Secondary battery
By using an electrolyte containing water, lithium salt and specific additives in a lithium-ion secondary battery, and forming a coating with a silane coupling agent, the problem of self-discharge and narrow potential window of lithium-ion secondary battery at high voltage is solved. , achieving more stable battery performance and safety.
Patent Information
- Application Number
- CN202080024859.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-01-27
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2040-01-27
AI Technical Summary
Existing lithium-ion secondary batteries are difficult to operate stably at high voltages, and there are self-discharge problems. The potential window of the aqueous electrolyte is narrow, which affects the safety and charge and discharge characteristics of the battery.
Using an electrolyte containing water, lithium salts and specific additives, the additives including alkaline earth metal salts, dicarboxylic acids, carboxylic anhydrides and organic carbonates, the coating is formed by a silane coupling agent to inhibit the reduction and decomposition of water and the self-discharge of lithium ions. .
The potential window is effectively expanded, the battery stability and charge and discharge efficiency are improved, self-discharge is suppressed, the electrolyte is robust, and the battery safety is improved.
Smart Images

Figure CN113632287B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a secondary battery. Background Art
[0002] As a high-output, high-energy-density secondary battery, a lithium-ion secondary battery is widely used. The secondary battery includes a positive electrode, a negative electrode, and an electrolyte, and lithium ions are transferred between the positive electrode and the negative electrode to perform charging and discharging. In order to achieve high energy density, an organic solvent-based electrolyte is used in conventional secondary batteries.
[0003] However, organic solvents are generally flammable, and ensuring safety is an important issue. In addition, the ion conductivity of organic solvents is lower than that of aqueous solutions, and the rapid charge and discharge characteristics are insufficient, which is also a problem.
[0004] In view of such problems, research has been conducted on secondary batteries using an electrolyte solution containing water. However, secondary batteries using an electrolyte solution containing water have a narrow potential window and are difficult to operate stably at a high voltage.
[0005] As one of the methods for solving the problem of narrow potential window, for example, Patent Documents 1 and 2 disclose the use of aqueous solutions containing high concentrations of alkali salts as aqueous electrolytes for secondary batteries, and Patent Document 3 discloses the use of electrolytes containing high concentrations of alkali salts to which organic carbonates are added.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent No. 6423453
[0009] Patent Document 2: International Publication No. 2017 / 122597
[0010] Patent Document 3: Japanese Patent Application Publication No. 2018-73819 Summary of the invention
[0011] However, in order to further increase the voltage of secondary batteries using aqueous electrolytes, there is a demand for a wider potential window and an improvement in self-discharge characteristics.
[0012] Therefore, an object of the present disclosure is to suppress self-discharge in a secondary battery using an aqueous electrolyte.
[0013] A secondary battery as a first embodiment of the present disclosure comprises a positive electrode, a negative electrode and an electrolyte, wherein the electrolyte comprises water, a lithium salt and an additive, the additive comprises at least any one of an alkaline earth metal salt, a dicarboxylic acid, a carboxylic anhydride and an organic carbonate, the negative electrode comprises a negative electrode active material, and a silane coupling agent is attached to the surface of the negative electrode active material.
[0014] In addition, the secondary battery of the second embodiment of the present invention comprises a positive electrode, a negative electrode and an electrolyte, the electrolyte comprises water, a lithium salt and an additive, the additive comprises at least any one of an alkaline earth metal salt, a dicarboxylic acid, a carboxylic anhydride and an organic carbonate, the negative electrode comprises a negative electrode active material, and a coating based on reductive decomposition of a silane coupling agent is formed on the surface of the negative electrode active material.
[0015] According to the secondary battery of the present disclosure, self-discharge can be suppressed. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a schematic cross-sectional view showing an example of the secondary battery according to the present embodiment. DETAILED DESCRIPTION
[0017] Typically, the reduction decomposition of an aqueous electrolyte (essentially the reduction decomposition of water) occurs between about 2V based on Li and a potential lower than this potential. In addition, the charge and discharge reaction of negative electrode active materials such as carbon materials occurs at a potential lower than the reduction decomposition potential of water. Therefore, during the charging process, before the charging reaction of the negative electrode active material, the reduction decomposition of water occurs, and the charging current is consumed in the reaction, so the charging reaction of the negative electrode active material is hindered. Therefore, the inventors of the present invention conducted in-depth research and found that: by combining a silane coupling agent and a specific additive (alkaline earth metal salt, dicarboxylic acid, carboxylic anhydride, organic carbonate), the reduction decomposition of water can be suppressed, and self-discharge can be suppressed, thereby conceiving of a secondary battery in the manner shown below.
[0018] The secondary battery of the first embodiment of the present disclosure comprises a positive electrode, a negative electrode and an electrolyte, wherein the electrolyte comprises water, a lithium salt and an additive, wherein the additive comprises at least one of an alkaline earth metal salt, a dicarboxylic acid, a carboxylic anhydride and an organic carbonate, and the negative electrode comprises a negative electrode active material, and a silane coupling agent is attached to the surface of the negative electrode active material. The secondary battery of the first embodiment of the present disclosure suppresses the reduction and decomposition of water during charging, and the charging reaction of the negative electrode active material is performed, and further the reaction between the negative electrode active material and the electrolyte is suppressed, so that the self-discharge of lithium ions absorbed by the negative electrode active material and naturally released from the negative electrode active material is suppressed.
[0019] The secondary battery of the second mode of the present disclosure comprises a positive electrode, a negative electrode and an electrolyte, wherein the electrolyte comprises water, a lithium salt and an additive, wherein the additive comprises at least any one of an alkaline earth metal salt, a dicarboxylic acid, a carboxylic anhydride and an organic carbonate, and the negative electrode comprises a negative electrode active material, and a coating based on reduction decomposition of a silane coupling agent is formed on the surface of the negative electrode active material. The secondary battery of the second mode of the present disclosure is a secondary battery in a state after charging or after charge and discharge of the secondary battery of the first mode of the present disclosure. That is, by the secondary battery of the second mode of the present disclosure, the reduction decomposition of water during charging is also suppressed, the charging reaction of the negative electrode active material is carried out, and further the reaction of the negative electrode active material with the electrolyte is suppressed, and thus the self-discharge of lithium ions absorbed by the negative electrode active material and naturally released from the negative electrode active material is suppressed.
[0020] The mechanism of the effect of the first and second modes of the present disclosure varies depending on the type of additive combined with the silane coupling agent, but can be considered as follows according to the type of additive. When multiple additives are added, it is a mechanism of combining the effects of the additives. The type of additive here refers to alkaline earth metal salts, dicarboxylic acids, carboxylic anhydrides, organic carbonates, that is, the classification of additives.
[0021] <Alkaline earth metal salt>
[0022] When the silane coupling agent and the alkaline earth metal salt are combined, although it also varies depending on the type of the silane coupling agent used, during the initial charge, the reduction and decomposition of the alkaline earth metal salt and the reduction and decomposition of the silane coupling agent proceed in parallel, forming a composite film of the film derived from the silane coupling agent and the film derived from the alkaline earth metal salt. Examples of the film component derived from the alkaline earth metal salt include CaF 2 MgF 2 , SrF 2 and BaF 2 As the coating component derived from the silane coupling agent, at least one of the fluorides thereof is mainly LiF and SiO x Compared with LiF, CaF 2 MgF 2 , SrF 2 , BaF 2 Since the solubility in water is low, the combination with alkaline earth metal salts can improve the robustness of the coating derived from the silane coupling agent to the aqueous electrolyte. In addition, the presence of alkaline earth metal salts that undergo reduction and decomposition at a relatively high potential can significantly suppress the dissolved CO2 in the aqueous electrolyte. 2 , dissolved O 2 The electrochemical reduction reaction of Li 2 CO 3 , Li 2O formation. As a result, the ratio of components with low solubility in water (such as fluoride) in the aforementioned composite film can be increased, and the robustness to aqueous electrolyte can be improved. In addition, when combined with an alkaline earth metal salt that is reduced and decomposed in a potential region above the reduction decomposition potential region of the silane coupling agent, the reduction reaction of the silane coupling agent is suppressed, and unreacted or low-reduced silane coupling agent will remain in the film. As a result, the water-repellent effect of the residual silane coupling agent can inhibit the penetration of water into the surface of the negative electrode active material. Through the above effects, by combining the silane coupling agent and the alkaline earth metal salt, the ratio of components with low solubility in water in the film can be increased, the robustness of the film to the aqueous electrolyte can be improved, and an electrochemically stable film can be formed. Therefore, the reaction between the negative electrode active material and the electrolyte is suppressed, and the self-discharge of lithium ions naturally released from the negative electrode active material by the negative electrode active material can be suppressed. It should be noted that the composite film of the film derived from the silane coupling agent and the film derived from the alkaline earth metal salt has lithium ion conductivity, so during the charging process, the negative electrode active material can absorb and store lithium ions through the film. It should be noted that fluoroalkyl groups (F1s, 688.8eV (XPS)), C-Si-O groups (Si2p, 102.6eV (XPS)), O-Si-C groups (Si2p, 103.5eV (XPS)), etc. can be observed in the silane coupling agent with a low degree of reduction in the film.
[0023] <Dicarboxylic Acid, Carboxylic Anhydride>
[0024] In the case of a combination of a silane coupling agent and a dicarboxylic acid or a carboxylic anhydride, the dicarboxylic acid or the carboxylic anhydride undergoes reduction and decomposition at a relatively high potential, thereby significantly suppressing the amount of dissolved CO dissolved in the aqueous electrolyte. 2 , dissolved O 2 The electrochemical reduction reaction of Li 2 CO 3 , Li 2O formation. In addition, when combined with a dicarboxylic acid or carboxylic anhydride that is reductively decomposed in a potential region above the reductive decomposition potential region of the silane coupling agent, the reduction reaction of the silane coupling agent is suppressed, and unreacted or low-reduced silane coupling agent will remain in the film. As a result, the water-repellent effect of the residual silane coupling agent can inhibit the penetration of water to the surface of the negative electrode active material. Through the above effects, by combining a silane coupling agent with a dicarboxylic acid or carboxylic anhydride, the ratio of components with low solubility in water in the film can be increased, and in addition, the permeability of water to the surface of the negative electrode active material can be suppressed, thereby improving the robustness of the film to the aqueous electrolyte, thereby being able to form an electrochemically stable film. Therefore, the reaction of the negative electrode active material with the electrolyte is suppressed, and the self-discharge of lithium ions absorbed by the negative electrode active material and naturally released from the negative electrode active material is suppressed. It should be noted that the composite coating of the coating derived from the silane coupling agent and the coating derived from the dicarboxylic acid or carboxylic anhydride has lithium ion conductivity, so during charging, the negative electrode active material can absorb lithium ions through the coating.
