Non-aqueous electrolyte secondary battery and method for manufacturing the same

By using manganese lithium-containing transition metal composite oxide and FSO3 non-aqueous electrolyte in non-aqueous electrolyte secondary batteries, optimizing the surface area and distribution of the positive active material, combined with the design of the polyolefin layer electrode body, solves the problem of battery problems at low and high temperatures. The problem of insufficient performance is achieved, and efficient charge movement and battery capacity maintenance are achieved.

CN113228368BActive Publication Date: 2024-10-18SANYO ELECTRIC CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN201980083768.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-12-19
Publication Date
2024-10-18
Estimated Expiration
2039-12-19

Smart Images

  • Figure CN113228368B_ABST
    Figure CN113228368B_ABST
Patent Text Reader

Abstract

A nonaqueous electrolyte secondary battery having excellent low-temperature power characteristics and high-temperature storage characteristics is provided. A nonaqueous electrolyte secondary battery, comprising: a positive electrode plate having a positive electrode core and a positive electrode active material layer formed on the positive electrode core and containing a positive electrode active material; a negative electrode plate; a flat wound electrode body formed by winding the positive electrode plate and the negative electrode plate with a separator interposed therebetween; and a nonaqueous electrolyte, wherein the positive electrode active material is a lithium transition metal composite oxide containing manganese, and the BET specific surface area of ​​the positive electrode active material is 2.0 to 3.0 m 2 / g, and the total surface area of ​​the positive electrode active material contained in the positive electrode active material layer is 70 to 90 m 2 The total amount of FSO3 contained in the non-aqueous electrolyte is defined as A (μmol), and the total area of ​​the positive electrode active material contained in the positive electrode active material layer is defined as B (m 2 ), the value of A / B is 0.03~0.09(μmol / m 2 ).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a nonaqueous electrolyte secondary battery and a method for producing the same. Background Art

[0002] Non-aqueous electrolyte secondary batteries are used as driving power sources for hybrid electric vehicles (PHEV, HEV), electric vehicles (EV), etc. There is an increasing demand for improvement in the performance and reliability of non-aqueous electrolyte secondary batteries used for such driving power sources.

[0003] The non-aqueous electrolyte secondary battery used for driving power supply etc. can also be used in low temperature environment. Therefore, the non-aqueous electrolyte secondary battery used for driving power supply etc. is required to have excellent battery characteristics even in low temperature environment. In addition, the non-aqueous electrolyte secondary battery used for driving power supply etc. is sometimes kept in a high temperature state, therefore, it is required that the battery characteristics do not decrease even when kept in a high temperature state.

[0004] For example, Patent Document 1 listed below discloses a non-aqueous electrolyte solution containing a non-aqueous organic solvent containing propylene carbonate and lithium bis(fluorosulfonyl)imide for the purpose of improving low-temperature power characteristics.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2016-164879 Summary of the invention

[0008] Problem that the invention aims to solve

[0009] One object of the present invention is to provide a nonaqueous electrolyte secondary battery having excellent low-temperature power characteristics and high-temperature storage characteristics.

[0010] Solutions for solving problems

[0011] A nonaqueous electrolyte secondary battery according to one embodiment of the present invention includes:

[0012] A positive electrode plate comprising a positive electrode core and a positive electrode active material layer formed on the positive electrode core and containing a positive electrode active material;

[0013] Negative plate;

[0014] A flat wound electrode body, which is formed by winding the positive electrode plate and the negative electrode plate with a separator interposed therebetween; and

[0015] Non-aqueous electrolytes,

[0016] The positive electrode active material is a lithium transition metal composite oxide containing manganese.

[0017] The specific surface area of ​​the positive electrode active material is 2.0 to 3.0 m 2 / g,

[0018] The total surface area of ​​the positive electrode active material contained in the positive electrode active material layer is 70 to 80 m 2 ,

[0019] The FSO contained in the non-aqueous electrolyte 3 The total amount of the positive electrode active material is denoted as A (μmol), the total area of ​​the positive electrode active material contained in the positive electrode active material layer is denoted as B (m 2 )hour,

[0020] The value of A / B is 0.03~0.09 (μmol / m 2 ).

[0021] According to the above configuration, since the BET specific surface area of ​​the positive electrode active material is increased, the reaction area during charge and discharge is increased, and the charge transfer resistance during low-temperature discharge is reduced. In addition, the non-aqueous electrolyte contains a specific amount of FSO 3 , thus FSO 3 Coordinated on the surface of the positive electrode active material in a preferred state, the side reaction between the positive electrode active material and the non-aqueous electrolyte during high temperature storage can be more effectively suppressed. Therefore, the dissolution of manganese contained in the positive electrode active material can be effectively suppressed, and the generation of high-resistance deposits on the surface of the positive electrode active material can be effectively suppressed. Thus, a non-aqueous electrolyte secondary battery with excellent low-temperature power characteristics and high-temperature storage characteristics is obtained.

