed within target layer 28.

[0027] According to other embodiments, layer 28 is a semiconductor substrate. According to these embodiments of the present disclosure, one or more additional layers beneath layer 28 may be omitted. Therefore, according to these embodiments, as... Figure 1A The substrate 10, dielectric layer 14 and conductive feature 16 shown may not be present.

[0028] A hard mask 30 exists above the target layer 28, which can be formed from a dielectric material such as silicon oxide (e.g., an oxide formed from TEOS), silicon nitride, nitrogen-free antireflective coating (NFARC, an oxide), silicon carbide, silicon oxynitride, silicon oxycarbide, etc. Formation methods include plasma-enhanced chemical vapor deposition (PECVD), high-density plasma (HDP) deposition, chemical vapor deposition (CVD), atomic layer deposition (ALD), etc.

[0029] In some embodiments, the hard mask 30 may include multiple layers (see, for example...) Figure 19A and Figure 19B The bottom layer of the hard mask 30 can be a nitrogen-free antireflective coating (NFARC) and can be between approximately 6 nm and 30 nm thick. The next layer can be a hard mask material such as silicon nitride, titanium nitride, tantalum nitride, etc., and can be formed between approximately 20 nm and 25 nm thick. The next layer can be an oxide layer, such as silicon oxide, silicon carbide, silicon carbide, etc. formed by TEOS, and can be formed between approximately 20 nm and approximately 30 nm thick.

[0030] A hard mask 32 is formed on top of a hard mask 30. According to some embodiments of this disclosure, the hard mask 32 is in contact with the hard mask 30, and no additional layer is formed between the hard mask 32 and the hard mask 30. According to some embodiments of this disclosure, the hard mask 32 is formed of amorphous silicon or another material having high etch selectivity relative to the underlying hard mask 30. For example, when etching the hard mask 32, the etch selectivity (the ratio of the etch rate of the hard mask 32 to the etch rate of the hard mask 30) is greater than about 20 or greater than about 50. Throughout this specification, the hard mask 32 is also referred to as a core layer 32.

[0031] Figure 1A , Figure 1B and Figure 1C The first photolithography process is also shown. A photomask 33 is formed on the core layer 32, which has been patterned to form openings 35. 1A and 35 1BIt should be understood that, unless otherwise stated, any reference to photomasks used herein may include a single photoresist or a three-layer photomask. Therefore, photomask 33 may include a single photoresist or a three-layer photomask. The three layers may include a lower layer (sometimes referred to as the bottom layer), an intermediate layer above the lower layer, and an upper layer above the intermediate layer. According to some embodiments of this disclosure, the lower and upper layers are formed of a photoresist (which is formed of an organic material). The intermediate layer may be formed of an inorganic material, which may be a nitride (e.g., silicon nitride), an oxynitride (e.g., silicon oxynitride), an oxide (e.g., silicon oxide), etc. The intermediate layer has high etch selectivity relative to the upper and lower layers, thus the upper layer is used as an etch mask for patterning the intermediate layer, and the intermediate layer is used as an etch mask for patterning the lower layer.

[0032] For example, in a photolithography process, a photomask 33 is applied and patterned to form an opening 35 in a first region 100A. 1A And an opening 35 is formed in the second region 100B. 1B The corresponding steps are shown as follows Figure 25 Step 205 in the process flow shown. According to some embodiments of this disclosure, openings 351 are located between areas that are strips parallel to each other in the top view. Multiple openings can be formed separately from each other with different widths and different spacings. Relative to Figure 3A , Figure 3B and Figure 3C The spacing and width of the first region 100A and the second region 100B are discussed in more detail. The opening 35 in the first region 100A... 1A Opening 35 in the second region 100B 1B This indicates the intersection region where metallic features (e.g., metal lines) can be formed along the x-direction. Opening 35 in the first region 100A. 1A It can have a length dimension D between approximately 44 nm and approximately 100 nm. 1A and the width dimension D between approximately 6nm and approximately 20nm 2A Opening 35 in the second region 100B 1B It can have a length dimension D between approximately 50 nm and approximately 120 nm. 1B and the width dimension D between approximately 6nm and approximately 20nm 2B Size D 2A It can be related to size D 2B Same value. Adjacent openings 35 in region 100A. 1A The spacing between them can be between approximately 20 nm and approximately 38 nm. Adjacent openings 35 in the second region 100B. 1B The spacing between them can be larger than the spacing in the first region 100A, and can be between approximately 25 nm and approximately 45 nm. As described above, refer to the following... Figure 3A , Figure 3B and Figure 3C The spacing is shown.

[0033] exist Figure 2A , Figure 2B and Figure 2C In the process, an etching process is performed to remove the openings 35 in the photomask 33. 1A and opening 35 1B Extending into the mandrel layer 32. The corresponding steps are shown as follows. Figure 25 Step 210 in the process flow shown. Then, for example, the remaining photomask 33 is removed in an ashing step. The resulting structure is... Figure 2A , Figure 2B and Figure 2C As shown in the figure. The etching is anisotropic, resulting in openings 35 in the core layer 32. 1A and opening 35 1B It has the same or similar dimensions as the corresponding opening in photomask 33. According to some embodiments of this disclosure, opening 35... 1A and opening 35 1B Rectangular openings may be included. In some embodiments, a trimming process may be used prior to etching the mandrel layer 32, wherein the trimming process is an anisotropic etching process to further reduce the width of each pattern of the photomask 33.

[0034] According to some embodiments, etching of the mandrel layer 32 is performed in a process chamber (not shown) containing process gases such as CF4, HBr, Cl2, O2, or combinations thereof. The flow rate of the process gas can be in the range of about 3 sccm to about 500 sccm. The pressure of the process gas can be in the range of about 5 mTorr to about 50 mTorr. It should be understood that the values ​​referenced in this disclosure are examples and different values ​​may be used.

[0035] exist Figure 3A , Figure 3B and Figure 3C The second photolithography process is shown in the diagram. This is done on top of the core layer 32 and at the opening 35. 1A and 35 1B A photomask 34 is formed, which has been patterned as a photomask 34A in a first region 100A, a photomask 34B in a second region 100B, and a photomask 34C in a third region 100C. The corresponding steps are shown as follows. Figure 25 Step 205 in the process flow shown (following step 210): An opening 35 is formed in the first region 100A in the photomask 34. 2A Opening 35 in the second region 100B 2B According to some embodiments of this disclosure, opening 35 2Aand opening 35 2B The top view shows strips that are parallel to each other. The opening is 35 degrees. 1A and 35 1B Oriented in the x direction, opening 35 degrees 2A and 35 2B Towards the y direction.

[0036] Patterned features, such as stripes, are formed in photomasks 34A and 34B with two different widths and two different spacings. The spacing P of the patterned features in photomask 34A... 1A It can be between approximately 20 nm and approximately 38 nm. The width W of the patterned features of photomask 34A... 1A The spacing P of the patterned features of the photomask 34B can be between approximately 15 nm and approximately 45 nm. 1B It can be between approximately 25 nm and approximately 45 nm. The width W of the patterned features of the photomask 34B is... 1B It can be between approximately 20nm and approximately 55nm. Spacing P 1B Can compare spacing P 1A It increased by approximately 5nm to approximately 20nm. Width W 1B It can be compared to the width W 1A It increased by approximately 5nm to approximately 30nm. The photomask 34A has a relatively small spacing P. 1A and width W 1A It can be used to form a structure in subsequent processes that is based on a relatively large spacing P. 1B and width W 1B The formed metal lines are closer to each other.

[0037] It should be understood that although this description includes two different widths and two different spacings, any number of widths and spacings can be used by employing the process described below.

[0038] exist Figure 4A and Figure 4B In the process, an etching process is performed to transfer the patterns in photomasks 34A and 34B to mandrels 32A and 32B respectively, and to open the opening 35. 2A and opening 35 2B Extending into the mandrel layer 32. Mandrel 32B is in the second region 100B and corresponds to a fine pitch, while mandrel 32A is in the first region 100A and corresponds to an even finer pitch. One or more larger mandrel blocks 32C may also be etched into the mandrel layer 32. The corresponding steps are shown as follows: Figure 25 Step 210 in the process flow shown. Then, for example, the remaining photomask 34 is removed in an ashing step. The resulting structure is... Figure 4A and Figure 4B As shown in the diagram. It can be used in conjunction with the above regarding... Figure 2A , Figure 2B and Figure 2C The similar processes and materials discussed are used to complete the etching.

[0039] In some embodiments, a baking process may be performed to bake wafer 100. In embodiments using a baking process, the baking process is performed for a period of time between about 5 minutes and about 20 minutes. The baking temperature may be in the range between about 250°C and about 500°C. The baking process may restore or repair the material of mandrels 32A, 32B, and 32C, which may have been generated to etch.

[0040] It should be understood that although the above-described patterning process uses a first patterning step to form lines and openings in the mandrel layer 32 in one direction and a second patterning step to form lines and openings in the mandrel layer 32 in the vertical direction, these steps may be combined in some embodiments. They may also be performed in reverse order. In some embodiments, individual layers above the mandrel layer (e.g., the lower layer of photomask 34) may first be patterned in each direction to form a combined pattern mask, and then the mandrel layer may be etched using the combined pattern mask.

[0041] Figure 5A It is along Figure 5B The vertical cross-section of line AA is shown, and Figure 5B It is along Figure 5A The horizontal cross-section of line BB shown (not the top view). Figure 6B , Figure 7B , Figure 8B , Figure 11B , Figure 12B , Figure 13B , Figure 16B , Figure 17B , Figure 18B , Figure 19B , Figure 20B and Figure 21B A similar horizontal cross-section was also used in [the text]. Figure 5A and Figure 5B In this process, a spacer layer 38 is formed on wafer 100 in a blanket manner. The corresponding steps are shown as follows: Figure 25 Step 215 in the process flow shown. The material of the spacer layer 38 can be selected to have high etch selectivity relative to the hard mask 30. For example, the material of the spacer layer 38 can be selected from AlO, AlN, AlON, TaN, TiN, TiO, Si, SiO2, SiN, and other metals and metal alloys.