[0025] <Organic carbonate>
[0026] When a silane coupling agent is combined with an organic carbonate, especially when an aqueous electrolyte containing a high concentration of an alkali salt is used, in addition to water and lithium salts, the organic carbonate also participates in the solvation structure, thereby reducing the activity of water in the aqueous electrolyte, thereby improving the electrochemical stability of the water in the electrolyte. In addition, the presence of the organic carbonate can greatly suppress the dissolved CO in the aqueous electrolyte. 2 , dissolved O 2 The electrochemical reduction reaction of Li 2 CO 3 , Li 2O formation. In addition, although it also depends on the type of silane coupling agent used, by combining with an organic carbonate that is reductively decomposed at a lower potential than the silane coupling agent, the coating derived from the organic carbonate can be used to compensate for the defects of the coating derived from the silane coupling agent with a large molecular weight and a problem in the density of the coating after reductive decomposition, thereby improving the density of the coating derived from the silane coupling agent. Through the above effects, by combining the silane coupling agent with the organic carbonate, the effect of improving the electrochemical stability of water brought about by the addition of the organic carbonate and the effect brought about by the composite coating formation of the coating derived from the silane coupling agent and the coating derived from the organic carbonate can improve the robustness of the coating to the aqueous electrolyte, thereby being able to form an electrochemically stable coating. Therefore, the reaction between the negative electrode active material and the electrolyte is suppressed, and the self-discharge of the lithium ions absorbed by the negative electrode active material and naturally released from the negative electrode active material is suppressed. It should be noted that the composite film of the film derived from the silane coupling agent and the film derived from the organic carbonate has lithium ion conductivity, so during the charging process, the negative electrode active material can absorb and store lithium ions through the film. In addition, during the discharge process, the lithium ions absorbed and stored by the negative electrode active material can be released.
[0027] Hereinafter, embodiments of the secondary battery of the present disclosure will be described in detail.
[0028] The shape of the secondary battery of the present embodiment is not particularly limited, and examples thereof include a coin shape, a button shape, a sheet shape, a laminate shape, a cylindrical shape, a flat shape, and a square shape. Figure 1 It is a schematic cross-sectional view showing an example of the secondary battery according to the present embodiment. Figure 1 The secondary battery 20 shown includes: a cup-shaped battery case 21, a positive electrode 22 arranged on the upper part of the battery case 21, a negative electrode 23 arranged at a position opposite to the positive electrode 22 via a separator 24, a gasket 25 formed of an insulating material, and a sealing plate 26 arranged at the opening of the battery case 21 and sealing the battery case 21 with the aid of the gasket 25. Figure 1 In the secondary battery 20 shown, the space between the positive electrode 22 and the negative electrode 23 is filled with an electrolyte 27. The electrolyte 27, the positive electrode 22, the negative electrode 23, and the separator 24 will be described in detail below.
[0029] The electrolyte 27 contains water, lithium salts and additives (hereinafter, sometimes referred to as aqueous electrolyte). The aqueous electrolyte contains water that is not flammable, so the safety of the secondary battery using the aqueous electrolyte can be improved. From this point of view, the content of water in the electrolyte 27 is preferably 6% by mass or more, more preferably in the range of 8% by mass to 50% by mass, and more preferably in the range of 8.5% by mass to 21% by mass, relative to the total amount of the electrolyte 27. The electrolyte 27 may also contain solvents other than water. As solvents other than water, for example, ethers, nitriles, alcohols, ketones, amines, amides, sulfur compounds and hydrocarbons can be cited. Relative to the total amount of the electrolyte 27, the content of solvents other than water is preferably less than 50% by mass, more preferably less than 25% by mass.
[0030] As long as the lithium salt is a compound that can be dissolved in a solvent containing water and dissociated to allow lithium ions to exist in an aqueous electrolyte, any lithium salt can be used. The lithium salt preferably does not cause degradation of battery characteristics due to reaction with the materials constituting the positive electrode and the negative electrode. As such lithium salts, for example, salts with inorganic acids such as perchloric acid, sulfuric acid, and nitric acid, salts with halide ions such as chloride ions and bromide ions, and salts with organic anions containing carbon atoms in the structure can be cited.
[0031] Examples of the organic anions constituting the lithium salt include anions represented by the following general formulae (i) to (vi).
[0032] (R 1 SO 2 )(R 2 SO 2 )N - (i)
[0033] (R 1 , R 2 are independently selected from alkyl or halogen-substituted alkyl. 1 and R 2 They may bond to each other to form a ring.)
[0034] R 3 SO 3 - (ii)
[0035] (R 3 is selected from alkyl or halogen-substituted alkyl. )
[0036] R 4 CO 2 - (iii)
[0037] (R 4 is selected from alkyl or halogen-substituted alkyl. )
[0038] (R5 SO 2 ) 3 C - (iV)
[0039] (R 5 is selected from alkyl or halogen-substituted alkyl. )
[0040] [(R 6 SO 2 )N(SO 2 )N(R 7 SO 2 )] 2- (v)
[0041] (R 6 , R 7 is selected from alkyl or halogen-substituted alkyl. )
[0042] [(R 8 SO 2 )N(CO)N(R 9 SO 2 )] 2- (vi)
[0043] (R 8 , R 9 is selected from alkyl or halogen-substituted alkyl. )
[0044] In the above general formulae (i) to (vi), the carbon number of the alkyl group or the halogen-substituted alkyl group is preferably 1 to 6, more preferably 1 to 3, and even more preferably 1 to 2. The halogen in the halogen-substituted alkyl group is preferably fluorine. The number of halogen substitutions in the halogen-substituted alkyl group is equal to or less than the number of hydrogen atoms in the original alkyl group.
[0045] R 1 ~R 9 Each of them is, for example, a group represented by the following general formula (vii).
[0046] C n H a F b Cl c Br d I e (vii)
[0047] (n is an integer greater than or equal to 1, a, b, c, d, and e are integers greater than or equal to 0, and 2n+1=a+b+c+d+e is satisfied.)
[0048] Specific examples of the organic anion represented by the general formula (i) include bis(trifluoromethylsulfonyl)imide (TFSI; [N(CF 3 SO 2 ) 2 ]- ), bis(perfluoroethylsulfonyl)imide (BETI; [N(C 2 F 5 SO 2 ) 2 ] - ), (perfluoroethylsulfonyl)(trifluoromethylsulfonyl)imide ([N(C 2 F 5 SO 2 )(CF 3 SO 2 )] - ) etc. Specific examples of the organic anion represented by the general formula (ii) include CF 3 SO 3 - , C 2 F 5 SO 3 - As specific examples of the organic anion represented by the general formula (iii), for example, CF 3 CO 2 - , C 2 F 5 CO 2 - As specific examples of the organic anion represented by the general formula (iv), for example, tris(trifluoromethylsulfonyl)carbonate ([(CF 3 SO 2 ) 3 C] - ), tris(perfluoroethylsulfonyl)carbonic acid ([(C 2 F 5 SO 2 ) 3 C] - ) etc. Specific examples of the organic anion represented by the general formula (v) include sulfonylbis(trifluoromethylsulfonyl)imide ([(CF 3 SO 2 )N(SO 2 )N(CF 3 SO 2 )] 2- ), sulfonylbis(perfluoroethylsulfonyl)imide ([(C 2 F 5 SO 2 )N(SO 2 )N(C 2 F 5 SO 2 )] 2- ), sulfonyl (perfluoroethylsulfonyl) (trifluoromethylsulfonyl) imide ([(C2 F 5 SO 2 )N(SO 2 )N(CF 3 SO 2 )] 2- ) etc. Specific examples of the organic anion represented by the general formula (vi) include carbonylbis(trifluoromethylsulfonyl)imide ([(CF 3 SO 2 )N(CO)N(CF 3 SO 2 )] 2- ), carbonylbis(perfluoroethylsulfonyl)imide ([(C 2 F 5 SO 2 )N(CO)N(C 2 F 5 SO 2 )] 2- ), carbonyl(perfluoroethylsulfonyl)(trifluoromethylsulfonyl)imide ([(C 2 F 5 SO 2 )N(CO)N(CF 3 SO 2 )] 2- )wait.
[0049] Examples of organic anions other than those of the general formulae (i) to (vi) include bis(1,2-benzenediol(2-)-O,O')boric acid, bis(2,3-naphthalenediol(2-)-O,O')boric acid, bis(2,2'-biphenylediol(2-)-O,O')boric acid, and bis(5-fluoro-2-ol-1-benzenesulfonic acid-O,O')boric acid.
[0050] As the anion constituting the lithium salt, it is preferred to include a salt having an imide anion from the viewpoint of being able to effectively suppress the self-discharge of the battery. Suitable specific examples of the imide anion include, in addition to the imide anions exemplified as the organic anions represented by the general formula (i), bis(fluorosulfonyl)imide (FSI; [N(FSO 2 ) 2 ] - ), (fluorosulfonyl)(trifluoromethylsulfonyl)imide (FTI; [N(FSO 2 )(CF 3 SO 2 )] - )wait.
[0051] From the perspective of being able to effectively suppress the self-discharge of the battery, the lithium salt having lithium ions and imide anions can include, for example, bis(trifluoromethylsulfonyl)imide lithium (LiTFSI), bis(perfluoroethylsulfonyl)imide lithium (LiBETI), (perfluoroethylsulfonyl) (trifluoromethylsulfonyl)imide lithium, bis(fluorosulfonyl)imide lithium (LiFSI), (fluorosulfonyl) (trifluoromethylsulfonyl)imide lithium (LiFTI), etc. These can be used alone or in combination of two or more.
