Radio wave absorbers and composites

By using a combination of magnetic powder and adhesive in the radio wave absorber, especially a magnetic hexagonal ferrite powder, the problem that the radio wave absorber in the prior art is difficult to increase the reflection and transmission attenuation amounts at the same time is solved. , realizes efficient radio wave absorption effect and meets the absorption needs of the millimeter band.

CN113795897BActive Publication Date: 2024-11-19FUJIFILM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080033792.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-05-14
Filing Date
2020-03-18
Publication Date
2024-11-19
Estimated Expiration
2040-03-18

AI Technical Summary

Technical Problem

In the case where the existing radio wave absorber does not use a metal layer, it is difficult to simultaneously increase the reflection attenuation amount and the transmission attenuation amount at the same time. Especially in the millimeter band, the reflection attenuation amount and the transmission attenuation amount must reach more than 10 dB.

Method used

Design an electric wave absorber, which contains a magnetic powder and a binder, the filling rate of the magnetic powder is less than 35% by volume, and is passed through a specific magnetic lead-type hexagonal ferrite powder and adhesive The mixture combination meets the specific thickness and filling rate relationship, ensures that the thickness and filling rate of the radio wave absorbing layer meet the conditions of 0.65≤(P/100)×Q, and achieves efficient radio wave absorption.

Benefits of technology

The reflection attenuation amount and transmission attenuation amount in the millimeter band are achieved with an effect of reaching more than 10 dB, ensuring efficient absorption of radio waves, and avoiding deterioration and cost problems caused by the use of metal layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003339258900000301
    Figure BDA0003339258900000301
  • Figure BDA0003339258900000311
    Figure BDA0003339258900000311
Patent Text Reader

Abstract

The present invention provides a radio wave absorber and a composite, wherein the radio wave absorber does not have a metal layer, and the transmission attenuation and reflection attenuation in the millimeter wave band are both above 10 dB. The present invention provides a radio wave absorber and a composite, wherein the radio wave absorber has a radio wave absorption layer including magnetic powder and a binder, and does not have a metal layer, wherein the filling rate of the magnetic powder in the radio wave absorption layer is 35 volume % or less, and when the filling rate of the magnetic powder in the radio wave absorption layer is set to P volume % and the thickness of the radio wave absorption layer is set to Q mm, the relationship of 0.65≤(P / 100)×Q is satisfied.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an electric wave absorber and a composite. Background Art

[0002] In recent years, with the diversification of the use of high-frequency radio waves in electronic toll collection systems (ETC), advanced cruise-assist highway systems (AHS), satellite broadcasting, etc., malfunctions and failures of electronic devices caused by radio wave interference have become a problem. In order to reduce the impact of such radio wave interference on electronic devices, a process is carried out in which a radio wave absorber absorbs unnecessary radio waves to prevent the reflection of radio waves.

[0003] For example, Patent Document 1 discloses a radio wave absorbing sheet comprising a flexible radio wave absorbing layer including a particulate radio wave absorbing material and a resin adhesive, wherein the radio wave absorbing material is a magnetic iron oxide that generates magnetic resonance in a frequency band above the millimeter wave band, and the easy magnetization axis of the radio wave absorbing material is oriented by a magnetic field along one direction within the plane of the radio wave absorbing sheet.

[0004] Previous technical literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2018-56492 Summary of the invention

[0007] Technical issues to be solved by the invention

[0008] The radio wave absorber is required to have both high reflection loss and high transmission loss. Specifically, both the reflection loss and the transmission loss are required to be 10 dB or more.

[0009] As a method for increasing the reflection attenuation of the radio wave absorber, there is a method of setting a reflection layer for reflecting the radio wave on the side opposite to the side where the radio wave of the radio wave absorbing layer is incident (the so-called back side). The reflection layer usually uses a layer containing metal (the so-called metal layer), but in recent years, from the perspective of recycling, there is a trend to avoid using the metal layer. In addition, in the radio wave absorber with a metal layer, there are problems such as the radio wave absorbing layer and the metal layer are easily peeled off, the metal layer itself is easily degraded, and the cost becomes high. Therefore, it is desired to design a radio wave absorber without a metal layer.