[0042] For example Figure 5A and Figure 5BAs shown, the spacer layer 38 is formed as a conformal layer, and the thicknesses of the horizontal and vertical portions of the spacer layer 38 are close to each other, for example, the difference is less than about 20%. The spacer layer 38 can be deposited using a conformal deposition method (e.g., CVD or ALD). According to some embodiments, the thickness T of the spacer layer 38 above the mandrel 32A is... 1A In Approximate With the agreement Within the range, for example, approximately With the agreement Between. The thickness T of the spacer layer 38 above the mandrel 32B. 1B With thickness T 1A The same. Because the spacing in the first region 100A is different from the spacing in the second region 100B, the thickness T can be changed by altering the spacer layer 38. 1B Greater than thickness T 1A As described in this article. Figure 5B As shown, the spacer layers 38 may be joined together across the gap 38g. In other embodiments, the spacer layers 38 may not be joined together across the gap 38g.

[0043] exist Figure 6A and Figure 6B In this process, a photomask 142 can be formed on wafer 100 and patterned to expose a first region 100A while remaining on a second region 100B. The corresponding steps are shown as follows: Figure 25 Step 220 in the illustrated process flow. In some embodiments, the photomask 142 may be a three-layer photomask, including a lower layer 138 and an intermediate layer 140. The upper layer is patterned and used to pattern the intermediate layer 140, and then the intermediate layer 140 is used to pattern the lower layer 138. The materials and processes used to form and pattern the photomask 142 may be similar to those described above. Figure 1A and Figure 1B The materials and processes discussed will not be repeated here.

[0044] exist Figure 7A and Figure 7B In the process, a trimming process is performed to reduce the thickness T of the spacer layer 38 in the first region 100A. 1A The corresponding steps are shown as follows Figure 25 Step 225 in the illustrated process flow. The trimming process can be performed using either dry or wet etching, which will isotropically erode the exposed spacer layer 38 in a substantially uniform manner. In the case of using dry etching, example etchants used to trim the spacer layer 38 may include fluorine-reactive gases, such as fluorocarbon-based etchants (C... x F yProcess gases include NF3, SF6, Cl2, and HBr. Other process gases can be combined with fluorocarbon-based etchants, such as oxygen (O2), nitrogen (N2), argon (Ar), and combinations thereof. In this embodiment, the process gas used to pattern the spacer layer 38 may be hydrogen-free. In the case of wet etching, example etchants used to trim the spacer layer 38 may include an HF solution or another suitable etchant.

[0045] The finishing process can be carried out from the thickness T of the spacer layer 38. 1A Remove approximately Peace Treaty Between, for example, about Peace Treaty Between. The resulting thickness T 2A It can be done in about Peace Treaty Between, for example, about Peace Treaty between.

[0046] exist Figure 8A and Figure 8B In this process, photomask 142 can be removed using any suitable technique. The corresponding steps are shown as follows: Figure 25 Step 230 in the illustrated process flow. In some embodiments, the photomask 142 can be removed by cleaning or etching, and in other embodiments, an ashing process can be used to remove the photomask 142. The spacer layer 38 in the second region 100B has a thickness T. 1B Same thickness T 2B However, the spacer layer 38 in the first region 100A now has a thickness T greater than before. 1A Thinner and also thicker than T 2B Thinner thickness T 2A In this process, at the edge of the photomask 142 above the spacer layer 38, a height of T can be formed. 2B -T 2A The step, the height of which corresponds to the amount trimmed from the spacer layer 38 in the first region 100A.

[0047] Figure 9A and Figure 9B ,to Figure 12A and Figure 12B An optional process for forming a recovery material or sacrificial material on a portion of the spacer layer is shown. This can be accomplished as a wire cutting process to fill the portion of the spacer layer 38 that will ultimately cause a wire break in the subsequently formed metal wire. The corresponding steps are shown as follows. Figure 26Steps 260, 262, 264, and 266 in the illustrated process flow. These same processes can be used in any of the embodiments described herein, for example, before or after etching the spacer layer 38 to form the spacer.

[0048] Including cross-sectional views and top views Figure 9A and Figure 9B In this process, a photomask 152 is formed on and patterned on wafer 100. The upper layer 150 (or intermediate layer) of the photomask 152 is patterned to form openings 153, which correspond to the dicing regions of subsequently formed metal lines. The corresponding steps are shown as follows. Figure 26 Step 260 in the process flow shown. This can be used in conjunction with the above regarding... Figure 1A and Figure 1B The processes and materials discussed in photomask 34 are similar to those used to form and pattern photomasks 152, and will not be repeated here.

[0049] Including cross-sectional views and top views Figure 10A and Figure 10B In the middle, opening 153 extends into the lower layer 148 of photomask 152, exposing spacer layer 38. Opening 153 can be used in conjunction with the above-mentioned... Figure 1A and Figure 1B The processes and materials discussed are similar to those used in the extension. In some embodiments, spacer layer 38 may have been etched into spacers, and in some embodiments, mandrels 32A and 32B may have been removed, for example if the process is in... Figure 25 After step 235 or step 240. For example... Figure 10A and Figure 10B As shown, openings 153 may span multiple mandrels 32A and / or 32B. Additionally, it should be understood that although openings 153 are shown formed along the x-direction, they may also be formed in the vertical direction (y-direction) in the same step or in separate steps. The upper layer 150 of photoresist 152 may be removed in the process of patterning the lower layer 148, or may be removed by a separate etching process.

[0050] Including vertical and horizontal cross-sectional views Figure 11A and Figure 11B In this process, sacrificial material 154 (sometimes also called reverse material) is deposited on top of the substrate 148 and into the opening 153. The corresponding steps are shown as follows: Figure 26Step 264 in the illustrated process flow. In some embodiments, sacrificial material 154 is also deposited on intermediate layer 150. In other embodiments, intermediate layer 150 is removed prior to the deposition of sacrificial material 154. In various embodiments, sacrificial material 154 comprises inorganic materials. For example, sacrificial material 154 may be an inorganic oxide, such as titanium oxide, tantalum oxide, silicon oxide, etc. In some embodiments, the inorganic material is a low-temperature oxide (LTO). As used herein, the term "LTO" refers to an oxide deposited using a relatively low process temperature (e.g., 200°C or lower). In some embodiments, sacrificial material 154 may comprise a nitride, such as silicon nitride or silicon oxynitride, etc. Sacrificial material 154 may be selected to have sufficient etch selectivity for spacer layer 38 relative to the same etch process. For example, in some embodiments, the ratio of the etch rate of sacrificial material 154 to the etch rate of spacer layer 38 relative to the same etch process is at least 0.7.

[0051] The sacrificial material 154 can be formed using semiconductor film deposition processes such as CVD, PVD, and ALD. The semiconductor film deposition process can be a conformal process, forming on the sidewalls and bottom surface of the opening 153 (see [link to documentation]). Figure 10A and Figure 10B As deposition continues, portions of the sacrificial material 154 on the opposite sidewalls of the opening 153 can merge, thereby filling the opening 153. As a result of the semiconductor film deposition process, the top surface of the sacrificial material 154 may not be flat, such as... Figure 11A and Figure 11B As shown.

[0052] Including cross-sectional views and top views Figure 12A and Figure 12B In the etching process, the photomask 152 is removed and the sacrificial material 154 is trimmed. The corresponding steps are shown as follows: Figure 26 Step 266 in the illustrated process flow. First, a planarization process (e.g., chemical mechanical polishing (CMP), dry etching, a combination thereof, etc.) is performed to remove excess portion of the sacrificial material 154 outside the opening 153. In embodiments where the sacrificial material 154 is formed on an intermediate layer 150, the planarization process may also remove the intermediate layer 150. After the planarization process, the bottom layer 148 is exposed, and the top surfaces of the sacrificial material 154 and the bottom layer 148 may be planar and coplanar. In some embodiments, the planarization process may also remove divots formed in the sacrificial material 154.

[0053] Next, an ashing process is used to remove the underlayer 148. After removing the underlayer 148, the pillars of the sacrificial material 154 are retained. The remaining sacrificial material 154 masks selected areas of the spacer layer 38. In some embodiments, the sacrificial material 154 can extend from a first sidewall portion of the spacer layer 38 on a first mandrel 32A or 32B to a second sidewall portion of the spacer layer 38 on a second corresponding mandrel 32A or 32B.

[0054] The sacrificial material 154 can then be trimmed in the etch-back process to achieve the desired profile. In some embodiments, trimming the sacrificial material 154 causes it to recess below the top surface of the spacer layer 38, for example, below the top surfaces of the mandrels 32A and 32B. Trimming the sacrificial material 154 may expose a portion of the spacer layer 126 above the mandrel 124. In some embodiments, trimming the sacrificial material 154 may also reduce at least the cross-sectional area BB( Figure 12B The width of the sacrificial material 154 in ).

[0055] Trimming the sacrificial material 154 may include a dry etching process, or a combination of a dry etching process and a wet etching process. Embodiments of dry etching processes for trimming the sacrificial material 154 may include the use of a fluorocarbon-based etchant (e.g., CF4). Other process gases may be used in combination with fluorocarbon-based etchants, such as oxygen (O2), nitrogen (N2), argon (Ar), and combinations thereof. Embodiments of wet etching processes for trimming the sacrificial material 154 may include the use of dilute hydrofluoric acid as an etchant. The desired shape of the sacrificial material 154 may be achieved, for example, by controlling the concentration and duration of the trimming process.