[0052] Specific examples of other lithium salts include CF 3 SO 3 Li, C 2 F 5 SO 3 Li, CF 3 CO 2 Li, C 2 F 5 CO 2 Li, (CF 3 SO 2 ) 3 CLi, (C 2 F 5 SO 2 ) 3 CLi, (C 2 F 5 SO 2 ) 2 (CF 3 SO 2 )CLi、(C 2 F 5 SO 2 )(CF 3 SO 2 ) 2 CLi, [(CF 3 SO 2 )N(SO 2 )N(CF 3 SO 2 )]Li 2 、[(C 2 F 5 SO 2 )N(SO 2 )N(C 2 F 5 SO 2 )]Li 2 、[(C 2 F 5 SO 2 )N(SO 2 )N(CF 3 SO 2 )]Li2 ,[(CF 3 SO 2 )N(CO)N(CF 3 SO 2 )]Li 2 、[(C 2 F 5 SO 2 )N(CO)N(C 2 F 5 SO 2 )]Li 2 、[(C 2 F 5 SO 2 )N(CO)N(CF 3 SO 2 )]Li 2 、Lithium bis(1,2-benzenediol (2-)-O,O')borate、Lithium bis(2,3-naphthaleneediol (2-)-O,O')borate、Lithium bis(2,2'-biphenylediol (2-)-O,O')borate、Lithium bis(5-fluoro-2-ol-1-benzenesulfonic acid-O,O')borate、Lithium perchlorate (LiClO 4 ), lithium chloride (LiCl), lithium bromide (LiBr), lithium hydroxide (LiOH), lithium nitrate (LiNO 3 ), lithium sulfate (Li 2 SO 4 ), lithium sulfide (Li 2 S), lithium hydroxide (LiOH), etc. These may be used alone or in combination of two or more.
[0053] The additive includes at least any one of an alkaline earth metal salt, a dicarboxylic acid, a carboxylic anhydride, and an organic carbonate.
[0054] Any alkaline earth metal salt can be used as long as it is a compound that can be dissolved in a solvent containing water and dissociated, thereby causing alkaline earth metal cations to be present in the aqueous electrolyte. The alkaline earth metal salt preferably does not cause degradation of the battery characteristics due to reaction with the materials constituting the positive electrode and the negative electrode. Alkaline earth metal salts include salts of alkaline earth metals and anions. As alkaline earth metals, calcium, magnesium, strontium, and barium can be mentioned. Among them, calcium, magnesium, and strontium are preferred, and calcium is most preferred. This is because fluoride (CaF), which is the main coating component derived from the alkaline earth metal salt formed during the initial charge, 2 MgF 2 , SrF 2 , BaF 2 ) in water, CaF 2 MgF 2 , SrF 2 Lower, CaF 2Lowest. Low solubility in water means that the robustness of the coating to the aqueous electrolyte can be improved, and an electrochemically stable coating can be formed. Since an electrochemically stable coating can be formed, the reaction between the negative electrode active material and the electrolyte can be suppressed, and the self-discharge of lithium ions naturally released from the negative electrode active material by the lithium ions absorbed by the negative electrode active material can be suppressed. As the alkaline earth metal salt, an alkaline earth metal salt that is reduced and decomposed at a potential higher than the reduction and decomposition potential of water is appropriate. The alkaline earth metal salt can be used alone or in combination of two or more. The anion component can include, for example, anions represented by the following general formulas (viii) to (xi).
[0055] (R 10 SO 2 )(R 11 SO 2 )N - (viii)
[0056] (R 10 , R 11 are independently selected from alkyl or halogen-substituted alkyl. 10 and R 11 They may bond to each other to form a ring.)
[0057] R 12 SO 3 - (ix)
[0058] (R 12 is selected from alkyl or halogen-substituted alkyl. )
[0059] R 13 CO 2 - (x)
[0060] (R 13 is selected from alkyl or halogen-substituted alkyl. )
[0061] (R 14 SO 2 ) 3 C - (xi)
[0062] (R 14 is selected from alkyl or halogen-substituted alkyl. )
[0063] In the above general formulae (viii) to (xi), the carbon number of the alkyl group or the halogen-substituted alkyl group is preferably 1 to 6, more preferably 1 to 3, and even more preferably 1 to 2. The halogen in the halogen-substituted alkyl group is preferably fluorine. The number of halogen substitutions in the halogen-substituted alkyl group is equal to or less than the number of hydrogen atoms in the original alkyl group.
[0064] R 10 ~R 14Each of them is, for example, a group represented by the following general formula (xii).
[0065] C n H a F b Cl c Br d I e (xii)
[0066] (n is an integer greater than or equal to 1, a, b, c, d, and e are integers greater than or equal to 0, and 2n+1=a+b+c+d+e is satisfied.)
[0067] Specific examples of the organic anion represented by the general formula (viii) include bis(trifluoromethylsulfonyl)imide (TFSI; [N(CF 3 SO 2 ) 2 ] - ), bis(perfluoroethylsulfonyl)imide (BETI; [N(C 2 F 5 SO 2 ) 2 ] - ), (perfluoroethylsulfonyl)(trifluoromethylsulfonyl)imide ([N(C 2 F 5 SO 2 )(CF 3 SO 2 )] - ) etc. Specific examples of the organic anion represented by the general formula (ix) include CF 3 SO 3 - , C 2 F 5 SO 3 - As specific examples of the organic anion represented by the general formula (x), for example, CF 3 CO 2 - , C 2 F 5 CO 2 - As specific examples of the organic anion represented by the general formula (xi), for example, tris(trifluoromethylsulfonyl)carbonate ([(CF 3 SO 2 ) 3 C] - ), tris(perfluoroethylsulfonyl)carbonic acid ([(C 2 F 5 SO 2 ) 3 C]- ), bis(perfluoroethylsulfonyl)(trifluoromethylsulfonyl)carbonic acid ([(C 2 F 5 SO 2 ) 2 (CF 3 SO 2 )C] - ), (perfluoroethylsulfonyl)bis(trifluoromethylsulfonyl)carbonic acid ([(C 2 F 5 SO 2 )(CF 3 SO 2 ) 2 C] - )wait.
[0068] Examples of organic anions other than those of the general formulae (viii) to (xi) include bis(1,2-benzenediol (2-)-O,O')boric acid, bis(2,3-naphthalenediol (2-)-O,O')boric acid, bis(2,2'-biphenylediol (2-)-O,O')boric acid, and bis(5-fluoro-2-ol-1-benzenesulfonic acid-O,O')boric acid.
[0069] As anions constituting the alkaline earth metal salt, it is preferred to include a salt having an imide anion from the viewpoint of being able to effectively suppress the self-discharge of the battery. Suitable specific examples of the imide anion include, in addition to the imide anions exemplified as the organic anions represented by the general formula (viii), bis(fluorosulfonyl)imide (FSI; [N(FSO 2 ) 2 ] - ), (fluorosulfonyl)(trifluoromethylsulfonyl)imide (FTI; [N(FSO 2 )(CF 3 SO 2 )] - )wait.
[0070] From the viewpoint of being able to effectively suppress the self-discharge of the battery, the alkaline earth metal salt having an alkaline earth metal and an imide anion includes calcium bis(trifluoromethylsulfonyl)imide (CaTFSI), calcium bis(perfluoroethylsulfonyl)imide (CaBETI), calcium (perfluoroethylsulfonyl)(trifluoromethylsulfonyl)imide, calcium bis(fluorosulfonyl)imide (CaFSI), calcium (fluorosulfonyl)(trifluoromethylsulfonyl)imide (CaFTI), magnesium bis(trifluoromethylsulfonyl)imide (MgTFSI), magnesium bis(perfluoroethylsulfonyl)imide (MgBETI), (perfluoroethylsulfonyl) (trifluoromethylsulfonyl) magnesium imide, bis(fluorosulfonyl) magnesium imide (MgFSI), (fluorosulfonyl) (trifluoromethylsulfonyl) magnesium imide (MgFTI), bis(trifluoromethylsulfonyl) strontium imide (SrTFSI), bis(perfluoroethylsulfonyl) strontium imide (SrBETI), (perfluoroethylsulfonyl) (trifluoromethylsulfonyl) strontium imide, bis(fluorosulfonyl) strontium imide (SrFSI), (fluorosulfonyl) (trifluoromethylsulfonyl) strontium imide (SrFTI), etc. These can be used alone or in combination of two or more. Among them, calcium salts are particularly preferred. This is because: in the main coating component formed by reduction decomposition, CaF 2 Since the solubility in water is the lowest, the electrochemical stability of the film to the aqueous electrolyte can be improved. As the alkaline earth metal salt, an alkaline earth metal salt that undergoes reduction decomposition at a potential higher than the reduction decomposition potential of water is more suitable.
[0071] Specific examples of other alkaline earth metal salts include Ca[CF 3 SO 3 ] 2 , Ca[C 2 F 5 SO 3 ] 2 , Ca[CF 3 CO 2 ] 2 , Ca[C 2 F 5 CO 2 ] 2 , Ca[(CF 3 SO 2 ) 3 C] 2 , Ca[(C 2 F 5 SO 2 ) 3 C] 2 , Ca[(C 2 F 5 SO 2 ) 2 (CF3 SO 2 )C] 2 , Ca[(C 2 F 5 SO 2 )(CF 3 SO 2 ) 2 C] 2 、Calcium bis(1,2-benzenediol (2-)-O,O')borate、Calcium bis(2,3-naphthalenediol (2-)-O,O')borate、Calcium bis(2,2'-biphenylenediol (2-)-O,O')borate、Calcium bis(5-fluoro-2-ol-1-benzenesulfonic acid-O,O')borate、Calcium perchlorate (Ca(ClO 4 ) 2 ), calcium chloride (CaCl 2 ), calcium bromide (CaBr 2 ), calcium hydroxide (Ca(OH) 2 ), calcium nitrate (Ca(NO 3 ) 2 ), calcium sulfate (CaSO 4 ), calcium sulfide (CaS), calcium hydroxide (Ca(OH) 2 ),Mg[CF 3 SO 3 ] 2 Mg[C 2 F 5 SO 3 ] 2 Mg[CF 3 CO 2 ] 2 Mg[C 2 F 5 CO 2 ] 2 Mg[(CF 3 SO 2 ) 3 C] 2 Mg[(C 2 F 5 SO 2 ) 3 C] 2 Mg[(C 2 F 5 SO 2 ) 2 (CF 3 SO 2 )C] 2 Mg[(C 2 F 5 SO 2 )(CF 3 SO2 ) 2 C] 2 、Bis(1,2-benzenediol (2-)-O,O') magnesium borate、Bis(2,3-naphthalenediol (2-)-O,O') magnesium borate、Bis(2,2'-biphenylenediol (2-)-O,O') magnesium borate、Bis(5-fluoro-2-ol-1-benzenesulfonic acid-O,O') magnesium borate、Magnesium perchlorate (Mg(ClO 4 ) 2 ), magnesium chloride (MgCl 2 ), magnesium bromide (MgBr 2 )、Magnesium hydroxide (Mg(OH) 2 ), magnesium nitrate (Mg(NO 3 ) 2 ), magnesium sulfate (MgSO 4 ), magnesium sulfide (MgS), magnesium hydroxide (Mg(OH) 2 ), Sr[CF 3 SO 3 ] 2 , Sr[C 2 F 5 SO 3 ] 2 , Sr[CF 3 CO 2 ] 2 , Sr[C 2 F 5 CO 2 ] 2 、Sr[(CF 3 SO 2 ) 3 C] 2 、Sr[(C 2 F 5 SO 2 ) 3 C] 2 、Sr[(C 2 F 5 SO 2 ) 2 (CF 3 SO 2 )C] 2 、Sr[(C 2 F 5 SO 2 )(CF 3 SO 2 ) 2 C] 2, strontium bis(1,2-benzenediol (2-)-O,O')borate, strontium bis(2,3-naphthaleneediol (2-)-O,O')borate, strontium bis(2,2'-biphenylediol (2-)-O,O')borate, strontium bis(5-fluoro-2-ol-1-benzenesulfonic acid-O,O')borate, strontium perchlorate (Sr(ClO 4 ) 2 ), Strontium chloride (SrCl 2 ), Strontium bromide (SrBr 2 ), Strontium hydroxide (Sr(OH) 2 ), strontium nitrate (Sr(NO 3 ) 2 ), strontium sulfate (SrSO 4 ), strontium sulfide (SrS), strontium hydroxide (Sr(OH) 2 ) etc. These can be used alone or in combination of two or more. Among them, calcium salts are particularly preferred. This is because: among the main coating components formed by reduction decomposition, CaF 2 The solubility in water is the lowest, and the electrochemical stability of the film to the aqueous electrolyte can be improved. As the alkaline earth metal salt, an alkaline earth metal salt that undergoes reduction decomposition at a potential higher than the reduction decomposition potential of water is suitable.