[0010] However, in a commonly used dielectric radio wave absorber, when no metal layer is provided, when an attempt is made to ensure transmission attenuation, reflection attenuation decreases.

[0011] In a radio wave absorber having no metal layer, it has been difficult to increase both the reflection attenuation and the transmission attenuation at the same time.

[0012] Regarding the above-mentioned points, Patent Document 1 does not focus on the problems when a metal layer is provided, and does not mention increasing both the reflection attenuation and the transmission attenuation in a radio wave absorber without a metal layer.

[0013] An object of one embodiment of the present invention is to provide a radio wave absorber having no metal layer and having both a transmission attenuation and a reflection attenuation of 10 dB or more in a millimeter wave band.

[0014] Another embodiment of the present invention aims to provide a composite material for producing the above-mentioned radio wave absorber.

[0015] Means for solving technical problems

[0016] Means for solving the above-mentioned problems include the following aspects.

[0017] <1> A radio wave absorber having a radio wave absorbing layer containing magnetic powder and a binder and having no metal layer, wherein:

[0018] The filling rate of the magnetic powder in the radio wave absorbing layer is 35 volume % or less,

[0019] When the filling rate of the magnetic powder in the radio wave absorbing layer is P volume % and the thickness of the radio wave absorbing layer is Q mm, the relationship of 0.65≤(P / 100)×Q is satisfied.

[0020] <2> according to <1> The radio wave absorber, wherein

[0021] The radio wave absorbing layer has a thickness of 10 mm or less, and a filling rate of 8 volume % or more and 35 volume % or less.

[0022] <3> according to <1> or <2> The radio wave absorber, wherein

[0023] The radio wave absorbing layer has a thickness of 5 mm or less, and a filling rate of 15 volume % or more and 35 volume % or less.

[0024] <4> according to <1> to <3> The radio wave absorber as described in any one of the preceding claims, wherein:

[0025] The magnetic powder includes powder of magnetoplumbite hexagonal ferrite.

[0026] <5> according to <1> to <4> The radio wave absorber as described in any one of the preceding claims, wherein:

[0027] The magnetic powder includes powder of magnetoplumbite hexagonal ferrite represented by the following formula (1).

[0028] [Chemical formula 1]

[0029] AFe (12-x) Al x O 19 ……(Formula 1)

[0030] In formula (1), A represents at least one metal element selected from the group consisting of Sr, Ba, Ca and Pb, and x satisfies 1.5≤x≤8.0.

[0031] <6> according to <5> The radio wave absorber, wherein

[0032] A in the above formula (1) is Sr.

[0033] <7> according to <5> or <6> The radio wave absorber, wherein

[0034] In the above formula (1), x satisfies 1.5≤x≤6.0.

[0035] <8> according to <1> to <7> The radio wave absorber as described in any one of the preceding claims, wherein:

[0036] In the particle size distribution of the magnetic powder measured by laser diffraction scattering method, the mode value is defined as the mode diameter and the cumulative 10% diameter is defined as D 10 , and the cumulative 90% diameter is set to D 90 When the mode diameter is 5 μm or more and less than 10 μm, and (D 90 -D 10 ) / mode diameter ≤3.0.

[0037] <9> according to <1> to <8> The radio wave absorber described in any one of the above has a planar shape.

[0038] <10> according to <1> to <8> The radio wave absorber described in any one of the above has a three-dimensional shape.

[0039] <11> A composite material for manufacturing <1> to <10> The radio wave absorber described in any one of the above aspects, wherein the composite contains magnetic powder and a binder, and the filling rate of the magnetic powder is 35 volume % or less.