[0056] Includes both vertical and horizontal cross-sectional views. Figure 13A and Figure 13B In this process, anisotropic etching is performed to remove the horizontal portions of the spacer layer 38, while the vertical portions of the spacer layer 38 are retained. The corresponding steps are shown as follows: Figure 25 Step 235 in the illustrated process flow. Hereinafter, the remaining portions of spacer layer 38 are referred to as spacers 40A and 40B, wherein spacer 40A is located in a first region 100A and spacer 40B is located in a second region 100B. In some embodiments, etching of spacer layer 38 utilizes a dry etching process using a suitable etchant (e.g., CH4, Cl2, combinations thereof, etc.). During the dry etching process, other process gases, such as nitrogen (N2), may be used in conjunction with the etchant. The dry etching process can be anisotropic and etch the exposed lateral portions of spacer layer 38 without significantly removing the vertical portions of spacer layer 38.

[0057] like Figure 13AAs shown, spacer 40A is on the side wall of mandrel 32A, and spacer 40B is on the side wall of mandrel 32B. (Reference) Figure 13B Spacers 40A and 40B may include longitudinal portions along the x and y directions and may be formed in various shapes. In some embodiments, spacers 40A and 40B may include longitudinal portions forming non-zero angles with respect to the x and y directions, or may include curved portions, circular portions, annular portions, etc.

[0058] In embodiments utilizing sacrificial material 154, spacers 41A and 41B comprise portions of spacer layers 38 on the sidewalls of mandrels 32A and 32B, respectively, and portions of sacrificial material 154 filling the gaps in the spacer layers 38. As a result, spacers 41A and 41B will define the wire cut within the subsequently formed metal wire.

[0059] Figure 14A and Figure 14B ,to Figure 16A and Figure 16B An optional holding process is shown for holding portions of the mandrel layer 32 to assist in patterning the underlying hard mask 30. In embodiments where a holding process is not used, an etching process can be used to remove portions of the exposed mandrels 32A and 32B. The corresponding steps are shown as follows. Figure 25 Step 240 in the process flow 200 shown. Optional holding processes include steps shown as steps 268, 270, and 272. Figure 27 Step 240 in the process flow shown. These same processes can be used to remove the mandrel in any of the embodiments described herein.

[0060] Including cross-sectional views and top views Figure 14A and Figure 14B In this process, a photomask 162 is formed on and patterned over wafer 100. The upper layer 160 (or intermediate layer) of the photomask 162 is patterned to form openings 163 corresponding to areas of the core layer 32 that should be removed. The covered areas (e.g., retaining areas 164) correspond to other wire cuts in subsequently formed metal lines. The corresponding steps are shown as follows: Figure 27 Step 268 in the process flow shown. This can be used in conjunction with the above regarding... Figure 1A and Figure 1B The processes and materials discussed in photomask 34 are similar to those used to form and pattern photomasks 162, and will not be repeated here.

[0061] Including vertical and horizontal cross-sectional views Figure 15A and Figure 15BIn this configuration, opening 163 extends into the lower layer 158 of photomask 162, exposing the core layer 32. Portions of spacers 40A and 40B are also exposed. The retained area of ​​the core layer 32 (retaining area 164) continues to be covered by photomask 162. This can be achieved using the methods described above. Figure 1A and Figure 1B The processes and materials discussed are similar to those used to extend the opening 163. The retaining region 164 may span multiple mandrels 32A and / or 32B and may also cover a portion of the mandrel layer 32C. The upper layer 160 of the photoresist 162 may be removed in the process of patterning the lower layer 158, or may be removed by a separate etching process.

[0062] Includes both cross-sectional and top-view views. Figure 16A and Figure 16B In the etching step, the mandrel layer 32 is selectively etched to remove the exposed mandrels 32A, 32B, and 32C, thereby forming an opening 43A in the first region 100A, an opening 43B in the second region 100B, and an opening 43C in the third region 100C. The corresponding steps are shown as follows: Figure 27 Step 272 in the illustrated process flow. According to some embodiments, etching is performed using wet etching or dry etching. The appropriate etchant may include an HF solution, or a mixture of NF3 and NH3 gases, and the suitable etchant depends on the material of the core layer 32. In embodiments where a holding process is not used to form the holding region 164, etching may be performed without using any photoresist to cover the wafer 100.

[0063] This process can achieve several different spacer widths. After the trimming process, the width and thickness T of spacer 40A are... 2A The width and thickness T of spacer 40B are roughly the same. 2B They are roughly the same. The width of spacer 41A is twice the width of spacer 40A plus the width between spindles 32A. Spacer 41C includes the width of spacer 40A or spacer 40B plus the width of holding region 164 in the third region 100C. Spacer 41C includes spacer 40A plus holding region 164.

[0064] Includes both cross-sectional and top-view views. Figure 17A and Figure 17B In this process, spacers 40A, 40B, 41A, 41B, and 41C together serve as a mask to etch the hard mask 30. The corresponding steps are shown as follows: Figure 25Step 245 in the illustrated process flow. A hard mask 30 is etched to include a patterned hard mask 30 in each of a first region 100A, a second region 100B, and a third region 100C. With the hard mask 30 patterned, an opening 44A is formed in the first region 100A, an opening 44B is formed in the second region 100B, and an opening 44C is formed in the third region 100C. Openings 44A, 44B, and 44C correspond to openings that will be formed in the target layer 28. Openings 44A, 44B, and 44C correspond to the spacing between openings in the target layer 28. Since spacers 40A and 40B can use different widths, the subsequently formed metal lines can have flexible spacing.

[0065] References include both cross-sectional and top views. Figure 18A and Figure 18B Similar to Figure 17A and Figure 17B The sacrificial material 154 is shown in another position, adjacent to the mandrel 32C and the associated holding region 164. By combining the above-described techniques, the spacer 41C may include the holding region 164, the spacer 40A, and the sacrificial material 154.

[0066] References include both cross-sectional and top views. Figure 19A and Figure 19B According to some embodiments, the hard mask layer 30 is shown as three distinct layers. (See above regarding...) Figure 1A In the discussion, mask 30A may be NFARC, mask 30B may be a hard mask, and mask 40A may be an oxide, etc. Each mask layer of the hard mask 30 may be etched sequentially to extend openings 43A, 43B, and 43C therein using a suitable etchant.

[0067] refer to Figure 20A and Figure 20B The openings 43A, 43B, and 43C in mask 30C are transferred to the underlying layer 30B. Any suitable technique can be used, such as a suitable etching process. The remaining spacer layer 38, sacrificial material 154, and mandrel layer 30 can also be removed by etching, grinding, or by a CMP process.

[0068] refer to Figure 21A and Figure 21B The openings 43A, 43B, and 43C in mask 30B are transferred to the underlying layer 30A. Any suitable technique can be used, such as a suitable etching process.

[0069] Figure 22A and Figure 22B It shows Figure 17A and Figure 17B Afterwards, or Figure 21A and Figure 21B Subsequent processes. Openings 44A, 44B, and 44C define the areas of target layer 28 that will be removed.

[0070] exist Figure 23A and Figure 23B In this process, a patterned hard mask 30 or 30A is used as an etching mask to etch the target layer 28, thereby forming trenches 46A and 46B. The corresponding steps are shown as follows: Figure 25 Step 250 in the illustrated process flow. In some embodiments, a mask layer may be deposited and patterned to protect the third region 100C before etching the target layer 28. Additional process steps may also be performed to define and etch the target layer 28 to form a via opening 48 beneath the trench 46. The etch stop layer 26 is also etched. The conductive feature 16 is exposed through the via opening 48. Next, the patterned hard mask 30 or 30A is removed. Alternatively, the patterned hard mask 30 or 30A is removed during or after subsequent planarization to form the metal line 50 and via 52, as shown. Figure 23A and Figure 23B As shown.

[0071] exist Figure 24A and Figure 24B In this process, the trench 46 and the through-hole opening 48 are filled with one or more conductive materials to form the metal wire 50 and the through-hole 52. The corresponding steps are shown as follows: Figure 25 Step 255 in the process flow shown. This formation can be achieved using a dual damascene process, wherein a conductive barrier layer, such as titanium nitride, titanium, tantalum nitride, tantalum, etc., is formed on the sidewalls and bottom of the trench 46 and the via opening 48. The remaining portions of the trench 46 and the via opening 48 are then filled with a conductive material, which may include copper or a copper alloy, or another conductive material. Chemical mechanical polishing (CMP) is then performed to remove the barrier layer and excess filler metal, forming the metal line 50 and the via 52, as shown. Figure 23A and Figure 23B As shown. Metal wire 50 and through-hole 52 are electrically connected to the conductive feature 16 below. (As illustrated...) Figure 24A As shown, CMP can stop on target layer 28, or on patterned hard masks 30A and 30B if they have not yet been removed.

[0072] According to an alternative embodiment of this disclosure, target layer 28 is a semiconductor substrate. Therefore, Figure 1A , Figure 1B and Figure 1C ,to Figure 24A and Figure 24B The process steps shown can be used to form trenches in the target layer 28 and fill the trenches with a dielectric material to form a shallow trench isolation (STI) region.

[0073] Figure 24B A top view of the metal line 50 formed in the target layer 28 is shown. The metal line 50 includes two spacings S1 and S2, with spacing S2 being larger than spacing S1. Spacing S2 is determined by the thickness T of the spacer 40B. 2B ( Figure 8A The spacing S1 can be adjusted by adjusting the trimming amount of the spacer layer 38 in the first region 100A, as described above. Therefore, embodiments of this disclosure offer the flexibility to adjust the spacing between metal lines to different values.