[0022] It should be noted that FSO contained in the non-aqueous electrolyte 3 It can exist in the form of fluorosulfonates such as lithium fluorosulfonate. In addition, FSO contained in the non-aqueous electrolyte 3 Can exist in the form of fluorosulfonate anion.

[0023] The value of A / B is preferably 0.05 to 0.07 (μmol / m 2 ). As a result, a non-aqueous electrolyte secondary battery with better low-temperature power characteristics and high-temperature storage characteristics is achieved.

[0024] The amount of manganese contained in the lithium transition metal composite oxide is preferably 10 to 40 mol % relative to the total amount of transition metals contained in the lithium transition metal composite oxide.

[0025] The lithium transition metal composite oxide preferably contains nickel and cobalt.

[0026] Preferably, a wound positive electrode core exposed portion is provided at one end of the flat wound electrode body.

[0027] The other end of the flat wound electrode body is provided with an exposed portion of the wound negative electrode core, thereby achieving a non-aqueous electrolyte secondary battery with better low-temperature power characteristics.

[0028] More preferably, a separator having a polyolefin layer is disposed between the positive electrode plate and the negative electrode plate, the surface of the negative electrode active material layer is in direct contact with the polyolefin layer, and the thickness of the separator is 14 to 23 μm. Thus, a non-aqueous electrolyte secondary battery with better initial low-temperature power characteristics is obtained.

[0029] In a method for producing a nonaqueous electrolyte secondary battery according to one aspect of the present invention, the nonaqueous electrolyte secondary battery includes:

[0030] A positive electrode plate comprising a positive electrode core and a positive electrode active material layer formed on the positive electrode core and containing a positive electrode active material;

[0031] Negative plate;

[0032] A flat wound electrode body, which is formed by winding the positive electrode plate and the negative electrode plate with a separator interposed therebetween;

[0033] nonaqueous electrolyte; and,

[0034] a battery case for housing the wound electrode body and the non-aqueous electrolyte,

[0035] The manufacturing method comprises the following steps:

[0036] The process of manufacturing the electrode body including the positive electrode plate, wherein the positive electrode active material is a lithium transition metal composite oxide including manganese, and the BET specific surface area of ​​the positive electrode active material is 2.0 to 3.0 m 2 / g, the total surface area of ​​the positive electrode active material contained in the positive electrode active material layer is 70 to 80 m 2 ;and,

[0037] The electrode body and the FSO 3 The non-aqueous electrolyte is disposed in the battery case.

[0038] The FSO contained in the non-aqueous electrolyte 3 The total amount of the positive electrode active material is denoted as A (μmol), the total area of ​​the positive electrode active material contained in the positive electrode active material layer is denoted as B (m 2 )hour,

[0039] The value of A / B is 0.03~0.09 (μmol / m 2 ).

[0040] Effects of the Invention

[0041] According to the present invention, a nonaqueous electrolyte secondary battery having excellent low-temperature power characteristics and high-temperature storage characteristics can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 1 is a schematic front view showing the inside of the battery with the front portion of the battery case and the front portion of the insulating sheet of the nonaqueous electrolyte battery according to the embodiment removed.

[0043] Figure 2 It is a top view of the nonaqueous electrolyte battery according to the embodiment.

[0044] Figure 3 (a) is a top view of the positive electrode plate according to the embodiment. Figure 3 (b) is a cross-sectional view along line IIIB-IIIB of (a).

[0045] Figure 4 (a) is a plan view of the negative electrode plate according to the embodiment. Figure 4 (b) is a cross-sectional view along line IVB-IVB of (a). DETAILED DESCRIPTION

[0046] The embodiments of the present invention will be described in detail below. However, the embodiments described below are examples of the present invention, and the present invention is not limited to the embodiments.

[0047] First, use Figure 1 and Figure 2 The structure of the square non-aqueous electrolyte secondary battery 100 according to the embodiment will be described. Figure 1 and Figure 2 As shown, the square non-aqueous electrolyte secondary battery 100 of the embodiment comprises: an outer shell 1 having an opening and a bottomed cylindrical shape, and a sealing plate 2 for sealing the opening of the outer shell 1. The outer shell 1 and the sealing plate 2 constitute a battery shell 200. The outer shell 1 contains a flat wound electrode body 3 formed by winding a strip-shaped positive electrode plate 4 and a strip-shaped negative electrode plate 5 with a strip-shaped separator (not shown) therebetween, and a non-aqueous electrolyte. The wound electrode body 3 has a wound positive electrode core exposed portion 4d at one end and a wound negative electrode core exposed portion 5c at the other end.

[0048] The positive electrode core exposed portion 4d is connected to the positive electrode collector 6, which is electrically connected to the positive electrode terminal 7. An inner insulating member 10 is disposed between the positive electrode collector 6 and the sealing plate 2, and an outer insulating member 11 is disposed between the positive electrode terminal 7 and the sealing plate 2.

[0049] The negative electrode core exposed portion 5c is connected to the negative electrode collector 8, which is electrically connected to the negative electrode terminal 9. An inner insulating member 12 is disposed between the negative electrode collector 8 and the sealing plate 2, and an outer insulating member 13 is disposed between the negative electrode terminal 9 and the sealing plate 2.