[0040] Effects of the Invention

[0041] According to one embodiment of the present invention, a radio wave absorber and a composite are provided, wherein the radio wave absorber has no metal layer and has a transmission attenuation and a reflection attenuation in a millimeter wave band of 10 dB or more.

[0042] According to another embodiment of the present invention, a composite material for manufacturing the above-mentioned radio wave absorber is provided. DETAILED DESCRIPTION

[0043] Hereinafter, an example of an embodiment of a radio wave absorber to which the present invention is applied will be described. However, the present invention is not limited to the following embodiment at all, and can be implemented with appropriate modifications within the scope of the purpose of the present invention.

[0044] In the present invention, a numerical range expressed using "to" indicates a range including the numerical values ​​described before and after "to" as the minimum value and the maximum value, respectively.

[0045] In the numerical ranges recorded in stages in the present invention, the upper limit or lower limit recorded in a certain numerical range can be replaced by the upper limit or lower limit of the numerical range recorded in other stages. In addition, in the numerical ranges recorded in the present invention, the upper limit or lower limit recorded in a certain numerical range can also be replaced by the value shown in the embodiments.

[0046] In the present invention, a combination of two or more preferred embodiments is a more preferred embodiment.

[0047] In the present invention, when there are plural kinds of substances corresponding to each component, the amount of each component represents the total amount of the plural kinds of substances unless otherwise specified.

[0048] In the present invention, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process can be achieved.

[0049] In the present invention, the conversion factor from the non-SI unit "Oe" to the SI unit "A / m" is set to "10 3 / 4π". Here, "π" is set to 3.1416.

[0050] In the present invention, the conversion from the non-SI unit "emu" to the SI unit "A·m 2 The conversion factor of " is set to "10 -3 ”.

[0051] [Radio wave absorber]

[0052] The radio wave absorber of the present invention has a radio wave absorbing layer containing magnetic powder and a binder and does not have a metal layer. The filling rate of the magnetic powder in the radio wave absorbing layer is 35 volume % or less. When the filling rate of the magnetic powder in the radio wave absorbing layer is set to P volume % and the thickness of the radio wave absorbing layer is set to Q mm, the relationship of 0.65≤(P / 100)×Q is satisfied.

[0053] The radio wave absorber of the present invention has a radio wave absorption layer containing magnetic powder and a binder, the filling rate of the magnetic powder in the radio wave absorption layer is 35 volume % or less, and when the filling rate of the magnetic powder in the radio wave absorption layer is set to P volume % and the thickness of the radio wave absorption layer is set to Qmm, the relationship of 0.65≤(P / 100)×Q is satisfied. Therefore, although there is no metal layer, the transmission attenuation and reflection attenuation in the millimeter wave band are both above 10 dB.

[0054] According to the radio wave absorber in which both the transmission attenuation and the reflection attenuation are 10 dB or more, at least 90% of the radio waves can be absorbed.

[0055] - Composition of radio wave absorbers -

[0056] The radio wave absorber of the present invention has a radio wave absorbing layer but does not have a metal layer.

[0057] In the present invention, the "metal layer" is a layer containing metal, and refers to a layer that substantially reflects radio waves. Here, "substantially reflects radio waves" means, for example, reflecting 90% or more of incident radio waves.

[0058] The metal layer may be a metal plate, a metal foil, or the like, and may be a metal thin film formed by vapor deposition, for example. The metal layer is usually formed on the side of the radio wave absorbing layer opposite to the side on which the radio wave is incident.

[0059] In addition, a layer corresponding to the radio wave absorbing layer is not included in the "metal layer" in the present invention.

[0060] The radio wave absorber of the present invention may have a layer other than the radio wave absorbing layer (so-called other layer) as necessary within a range not impairing the effect of the radio wave absorber of the present invention.

[0061] Examples of the other layers include a protective layer, an adhesive layer, and a release layer.

[0062] Furthermore, the radio wave absorber of the present invention may include a non-metal reflective layer as another layer within a range not impairing the effect of the radio wave absorber of the present invention, but an embodiment without the non-metal reflective layer is preferred.