[0074] In the above about Figure 1A , Figure 1B and Figure 1C ,to Figure 25 In the process discussed, when the spacer layer 38 is formed (see...) Figure 5A and Figure 5B Due to the relative thickness of the spacer layers 38, there is a risk that the vertical supports of the spacer layers 38 may merge together in the first region 100A. Furthermore, due to the size and spacing of the spacer layers 38, when performing trimming processes (see...),... Figure 7A and Figure 7B The spacer layer 38 may suffer from a horning effect at a 90-degree angle, where the spacer layer 38 forms a sharp corner shape at the corner. This sharp corner shape may cause defects in subsequent patterning steps and the formation of the metal line 50.

[0075] In other embodiments, sharp corners may be reduced or eliminated. Figure 28A and Figure 28B ,to Figure 36 A cross-sectional view is shown of an intermediate stage in the formation of features such as metal wires according to some embodiments of the present disclosure. Figure 28A and Figure 28B ,to Figure 36 The process reduces or eliminates sharp corner effects. Unless otherwise stated, the materials and forming methods of the components in these embodiments are the same as those in… Figure 1A , Figure 1B and Figure 1C ,to Figure 25 The same components, indicated by the same reference numerals in the illustrated embodiments, are substantially the same. Therefore, they can be compared with those in the embodiments shown. Figure 1A , Figure 1B and Figure 1C ,to Figure 24A and Figure 24B The discussion of the illustrated embodiments contains information about Figure 28A and Figure 28B ,to Figure 36 Details of the manufacturing process and materials used for the same components shown.

[0076] Figure 28A It is along Figure 28B The vertical cross-section of line AA is shown, and Figure 28B It is along Figure 28A The horizontal cross-section of line BB shown (not the top view). Figure 29B , Figure 30B , Figure 31B and Figure 32B A similar horizontal cross section was also used. Figure 28A and Figure 28B This shows the process after depositing spacer layer 38 on mandrels 32A and 32B. Figure 5A and Figure 5B Wafer 100. The corresponding steps are shown as follows. Figure 36 Step 315 in the illustrated process flow. Therefore, step 305 is... Figure 25 Step 205 is essentially the same, and step 310 is essentially the same as step 210. Therefore, substrate 10, device 12, dielectric layer 14, conductive feature 16, etch stop layer 26, target layer 28, hard mask 30, and mandrels 32A and 32B refer to the components of the substrate 10, device 12, dielectric layer 14, conductive feature 16, etch stop layer 26, target layer 28, hard mask 30, and mandrels 32A and 32B. Figure 1A , Figure 1B and Figure 1C as well as Figure 2A , Figure 2B and Figure 2C Similar features are shown, and will not be repeated here.

[0077] You can use something like Figure 5A and Figure 5B The spacer layer 238 is formed using the same process and materials as spacer layer 38, but the spacer layer 238 is not deposited as thickly as spacer layer 38. Because spacer layer 238 is not deposited thickly, the risk of undesirable coalescence and sharp corner effects is reduced or eliminated. According to some embodiments, the thickness T of spacer layer 238 above mandrel 32A is... 3A In Approximate Peace Treaty Within the range, for example, approximately and Between. The thickness T of the spacer layer 238 above the mandrel 32B. 3B With thickness T 3A same.

[0078] exist Figure 29A and Figure 29B In this process, a photomask 142 can be formed on wafer 100 and patterned to expose a first region 100A while preserving a second region 100B. The corresponding steps are shown as follows: Figure 36 Step 320 in the process flow shown. This can be used in conjunction with the above regarding... Figure 6A and Figure 6BThe processes and materials discussed are similar to those used to manufacture photomasks 142, and will not be repeated here.

[0079] exist Figure 30A and 30B In the process, a trimming process is performed to reduce the thickness T of the spacer layer 38 in the first region 100A. 3A The corresponding steps are shown as follows Figure 36 Step 325 in the process flow shown. The finishing process can be performed using either dry etching or wet etching processes, as described above. Figure 7A and Figure 7B The trimming process can be adjusted from the thickness T of the spacer layer 38. 3A Remove approximately Peace Treaty Between, for example, about Peace Treaty Between. The resulting thickness T 4A It can be done in about Peace Treaty Between, for example, about Peace Treaty between.

[0080] exist Figure 31A and Figure 31B In this process, photomask 142 can be removed using any suitable technique, such as those mentioned above. Figure 8A and Figure 8B The discussed steps are shown below. Figure 36 Step 330 in the process flow shown. The thickness T of the spacer layer 238 in the second region 100B. 4B With thickness T 3B Same. However, the spacer layer 238 in the first region 100A now has a thickness T greater than before. 3A Thinner and also thicker than T 4B Thinner thickness T 4A In this process, at the edge of the photomask 142 above the spacer layer 38, a height of T can be formed. 4B -T 4A The step, the height of which corresponds to the amount trimmed from the spacer layer 238 in the first region 100A.

[0081] exist Figure 32A and Figure 32B In, similar to Figure 5A and Figure 5B The process and materials of spacer layer 38 are used to form the second spacer layer 239. The corresponding steps are shown as follows. Figure 36 Step 333 in the process flow shown. The thickness of the second spacer layer 239 can be approximately... and Between, for example, about and Between. Because the spacer layer 238 is trimmed in the first region 100A, the total thickness of the combined spacer layer 242 is different in the first region 100A and the second region 100B. According to some embodiments, the thickness T of the combined spacer layer 242 above the mandrel 32A is... 5A In Approximate Peace Treaty Within the range, for example, approximately Peace Treaty Between. The thickness T of the combined spacer layer 242 above the mandrel 32B. 5B In Approximate Peace Treaty Between, for example, about Peace Treaty between.

[0082] In some embodiments, the second spacer layer 239 may be formed using the same materials and processes as those used to form the first spacer layer 238. In such embodiments, even though the second spacer layer 239 may be formed of the same material as the spacer layer 238, an interface between the spacer layer 238 and the second spacer layer 239 may be observed. In some embodiments, the materials of the spacer layer 238 and the second spacer layer 239 may be formed such that a visible interface is not observed. In other embodiments, different materials and / or processes may be used to form the second spacer layer 239, in which case an interface is maintained between the spacer layer 238 and the second spacer layer 239.

[0083] Before etching the spacer layer, the above-mentioned procedures can be performed. Figure 9A and Figure 9B ,to Figure 12A and Figure 12B The process for forming the sacrificial material 154.

[0084] According to some embodiments, when the second spacer layer 239 is deposited, the second spacer layer 239 does not merge across the gap 239g. According to other embodiments, when the second spacer layer 239 is deposited, the second spacer layer 239 does merge across the gap 239g. Those skilled in the art will understand that other drawings can be modified according to such embodiments.

[0085] Includes both cross-sectional and top-view views. Figure 33A and Figure 33B In this process, anisotropic etching is performed to remove the horizontal portion of the combined spacer layer 242, while the vertical portion of the combined spacer layer 242 is retained. The corresponding steps are shown as follows: Figure 36Step 335 in the process flow shown. The remaining portions of the combined spacer layer 242 will hereinafter be referred to as spacers 40A and 40B, wherein spacer 40A is in the first region 100A and spacer 40B is in the second region 100B. The process for etching the combined spacer layer 242 can be used with… Figure 13A and Figure 13B The etching of spacer layer 38 in the middle uses similar materials and processes, and will not be repeated.

[0086] like Figure 33A As shown, spacer 40A is on the side wall of mandrel 32A and spacer 40B is on the side wall of mandrel 32B. (Reference) Figure 33B Spacers 40A and 40B may include longitudinal portions along the x and y directions and may be formed in various shapes. In some embodiments, spacers 40A and 40B may include longitudinal portions forming non-zero angles with respect to the x and y directions, or may include curved portions, circular portions, annular portions, etc.

[0087] Figure 34A and Figure 34B The formation of masks 158 / 162 with holding region 164 is shown. The formation of masks 158 / 162 is related to the above regarding... Figure 14A and Figure 14B ,to Figure 16A and Figure 16B The discussion is similar, and details will not be repeated. In the illustrated embodiment, Figure 34B The retaining region 164 is shown in the second region 100B. Masks 158 / 162 are used to protect the areas of the mandrel layer 32 that are not removed.

[0088] Includes both cross-sectional and top-view views. Figure 35A and Figure 35B In the etching step, mandrels 32A and 32B are selectively etched using masks 158 / 162 to remove mandrels 32A and 32B, thereby forming openings 43A between spacers 40A and 43B between spacers 40B. The corresponding steps are shown as follows: Figure 36 Step 340 in the process flow shown. Mandrels 32A and 32B can be used with the methods described above. Figure 16A and Figure 16B The similar processes and materials discussed for removal will not be repeated. The width and thickness T of spacer 40A. 5A The width and thickness T of spacer 40B are roughly the same. 5B They are roughly the same.

[0089] As in Figure 36 The process of using spacers 40A and 40B to etch the hard mask 30, as referenced in step 345 of the process flow, can be compared with the above-mentioned process. Figure 17A and Figure 17B ,to Figure 22A and Figure 22B The etching process for the hard mask 30 is the same and will not be repeated.

[0090] As in Figure 36 The process of using a hard mask 30 to etch the target layer 28, as referenced in step 350 of the process flow, can be compared with the above reference. Figure 23A and Figure 23B The etching process for target layer 28 described herein is the same and will not be repeated.

[0091] As in Figure 36 The process for forming the metal wire 50 and the through hole 52, as referenced in step 355 of the process flow, can be compared with the above reference. Figure 24A and Figure 24B The processes for forming metal wires 50 and 52 described above are the same and will not be repeated. Thus, similar to the above... Figure 24B The formed metal wire (e.g., metal wire 50) includes two intervals S1 and S2 (see...). Figure 24A Furthermore, the interval S2 is greater than the interval S1. The interval S2 is determined by the thickness T of the spacer 40B. 5B ( Figure 35A The spacing S1 can be adjusted by adjusting the trimming amount of the spacer layer 238 in the first region 100A, followed by the deposition of a second spacer layer on top of the spacer layer 238. Therefore, embodiments of this disclosure offer the flexibility to adjust the spacing between metal lines to different values.