[0050] An insulating sheet 14 made of resin is disposed between the wound electrode body 3 and the outer shell 1. The sealing plate 2 is provided with a gas discharge valve 15 that breaks when the pressure in the battery case 200 exceeds a predetermined value and discharges the gas in the battery case 200 to the outside of the battery case 200. In addition, a non-aqueous electrolyte injection hole 16 is formed in the sealing plate 2. The non-aqueous electrolyte injection hole 16 is sealed by a sealing member 17 after a non-aqueous electrolyte is injected into the battery case 200.

[0051] Next, a method for manufacturing the nonaqueous electrolyte secondary battery 100 will be described.

[0052] [Production of positive electrode plate]

[0053] LiNi as the positive electrode active material 0.35 Co 0.35 Mn 0.30 O 2 The lithium transition metal electrode composite oxide shown, carbon powder as a conductive material, and polyvinylidene fluoride (PVdF) as a binding material are mixed with N-methyl-2-pyrrolidone (NMP) as a dispersion medium to prepare a positive electrode mixture slurry. Here, the mass ratio of the positive electrode active material, the conductive material, and the binding material contained in the positive electrode mixture slurry is set to 90.3:7.0:2.7.

[0054] The positive electrode mixture slurry prepared by the above method is applied to both sides of an aluminum foil with a thickness of 15 μm as a positive electrode core by a die coater. After that, the positive electrode mixture slurry is dried and the NMP as a dispersion medium is removed. The positive electrode active material layer is compressed using a pair of compression rollers. Then, the positive electrode core exposed portion without a positive electrode active material layer formed on both sides along the length direction is cut into a specified size as a positive electrode plate.

[0055] like Figure 3 As shown in (a) and (b), a positive electrode active material layer 4b containing a positive electrode active material is formed on both sides of the positive electrode core 4a. A positive electrode core exposed portion 4d is provided at one end in the width direction of the positive electrode plate 4 where the positive electrode active material layer 4b is not formed on both sides of the positive electrode core 4a. Figure 3 As shown in (a) and (b), in the positive electrode core 4a, a positive electrode protective layer 4c is provided near the end of the positive electrode active material layer 4b in the width direction. The positive electrode protective layer 4c preferably contains ceramic particles and a binder.

[0056] [Manufacturing of negative electrode plate]

[0057] Graphite powder as a negative electrode active material, carboxymethyl cellulose (CMC) as a thickener, and styrene-butadiene rubber (SBR) as a binder were dispersed in water at a mass ratio of 99.2:0.6:0.2 to prepare a negative electrode mixture slurry.

[0058] The negative electrode mixture slurry prepared by the above method is applied to both sides of a copper foil with a thickness of 8 μm as a negative electrode core by a die coater. Next, the negative electrode mixture slurry is dried to remove the water as a dispersion medium, and the negative electrode active material layer is compressed to a predetermined thickness by a roller press. Then, the negative electrode core exposed portion without a negative electrode active material layer formed on both sides along the length direction is cut into a predetermined size to form a negative electrode plate at one end in the width direction of the negative electrode plate.

[0059] like Figure 4 As shown in (a) and (b), negative electrode active material layers 5b containing negative electrode active material are formed on both sides of negative electrode core 5a. A negative electrode core exposed portion 5c where negative electrode active material layers 5b are not formed on both sides of negative electrode core 5a is provided at one end in the width direction of negative electrode plate 5.

[0060] [Production of Flat Wound Electrode Body]

[0061] The strip-shaped positive electrode plate 4 and the strip-shaped negative electrode plate 5 produced by the above method are wound with a strip-shaped separator having a three-layer structure of polypropylene / polyethylene / polypropylene having a thickness of 16 μm, and then press-formed into a flat shape to produce a flat wound electrode body 3. At this time, a wound positive electrode core exposed portion 4d is formed at one end of the flat wound electrode body 3 in the winding axis direction, and a negative electrode core exposed portion 5c is formed at the other end.

[0062] [Adjustment of non-aqueous electrolyte]

[0063] A mixed solvent was prepared in which ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), and methylene propionate (MP) were mixed in a volume ratio (25°C, 1 atm) of 25:37:35:3. LiPF was added as a solute to the mixed solvent. 6 The concentration was adjusted to 1.15 mol / L, and lithium fluorosulfonate was further added as a non-aqueous electrolyte.

[0064] [Installation of terminals and current collectors on sealing plates]

[0065] An external insulating member 11 is arranged on the outer side of the battery at the positive terminal mounting hole of the sealing plate 2. An internal insulating member 10 and a positive electrode collector 6 are arranged on the inner side of the battery at the positive terminal mounting hole of the sealing plate 2. Thereafter, the positive terminal 7 is embedded from the outer side of the battery into the through hole of the external insulating member 11, the positive terminal mounting hole of the sealing plate 2, the through hole of the internal insulating member 10, and the through hole of the positive electrode collector 6. Then, the front end side of the positive terminal 7 is riveted to the positive electrode collector 6. Thereafter, the riveted portion of the positive terminal 7 is welded and connected to the positive electrode collector 6.