[0063] - Shape of the radio wave absorber -

[0064] The radio wave absorber of the present invention may have a planar shape or a three-dimensional shape.

[0065] The planar shape is not particularly limited, and examples thereof include a sheet shape, a film shape, and the like.

[0066] Examples of the three-dimensional shape include a tube shape (a circular tube shape, a square tube shape, etc.), a trumpet shape, and a box shape (where one surface is open).

[0067] 〔Radio wave absorbing layer〕

[0068] The radio wave absorbing layer contains magnetic powder and a binder.

[0069] The components contained in the radio wave absorbing layer will be described in detail later.

[0070] The filling rate of the magnetic powder in the radio wave absorbing layer is 35 volume % or less, preferably 8 volume % or more and 35 volume % or less, more preferably 15 volume % or more and 35 volume % or less, further preferably 20 volume % or more and 35 volume % or less, and particularly preferably 25 volume % or more and 35 volume % or less.

[0071] When the filling rate of the magnetic powder in the radio wave absorbing layer is 35 volume % or less, the radio wave absorber can achieve a reflection loss of 10 dB or more even without having a metal layer.

[0072] The filling rate of the magnetic powder in the radio wave absorbing layer is a value measured and calculated by the following method using a scanning electron microscope (SEM).

[0073] The radio wave absorbing layer was cut into a size of 5 mm x 5 mm. After the cut radio wave absorbing layer was pasted on a workbench, the cross section was processed in the thickness direction using a focused ion beam (FIB). After the processed radio wave absorbing layer was placed on the workbench so that the cross section was at the top, a cross-sectional SEM image with a field of view of 30 μm x 40 μm was obtained using a field emission scanning electron microscope (FE-SEM) at a voltage of 15 kV and an observation magnification of 3,000 times. The obtained cross-sectional SEM image was binarized to obtain the ratio of the magnetic powder and calculate the filling rate of the magnetic powder.

[0074] The above operation was repeated five times by changing the cutting position of the radio wave absorbing layer, and the arithmetic mean of the calculated values ​​was taken as the filling rate of the magnetic powder in the radio wave absorbing layer. The arithmetic mean was rounded off to the first decimal place.

[0075] As the focused ion beam (FIB) apparatus, for example, a high-performance focused ion beam (FIB) apparatus (product name: MI4050) from Hitachi, Ltd. can be preferably used. However, the focused ion beam (FIB) apparatus is not limited thereto.

[0076] As the field emission scanning electron microscope (FE-SEM), for example, a field emission scanning electron microscope (product name: SU-8220) manufactured by Hitachi, Ltd. can be preferably used. However, the field emission scanning electron microscope (FE-SEM) is not limited thereto.

[0077] In the radio wave absorption layer, when the filling rate of the magnetic powder in the radio wave absorption layer is set to P volume % and the thickness of the radio wave absorption layer is set to Q mm, the relationship of 0.65≤(P / 100)×Q is satisfied, preferably the relationship of 0.65≤(P / 100)×Q≤5.0 is satisfied, more preferably the relationship of 0.65≤(P / 100)×Q≤3.5 is satisfied, further preferably the relationship of 0.65≤(P / 100)×Q≤1.75 is satisfied, and particularly preferably the relationship of 0.65≤(P / 100)×Q≤1.0 is satisfied.

[0078] If the relationship of 0.65≤(P / 100)×Q is satisfied, the radio wave absorber can achieve a transmission attenuation of 10 dB or more.

[0079] The thickness of the radio wave absorbing layer is not particularly limited as long as the above relationship of "0.65≤(P / 100)×Q" is satisfied.

[0080] For example, from the viewpoint of the degree of freedom of the installation position, the thickness of the radio wave absorbing layer is preferably 20 mm or less, more preferably 10 mm or less, and further preferably 5 mm or less.

[0081] The lower limit of the thickness of the radio wave absorbing layer is not particularly limited, but is preferably 2 mm or more from the viewpoint of mechanical properties, for example.