[0092] In the above about Figure 1A , Figure 1B and Figures 1C to 27 and about Figure 28A and Figures 28B to 36 In the processes discussed, in each case, the spacer layer 38 is trimmed to achieve different thicknesses of the spacer layer 38 in different regions of wafer 100. The remaining figures depict other embodiments in which a pad layer is used over the spacer layer in selected regions of wafer 100. Furthermore, optional wire cutting processes are described, which can be applied to all processes of the embodiments described herein. The wire cutting process can use additional pad material to modify the spacer pattern to produce metal wire cuts. Additionally, optional patterning of the third region 100C is described, which can be applied to all processes of the embodiments described herein (similarly, optional patterning of the third region 100C can be omitted, as described with respect to the above figures).

[0093] Figure 37A and Figure 37B ,to Figure 48Cross-sectional views are shown of intermediate stages in the formation of features such as metal wires according to some embodiments of this disclosure. Unless otherwise stated, the materials and formation methods of the components in these embodiments are similar to those in… Figure 1A , Figure 1B and Figure 1C ,to Figure 27 The same components, indicated by the same reference numerals in the illustrated embodiments, are substantially the same. Therefore, they can be used in conjunction with... Figure 1A , Figure 1B and Figure 1C ,to Figure 27 The discussion of the illustrated embodiments contains information about Figure 37A and Figure 37B ,to Figure 48 Details of the manufacturing process and materials used for the same components shown.

[0094] Figure 37A It is along Figure 37B The vertical section of line AA shown, and Figure 37B yes Figure 37A A top view of wafer 100 in the image. Figure 37A and Figure 37B It shows the relationship with Figure 1A , Figure 1B and Figure 1C The structure is similar to the one shown. Therefore, substrate 10, device 12, dielectric layer 14, conductive feature 16, etch stop layer 26, target layer 28, and hard mask 30 refer to the structure shown. Figure 1A , Figure 1B and Figure 1C The features shown are similar to those shown, and will not be repeated.

[0095] Figure 37A and Figure 37B One or more photolithography processes are also shown. A first photolithography process can be performed and then the mandrel layer 32 can be patterned to form an opening therein in a first orientation, as described above regarding Figure 1A , Figure 1B , Figure 1C , Figure 2A , Figure 2B and Figure 2C As shown. The corresponding steps are shown as follows. Figure 48 Steps 405 and 410 in the illustrated process flow 400. After the first photolithography process, a second photolithography process can be performed to form an opening therein in a second orientation. A process similar to... Figure 3A and Figure 3B The photomask 34 is formed and patterned using the process and materials described. For example, in a photolithography process, the photomask 34 is applied and patterned as a photomask 34A in a first region 100A, a photomask 34B in a second region 100B, and a photomask 34C in a third region 100C. The corresponding steps are shown as follows: Figure 48 Step 405 of the process flow 400 shown. An opening 35A in the first region 100A and an opening 35B in the second region 100B are formed in the photomask 34. According to some embodiments of this disclosure, the top view shape of the openings 35 is strips parallel to each other. The photomask 34C in the third region 100C (in which no metal strips are formed) can be used to control the pattern loading effect. The photomask 34C can also be used for the above-mentioned... Figure 28A and Figure 28B ,to Figure 36 Examples discussed.

[0096] The patterned features (e.g., stripes) of photomasks 34A and 34B are formed with two different widths and two different spacings, and their dimensions and spacing are similar to those described above. Figure 1A and Figure 1B The discussion.

[0097] exist Figure 38A and Figure 38B In this process, an etching process is performed to extend openings 35A and 35B into the core layer 32, while transferring the patterns in photomasks 34A and 34B into the core layer 32 to form cores 32A and 32B, respectively. Core 32B is located in the second region 100B and corresponds to a finer pitch, while core 32A is located in the first region 100A and corresponds to an even finer pitch. Furthermore, a hard mask 32C is formed in the third region 100C. The corresponding steps are shown as follows: Figure 48 Step 410 in the process flow 400 shown. Then, for example, the remaining photomask 34 is removed in an ashing step. The resulting structure is... Figure 38A and Figure 38B As shown above. Similar to the above, it can be used... Figure 4A and Figure 4B The processes and materials used to perform etching, as discussed above, will not be repeated. In some embodiments, similar to those described above... Figure 4A and Figure 4B The process discussed can be a trimming process before etching the mandrel layer 32 and a baking process after etching the mandrel layer 32.

[0098] Figure 39A It is along Figure 39B The vertical cross-section of line AA is shown, and Figure 39B It is along Figure 39A The horizontal cross-section of line BB shown (not the top view). Figure 40B , Figure 41B , Figure 42B , Figure 43B and Figure 44B A similar horizontal cross section was also used in the middle. Figure 39A and Figure 39BThis illustrates the deposition of spacer layer 38 over mandrels 32A and 32B and over hard mask 32C. Figure 38A and Figure 38B Wafer 100. The corresponding steps are shown as follows. Figure 48 Step 415 in the process flow 400 shown.

[0099] Can be used with Figure 5A and Figure 5B The spacer layer 38 is formed using a similar process and materials, the difference being that the spacer layer 38 is not deposited as... Figure 5A and Figure 5B The spacer layer 38 is that thick. Because the spacer layer 38 is not deposited thickly, the risk of undesirable coalescence and sharp corner effects is reduced or eliminated. According to some embodiments, the thickness T of the spacer layer 38 above the mandrel 32A is... 6A In Approximate With the agreement Within the range, for example, approximately and Between. The thickness T of the spacer layer 38 above the mandrel 32B. 6B And the thickness T above the hard mask 32C 6C With thickness T 6A same.

[0100] exist Figure 40A and Figure 40B In this process, a photomask 142 can be formed on wafer 100 and patterned to expose the second region 100B while remaining on the first region 100A. The corresponding steps are shown as follows: Figure 48 Step 420 in the process flow 400 shown above can be used. Figure 6A and Figure 6B The processes and materials discussed for manufacturing photomask 142 will not be repeated here.

[0101] exist Figure 41A and Figure 41B In this process, a pad layer 144 is deposited on top of a photomask 142 and a spacer layer 38. The corresponding steps are shown as follows: Figure 48Step 425 in the process flow 400 shown. The liner layer may also be referred to as a spacer layer. In some embodiments, the intermediate layer 140 may be removed before depositing the liner layer 144, such that the liner layer 144 is formed directly on the uppermost surface of the substrate 138. The liner layer 144 may include an inorganic material. For example, the liner layer 144 may be an inorganic oxide, such as titanium oxide, tantalum oxide, silicon oxide, etc. In some embodiments, the inorganic material is a low-temperature oxide (LTO). In some embodiments, the liner layer 144 may include a nitride, such as silicon nitride or silicon oxynitride, etc. The liner layer 144 may be selected to have sufficient etch selectivity for the spacer layer 38 relative to the same etch process. For example, in some embodiments, the ratio of the etch rate of the liner layer 144 to the etch rate of the spacer layer 38 relative to the same etch process is at least 0.7.

[0102] The pad layer 144 can be formed using semiconductor film deposition processes such as CVD, PVD, and ALD. The semiconductor film deposition process can be a conformal process, forming on the sidewalls and bottom surface of the opening 35B. The pad layer 144 can be formed to a thickness T. 7B In Approximate With the agreement Between, but other values ​​can be expected and used.

[0103] exist Figure 42A and Figure 42B In this process, an ashing process or a wet etching process is used to remove the underlying layer 138. The corresponding steps are shown as follows: Figure 48 Step 430 of the process flow 400 shown. When the bottom layer 138 is removed, the padding layer 144 above the bottom layer 138 is also removed. The padding layer 144 remains above the spacer layer 38 in the second region 100B. In some embodiments, only a portion of the padding layer 144 remains on the sidewall of the opening 35B (and in some embodiments, the bottom surface). The remaining portion of the padding layer 144 is used to pad the width of the spacer layer 38 in the second region 100B.

[0104] exist Figure 42A and Figure 42B The image also shows residue 146 remaining on the third region 100C. Residue 146 can generate a self-removable photomask 142 and / or a padding layer 144. The cleaning process may individually damage the padding layer 144, thus masking the first region 100A and the second region 100B to clean residue 146. In some embodiments, a separate cleaning process is not required, and residue 146 can be cleaned in a continuous process step. Specifically, if a sacrificial material 154 is formed (e.g., regarding...), Figure 9A and Figure 9B ,to Figure 12A and Figure 12BAs described, a separate photomask 152 is not required for cleaning (e.g., regarding...). Figure 43A and Figure 43B (as described), because it can be used Figure 9A and Figure 9B ,to Figure 11A and Figure 11B Photomask 152.

[0105] If a residue removal process is performed, then in Figure 43A and 43B In this process, a photomask 152 is formed on wafer 100 and patterned to expose the third region 100C and the residue 146. The corresponding steps are shown as follows: Figure 48 Step 435 in the process flow 400 shown. This can be used in conjunction with the above regarding... Figure 6A and Figure 6B The processes and materials used to form and pattern photomasks 152 are similar to those discussed for photomask 142, and will not be repeated here.