[0066] An external insulating member 13 is arranged on the outer side of the battery at the negative terminal mounting hole of the sealing plate 2. An internal insulating member 12 and a negative electrode collector 8 are arranged on the inner side of the battery at the negative terminal mounting hole of the sealing plate 2. Thereafter, the negative terminal 9 is inserted from the outer side of the battery into the through hole of the external insulating member 13, the negative terminal mounting hole of the sealing plate 2, the through hole of the internal insulating member 12, and the through hole of the negative electrode collector 8. Then, the front end side of the negative terminal 9 is riveted to the negative electrode collector 8. Thereafter, the riveted portion of the negative terminal 9 is welded and connected to the negative electrode collector 8.

[0067] [Connection between current collector and wound electrode body]

[0068] The positive electrode current collector 6 is welded to the exposed positive electrode core portion 4d of the wound electrode body 3. The negative electrode current collector 8 is welded to the exposed negative electrode core portion 5c of the wound electrode body 3. Resistance welding, ultrasonic welding, laser welding, etc. can be used for welding.

[0069] [Insertion of the wound electrode body into the outer casing]

[0070] The wound electrode body 3 is covered with a resin insulating sheet 14 and is inserted into the outer case 1 . Thereafter, the outer case 1 and the sealing plate 2 are welded to seal the opening of the outer case 1 with the sealing plate 2 .

[0071] [Non-aqueous electrolyte injection hole / seal]

[0072] The nonaqueous electrolyte prepared in the above manner is injected from the nonaqueous electrolyte injection hole 16 provided in the sealing plate 2, and then the nonaqueous electrolyte injection hole 16 is sealed with a blind rivet as a sealing member 17. The nonaqueous electrolyte secondary battery 100 is manufactured as described above.

[0073] [Example 1]

[0074] A nonaqueous electrolyte secondary battery having the following structure was prepared in the same manner as the nonaqueous electrolyte secondary battery 100 as a nonaqueous electrolyte secondary battery of Example 1.

[0075] 1.0 mass % of lithium fluorosulfonate was added to the non-aqueous electrolyte so that the FSO contained in the non-aqueous electrolyte injected into the battery case 200 3 The total amount A (μmol) of FSO is 3.77 μmol. 3 The total amount can be adjusted by the content ratio of lithium fluorosulfonate in the non-aqueous electrolyte and the amount of the non-aqueous electrolyte injected into the battery case 200 .

[0076] In addition, the BET specific surface area is 2.46 m 2 / g of positive electrode active material, the total surface area B (m 2 ) is 77.00(m 2 ). It should be noted that the total surface area of ​​the positive electrode active material can be calculated from the BET specific surface area of ​​the positive electrode active material and the total mass of the positive electrode active material contained in the positive electrode active material layer 4 b.

[0077] [Example 2]

[0078] A nonaqueous electrolyte secondary battery having the following structure was prepared in the same manner as the nonaqueous electrolyte secondary battery 100 as a nonaqueous electrolyte secondary battery of Example 2.

[0079] 1.0 mass % of lithium fluorosulfonate was added to the non-aqueous electrolyte so that the FSO contained in the non-aqueous electrolyte injected into the battery case 200 3 The total amount A (μmol) was 4.71 μmol. In addition, the BET specific surface area was 2.46 m 2 / g of positive electrode active material, the total surface area B (m 2 ) is 77.00(m 2 ).

[0080] [Example 3]

[0081] A nonaqueous electrolyte secondary battery having the following structure was produced in the same manner as the nonaqueous electrolyte secondary battery 100 as a nonaqueous electrolyte secondary battery of Example 3.

[0082] 1.0 mass % of lithium fluorosulfonate was added to the non-aqueous electrolyte so that the FSO contained in the non-aqueous electrolyte injected into the battery case 200 3 The total amount A (μmol) was 5.66 μmol. In addition, the BET specific surface area was 2.46 m 2 / g of positive electrode active material, the total surface area B (m 2 ) is 77.00(m 2 ).

[0083] [Comparative Example 1]

[0084] A nonaqueous electrolyte secondary battery of Comparative Example 1 was prepared by the same method as the nonaqueous electrolyte secondary battery 100 having the following structure.

[0085] No lithium fluoride sulfonate is added to the non-aqueous electrolyte, so that the non-aqueous electrolyte injected into the battery case 200 does not contain FSO 3 In addition, the BET specific surface area is 2.38 m 2 / g of positive electrode active material, the total surface area B (m 2 ) is 83.87(m 2 ).

[0086] [Comparative Example 2]

[0087] A nonaqueous electrolyte secondary battery of Comparative Example 2 was prepared by the same method as the nonaqueous electrolyte secondary battery 100 described above and having the following structure.