[0072] Among the above, calcium bis(trifluoromethylsulfonyl)imide, magnesium bis(trifluoromethylsulfonyl)imide, strontium bis(trifluoromethylsulfonyl)imide, etc. are preferred from the viewpoint of being able to effectively suppress the self-discharge of the battery. Among them, calcium bis(trifluoromethylsulfonyl)imide, etc., which are calcium salts, are most preferred. This is because: in the solubility of fluoride, which is a coating component formed by reduction decomposition, in water, CaF 2 MgF 2 , SrF 2 Lower, CaF 2 The lowest. In addition, it is because the reduction decomposition is carried out at a potential higher than the hydrolysis potential. The reason why the bis(trifluoromethylsulfonyl)imide anion is preferred is because it is suitable when adjusting a high-concentration aqueous electrolyte. In addition, it is suitable from the viewpoint of forming a fluoride at a potential higher than the hydrolysis potential.
[0073] The alkaline earth metal salt may be, for example, 0.1% by mass or more and 5.0% by mass or less, preferably 0.5% by mass or more and 3.0% by mass or less, relative to the total amount of the aqueous electrolyte. By setting the above range, the self-discharge of the battery can sometimes be effectively suppressed without damaging the lithium ion conductivity of the aqueous electrolyte. When the addition amount is greater than 5.0wt.%, the lithium ion conductivity is sometimes reduced. On the other hand, when it is less than 0.1wt.%, a sufficient effect may sometimes not be obtained.
[0074] Dicarboxylic acids include, for example, succinic acid, glutaric acid, phthalic acid, maleic acid, citraconic acid, glutaconic acid, itaconic acid, diglycolic acid, etc. As carboxylic anhydrides, for example, succinic anhydride, glutaric anhydride, phthalic anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, diglycolic anhydride, etc. can be mentioned. Among the above, from the perspective of being able to effectively suppress the self-discharge of the battery, succinic acid, succinic anhydride, maleic acid, maleic anhydride, diglycolic acid, glutaric acid, etc. are preferred. Among them, succinic acid, succinic anhydride, maleic acid, maleic anhydride, diglycolic acid are preferred. This is because: although it also varies depending on the type of silane coupling agent used, it is preferred from the perspective of being able to be reduced and decomposed above the reduction decomposition potential of water and above the reduction decomposition potential region of the silane coupling agent. The reduction decomposition of glutaric acid is carried out competitively with the reduction decomposition of water, so the effect is reduced.
[0075] Relative to the total amount of the aqueous electrolyte, the dicarboxylic acid or carboxylic anhydride can be, for example, 0.1 mass % or more and 5.0 mass % or less, preferably 0.5 mass % or more and 3.0 mass % or less. By setting it to the above range, the self-discharge characteristics of the battery can sometimes be effectively suppressed without damaging the lithium ion conductivity of the aqueous electrolyte. When the addition amount is greater than 5.0wt.%, the lithium ion conductivity is sometimes reduced. In addition, there is a concern that the ratio of the components of the coating derived from the silane coupling agent in the coating is reduced and the resistance of the coating is increased. On the other hand, when it is less than 0.1wt.%, sometimes a sufficient effect cannot be obtained.
[0076] Examples of organic carbonates include cyclic carbonates such as ethylene carbonate, propylene carbonate, vinylene carbonate (vinylidene carbonate), and butylene carbonate; chain carbonates such as dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate; and fluorinated carbonates containing fluorine as a constituent element such as fluoroethylene carbonate, fluorodimethyl carbonate, and methyl fluoropropionate (FMP).
[0077] From the perspective of suppressing the self-discharge of the battery, improving the charge and discharge efficiency of the battery, etc., organic carbonates are preferred among the additives, and in particular, cyclic carbonates and fluorinated carbonates containing fluorine as constituent elements are preferred among the organic carbonates exemplified above. In addition, from the perspective of suppressing the reduction of the self-discharge of the battery, improving the charge and discharge efficiency of the battery, etc., the organic carbonate is preferably reduced and decomposed at a potential lower than the reduction and decomposition potential of the silane coupling agent described later. The reduction and decomposition potential of the organic carbonate also depends on the type of the silane coupling agent, but is preferably less than 2.2V based on the Li standard. As organic carbonates that are reduced and decomposed below 2.2V based on the Li standard, for example, dimethyl carbonate, fluoroethylene carbonate, etc. can be cited. Organic carbonates are reduced and decomposed at a potential lower than that of the silane coupling agent, so that the defects of the coating derived from the silane coupling agent can be compensated by the coating derived from the organic carbonate, and the compactness of the coating can be improved. That is, the coating based on the reductive decomposition of the organic carbonate is deposited on the coating based on the reductive decomposition of the silane coupling agent. As a result, the peak intensity of the bond energy (686 eV) derived from LiF in the F1s spectrum of XPS is set to I C The peak intensity of the bond energy (688.8 eV) derived from the unreacted silane coupling agent CF species (fluoroalkyl) is set as I D When the peak intensity of the surface layer on the electrolyte side of the coating is I C >I D . As a result, the reaction between the negative electrode active material and the electrolyte is suppressed, so the self-discharge of lithium ions absorbed by the negative electrode active material and naturally released from the negative electrode active material is suppressed, which can improve the charge and discharge efficiency of the battery. By adding an organic carbonate containing fluorine as a constituent element as an organic carbonate, the ratio of components containing fluorine and having low solubility in water (such as LiF) can be increased, and the robustness to the aqueous electrolyte can be further improved, and further, there is a tendency to form an electrochemically stable film.
[0078] The organic carbonate is preferably present in a molar ratio of 1:0.01 to 1:5 relative to the lithium salt, more preferably in a molar ratio of 1:0.05 to 1:1, and water is preferably present in a molar ratio of 1:0.5 to 1:4 relative to the lithium salt, more preferably in a molar ratio of 1:1 to 1:2.5. By setting the above range, the reduction of the self-discharge of the battery can sometimes be effectively suppressed, or the charge and discharge efficiency of the battery can be further improved.
[0079] The positive electrode 22, for example, comprises a positive electrode current collector and a positive electrode composite material layer formed on the positive electrode current collector. As the positive electrode current collector, a foil of a metal that is electrochemically stable and chemically stable within the potential range of the positive electrode, and a thin film having the metal disposed on the surface layer, etc. can be used. The form of the positive electrode current collector is not particularly limited, and for example, a porous body such as a mesh body, a punched sheet, and a porous metal mesh of the metal can also be used. As the material of the positive electrode current collector, a known metal that can be used for a secondary battery using an aqueous electrolyte can be used. As such a metal, for example, stainless steel, Al, an aluminum alloy, Ti, etc. can be cited. From the viewpoint of current collection, mechanical strength, etc., the thickness of the positive electrode current collector is, for example, preferably 3 μm or more and 50 μm or less.
[0080] The positive electrode composite material layer contains a positive electrode active material. In addition, the positive electrode composite material layer may also contain a binder, a conductive material, and the like.
[0081] Examples of positive electrode active materials include lithium transition metal oxides containing lithium (Li) and transition metal elements such as cobalt (Co), manganese (Mn) and nickel (Ni). Examples of positive electrode active materials include transition metal sulfides, metal oxides, lithium iron phosphate (LiFePO 4 ), lithium iron pyrophosphate (Li 2 FeP 2 O 7 ) and other lithium-containing polyanion compounds containing one or more transition metals, sulfur compounds (Li 2 S), oxygen, oxygen-containing metal salts such as lithium oxide, etc. As the positive electrode active material, preferably a lithium-containing transition metal oxide, preferably containing at least one of Co, Mn and Ni as a transition metal element.
[0082] Lithium transition metal oxides may also include other added elements besides Co, Mn and Ni, for example, aluminum (Al), zirconium (Zr), boron (B), magnesium (Mg), scandium (Sc), yttrium (Y), titanium (Ti), iron (Fe), copper (Cu), zinc (Zn), chromium (Cr), lead (Pb), tin (Sn), sodium (Na), potassium (K), barium (Ba), strontium (Sr), calcium (Ca), tungsten (W), molybdenum (Mo), niobium (Nb) and silicon (Si), etc.
[0083] Specific examples of lithium transition metal oxides include Li x CoO 2 , Li x NiO 2 , Li x MnO 2 , Li x Co y Ni 1-y O 2 , Lix Co y M 1-y O z , Li x Ni 1-y M y O z , Li x Mn 2 O 4 , Li x Mn 2-y M y O 4 、LiMPO 4 , Li 2 MPO 4 F (in each chemical formula, M is at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb and B, 0<x≤1.2, 0<y≤0.9, 2.0≤z≤2.3). Lithium transition metal oxides can be used alone or in combination. From the viewpoint of high capacity, lithium transition metal oxides preferably contain more than 80 mol% Ni relative to the total amount of transition metals other than lithium. In addition, from the viewpoint of the stability of the crystal structure, lithium transition metal oxides are more preferably Li a Ni b Co c Al d O 2 (0<a≤1.2, 0.8≤b<1, 0<c<0.2, 0<d≤0.1, b+c+d=1).