[0106] exist Figure 44A and Figure 44B In this process, a reverse etching process can be used to remove residue 146. The corresponding steps are shown as follows: Figure 48 Step 440 in the illustrated process flow 400. In some embodiments, the etch-back process may utilize a dry (e.g., plasma) etching process, a wet etching process, or a combination thereof. The plasma etching process may include the use of fluorocarbons (C... x F y ) gas, chlorofluorocarbons (C x Cl y F z ) gas, carbon chloride (C x Cl y The wet etching process may include the use of one or more solutions of the following: Standard Clean-1 (SC1), Standard Clean-2 (SC2), sulfuric acid-hydrogen peroxide mixture (SPM), dilute hydrofluoric acid (dHF), hydrogen peroxide (H2O2), buffered oxide etch (BOE) solution, hydrogen chloride (HCl) acid, etc., or combinations thereof. The temperature of the solution may be in the range of about 20°C to about 90°C, and the duration of substrate immersion in the solution may be in the range of about 10 seconds to about 120 seconds. In some embodiments, the back etching process may remove the intermediate layer 150 of the photomask 152 (e.g., gas, etc.). Figure 44A and Figure 44B (as shown) and / or the lower layer 148. In some embodiments, the lower layer 148 may be removed using an ashing process and / or one or more cleaning processes.

[0107] Before etching spacer layer 38 and combined spacer layer 244, the above-mentioned procedures can be performed. Figure 9A and Figure 9B ,to Figure 12A and Figure 12B The process for forming the sacrificial material 154.

[0108] Includes both cross-sectional and top-view views. Figure 45A and Figure 45B In this process, anisotropic etching is performed to remove the horizontal portions of the spacer layer 38 in the first region 100A and the combined spacer layer 38 and the pad layer 144 (together forming the combined spacer layer 244) in the second region 100B, while the vertical portions of the spacer layer 38 and the combined spacer layer 244 are retained. The corresponding steps are shown as follows: Figure 48 Step 445 in the process flow 400 shown. In the following text, the remainder of the spacer layer 38 in the first region 100A is referred to as spacer 40A, and the remainder of the combined spacer layer 244 in the second region 100B is referred to as spacer 40B. The process for etching the combined spacer layer 242 can be used with... Figure 13A and Figure 13B The etching of spacer layer 38 in the middle uses similar materials and processes, and will not be repeated here.

[0109] like Figure 45A As shown, spacer 40A is on the sidewall of mandrel 32A, and spacer 40B is on the sidewall of mandrel 32B. In some embodiments, hard mask 32C may also have spacers 40A and 40B formed on its sidewalls. (See reference) Figure 45B Spacers 40A and 40B may include longitudinal portions along the x and y directions and may be formed in various shapes. In some embodiments, spacers 40A and 40B may include longitudinal portions forming non-zero angles with respect to the x and y directions, or may include curved portions, circular portions, annular portions, etc.

[0110] Figure 46A and Figure 46B The formation of masks 158 / 162 with holding region 164 is shown. The formation of masks 158 / 162 is similar to that described above. Figure 14A and Figure 14B ,to Figure 16A and Figure 16B The details discussed will not be repeated here. In the illustrated embodiment, Figure 46B The retaining region 164 is shown in the second region 100B. Masks 158 / 162 are used to protect the areas of the mandrel layer 32 that are not removed.

[0111] Includes both cross-sectional and top-view views. Figure 47A and Figure 47BIn the etching step, mandrels 32A and 32B are selectively etched using masks 158 / 162 to remove mandrels 32A and 32B, thereby forming an opening 43A between spacers 40A and an opening 43B between spacers 40B. In some embodiments, hard mask 32C is also removed, thereby forming an opening 43C (indicated in parentheses) between spacers 40A and spacers 40B in the third region 100C. The corresponding steps are shown as follows: Figure 48 Step 450 in the process flow 400 shown. Mandrels 32A and 32B, and hard mask 32C can be used in accordance with the above-mentioned... Figure 16A and Figure 16B The processes and materials discussed for removal will not be repeated. The width T of spacer 40A. 8A With thickness T 6A Roughly the same. The width T of spacer 40B 8B With thickness T 6B +T 7B Broadly the same (minus the parts from about) Figure 45A and Figure 45B The loss from the spacer etching process is approximately and between).

[0112] Figure 48 The remaining processes and related Figure 25 The described processes are similar and can be performed using similar processes and materials, therefore they will not be repeated. For example, such as... Figure 48 The steps shown in step 455 of the process flow 400 are similar to those shown in the example. Figure 25 The steps in step 245 of the process flow shown are similar; for example... Figure 48 The steps shown in step 460 of the process flow 400 are similar to those shown in the example. Figure 25 The steps in step 250 of the process flow shown are similar; and as shown Figure 48 The steps shown in step 465 of the process flow 400 are similar to those shown in the example. Figure 25 The steps in step 255 of the process flow shown are similar. Therefore, similar to the above regarding... Figure 24A and Figure 24B The metal wire being discussed (e.g., metal wire 50) comprises two intervals S1 and S2, with interval S2 being larger than interval S1.

[0113] Figure 49A and Figure 49B ,to Figure 55 Cross-sectional views are shown of intermediate stages in the formation of features such as metal wires according to some embodiments of this disclosure. Unless otherwise stated, the materials and formation methods of the components in these embodiments are similar to those in… Figure 1A , Figure 1B and Figure 1C ,to Figure 27 The same components, indicated by the same reference numerals in the illustrated embodiments, are substantially the same. Therefore, they can be referred to in the following... Figure 1A , Figure 1B and Figure 1C ,to Figure 27 The discussion of the illustrated embodiments contains information about Figure 49A and Figure 49B ,to Figure 55 Details of the manufacturing process and materials used for the same components shown.

[0114] Figure 49A It is along Figure 49B The vertical cross-section of line AA is shown, and Figure 49B It is along Figure 49A The horizontal cross-section of line BB is shown. Figure 50B and Figure 51B A similar horizontal cross section was also used in the middle. Figure 49A and Figure 49B This illustrates the deposition of spacer layer 38 over mandrels 32A and 32B and over hard mask 32C, and the deposition of liner layer 144 over spacer layer 38. Figure 39A and Figure 39B Wafer 100. The corresponding steps are shown as follows. Figure 55 Step 620 in the process flow shown. Therefore, step 605 is... Figure 48 Step 405 is essentially the same, step 610 is essentially the same as step 410, and step 615 is essentially the same as step 415. Therefore, substrate 10, device 12, dielectric layer 14, conductive feature 16, etch stop layer 26, target layer 28, hard mask 30, mandrels 32A and 32B, and hard mask 32C refer to the components of the substrate 10, device 12, dielectric layer 14, conductive feature 16, etch stop layer 26, target layer 28, hard mask 30, mandrels 32A and 32B, and hard mask 32C. Figure 37A and Figure 37B ,as well as Figure 38A Similar features to those shown in Figure 38 will not be repeated here. According to some embodiments, the thickness T of the spacer layer 38 above the mandrels 32A and 32B and the hard mask 32C... 9A In Approximate With the agreement Within the range, for example, approximately With the agreement Between, but other values ​​can be expected and used.

[0115] The liner layer 144 is deposited on top of the spacer layer 38. The corresponding steps are shown as follows: Figure 55 Step 620 in the process flow 600 shown. The liner layer can also be called a spacer layer. It can be used in accordance with the above regarding... Figure 41A and Figure 41BThe similar processes and materials used to form the liner layer 144 discussed herein will not be repeated. The liner layer 144 may be formed to a thickness T. 10A In Approximate With the agreement Between, but other values ​​can be expected and used.

[0116] exist Figure 50A and Figure 50B In this process, a photomask 142 can be formed on wafer 100 and patterned to expose a first region 100A while remaining on a second region 100B. The corresponding steps are shown as follows: Figure 55 Step 625 in the process flow 600 shown. This can be used in conjunction with the above regarding... Figure 6A and Figure 6B The similar processes and materials discussed for manufacturing photomasks 142 will not be repeated.

[0117] exist Figure 51A and Figure 51B The portion of the pad layer 144 exposed from the photomask 142 can be removed using any suitable technique (e.g., wet etching or dry etching (e.g., plasma etching), or a combination thereof). The corresponding steps are shown as follows: Figure 55 Step 630 in the process flow 600 shown. The plasma etching process may include the use of fluorocarbons (C... x F y ) gas, chlorofluorocarbons (C x Cl y F z The wet etching process may include the use of one or more solutions of the following: Standard Clean-1 (SC1), Standard Clean-2 (SC2), sulfuric acid-hydrogen peroxide mixture (SPM), dilute hydrofluoric acid (dHF), hydrogen peroxide (H2O2), buffered oxide etching (BOE) solution, hydrogen chloride (HCl) acid, etc., or combinations thereof. The solution temperature may be in the range of about 20°C to about 90°C, and the substrate immersion time in the solution may be in the range of about 10 seconds to about 120 seconds.

[0118] exist Figure 52A and Figure 52B In this process, an ashing process or a wet etching process is used to remove the photomask 142, and the spacer layer and the pad layer are etched to form spacers. The corresponding steps are shown as follows: Figure 55 Steps 635 and 640 in the process flow 600 shown. After removing the photomask 142, the padding layer 144 remains on top of the spacer layer 38 in the second region 100B. The padding layer 144 is used to pad the width of the spacer layer 38 in the second region 100B.

[0119] Before etching spacer layer 38 and combined spacer layer 244, the above-mentioned procedures can be performed. Figure 9A and Figure 9B ,to Figure 12A and Figure 12B The process for forming the sacrificial material 154.

[0120] In addition Figure 52A and Figure 52B In this process, anisotropic etching is performed to remove the horizontal portions of the spacer layer 38 in the first region 100A and the combined spacer layer 38 and the pad layer 144 (together forming the combined spacer layer 244) in the second region 100B, while the vertical portions of the spacer layer 38 and the combined spacer layer 244 are retained. The corresponding steps are shown as follows: Figure 55 Step 640 in the process flow 600 shown. In the following text, the remainder of the spacer layer 38 in the first region 100A is referred to as spacer 40A, and the remainder of the combined spacer layer 244 in the second region 100B is referred to as spacer 40B. The process for etching the combined spacer layer 242 can be used with... Figure 16A and Figure 16B The etching of spacer layer 38 in the middle uses similar materials and processes, and will not be repeated here.