[0082] The thickness of the electromagnetic wave absorbing layer is a value measured using a digital length measuring machine, and specifically, is the arithmetic mean of the values ​​measured at arbitrarily selected nine positions.

[0083] As the digital length measuring machine, for example, a digital length measuring machine (product name: Litematic (registered trademark) VL-50A) manufactured by Mitutoyo Corporation can be preferably used. However, the digital length measuring machine is not limited to this.

[0084] As a method for satisfying the relationship of 0.65≤(P / 100)×Q, for example, it is preferred that the thickness of the radio wave absorption layer is 10 mm or less, and the filling rate of the magnetic powder in the radio wave absorption layer is 8 volume % or more and 35 volume % or less. It is more preferred that the thickness of the radio wave absorption layer is 5 mm or less, and the filling rate of the magnetic powder in the radio wave absorption layer is 15 volume % or more and 35 volume % or less. It is further preferred that the thickness of the radio wave absorption layer is 2 mm or more and 5 mm or less, and the filling rate of the magnetic powder in the radio wave absorption layer is 20 volume % or more and 35 volume % or less.

[0085] <Magnetic Powder>

[0086] The radio wave absorbing layer contains magnetic powder.

[0087] The magnetic powder is not particularly limited, and examples thereof include powders of ferrite, iron oxide, cobalt, chromium oxide, and the like.

[0088] For example, from the viewpoint of radio wave absorption performance, the magnetic powder preferably includes magnetoplumbite hexagonal ferrite powder (hereinafter also referred to as "magnetoplumbite hexagonal ferrite powder"), and more preferably magnetoplumbite hexagonal ferrite powder.

[0089] Magneto-plumbite hexagonal ferrite is usually composed of the formula A 1 Fe 12 O 19 (Where A 1 Represents metal elements such as Sr, Ba, Ca, Pb, etc. ) represented by a compound.

[0090] However, in the concept of "magnetoplumbite-type hexagonal ferrite" in the present invention, in addition to the composition formula A 1 Fe 12 O 19 In addition to the magnetoplumbite type hexagonal ferrite represented by the formula (1) described later, magnetoplumbite type hexagonal ferrite is also included.

[0091] For example, from the perspective of operability and handling, A 1 Preferably, it is at least one metal element selected from the group consisting of Sr, Ba, Ca and Pb.

[0092] For example, from the perspective of having excellent magnetic properties and excellent radio wave absorption performance in high frequency bands, the magnetic powder preferably includes powder of magnetoplumbite-type hexagonal ferrite represented by the following formula (1), and is preferably powder of magnetoplumbite-type hexagonal ferrite represented by formula (1).

[0093] Hereinafter, the magnetoplumbite hexagonal ferrite represented by formula (1) is referred to as “specific magnetoplumbite hexagonal ferrite.” Furthermore, powder of the specific magnetoplumbite hexagonal ferrite is also referred to as “specific magnetoplumbite hexagonal ferrite powder.”

[0094] [Chemical formula 2]

[0095] AFe (12-x) Al x O 19 ……(Formula 1)

[0096] In formula (1), A represents at least one metal element selected from the group consisting of Sr, Ba, Ca and Pb, and x satisfies 1.5≤x≤8.0.

[0097] In the formula (1), as long as A is at least one metal element selected from the group consisting of Sr, Ba, Ca and Pb, the type and amount of the metal element are not particularly limited.

[0098] For example, from the viewpoint of operability and handling properties, A in formula (1) is preferably at least one metal element selected from the group consisting of Sr, Ba, and Ca.

[0099] Furthermore, for example, from the viewpoint of exhibiting excellent radio wave absorption performance near 79 GHz, A in the formula (1) preferably contains Sr, and more preferably is Sr.

[0100] In the formula (1), x satisfies 1.5≤x≤8.0, preferably satisfies 1.5≤x≤6.0, more preferably satisfies 1.5≤x≤4.0, and further preferably satisfies 1.5≤x≤3.0.