[0084] As conductive material, known conductive material for improving the conductivity of positive composite material layer can be used, such as carbon black, acetylene black, Ketjen black, graphite, carbon nanofiber, carbon nanotube, graphene and other carbon materials can be cited. As binding material, known binding material for maintaining the good contact state of positive active material and conductive material, and improving the bonding property of positive active material and the like to the positive current collector surface can be used, such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF) and other fluororesins, polyacrylonitrile (PAN), polyimide, acrylic resin, polyolefin, carboxymethyl cellulose (CMC) or its salt, styrene-butadiene rubber (SBR), polyethylene oxide (PEO), polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP) and the like can be cited.
[0085] The positive electrode 22 can be manufactured, for example, by coating a positive electrode composite material slurry containing a positive electrode active material, a binder, a conductive material, etc. on a positive electrode current collector, and drying and rolling the coating to form a positive electrode composite material layer on the positive electrode current collector.
[0086] The negative electrode 23, for example, includes a negative electrode collector and a negative electrode composite material layer formed on the negative electrode collector. As the negative electrode collector, a foil of a metal that is electrochemically stable and chemically stable within the potential range of the negative electrode, and a thin film of the metal disposed on the surface layer, etc. can be used. The form of the negative electrode collector is not particularly limited, and for example, a porous body such as a mesh body, a punched sheet, and a porous metal mesh of the metal can also be used. As the material of the negative electrode collector, a known metal that can be used for a secondary battery using an aqueous electrolyte can be used. As such a metal, for example, Al, Ti, Mg, Zn, Pb, Sn, Zr, In, etc. can be cited. These can be used alone, or two or more alloys can be used, and the material can be composed of at least one as the main component. In addition, when containing two or more elements, it is not necessary to be alloyed. From the viewpoint of current collection, mechanical strength, etc., the thickness of the negative electrode collector is preferably, for example, 3 μm or more and 50 μm or less.
[0087] The negative electrode composite material layer includes a negative electrode active material. A silane coupling agent described below is attached to the surface of the negative electrode active material. In addition, the negative electrode composite material layer may also include a binding material, a conductive material, etc. The conductive material and the binding material may use the same materials as those on the positive electrode side.
[0088] The negative electrode active material can use a known negative electrode active material that can be used for a secondary battery using a non-aqueous electrolyte in the past. Examples of such negative electrode active materials include carbonaceous materials such as natural graphite (graphite), artificial graphite (graphite), soft carbon, hard carbon and other amorphous carbon. As another example, metal compounds such as alloys containing lithium elements, metal oxides, metal sulfides, and metal nitrides, silicon, etc. can be mentioned. For example, as alloys containing lithium elements, examples such as lithium aluminum alloys, lithium tin alloys, lithium lead alloys, and lithium silicon alloys can be mentioned. In addition, as metal oxides containing lithium elements, examples such as lithium titanate (Li 4 Ti 5 O 12 Etc.). In addition, as metal nitrides containing lithium elements, for example, lithium cobalt nitride, lithium iron nitride, lithium manganese nitride, etc. can be cited. Furthermore, sulfur compounds can also be exemplified. These negative electrode active materials can be used alone or in combination of two or more. By the secondary battery 20 of this embodiment, the reduction reaction of water is suppressed, so carbon materials, lithium tin alloy materials, lithium silicon alloy materials, etc., which were previously more difficult, can be used as negative electrode active materials for batteries using aqueous electrolytes. In addition, carbon material can be used as the main component. It should be noted that the main component refers to the component with the highest content in the negative electrode active material.
[0089] The negative electrode 23 can be manufactured, for example, by coating a negative electrode composite material slurry containing a negative electrode active material, a binder, etc. on a negative electrode current collector, and drying and rolling the coating film to form a negative electrode composite material layer on the negative electrode current collector.
[0090] The silane coupling agent attached to the surface of the negative electrode active material is reduced and decomposed during the initial charging process of the secondary battery. In addition, an electrochemically stable coating is formed on the surface of the negative electrode active material through the reduction and decomposition of the silane coupling agent. The coating is an electrochemically stable coating, so water reduction and decomposition will hardly occur with the coating as an active point. In addition, since it is a coating that is chemically stable to the aqueous electrolyte, the corrosion caused by the aqueous electrolyte is suppressed, and the contact of the aqueous electrolyte with the surface of the negative electrode active material can be suppressed. It should be noted that the coating derived from the silane coupling agent has lithium ion conductivity, so during the charge and discharge process, lithium ions are absorbed and released by the negative electrode active material through the coating.
[0091] From the perspective of inhibiting the reduction decomposition of water and inhibiting the self-discharge of the battery, the silane coupling agent preferably contains fluorine as a constituent element, and preferably undergoes reduction decomposition at a potential higher than the reduction decomposition potential of water. From the perspective of facilitating the reduction decomposition of water, the reduction decomposition potential of the silane coupling agent is based on the Li standard (vs. Li / Li + ) is preferably 2.1V or more, more preferably 2.2V or more, and more preferably 2.4V or more. This is because it is preferred from the viewpoint of avoiding competitive reduction and decomposition of water, so that it is completely covered by a dense film before reaching the reduction and decomposition potential of water. The upper limit value is not particularly limited, for example, it is preferably 3V or less based on Li. This is because the potential at which the negative electrode current collector does not undergo oxidative dissolution is ideal.
[0092] In addition, from the viewpoint of inhibiting the reduction decomposition of water and inhibiting the self-discharge of the battery, the silane coupling agent containing fluorine as a constituent element is preferably a fluoroalkylsilane, and more preferably a fluoroalkylsilane that is reduction-decomposed at a potential higher than the reduction decomposition potential of water. Specifically, a fluoroalkylsilane represented by the following chemical formula is preferred.
[0093]
[0094] (wherein, Y1 is a fluoroalkyl group having 3 to 10 carbon atoms and 7 to 21 fluorine atoms, which may be linear or branched, and may contain at least one of an ether bond, an ester bond, a peptide bond, a vinyl bond, a sulfonamide bond, and a hydrogen atom, and Y2 is (CH 2 ) n Indicates that n is an integer of 0 to 6, Y2 may be linear or branched, and R1, R2 and R3 are each independently an alkoxy group, an alkyl group, an amino group, a halogen atom, or a hydrogen atom).
[0095] The carbon number and fluorine number of Y1 are preferably 5 to 8 and 11 to 17, respectively, from the viewpoints of reducing and decomposing at a potential higher than the reducing and decomposing potential of water and facilitating the suppression of reducing and decomposing water.
[0096] Examples of the fluoroalkylsilane in which Y1 is a fluoroalkyl group having a peptide bond include N-(3-trimethoxysilylpropyl)perfluorohexanamide.
[0097]
[0098] Examples of the fluoroalkylsilane in which Y1 is a fluoroalkyl group having a vinyl bond include hexafluorododec-11-en-1-yltrimethoxysilane.
[0099]
[0100] Examples of the fluoroalkylsilane in which Y1 is a fluoroalkyl group having a sulfonamide bond include 3-perfluorooctylsulfonylaminopropyltriethoxysilane.
[0101]
[0102] Examples of the fluoroalkylsilane in which Y1 is a fluoroalkyl group having a hydrogen atom include dodecafluoroheptyl-propyltrimethoxysilane and dodecafluoroheptyl-propylmethyldimethoxysilane.
[0103]
[0104] Examples of the fluoroalkylsilane in which Y1 is a branched fluoroalkyl group include triethoxy[5,5,6,6,7,7,7-heptafluoro-4,4-bis(trifluoromethyl)heptyl]silane.
[0105]
[0106] Examples of the fluoroalkylsilane in which Y2 is a branched chain include 4-methyl-(perfluorohexylethyl)propyltrimethoxysilane.
[0107]
[0108] As the fluoroalkylsilane, it is more preferable that Y1 is C n F 2n+1 (5≤n≤10), more preferably R1, R2 and R3 are each independently OC n H 2n+1 (1≤n≤5) or C n H 2n+1(1≤n≤5). The longer the alkyl chain length of Y1, the more preferred it is. This is because it can increase the fluorination rate in the silane coupling agent and increase the amount of fluorine in the coating. R1, R2 and R3 are more preferably fluoroalkylsilanes containing methoxy groups. This is because it can further increase the reactivity with the hydrophilic groups such as hydroxyl groups on the surface of the above-mentioned negative electrode active material. Specifically, the fluoroalkylsilane is more preferably C 5 F 11 CH 2 CH 2 -Si(OCH 3 ) 3 , C 6 F 13 CH 2 CH 2 -Si(OCH 3 ) 3 , C 8 F 17 CH 2 CH 2 -Si(OCH 3 ) 3 At least one of the following.
[0109] The content of the silane coupling agent is preferably in the range of 0.01 mass % to 10 mass % relative to the mass of the negative electrode active material. By setting the content of the silane coupling agent to the above range, the self-discharge of the battery can be further suppressed. When the amount of the silane coupling agent is less than 0.01 mass %, it is difficult to completely cover the surface of the negative electrode active material with the coating derived from the silane coupling agent. As a result, there is a concern that the decomposition of the aqueous electrolyte cannot be blocked by the coating derived from the silane coupling agent and the potential window on the reduction side cannot be expanded. In addition, when the added amount is greater than 10wt.%, it is better from the point of view of covering the surface of the negative electrode active material with a coating derived from the silane coupling agent, but there is a concern that the lithium ion conductivity in the coating is damaged, that is, the resistance is increased. The amount of the silane coupling agent can be calculated by using the Stuart-Briegleb molecular model according to the BET specific surface area (m 2 / g), the molecular weight of the silane coupling agent (g / mol), and the minimum estimated amount required is calculated using the following formula. From the viewpoint of completely covering the surface of the negative electrode active material with a film derived from the silane coupling agent, it is ideal to use a silane coupling agent above the amount calculated by the following formula.