[0088] 1.0 mass % of lithium fluorosulfonate was added to the non-aqueous electrolyte so that the FSO contained in the non-aqueous electrolyte injected into the battery case 200 3 The total amount A (μmol) was 4.15 μmol. In addition, the BET specific surface area was 1.32 m 2 / g of positive electrode active material, the total surface area B (m 2 ) is 42.90(m 2 ).

[0089] [Comparative Example 3]

[0090] A nonaqueous electrolyte secondary battery of Comparative Example 3 was prepared by the same method as the nonaqueous electrolyte secondary battery 100 described above and having the following structure.

[0091] 1.0 mass % of lithium fluorosulfonate was added to the non-aqueous electrolyte so that the FSO contained in the non-aqueous electrolyte injected into the battery case 200 3 The total amount A (μmol) was 1.04 μmol. In addition, the BET specific surface area was 1.32 m 2 / g of positive electrode active material, the total surface area B (m 2 ) is 42.90(m 2 ).

[0092] [Comparative Example 4]

[0093] A nonaqueous electrolyte secondary battery of Comparative Example 4 was prepared by the same method as the nonaqueous electrolyte secondary battery 100 having the following structure.

[0094] The non-aqueous electrolyte injected into the battery case 200 does not contain FSO 3 In addition, the BET specific surface area is 1.33 m 2 / g of positive electrode active material, the total surface area B (m 2 ) is 46.87(m 2 ).

[0095] The following tests were performed on the nonaqueous electrolyte secondary batteries of Examples 1 to 3 and Comparative Examples 1 to 4.

[0096] <Measurement of Low-Temperature Power Characteristics>

[0097] For non-aqueous electrolyte secondary batteries, charge at a charging current of 4.0A at 25°C until the state of charge (SOC) reaches 27%. Then, place the non-aqueous electrolyte secondary battery at -35°C for 5 hours. After that, discharge at currents of 12A, 24A, 36A, 48A, 60A, and 72A for 10 seconds at -35°C, and measure the voltage of each battery. Plot each current value and battery voltage, and calculate the power (W) from the IV characteristics during discharge as a low-temperature power characteristic. It should be noted that the state of charge that deviates due to discharge can be restored to its original state of charge by charging at a constant current of 0.4A.

[0098] <High-temperature storage characteristics measurement>

[0099] For non-aqueous electrolyte secondary batteries, at 25°C, constant current charging is performed at a current of 4.0A until 4.1V, and then constant voltage charging is performed at 4.1V for 2 hours. After that, constant current discharge is performed at a current of 2A until 3.0V, and then constant voltage discharge is performed at 3.0V for 3 hours, and the discharge capacity at this time is measured, and the discharge capacity is used as the battery capacity before the high-temperature storage test. In addition, at 25°C, charge at a charging current of 4.0A until the state of charge becomes 56%, and place it in an environment of -10°C for 5 hours. After that, the difference in battery voltage after discharging at a current of 60A for 10 seconds is divided by the discharge current (60A) to calculate the low-temperature discharge resistance before the high-temperature storage test.

[0100] Low temperature discharge resistance before high temperature storage test = (voltage before discharging at 60A for 10 seconds - battery voltage after discharging at 60A for 10 seconds) / discharge current (60A)

[0101] Next, the battery was charged at a charging current of 4.0A until the state of charge reached 80% at 25°C, and then placed at 75°C for 60 days. After that, the battery was charged at a constant current of 3.8 to 4.0A at 25°C until 4.1V, and then charged at a constant voltage of 4.1V for 2 hours. After that, the battery was discharged at a constant current of 4.0A until 3.0V, and then discharged at a constant voltage of 3.0V for 3 hours, and the discharge capacity at this time was measured as the battery capacity after the high-temperature storage test. The ratio of the battery capacity after the high-temperature storage test to the battery capacity before the high-temperature storage test was calculated as the high-temperature storage capacity retention rate. In addition, the battery was charged at a charging current of 4.0A at 25°C until the state of charge reached 56%, and then placed at -10°C for 5 hours. The difference in battery voltage after discharging at a current of 60A for 10 seconds was divided by the discharge current (60A), and thus the low-temperature discharge resistance after high-temperature storage was obtained.

[0102] Low-temperature discharge resistance after high-temperature storage test = (voltage before discharging at 60A for 10 seconds - battery voltage after discharging at 60A for 10 seconds) / discharge current (60A)

[0103] High temperature storage capacity maintenance rate (%) = battery capacity after high temperature storage test ÷ battery capacity before high temperature storage test × 100

[0104] High temperature storage resistance increase rate (%) = low temperature discharge resistance after high temperature storage ÷ low temperature discharge resistance before storage test × 100

[0105] <Cycle Characteristics Measurement>

[0106] For non-aqueous electrolyte secondary batteries, at 25°C, constant current charging is performed at a current of 4.0A until 4.1V, and then constant voltage charging is performed at 4.1V for 2 hours. Afterwards, constant current discharge is performed at a current of 2.0A until 3.0V, and then constant voltage discharge is performed at 3.0V for 3 hours, and the discharge capacity at this time is measured, and the discharge capacity is used as the battery capacity before the cycle test. In addition, at 25°C, charge at a charging current of 4.0A until the state of charge becomes 56%, and place it at -10°C for 5 hours. Afterwards, the difference in battery voltage after discharging at a current of 60A for 10 seconds is divided by the discharge current (60A) to calculate the low-temperature discharge resistance before the cycle test.