[0121] like Figure 52A As shown, spacer 40A is on the sidewall of mandrel 32A, and spacer 40B is on the sidewall of mandrel 32B. In some embodiments, hard mask 32C may also have spacers 40A and 40B formed on its sidewalls. (See reference) Figure 52B Spacers 40A and 40B may include longitudinal portions along the x and y directions and may be formed in various shapes. In some embodiments, spacers 40A and 40B may include longitudinal portions forming non-zero angles with respect to the x and y directions, or may include curved portions, circular portions, annular portions, etc. Since the padding layer 144 in the first region 100A is removed, the hard mask 32C may also have a stepped upper surface. The height of spacer 40B may also be approximately greater than the height of spacer 40A. to approximately

[0122] Figure 53A and Figure 53B The formation of masks 158 / 162 with holding region 164 is shown. The formation of masks 158 / 162 is related to the above regarding... Figure 14A and Figure 14B ,to Figure 16A and Figure 16B The discussion is similar, and the details will not be repeated. In the illustrated embodiment, Figure 53BThe retaining region 164 is shown in the second region 100B. Masks 158 / 162 are used to protect the areas of the mandrel layer 32 that are not removed.

[0123] Includes both cross-sectional and top-view views. Figure 54A and Figure 54B In the etching step, mandrels 32A and 32B are selectively etched to remove them, thereby forming an opening 43A between spacers 40A and an opening 43B between spacers 40B. In some embodiments, hard mask 32C is also removed, thereby forming an opening 43C (indicated in parentheses) between spacers 40A and spacers 40B in the third region 100C. The corresponding steps are shown as follows: Figure 55 Step 645 in the process flow 600 shown. Mandrels 32A and 32B, and hard mask 32C can be used in accordance with the above... Figure 8A and Figure 8B The similar processes and materials discussed for removal will not be repeated. The width T of spacer 40A. 11A With thickness T 9A Roughly the same. The width T of spacer 40B 11B With thickness T 9A +T 10A Roughly the same (minus the parts from about) Figure 52A and Figure 52B The loss from the spacer etching process is approximately and between).

[0124] Figure 55 The remaining processes are similar to those regarding Figure 25 The same process is described, and can be performed using similar processes and materials, therefore it will not be repeated. For example, as... Figure 55 The steps in step 650 of the process flow 600 shown are the same as those shown in the example. Figure 25 The steps in step 245 of the process flow shown are similar; for example... Figure 55 The steps in step 655 of the process flow 600 shown are the same as those shown in the example. Figure 25 The steps in step 250 of the process flow shown are similar; and as shown Figure 55 The steps in step 660 of the process flow 600 shown are the same as those shown in the example. Figure 25 The steps in step 255 of the process flow shown are similar. Therefore, similar to the above regarding... Figure 24A and Figure 24B The formed metal wire (e.g., metal wire 50) includes two intervals S1 and S2, and the interval S2 is greater than the interval S1.

[0125] Embodiments of this disclosure advantageously provide the ability to have multiple spaced-apart mandrels and spacers of various sizes on the same wafer. After depositing an initial spacer layer over mandrels of different sizes, the spacer layer can be manipulated and modified so that a portion of the spacer layer is thicker over wider and / or more widely spaced mandrels, while a portion of the spacer layer is thinner over narrower and / or more closely spaced mandrels. By utilizing spacer layers with multiple widths, subsequently formed metal lines can have isolation between lines tailored to the width of the spacers. For example, this allows the wafer to have multiple types of line signal transmission and isolation within the same interconnect layer. Adjusting the spacer dimensions also allows for designs with different capacitive effects between adjacent metal lines. For example, in embodiments where capacitive leakage between metal lines is less of a concern in some areas of the device design than in other areas, the isolation spacing between metal lines in those areas can be smaller, while it can be larger in other areas. As a result, the spacing between the formed features can be adjusted, and the flexibility of feature formation is improved.

[0126] One embodiment is a method including patterning a first mandrel layer over a target layer to form a first mandrel and a second mandrel, the width of the first mandrel being greater than the width of the second mandrel. The method further includes depositing a spacer layer over the first and second mandrels. The method further includes forming a mask layer over the spacer layer and the first mandrel. The method further includes thinning the spacer layer over the second mandrel. The method further includes removing the mask layer. The spacer layer is etched to form a spacer etch mask, the spacer etch mask including a first spacer contacting a sidewall of the first mandrel and a second spacer contacting a sidewall of the second mandrel, the width of the first spacer being greater than the width of the second spacer. The method further includes etching the target layer based on the spacer etch mask. In one embodiment, the method may include depositing a second spacer layer over the first spacer layer after removing the mask layer. In one embodiment, the method may include forming a first metal line in a first region of the target layer corresponding to the first mandrel; and forming a second metal line in a second region of the target layer corresponding to the second mandrel, the second metal line being spaced further apart than the first metal line. In one embodiment, the method may include forming a second mask layer over a spacer layer and a first mandrel; patterning the second mask layer to expose a kerf region; depositing a sacrificial material in the kerf region; and removing the second mask layer, the sacrificial material becoming part of a spacer etching mask. In one embodiment, the method may include using a spacer etching mask to etch a hard mask beneath the spacer etching mask; and using the hard mask to etch a target layer. In one embodiment, the first spacer is wider than the second spacer. and between.

[0127] Another embodiment is a method including patterning a first mandrel layer over a target layer to form a first mandrel and a second mandrel, the width of the first mandrel being greater than the width of the second mandrel. A spacer layer is deposited over the first and second mandrels. A mask layer is formed over the spacer layer and the second mandrel, a portion of the spacer layer over the first mandrel being exposed from the mask layer. A pad layer is deposited over the mask layer and the exposed spacer layer, and the mask layer is removed. The method further includes etching the spacer layer and the pad layer over the first mandrel to form a first spacer etch mask including first spacers, and etching the spacer layer over the second mandrel to form a second spacer mask including second spacers, each of the first spacers being wider than the second spacers. The method further includes etching the target layer based on the first and second spacer etch masks. In one embodiment, the method includes forming a second mask layer after removing the mask layer; patterning the second mask layer to provide an opening in the second mask layer that exposes residue of the pad layer; and removing the residue of the pad layer. In one embodiment, the first spacer mask or the second spacer mask may include pillars of sacrificial material. In one embodiment, the pad layer and the sacrificial material may include the same material. In one embodiment, the target layer may include a semiconductor material. In one embodiment, patterning the first mandrel layer includes patterning the first mandrel layer to form a hard mask between the first mandrel and the second mandrel. In one embodiment, the method may include removing a horizontal portion of the pad layer from above the first mandrel, with the remaining vertical portion of the pad layer disposed on the sidewall of the spacer layer.

[0128] Another embodiment is a method comprising forming a first set of mandrels in a first region of a wafer and forming a second set of mandrels in a second region of the wafer, the spacing of the first set of mandrels being wider than the spacing of the second set of mandrels. The method further comprises depositing a first spacer layer over the first and second sets of mandrels, and depositing a second spacer layer over the first and second sets of mandrels. A mask is formed over the first region. The second spacer layer over the second set of mandrels in the second region is removed, and then the mask is removed. The method further comprises etching the first spacer layer in the second region and etching the first and second spacer layers in the first region to form a spacer mask including a first spacer in the first region and a second spacer in the second region, the first spacer being wider than the second spacer. The first and second sets of mandrels are removed. A target layer is etched beneath the spacer mask. In one embodiment, the method may include etching a hard mask layer directly beneath the spacer mask and using the hard mask layer to etch the target layer. In one embodiment, the spacing between adjacent lines in the first region is greater than the spacing between adjacent metal lines in the second region. In one embodiment, the second spacer layer may include a different material than the first spacer layer. In one embodiment, a spacer in the first spacer contacts one side of the hard mask, and a spacer in the second spacer contacts the opposite side of the hard mask. In one embodiment, the first spacer is higher than the second spacer.

[0129] The foregoing has outlined features of several embodiments to enable those skilled in the art to better understand various aspects of this disclosure. Those skilled in the art should understand that they can readily use this disclosure as a basis for designing or modifying other processes and structures to achieve the same purposes and / or the same advantages of the embodiments described herein. Those skilled in the art should also recognize that such equivalent constructions do not depart from the spirit and scope of this disclosure, and that various changes, substitutions, and modifications can be made herein without departing from the spirit and scope of this disclosure.

[0130] Example 1. A method for forming a semiconductor device, comprising: patterning a first mandrel layer over a target layer to form a first mandrel and a second mandrel, the width of the first mandrel being greater than the width of the second mandrel; depositing a spacer layer over the first mandrel and the second mandrel; forming a mask layer over the spacer layer and the first mandrel; thinning the spacer layer over the second mandrel; removing the mask layer; etching the spacer layer to form a spacer etching mask, the spacer etching mask including a first spacer contacting a sidewall of the first mandrel and a second spacer contacting a sidewall of the second mandrel, the width of the first spacer being greater than the width of the second spacer; and etching the target layer based on the spacer etching mask.

[0131] Example 2. The method according to Example 1 further includes: after removing the mask layer, depositing a second spacer layer on top of the first spacer layer.

[0132] Example 3. The method according to Example 1 further includes: forming a first metal wire in a first region of the target layer, the first region corresponding to the first mandrel; and forming a second metal wire in a second region of the target layer, the second region corresponding to the second mandrel, the second metal wire being spaced further apart from each other than the first metal wire.