[0110] Amount of silane coupling agent (g)
[0111] = weight of negative electrode active material (g) × specific surface area of negative electrode active material (m 2 / g)÷Minimum coverage area of silane coupling agent (m 2 / g)
[0112] Minimum coverage area of silane coupling agent (m 2 / g)
[0113] =6.02×10 23 ×13×10 -20 ÷Molecular weight of silane coupling agent (g / mol)
[0114] Methods for attaching the silane coupling agent to the surface of the negative electrode active material include, for example, a method of directly spraying a solution of the silane coupling agent on the negative electrode composite material layer of the negative electrode 23 and drying it, a method of vaporizing the solution of the silane coupling agent and contacting the vaporized silane coupling agent with the negative electrode composite material layer of the negative electrode 23, etc. It is preferred to ozone the negative electrode composite material layer containing the negative electrode active material before attaching the silane coupling agent to the surface of the negative electrode active material. As methods for ozone treatment, for example, UV ozone treatment, atmospheric plasma treatment, etc. can be cited. Among them, UV ozone treatment is preferred. UV ozone treatment is performed, for example, using a UV cleaning surface modification device (ASM1101N) (Asumi Technology Research Co., Ltd.). It should be noted that the silane coupling agent can be attached to the powder of the negative electrode active material before making the negative electrode 23, or the silane coupling agent can be added to the negative electrode composite material slurry so that it adheres to the surface of the negative electrode active material.
[0115] After the secondary battery 20 of the present embodiment is charged, a coating film derived from a silane coupling agent, such as LiF, SiO x (0<x<2), Li 2 CO 3 , Li 2 O and other components. It is believed that the film contains LiF, SiO x (0<x<2), thereby being electrochemically stable, and on the other hand, forming a coating showing lithium ion conductivity. It should be noted that by using the above-mentioned fluoroalkylsilane as a silane coupling agent, LiF and SiO in the coating x The ratio of (0<x<2) tends to increase.
[0116] For the above SiO x In general, it is preferred that the valence of Si changes from the surface side of the coating to the deepest side to a low valence. In addition, the above-mentioned LiF is preferably present more heavily on the deepest side of the coating. The deepest side of the coating refers to the contact surface side with the surface of the negative electrode active material. That is, the peak intensity of the bond energy (686 eV) derived from LiF in the F1s spectrum of XPS is set to I A The peak intensity of the bond energy (688.8 eV) from the unreacted silane coupling agent (fluoroalkyl) is set as I B When the peak intensity increases from the deepest side of the coating to the surface layer on the electrolyte side, A >I BChange to I A <I B . These characteristics are achieved, for example, by using the aforementioned fluoroalkylsilane as a silane coupling agent. In addition, a coating having these characteristics means that unreacted or low-reduced silane coupling agent remains on the surface of the electrolyte side, and the surface layer of the coating on the electrolyte side becomes water-repellent due to the effect of the remaining unreacted or low-reduced silane coupling agent. As a result, the penetration of water to the surface of the negative electrode active material can be suppressed in the coating, resulting in an electrochemically stable coating. By adding an additive that forms a coating by reduction decomposition at a potential above the reduction decomposition potential region of the silane coupling agent, the amount of residual unreacted or low-reduced silane coupling agent can be greatly increased. Examples of such additives include alkaline earth metal salts, dicarboxylic acids, and carboxylic anhydrides. When only alkaline earth metal salts, dicarboxylic acids, and carboxylic anhydrides are added to the electrolyte, almost no CaF derived from CaTFSI is formed before the hydrolysis potential. 2 , LiF derived from LiTFSI anion, most of the coating components are Li that is highly soluble in water 2 CO 3 , Li 2 O.
[0117] After the secondary battery 20 of the present embodiment is charged, the coating film derived from the silane coupling agent formed on the surface of the negative electrode active material may further include fluoride (CaF) corresponding to the type of the alkaline earth metal when the additive includes an alkaline earth metal salt. 2 MgF 2 , SrF 2 , BaF 2 Fluoride (CaF) as a coating component derived from alkaline earth metal salts 2 MgF 2 , SrF 2 , BaF 2 ) has a lower solubility in water than LiF, which is a fluoride derived from a silane coupling agent. Therefore, by combining with an alkaline earth metal salt, the robustness of the film derived from the silane coupling agent to the aqueous electrolyte can be improved. In addition, by the presence of an alkaline earth metal salt that is reductively decomposed at a higher potential, the dissolved CO dissolved in the aqueous electrolyte can be suppressed. 2 , dissolved O 2 The electrochemical reduction reaction of Li 2 CO 3 , Li 2O formation. In addition, when using an alkaline earth metal salt that is reductively decomposed at a potential above the reductive decomposition potential region of the silane coupling agent, the reduction reaction of the silane coupling agent is suppressed, and a large amount of unreacted or low-reduced sites of the silane coupling agent (fluoroalkyl (F1s, 688.8eV (XPS)), C-Si-O group (Si2p, 102.6eV (XPS)), O-Si-C group (Si2p, 103.5eV (XPS)), etc.) can be intentionally left in the film. As a result, the unreacted or low-reduced sites of the silane coupling agent remain in the film, and the penetration of water into the surface of the negative electrode active material can be suppressed. Through the above effects, the robustness to aqueous electrolytes can be further improved, resulting in an electrochemically stable film. This is because: when only alkaline earth metal salts are added to the electrolyte, when the film is formed, it is impossible to avoid the contact of water with the surface of the negative electrode active material, and it is impossible to suppress the dissolution of CO 2 , dissolved O 2 The electrochemical reduction reaction turns into Li 2 CO 3 , Li 2 The coating has a high O content. Therefore, before the reduction and decomposition of water begins, it is not possible to form an electrochemically stable coating that is sufficiently robust to the aqueous electrolyte. 2 CO 3 , Li 2 In order to reduce the O component ratio, it is necessary to combine with the following silane coupling agent, which can form a uniform coating on the entire surface of the negative electrode active material during the initial charge in a state where the silane coupling agent is attached to the surface of the negative electrode active material in advance and water is prevented from contacting the surface of the negative electrode active material. In addition, in order to avoid water contacting the surface of the negative electrode active material, it is necessary to combine with an alkaline earth metal salt that is reductively decomposed above the reductive decomposition potential region of the silane coupling agent.
[0118] After charging of the secondary battery 20 of the present embodiment, the coating film derived from the silane coupling agent formed on the surface of the negative electrode active material can suppress the dissolved CO dissolved in the aqueous electrolyte when the additive includes dicarboxylic acid or carboxylic anhydride. 2 , dissolved O 2 The electrochemical reduction reaction of Li 2 CO 3 , Li 2O formation. In addition, when a dicarboxylic acid or carboxylic anhydride that is reductively decomposed at a potential above the reductive decomposition potential region of the silane coupling agent is present, the reduction reaction of the silane coupling agent is suppressed, and a large amount of unreacted or low-reduced sites of the silane coupling agent (fluoroalkyl (F1s, 688.8eV (XPS)), C-Si-O group (Si2p, 102.6eV (XPS)), O-Si-C group (Si2p, 103.5eV (XPS)), etc.) can be intentionally left in the film. As a result of the unreacted or low-reduced sites of the silane coupling agent remaining in the film, the penetration of water into the surface of the negative electrode active material can be suppressed. Through the above effects, the robustness to aqueous electrolytes can be further improved to form an electrochemically stable film. This is because: when only dicarboxylic acids and carboxylic anhydrides are added to the electrolyte, LiF derived from LiTFSI anions can hardly be formed before the reductive decomposition of water, and most of the coating components become Li with high solubility in water. 2 CO 3 , Li 2 O, before the reduction and decomposition of water begins, it is impossible to form an electrochemically stable film that is sufficiently robust to the aqueous electrolyte on the surface of the negative electrode active material. In a state where the silane coupling agent is attached to the surface of the negative electrode active material in advance and water intrusion into the surface of the negative electrode active material is avoided, it is necessary to form a uniform film on the entire surface of the negative electrode active material during the initial charge. In addition, it is important to select a dicarboxylic acid or carboxylic anhydride that is reductively decomposed above the reductive decomposition potential region of the silane coupling agent.
[0119] As long as the separator 24 has the function of allowing lithium ions to pass through and electrically separating the positive electrode and the negative electrode, there is no particular limitation. For example, a porous sheet composed of a resin, an inorganic material, etc. can be used. As specific examples of porous sheets, microporous films, woven fabrics, non-woven fabrics, etc. can be cited. As materials for the separator, olefin resins such as polyethylene and polypropylene, polyamide, polyamide-imide, cellulose, etc. can be cited. As inorganic materials constituting the separator, glasses and ceramics such as borosilicate glass, silicon dioxide, aluminum oxide, and titanium oxide can be cited. The separator can also be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin resin. In addition, it can also be a multilayer separator comprising a polyethylene layer and a polypropylene layer, and a separator formed by coating the surface of the separator with materials such as aramid resins and ceramics can also be used.
[0120] Example
[0121] Hereinafter, the present disclosure will be further described by way of examples, but the present disclosure is not limited to these examples.
[0122] <Example 1>
[0123] [negative electrode]
[0124] Hard carbon as a negative electrode active material and PVDF as a binder were mixed in N-methyl-2-pyrrolidone (NMP) at a solid content mass ratio of 96:4 to prepare a negative electrode composite material slurry. Next, the negative electrode composite material slurry was applied to a negative electrode collector formed of copper foil, and after the coating was dried, it was rolled using a calendering roll to produce an electrode.
[0125] A fluoroalkylsilane solution (composition: CF 3 (CF 2 ) 7 CH 2 CH 2 -Si-(OCH 3 ) 3 ) and the electrode are placed in a metal container with a lid, and the metal container is placed in a thermostatic bath and heated at 120°C for 12 hours in a drying room (dew point: below -40°C). Through this treatment, the fluoroalkylsilane is volatilized and adhered to the surface of the negative electrode active material constituting the electrode. The electrode after the above treatment is cut into a specified size to obtain a negative electrode. The coating amount and packing density of the negative electrode are 32.3g / m 2 , 1.0gcm -3 .
[0126] [positive electrode]
[0127] LiCoO as the positive electrode active material 2 , carbon black as a conductive material and PVdF as a binder are mixed in NMP at a mass ratio of 94:3:3 to prepare a positive electrode composite material slurry. Next, the positive electrode composite material slurry is coated on the positive electrode collector formed by Ti foil, and after the coating film is dried, it is rolled by a calendering roller. Then, it is cut into a specified electrode size to obtain a positive electrode. The coating amount and filling density of the positive electrode are 65.0g / cm 2 , 2.8gcm -3 .
[0128] [Electrolyte]
[0129] 1 mass % of calcium bis(trifluoromethylsulfonyl)imide (CaTFSI) was added to a solution in which a lithium salt (LITFSI:LIBETI=0.7:0.3 (molar ratio)) and water were mixed at a molar ratio of 1:2 to prepare an electrolyte solution.