[0107] Low temperature discharge resistance before cycle test = (voltage before discharge at 60A for 10 seconds - battery voltage after discharge at 60A for 10 seconds) / discharge current (60A)

[0108] Next, at 75°C, pulse charge and discharge were performed for 2500 cycles with a current of 32.5It (130A) or less for a period of less than 60 seconds. The battery after the pulse cycle was discharged under the same conditions as the battery capacity before the above cycle test, and the discharge capacity was measured as the battery capacity after the cycle test. Then, the cycle capacity maintenance rate was calculated according to the following formula.

[0109] Then, the discharge was performed under the same conditions as the low-temperature discharge resistance before the cycle test, and the low-temperature discharge resistance after the cycle test was calculated. Then, the resistance increase rate after the cycle was calculated according to the following formula.

[0110] Low temperature discharge resistance after cycle test = (voltage before discharge at 60A for 10 seconds - battery voltage after discharge at 60A for 10 seconds) / discharge current (60A)

[0111] Cycle capacity retention rate (%) = battery capacity after cycle test ÷ battery capacity before cycle test × 100

[0112] Cycle resistance increase rate (%) = low temperature discharge resistance after cycle test / low temperature discharge resistance before cycle test × 100

[0113] The test results of each nonaqueous electrolyte secondary battery are shown in Table 1. The low temperature power characteristics of each nonaqueous electrolyte secondary battery are expressed as relative values ​​with the low temperature power (W) of the nonaqueous electrolyte secondary battery of Example 1 being 100%.

[0114] [Table 1]

[0115]

[0116] The nonaqueous electrolyte secondary battery of Comparative Example 1 had a low high-temperature storage capacity retention rate and a high high-temperature storage resistance increase rate. This is believed to be because the nonaqueous electrolyte does not contain FSO 3 Therefore, when the non-aqueous electrolyte secondary battery is stored at a high temperature, a side reaction between the positive electrode active material surface and the non-aqueous electrolyte becomes easy to occur. This is believed to be because the manganese contained in the positive electrode active material is dissolved in the non-aqueous electrolyte due to the side reaction between the positive electrode active material surface and the non-aqueous electrolyte, the Li insertion and extraction sites in the positive electrode active material are reduced, and the growth of the high-resistance Li deposition part on the surface of the positive electrode active material is promoted.

[0117] The nonaqueous electrolyte secondary battery of Comparative Example 2 has low initial low-temperature power characteristics. FSO in the nonaqueous electrolyte 3 Total amount A (μmol) / total area B (m 2 ) is 0.1 (μmol / m 2 ), the BET specific surface area of ​​the positive electrode active material is 1.31m 2 When the BET specific surface area of ​​the positive electrode active material is small and the value of A / B is large, the charge transfer resistance at the interface between the nonaqueous electrolyte and the positive electrode active material is large, so it is considered that the initial low-temperature power characteristics are reduced.

[0118] The non-aqueous electrolyte secondary batteries of Comparative Examples 3 and 4 have low low-temperature power characteristics, low high-temperature storage capacity retention rate, high high-temperature storage resistance increase rate, low cycle capacity retention rate, and high cycle resistance increase rate. This is believed to be due to the small BET specific surface area of ​​the positive electrode active material and the high charge transfer resistance at the interface between the non-aqueous electrolyte and the positive electrode active material. In addition, the FSO in the non-aqueous electrolyte 3 Total amount A (μmol) / total area B (m 2 ) is small, and when the nonaqueous electrolyte secondary battery is stored or charged and discharged under high temperature, a side reaction between the positive electrode active material surface and the nonaqueous electrolyte is likely to occur. Therefore, it is believed that this is because the manganese contained in the positive electrode active material dissolves into the nonaqueous electrolyte, the Li insertion and extraction sites in the positive electrode active material are reduced, and the growth of the high-resistance Li deposition part on the surface of the positive electrode active material is promoted.

[0119] The BET specific surface area of ​​the positive electrode active material of the non-aqueous electrolyte secondary battery of Examples 1 to 3 is 2.0 to 3.0 m 2 / g, the total surface area of ​​the positive electrode active material contained in the positive electrode active material layer is 70 to 80 m 2 , FSO in non-aqueous electrolyte 3 Total amount A (μmol) / total area B (m 2 ) is 0.03~0.09(μmol / m2 )。Therefore, the charge-discharge reaction area of the positive electrode active material becomes larger, thereby reducing the charge movement resistance during low-temperature discharge, and due to FSO 3 Moreover, when stored at a high temperature or subjected to charge-discharge cycles, the side reaction between the surface of the positive electrode active material and the non-aqueous electrolyte can be effectively suppressed. Therefore, the dissolution of manganese from the positive electrode active material into the non-aqueous electrolyte can be effectively suppressed. In addition, the growth of the high-resistance Li deposition portion on the surface of the positive electrode active material is effectively suppressed.