[0133] Example 4. The method according to Example 1 further includes: forming a second mask layer over the spacer layer and the first mandrel; patterning the second mask layer to expose a cut line region; depositing a sacrificial material in the cut line region; and removing the second mask layer, the sacrificial material becoming part of the spacer etching mask.

[0134] Example 5. The method according to Example 1 further includes: using the spacer etch mask to etch a hard mask below the spacer etch mask; and using the hard mask to etch the target layer.

[0135] Example 6. The method according to Example 1, wherein the first spacer is wider than the second spacer. and between.

[0136] Example 7. A method for forming a semiconductor device, comprising: patterning a first mandrel layer over a target layer to form a first mandrel and a second mandrel, the width of the first mandrel being greater than the width of the second mandrel; depositing a spacer layer over the first mandrel and the second mandrel; forming a mask layer over the spacer layer and the second mandrel, a portion of the spacer layer over the first mandrel being exposed from the mask layer; depositing a pad layer over the mask layer and the exposed spacer layer; removing the mask layer; etching the spacer layer and the pad layer over the first mandrel to form a first spacer etch mask including first spacers, and etching the spacer layer over the second mandrel to form a second spacer mask including second spacers, each of the first spacers being wider than the second spacers; and etching the target layer based on the first spacer etch mask and the second spacer etch mask.

[0137] Example 8. The method according to Example 7 further includes: forming a second mask layer after removing the mask layer; patterning the second mask layer to provide an opening in the second mask layer that exposes the residue of the padding layer; and removing the residue of the padding layer.

[0138] Example 9. The method according to Example 7 further includes: forming a second mask layer after removing the mask layer; patterning the second mask layer to provide one or more openings in the second mask layer, each of the one or more openings exposing a region above a subset of the first mandrel or a subset of the second mandrel; depositing a sacrificial material in the one or more openings; and removing the second mask layer to leave pillars of the sacrificial material above the first mandrel or the second mandrel, wherein the first spacer mask or the second spacer mask includes pillars of the sacrificial material.

[0139] Example 10. The method according to Example 9, wherein the liner layer and the sacrificial material comprise the same material.

[0140] Example 11. The method according to Example 7, wherein the target layer comprises a semiconductor material.

[0141] Example 12. The method according to Example 7, wherein patterning the first mandrel layer includes patterning the first mandrel layer to form a hard mask between the first mandrel and the second mandrel.

[0142] Example 13. The method according to Example 7 further includes: removing a horizontal portion of the liner layer from the first mandrel, the remaining vertical portion of the liner layer being disposed on the sidewall of the spacer layer.

[0143] Example 14. A method for forming a semiconductor device, comprising: forming a first set of mandrels in a first region of a wafer; forming a second set of mandrels in a second region of the wafer, the spacing of the first set of mandrels being wider than the spacing of the second set of mandrels; depositing a first spacer layer over the first set of mandrels and the second set of mandrels; depositing a second spacer layer over the first set of mandrels and the second set of mandrels; forming a mask over the first region; removing the second spacer layer over the second set of mandrels in the second region; removing the mask; etching the first spacer layer in the second region and etching the first spacer layer and the second spacer layer in the first region to form a spacer mask including a first spacer in the first region and a second spacer in the second region, the first spacer being wider than the second spacer; removing the first set of mandrels and the second set of mandrels; and etching a target layer beneath the spacer mask.

[0144] Example 15. The method according to Example 14 further includes: etching a hard mask layer directly beneath the spacer mask, and using the hard mask layer to etch the target layer.

[0145] Example 16. The method according to Example 14 further includes: depositing a liner layer and a conductive filler within an opening in the target layer to form a first metal line in the first region and a second metal line in the second region, wherein the spacing between adjacent lines in the first region is greater than the spacing between adjacent metal lines in the second region.

[0146] Example 17. The method according to Example 14, wherein the second spacer layer comprises a material different from the first spacer layer.

[0147] Example 18. The method according to Example 14 further includes: forming a hard mask structure in a third region of the wafer, the hard mask structure being inserted between a mandrel in the first set of mandrels and a mandrel in the second set of mandrels, wherein a spacer in the first spacer contacts one side of the hard mask, and a spacer in the second spacer contacts the opposite side of the hard mask.

[0148] Example 19. The method according to Example 14, wherein the first spacer is higher than the second spacer.

[0149] Example 20. The method according to Example 14, wherein the first spacer includes a bottom and a first side portion and a second side portion, the first side portion including a portion of the first spacer layer, and the second side portion including a portion of the second spacer layer.

Claims

1. A method for forming a semiconductor device, include: patterning a first mandrel layer over the target layer to form a first mandrel and a second mandrel, the first mandrel having a width greater than a width of the second mandrel; depositing a spacer layer over the first mandrel and the second mandrel; forming a mask layer over the spacer layer and the first mandrel; thinning the spacer layer over the second mandrel; removing the mask layer; etching the spacer layer to form a spacer etch mask, the spacer etch mask comprising first spacers in contact with sidewalls of the first mandrel and second spacers in contact with sidewalls of the second mandrel, the first spacers having a width greater than a width of the second spacers; as well as The target layer is etched based on the spacer etch mask.

2. The method according to claim 1, further comprising: include: After said removing the mask layer, a second spacer layer is deposited over the first spacer layer.

3. The method according to claim 1, further comprising: include: forming a first metal line in a first region of the target layer, the first region corresponding to the first mandrel; as well as Second metal lines are formed in a second region of the target layer, the second region corresponding to the second mandrels, the second metal lines being spaced apart from each other by a greater distance than the first metal lines.

4. The method according to claim 1, further comprising: include: forming a second mask layer over the spacer layer and the first mandrels; patterning the second mask layer to expose the cut line area; depositing a sacrificial material in the region of the scribe line; as well as The second mask layer is removed and the sacrificial material becomes part of the spacer etch mask.

5. The method according to claim 1, further comprising: include: etching a hard mask beneath the spacer etch mask using the spacer etch mask; as well as The target layer is etched using the hard mask.

6. The method according to claim 1, in, The first spacer is wider than the second spacer and between.

7. A method for forming a semiconductor device, include: patterning a first mandrel layer over the target layer to form a first mandrel and a second mandrel, the first mandrel having a width greater than a width of the second mandrel; depositing a spacer layer over the first mandrel and the second mandrel; forming a mask layer over the spacer layer and the second mandrel, a portion of the spacer layer over the first mandrel being exposed from the mask layer; depositing a liner layer over the mask layer and the exposed spacer layer; removing the mask layer; etching the spacer layer and the liner layer over the first mandrel to form a first spacer etch mask including first spacers, and etching the spacer layer over the second mandrel to form a second spacer mask including second spacers, the first spacers being each wider than the second spacers; as well as The target layer is etched based on the first spacer etch mask and the second spacer etch mask.

8. The method according to claim 7, further comprising: include: After removing the mask layer, forming a second mask layer; patterning the second mask layer to provide an opening in the second mask layer, the opening exposing a residue of the liner layer; as well as The residue of the liner layer is removed.

9. The method according to claim 7, further comprising: include: After removing the mask layer, forming a second mask layer; patterning the second mask layer to provide one or more openings in the second mask layer, the one or more openings each exposing an area over a subset of the first mandrels or a subset of the second mandrels; depositing a sacrificial material in the one or more openings; as well as The second masking layer is removed, thereby leaving pillars of the sacrificial material over the first mandrel or the second mandrel, wherein the first spacer mask or the second spacer mask includes the pillars of sacrificial material.

10. The method according to claim 9, in, The liner layer and the sacrificial material include the same material.

11. The method according to claim 7, in, The target layer includes a semiconductor material.

12. The method according to claim 7, in, Patterning the first mandrel layer includes patterning the first mandrel layer to form a hard mask between the first mandrel and the second mandrel.

13. The method according to claim 7, further comprising: include: A horizontal portion of the liner layer is removed from over the first mandrel, with a remaining vertical portion of the liner layer disposed on a sidewall of the spacer layer.

14. A method for forming a semiconductor device, include: forming a first set of mandrels in a first region of the wafer; forming a second group of mandrels in a second region of the wafer, the mandrels of the first group having a wider spacing than the mandrels of the second group; depositing a first spacer layer over the first set of mandrels and the second set of mandrels; depositing a second spacer layer over the first set of mandrels and the second set of mandrels; forming a mask over the first region; removing the second spacer layer over the second set of mandrels in the second region; removing the mask; etching the first spacer layer in the second region and etching the first spacer layer and the second spacer layer in the first region to form a spacer mask including first spacers in the first region and second spacers in the second region, the first spacers being wider than the second spacers; removing the first set of mandrels and the second set of mandrels; as well as A target layer beneath the spacer mask is etched.

15. The method according to claim 14, further comprising: include: A hard mask layer directly below the spacer mask is etched, and the target layer is etched using the hard mask layer.

16. The method according to claim 14, further comprising: include: A liner layer and a conductive filler are deposited in the openings in the target layer to form a first metal line in the first region and a second metal line in the second region, wherein the spacing between adjacent lines in the first region is greater than the spacing between adjacent metal lines in the second region.

17. The method according to claim 14, in, The second spacer layer includes a different material than the first spacer layer.

18. The method according to claim 14, further comprising: include: A hard mask structure is formed in a third region of the wafer, the hard mask structure being inserted between one of the first group of mandrels and one of the second group of mandrels, wherein a spacer in the first spacers contacts one side of the hard mask and a spacer in the second spacers contacts an opposite side of the hard mask.

19. The method according to claim 14, in, The first spacer is taller than the second spacer.

20. The method according to claim 14, in, The first spacer includes a bottom portion and a first side portion and a second side portion, the first side portion includes a portion of the first spacer layer, and the second side portion includes a portion of the second spacer layer.