[0130] [Three-electrode battery cell]
[0131] A three-electrode battery cell containing the above electrolyte was constructed using the above negative electrode as a working electrode, the above positive electrode as a counter electrode, and Ag / AgCl (3M NaCl) as a reference electrode.
[0132] <Example 2>
[0133] In the preparation of the electrolyte solution, a three-electrode battery cell was constructed in the same manner as in Example 1 except that 1 mass % of maleic acid was added instead of calcium bis(trifluoromethylsulfonyl)imide.
[0134] <Example 3>
[0135] In the preparation of the electrolyte solution, a three-electrode battery cell was constructed in the same manner as in Example 1 except that 1 mass % of diglycolic acid was added instead of calcium bis(trifluoromethylsulfonyl)imide.
[0136] <Example 4>
[0137] In the preparation of the electrolyte solution, a three-electrode battery cell was constructed in the same manner as in Example 1 except that 1% by mass of glutaric acid was added instead of calcium bis(trifluoromethylsulfonyl)imide.
[0138] <Example 5>
[0139] In the preparation of the electrolyte solution, a three-electrode battery cell was constructed in the same manner as in Example 1 except that 1 mass % of succinic anhydride was added instead of calcium bis(trifluoromethylsulfonyl)imide.
[0140] <Example 6>
[0141] In the preparation of the electrolyte solution, a three-electrode battery cell was constructed in the same manner as in Example 1 except that 0.5 mass % of succinic acid and 0.5 mass % of maleic anhydride were added instead of calcium bis(trifluoromethylsulfonyl)imide.
[0142] <Comparative Example 1>
[0143] A three-electrode battery cell was constructed in the same manner as in Example 1 except that no treatment was performed to allow fluoroalkylsilane to adhere to the surface of the negative electrode active material in the preparation of the negative electrode (working electrode) and no calcium bis(trifluoromethylsulfonyl)imide was added in the preparation of the electrolyte.
[0144] <Comparative Examples 2 to 7>
[0145] In Comparative Examples 2 to 7, the negative electrodes (working electrodes) were prepared in the same manner as in Examples 1 to 6, except that the treatment for making fluoroalkylsilane adhere to the surface of the negative electrode active material was not performed.
[0146] <Comparative Example 8>
[0147] In the preparation of the electrolyte solution, a three-electrode battery cell was constructed in the same manner as in Example 1 except that calcium bis(trifluoromethylsulfonyl)imide was not added.
[0148] The OCP of the negative electrode was measured by linear sweep voltammetry using the three-electrode battery cells of Examples 1 to 6 and Comparative Examples 1 to 8. The measurement conditions are shown below.
[0149] Starting potential: OCV
[0150] Potential scanning range: -3.238V~OCV vs.Ag / AgCl(3M NaCl)
[0151] OCP measurement time: 30 minutes after potential scanning to -3.238 V vs. Ag / AgCl (3M NaCl)
[0152] Scan speed: 0.1mV / sec
[0153] Measurement temperature: 25℃
[0154] The results of the negative electrode OCP after 0 minute (OCP after the potential was scanned to -3.238 V), the negative electrode OCP after 1 minute (OCP after 1 minute after the potential was scanned to -3.238 V), the negative electrode OCP after 10 minutes (OCP after 10 minutes after the potential was scanned to -3.238 V), and the negative electrode OCP after 20 minutes (OCP after 20 minutes after the potential was scanned to -3.238 V) in Examples 1 to 6 and Comparative Examples 1 to 8 are shown in Table 1. The negative electrode OCP shown in Table 1 is converted to a lithium standard (vs. Li / Li + ) value.
[0155] [Table 1]
[0156]
[0157] Comparing Example 1 and Comparative Example 2, Example 2 and Comparative Example 3, Example 3 and Comparative Example 4, Example 4 and Comparative Example 5, Example 5 and Comparative Example 6, and Example 6 and Comparative Example 7, which have the same composition of the aqueous electrolyte in Table 1, the OCP of the negative electrode after 0 minutes to 20 minutes shows lower values in all the examples.
[0158] The examples show that by adding alkaline earth metal salts, dicarboxylic acids, and carboxylic anhydrides to the aqueous electrolyte in addition to fluoroalkyl silane on the surface of the negative electrode active material, the absorption and storage of lithium ions to the negative electrode active material is improved, and the absorbed lithium ions become easy to accumulate in the negative electrode active material. On the other hand, the OCP of the negative electrode of Comparative Examples 1 to 7 changes dramatically from 0 minutes to 20 minutes. This means that almost no absorption and storage of lithium ions occurs, or even if it occurs, the absorbed lithium ions are not accumulated in the negative electrode active material, but are released instantly. Therefore, for Examples 1 to 6 in which alkaline earth metal salts, dicarboxylic acids, and carboxylic anhydrides are added to the aqueous electrolyte in addition to attaching the silane coupling agent to the surface of the negative electrode active material, it can be said that self-discharge is suppressed compared to Comparative Examples 1 to 7 in which the silane coupling agent is not attached to the surface of the negative electrode active material. Furthermore, compared with Comparative Example 8 in which the silane coupling agent is attached to the surface of the negative electrode active material but alkaline earth metal salt, dicarboxylic acid, and carboxylic anhydride are not added to the aqueous electrolyte, Examples 1 to 6 have lower OCP values at the negative electrode after 10 minutes and 20 minutes. This means that even after 20 minutes, more lithium ions are accumulated in the negative electrode active material of Examples 1 to 6. Therefore, compared with Comparative Example 8 in which the above compounds are not added to the aqueous electrolyte, Examples 1 to 6 in which alkaline earth metal salt, dicarboxylic acid, and carboxylic anhydride are added to the aqueous electrolyte can be said to have more suppressed self-discharge. This is because: for Examples 1 to 6 in which only CaTFSI, maleic acid, diglycolic acid, glutaric acid, succinic anhydride, and succinic acid and maleic anhydride are added in addition to attaching fluoroalkyl silane, there is an additive that is reductively decomposed at a higher potential, thereby dissolving O 2 , dissolved CO 2 The electrochemical reduction reaction of Li 2 CO 3 , Li 2 O component ratio can improve the robustness of the film to the aqueous electrolyte and form an electrochemically stable film. On the other hand, in Comparative Examples 2 to 7 in which only CaTFSI, maleic acid, diglycolic acid, glutaric acid, succinic anhydride, and succinic acid and maleic anhydride were added, almost no CaTFSI-derived CaF was formed before the reduction and decomposition of water. 2 , LiF derived from LiTFSI, most of the coating components are Li that is highly soluble in water 2 CO 3 , Li 2 O. In Comparative Example 8 in which only fluoroalkylsilane was attached, the coating was derived from fluoroalkylsilane. Compared with the case where only CaTFSI, maleic acid, diglycolic acid, glutaric acid, succinic anhydride, and succinic acid and maleic anhydride were added before the reduction and decomposition of water, the surface of the negative electrode active material could be covered with a large amount of LiF. However, while the fluoroalkylsilane was reduced and decomposed, the water repellency of the surface of the negative electrode active material decreased, and the dissolved O2 , dissolved CO 2 The electrochemical reduction reaction takes place to form Li 2 CO 3 , Li 2 The coating with a high O component ratio. Therefore, for Comparative Examples 2 to 7 in which only CaTFSI, maleic acid, diglycolic acid, glutaric acid, succinic anhydride, and succinic acid and maleic anhydride were added, and Comparative Example 8 in which only fluoroalkylsilane was attached, the coating had low robustness to the aqueous electrolyte and became an electrochemically unstable coating. Therefore, it was difficult to significantly suppress self-discharge.
[0159] <Example 7>
[0160] A three-electrode battery cell was constructed in the same manner as in Example 1 except that the following electrolyte was used. 3.34 mass % of dimethyl carbonate (DMC) and 3.34 mass % of fluoroethylene carbonate (FEC) were added to a solution in which a lithium salt (LITFSI) and water were mixed in a molar ratio of 1:1.8 to prepare an electrolyte. It should be noted that the ratio of organic carbonate (DMC and FEC) to water was 0.22:1.8 in a molar ratio.
[0161] <Example 8>
[0162] A three-electrode battery cell was constructed in the same manner as in Example 1 except that the following electrolyte was used. 1.65 mass % of dimethyl carbonate (DMC) and 1.65 mass % of fluoroethylene carbonate (FEC) were added to a solution in which a lithium salt (LITFSI) and water were mixed in a molar ratio of 1:2 to prepare an electrolyte. It should be noted that the ratio of organic carbonate (DMC and FEC) to water was 0.11:2.0 in terms of molar ratio.
[0163] <Example 9>
[0164] A three-electrode battery cell was constructed in the same manner as in Example 1 except that the following electrolyte was used. 1.0 mass % of dimethyl carbonate (DMC) and 1.0 mass % of fluoroethylene carbonate (FEC) were added to a solution in which lithium salt (LITFSI:LIBETI=0.7:0.3) and water were mixed in a molar ratio of 1:2 to prepare an electrolyte. It should be noted that the ratio of organic carbonate (DMC and FEC) to water was 0.07:2.0 in molar ratio.
[0165] <Example 10>
[0166] A three-electrode battery cell was constructed in the same manner as in Example 1 except that the following electrolyte was used. 1.65 mass % of dimethyl carbonate (DMC) and 1.65 mass % of fluoroethylene carbonate (FEC) were added to a solution in which lithium salt (LITFSI:LIBETI=0.7:0.3) and water were mixed in a molar ratio of 1:2 to prepare an electrolyte. It should be noted that the ratio of organic carbonate (DMC and FEC) to water was 0.11:2.0 in terms of molar ratio.
[0167] <Example 11>
[0168] A three-electrode battery cell was constructed in the same manner as in Example 1 except that the following electrolyte solution was used.
[0169] An electrolyte solution was prepared by adding 1.0 mass % of fluoroethylene carbonate (FEC) to a solution of lithium salt (LITFSI:LIBETI=0.7:0.3) and water in a molar ratio of 1:2. The molar ratio of organic carbonate (FEC) to water was 0.03:2.0.
[0170] <Example 12>
[0171] A three-electrode battery cell was constructed in the same manner as in Example 1 except that the following electrolyte was used. 2.0 mass % of fluoroethylene carbonate (FEC) was added to a solution in which lithium salt (LITFSI:LIBETI=0.7:0.3) and water were mixed in a molar ratio of 1:2 to prepare an electrolyte. It should be noted that the molar ratio of organic carbonate (FEC) to water was 0.07:2.0.