[0120] Therefore, the non-aqueous electrolyte secondary batteries of Examples 1 to 3 have high low-temperature power characteristics, high high-temperature storage capacity retention rate, low high-temperature storage resistance increase rate, high cycle capacity retention rate, and low cycle resistance increase rate.

[0121] It should be noted that in the lithium transition metal composite oxide, the Li amount (mol) / transition metal (mol) is preferably 1.1 to 1.25.

[0122] The content ratio of lithium fluorosulfonate in the non-aqueous electrolyte is preferably 0.25 to 2.0% by mass, more preferably 0.5 to 1.5% by mass.

[0123] The packing density of the positive electrode active material layer is preferably 2.3 to 2.5 g / cm 3 , more preferably 2.4 to 2.5 g / cm 3 .

[0124] The lithium transition metal composite oxide preferably contains at least one of zirconium and tungsten.

[0125] <Other>

[0126] As the positive electrode active material, a lithium transition metal composite oxide is preferred. Examples of the lithium transition metal composite oxide include lithium cobalt oxide (LiCoO 2 ), lithium manganese oxide (LiMn 2 O 4 ), lithium nickel oxide (LiNiO 2 ), lithium nickel manganese composite oxide (LiNi 1- x Mn x O 2 (0 < x < 1)), lithium nickel cobalt composite oxide (LiNi 1-x Co x O 2 (0 < x < 1)), lithium nickel cobalt manganese composite oxide (LiNi x Co y Mn z O 2 (0 < x < 1, 0 < y < 1, 0 < z < 1, x + y + z = 1)), etc.

[0127] In addition, the above-mentioned lithium transition metal composite oxides may be added with Al, Ti, Zr, Nb, B, W, Mg, Mo, etc. For example, Li 1+a Ni x Co y Mn z M b O 2 A lithium transition metal composite oxide represented by (M = at least one element selected from Al, Ti, Zr, Nb, B, Mg and Mo, 0≤a≤0.2, 0.2≤x≤0.5, 0.2≤y≤0.5, 0.2≤z≤0.4, 0≤b≤0.02, a+b+x+y+z=1).

[0128] As the negative electrode active material, a carbon material capable of absorbing and releasing lithium ions can be used. As the carbon material capable of absorbing and releasing lithium ions, graphite, non-graphitizable carbon, graphitizable carbon, fibrous carbon, coke, and carbon black can be cited. Among them, graphite is particularly preferred. Furthermore, as non-carbon materials, silicon, tin, and alloys and oxides thereof can be cited.

[0129] As the non-aqueous solvent (organic solvent) of non-aqueous electrolyte, carbonates, lactones, ethers, ketones, esters, etc. can be used, and two or more of these solvents can be mixed and used. For example, cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate and other chain carbonates can be used. It is particularly preferred to use a mixed solvent of cyclic carbonate and chain carbonate. In addition, unsaturated cyclic carbonates such as vinylene carbonate (VC) can also be added to the non-aqueous electrolyte. It should be noted that the non-aqueous electrolyte more preferably includes propylene carbonate and methylene propionate (MP).

[0130] It should be noted that the non-aqueous electrolyte preferably contains lithium bis(oxalatoborate) (LiC 4 BO 8 ), lithium difluorophosphate (LiPF 2 O 2 ).

[0131] As the electrolyte salt of the non-aqueous electrolyte, those commonly used as electrolyte salts in conventional lithium-ion secondary batteries can be used. For example, LiPF 6 , LiBF 4 、LiCF 3 SO 3 、LiN(CF 3 SO 2 ) 2 、LiN(C 2 F 5 SO 2 )2 、LiN(CF 3 SO 2 )(C 4 F 9 SO 2 )、LiC(CF 3 SO 2 ) 3 、LiC(C 2 F 5 SO 2 ) 3 、LiAsF 6 、LiClO 4 , Li 2 B 10 Cl 10 , Li 2 B 12 Cl 12 、LiB(C 2 O 4 ) 2 、LiB(C 2 O 4 )F 2 、LiP(C 2 O 4 ) 3 、LiP(C 2 O 4 ) 2 F 2 、LiP(C 2 O 4 )F 4 etc. and mixtures thereof. Among them, LiPF is particularly preferred 6 In addition, the amount of the electrolyte salt dissolved in the non-aqueous solvent is preferably 0.5 to 2.0 mol / L.

[0132] As the separator, a porous separator made of polyolefins such as polypropylene (PP) and polyethylene (PE) is preferably used. Particularly preferably, a separator having a three-layer structure (PP / PE / PP, or PE / PP / PE) of polypropylene (PP) and polyethylene (PE) is used. In addition, a heat-resistant layer formed of inorganic particles such as alumina and a binder can be provided on the separator. In addition, a polymer electrolyte can be used as a separator.