[0172] <Example 13>
[0173] A three-electrode battery cell was constructed in the same manner as in Example 1 except that the following electrolyte was used. 2.0 mass % of vinylene carbonate (VC) was added to a solution in which lithium salt (LITFSI:LIBETI=0.7:0.3) and water were mixed in a molar ratio of 1:2 to prepare an electrolyte. It should be noted that the molar ratio of organic carbonate (VC) to water was 0.08:2.
[0174] <Comparative Examples 9 to 15>
[0175] In Comparative Examples 8 to 13, the negative electrodes (working electrodes) were prepared in the same manner as in Examples 7 to 13, except that the treatment for making fluoroalkylsilane adhere to the surface of the negative electrode active material was not performed.
[0176] Cyclic voltammetry was performed using the three-electrode battery cells of Examples 7 to 13 and Comparative Examples 9 to 15 to evaluate the charge and discharge efficiency of the first cycle. The measurement conditions are shown below.
[0177] Starting potential: OCV
[0178] First reentry potential: -2.950V vs.Ag / AgCl(3M NaCl)
[0179] (0.288V based on Li)
[0180] Second reentry potential: -0.238V vs.Ag / AgCl(3M NaCl)
[0181] (3V based on Li)
[0182] Number of cycles: 2 cycles
[0183] Scan speed: 0.5mV / sec
[0184] Measurement temperature: 25℃
[0185] Charge and discharge efficiency: (oxidation charge (C) / reduction charge (C)) × 100
[0186] (The reduction amount includes the reduction amount from the silane coupling agent and additives.)
[0187] In addition, linear sweep voltammetry was performed using the three-electrode battery cells of Examples 7 to 10 and Comparative Examples 9 to 12 to measure the OCP of the negative electrode. The measurement conditions are shown below.
[0188] Starting potential: OCV
[0189] Potential scanning range: -3.238V~OCV vs.Ag / AgCl(3M NaCl)
[0190] OCP measurement time: 30 minutes after potential scanning to -3.238 V vs. Ag / AgCl (3M NaCl)
[0191] Scan speed: 0.1mV / sec
[0192] Measurement temperature: 25℃
[0193] The results of the negative electrode OCP after 0 minutes (OCP after potential scanning to -3.238 V), the negative electrode OCP after 1 minute (OCP after 1 minute after potential scanning to -3.238 V), the negative electrode OCP after 10 minutes (OCP after 10 minutes after potential scanning to -3.238 V), the negative electrode OCP after 20 minutes (OCP after 20 minutes after potential scanning to -3.238 V), and the negative electrode OCP after 30 minutes (OCP after 30 minutes after potential scanning to -3.238 V) in Examples 7 to 10 and Comparative Examples 9 to 12 are shown in Table 2. The negative electrode OCP shown in Table 2 is converted to a lithium reference (vs. Li / Li + ) value.
[0194] [Table 2]
[0195]
[0196] Table 3 shows the results of the charge and discharge efficiency in the first cycle in Examples 7 to 13 and Comparative Examples 9 to 15.
[0197] [Table 3]
[0198]
[0199] Comparing Example 7 and Comparative Example 9, Example 8 and Comparative Example 10, Example 9 and Comparative Example 11, and Example 10 and Comparative Example 12, which have the same composition of the aqueous electrolyte in Table 2, the OCP of the negative electrode after 0 minutes to 30 minutes is lower in all the examples. Therefore, it can be said that the self-discharge of the secondary battery is further suppressed by combining the attachment of the silane coupling agent to the surface of the negative electrode active material and the addition of the organic carbonate to the aqueous electrolyte, compared with the addition of the organic carbonate to the aqueous electrolyte alone.
[0200] In addition, according to Table 3, for Examples 7 to 13 in which a silane coupling agent is attached to the surface of the negative electrode active material and an organic carbonate is added to the aqueous electrolyte, lithium absorption and release are performed even when the carbon material is used as the negative electrode active material, and the charge-discharge efficiency is calculated. On the other hand, in Comparative Examples 9 to 15 in which only an organic carbonate is added to the aqueous electrolyte, when the carbon material is used as the negative electrode active material, lithium absorption and release are performed, but lithium release is not performed, and the charge-discharge efficiency is 0.
[0201] Description of Reference Numerals
[0202] 20 Secondary batteries
[0203] 21 Battery housing
[0204] 22 Positive electrode
[0205] 23 Negative electrode
[0206] 24 Dividers
[0207] 25 Gasket
[0208] 26 Sealing plate
[0209] 27 Electrolyte
Claims
1. A secondary battery comprising: a positive electrode, a negative electrode and an electrolyte, The electrolyte solution comprises water, a lithium salt and an additive, wherein the additive comprises at least one of an alkaline earth metal salt, a dicarboxylic acid, a carboxylic anhydride and an organic carbonate. The negative electrode comprises a negative electrode active material, and a silane coupling agent is attached to the surface of the negative electrode active material. The silane coupling agent contains fluorine as a constituent element, The content of water in the electrolyte is 6 mass % or more and 50 mass % or less relative to the total amount of the electrolyte.
2. The secondary battery according to claim 1, wherein The negative electrode active material contains a carbon material as a main component.
3. The secondary battery according to claim 1 or 2, wherein: The silane coupling agent undergoes reductive decomposition at a potential higher than the reductive decomposition potential of water.
4. The secondary battery according to claim 3, wherein The silane coupling agent has a reduction decomposition potential of 2.1 V or more based on Li.
5. The secondary battery according to claim 1 or 2, wherein: The silane coupling agent is fluoroalkyl silane.
6. The secondary battery according to claim 5, wherein The fluoroalkylsilane is represented by the following chemical formula: In the formula, Y1 is a fluoroalkyl group having 3 to 10 carbon atoms and 7 to 21 fluorine atoms, which may be linear or branched, and may contain at least one of an ether bond, an ester bond, a peptide bond, a vinyl bond, a sulfonamide bond, and a hydrogen atom, and Y2 is (CH2) n It represents that n is an integer of 0 to 6, Y2 is linear or branched, and R1, R2 and R3 are each independently an alkoxy group, an alkyl group, an amino group, a halogen atom, or a hydrogen atom.
7. The secondary battery according to claim 5, wherein The fluoroalkylsilane comprises C5F 11 CH2CH2-Si(OCH3)3、C6F 13 CH2CH2-Si(OCH3)3、C8F 17 At least any one of CH2CH2-Si(OCH3)3.
8. The secondary battery according to claim 1 or 2, wherein: The content of the silane coupling agent is in a range of 0.01 mass % to 10 mass % relative to the mass of the negative electrode active material.
9. A secondary battery comprising: a positive electrode, a negative electrode and an electrolyte, The electrolyte solution comprises water, a lithium salt and an additive, wherein the additive comprises at least one of an alkaline earth metal salt, a dicarboxylic acid, a carboxylic anhydride and an organic carbonate. The negative electrode includes a negative electrode active material, and a coating film based on reductive decomposition of a silane coupling agent is formed on the surface of the negative electrode active material. The silane coupling agent contains fluorine as a constituent element.
10. The secondary battery according to claim 9, wherein The coating includes LiF and SiO x , 0<x<2.
11. The secondary battery according to claim 10, wherein The additive comprises an alkaline earth metal salt, The coating includes at least any one of CaF2, MgF2, SrF2 or BaF2.
12. The secondary battery according to any one of claims 9 to 11, wherein The coating contains a silane coupling agent containing a fluoroalkyl group.
13. The secondary battery according to any one of claims 9 to 11, wherein The coating comprises: at least one of a silane coupling agent and a silane coupling agent containing a fluoroalkyl group, The silane coupling agent and the silane coupling agent containing a fluoroalkyl group are more concentrated on the surface layer side of the electrolyte solution side of the film than on the deepest side of the film.
14. The secondary battery according to claim 13, wherein The coating comprises LiF, The peak intensity of the bond energy (686 eV) derived from LiF in the F1s spectrum of XPS is set to I A , the peak intensity of the bond energy (688.8 eV) derived from the fluoroalkyl group is set as I B When the peak intensity increases from the deepest side of the coating to the surface layer on the electrolyte side, A >I B Change to I A <I B .
15. The secondary battery according to any one of claims 9 to 11, wherein The additive comprises an organic carbonate, The coating film formed by reductive decomposition of the organic carbonate is deposited on the coating film formed by reductive decomposition of the silane coupling agent.
16. The secondary battery according to claim 12, wherein The additive comprises an organic carbonate, The coating comprises LiF, The peak intensity of the bond energy (686 eV) derived from LiF in the F1s spectrum of XPS is set to I C , the peak intensity of the bond energy (688.8 eV) derived from the fluoroalkyl group is set as I D When the peak intensity of the surface layer of the electrolyte side of the coating is I C >I D .
17. The secondary battery according to any one of claims 1 to 2 or 9 to 11, wherein The lithium salt includes a salt having a lithium ion and an imide anion.
18. The secondary battery according to any one of claims 1 to 2 or 9 to 11, wherein The lithium salt includes lithium bis(trifluoromethylsulfonyl)imide.
19. The secondary battery according to any one of claims 1 to 2 or 9 to 11, wherein The organic carbonate is present in an amount of 1: The water is present in a first molar ratio ranging from 0.01 to 1:5, and the water is present in a second molar ratio ranging from 1:0.5 to 1:4 relative to the lithium salt.
20. The secondary battery according to claim 19, wherein The first molar ratio is in the range of 1:0.05 to 1:
1.
21. The secondary battery according to claim 19, wherein The second molar ratio is in the range of 1:1 to 1:2.
5.
22. The secondary battery according to claim 19, wherein The organic carbonate is reductively decomposed at a potential lower than the reductive decomposition potential of the silane coupling agent.
23. The secondary battery according to claim 22, wherein: The organic carbonate has a reductive decomposition potential of 2.2 V or less based on Li.
24. The secondary battery according to any one of claims 1 to 2 or 9 to 11, wherein The organic carbonate includes a cyclic carbonate.
25. The secondary battery according to any one of claims 1 to 2 or 9 to 11, wherein The organic carbonate contains fluorine as a constituent element.
Citation Information
Patent Citations
Aqueous electrolytic solution for electrical storage device, and electrical storage device including said aqueous electrolytic solution
WO2017122597A1
Lithium-ion batteries
CN102292856A
Non-aqueous electrolyte secondary cell and method for manufacturing same
CN104247130A
Secondary battery, battery pack, and vehicle
CN109524713A
Nonaqueous electrolyte secondary battery and manufacture for electrode