[0133] It should be noted that the surface of the negative electrode active material layer is preferably in direct contact with the polyolefin layer of the separator, and the thickness of the separator is 14 to 23 μm. If this structure is adopted, a non-aqueous electrolyte secondary battery with better power characteristics is obtained. It should be noted that the thickness of the separator is more preferably 14 to 19 μm.

[0134] Description of Reference Numerals

[0135] 100…Non-aqueous electrolyte secondary battery

[0136] 200…Battery housing

[0137] 1…Outer shell

[0138] 2…Sealing plate

[0139] 3…Wound electrode body

[0140] 4…Positive plate

[0141] 4a…Positive electrode core

[0142] 4b…Positive electrode active material layer

[0143] 4c…Positive electrode protection layer

[0144] 4d…Positive electrode core exposed part

[0145] 5…Negative plate

[0146] 5a…Negative electrode core

[0147] 5b…Negative electrode active material layer

[0148] 5c…Negative electrode core exposed part

[0149] 6…Positive electrode collector

[0150] 7…Positive terminal

[0151] 8…Negative electrode current collector

[0152] 9…Negative terminal

[0153] 10…Inner side insulation member

[0154] 11…External insulation member

[0155] 12…Inner side insulation member

[0156] 13…External insulation member

[0157] 14…Insulation sheet

[0158] 15…Gas discharge valve

[0159] 16…Non-aqueous electrolyte injection hole

[0160] 17…Sealing member

Claims

1. A non-aqueous electrolyte secondary battery comprising: A positive electrode plate having a positive electrode core and a positive electrode active material layer formed on the positive electrode core and containing a positive electrode active material; Negative plate; a flat wound electrode body formed by winding the positive electrode plate and the negative electrode plate with a separator interposed therebetween; and Non-aqueous electrolytes, The positive electrode active material is a lithium transition metal composite oxide containing manganese, The BET specific surface area of ​​the positive electrode active material is 2.0 to 3.0 m 2 / g, The total surface area of ​​the positive electrode active material contained in the positive electrode active material layer is 70 to 80 m 2 , The total amount of FSO3 contained in the non-aqueous electrolyte is denoted by A μmol, and the total area of ​​the positive electrode active material contained in the positive electrode active material layer is denoted by Bm. 2 hour, The value of A / B is 0.03~0.09μmol / m 2 .

2. The nonaqueous electrolyte secondary battery according to claim 1, wherein The value of A / B is 0.05~0.07μmol / m 2 .

3. The nonaqueous electrolyte secondary battery according to claim 1 or 2, wherein: The amount of manganese contained in the lithium transition metal composite oxide is 10 to 40 mol % relative to the total amount of transition metals contained in the lithium transition metal composite oxide.

4. The nonaqueous electrolyte secondary battery according to claim 3, wherein: The lithium transition metal composite oxide includes nickel and cobalt.

5. The nonaqueous electrolyte secondary battery according to claim 1 or 2, wherein: A wound positive electrode core exposed portion is provided at one end of the flat wound electrode body. The other end of the flat wound electrode body is provided with a wound negative electrode core exposed portion.

6. The nonaqueous electrolyte secondary battery according to claim 1 or 2, wherein: A separator having a polyolefin layer is arranged between the positive electrode plate and the negative electrode plate. The surface of the negative electrode active material layer is in direct contact with the polyolefin layer. The separator has a thickness of 14 to 23 μm.

7. A method for manufacturing a non-aqueous electrolyte secondary battery, wherein: The non-aqueous electrolyte secondary battery comprises: A positive electrode plate having a positive electrode core and a positive electrode active material layer formed on the positive electrode core and containing a positive electrode active material; Negative plate; A flat wound electrode body, which is formed by winding the positive electrode plate and the negative electrode plate with a separator interposed therebetween; a nonaqueous electrolyte; and, a battery case for housing the wound electrode body and the nonaqueous electrolyte, The manufacturing method comprises the following steps: The step of preparing the electrode body including the positive electrode plate, wherein the positive electrode active material is a lithium transition metal composite oxide including manganese, and the BET specific surface area of ​​the positive electrode active material is 2.0 to 3.0 m 2 / g, the total surface area of ​​the positive electrode active material contained in the positive electrode active material layer is 70 to 80 m 2 ; and, The step of placing the electrode body and the non-aqueous electrolyte containing FSO 3 in the battery case, The total amount of FSO3 contained in the non-aqueous electrolyte is denoted by A μmol, and the total area of ​​the positive electrode active material contained in the positive electrode active material layer is denoted by Bm. 2 hour, The value of A / B is 0.03~0.09μmol / m 2 .

Citation Information

Patent Citations

  • Nonaqueous electrolyte and lithium secondary battery including the same

    JP2016164879A

  • Nonaqueous electrolyte secondary battery and method for manufacturing the same

    CN106299457A

  • Nonaqueous electrolyte secondary battery

    JP2015125833A