[0101] When x in the formula (1) is 1.5 or more, radio waves in a frequency band higher than 60 GHz can be absorbed.

[0102] When x in the formula (1) is 8.0 or less, the magnetoplumbite hexagonal ferrite has magnetic properties.

[0103] As specific magnetoplumbite-type hexagonal ferrite, SrFe (10.44) Al (1.56) O 19 、SrFe (10.00) Al (2.00) O 19 、SrFe (9.95) Al (2.05) O 19 、SrFe (9.85) Al (2.15) O 19 、SrFe (9.79) Al (2.21) O 19 、SrFe (9.74) Al (2.26) O 19 、SrFe (9.70) Al (2.30) O 19 、SrFe (9.58) Al (2.42) O 19 、SrFe (9.37) Al (2 . 63) O 19 、SrFe (9.33) Al (2.67) O 19 、SrFe (9.27) Al (2.73) O 19 、SrFe (7.88) Al (4.12) O 19 、SrFe ( 7.71) Al (4.29) O 19 、SrFe (7.37) Al (4.63) O 19 、SrFe (7.04) Al (4.96) O 19 、SrFe (6.25) Al (5.75) O 19 ,BaFe (9.50) Al (2.50) O 19 ,BaFe (10.05) Al (1.95) O 19 , CaFe (10.00) Al (2.00) O 19 、PbFe ( 9. 00) Al (3.00) O 19 , Sr (0.80) Ba (0.10) Ca (0.10) Fe (9.83) Al (2.17) O 19 , Sr (0.80) Ba (0.10) Ca (0.10) Fe (8.85) Al (3.15) O 19 wait.

[0104] For example, SrFe (10.00) Al (2.00) O 19 It is a specific magnetoplumbite hexagonal ferrite with a resonance frequency around 76.5 GHz. (9.70) Al (2.30) O 19 It is a specific magnetoplumbite hexagonal ferrite having a resonance frequency near 85.0 GHz.

[0105] The method for producing the specific magnetoplumbite hexagonal ferrite powder will be described later.

[0106] The composition of the magnetoplumbite hexagonal ferrite was confirmed by high-frequency inductively coupled plasma (ICP: Inductively Coupled Plasma) emission spectrometry.

[0107] Specifically, a pressure-resistant container containing 12 mg of sample powder and 10 mL of 4 mol / L (liter; hereinafter the same) hydrochloric acid aqueous solution is kept in an oven set at 120°C for 12 hours to obtain a solution. Next, 30 mL of pure water is added to the obtained solution, and then filtered using a 0.1 μm membrane filter. The elemental analysis of the filtrate thus obtained is performed using a high-frequency inductively coupled plasma (ICP) emission spectrophotometer. Based on the obtained elemental analysis results, the content of each metal atom relative to 100 atomic % of iron atoms is calculated. The composition is confirmed based on the calculated content.

[0108] As the ICP emission spectrometer, for example, IC PS-8100 (model) manufactured by Shimadzu Corporation can be preferably used. However, the ICP emission spectrometer is not limited thereto.

[0109] The crystal phase of the magnetoplumbite hexagonal ferrite may be a single phase or may not be a single phase. When the magnetoplumbite hexagonal ferrite is a specific magnetoplumbite hexagonal ferrite, the crystal phase is preferably a single phase.

[0110] When the aluminum content ratio is the same, the powder of specific magnetoplumbite-type hexagonal ferrite whose crystal phase is not a single phase (for example, the crystal phase is a two-phase) has a higher coercive force and tends to have better magnetic properties.

[0111] In the present invention, the case where “the crystal phase is a single phase” means that only one diffraction pattern showing the crystal structure of magnetoplumbite-type hexagonal ferrite of an arbitrary composition is observed in powder X-ray diffraction (XRD: X-Ray-Diffraction; the same applies hereinafter).

[0112] On the other hand, in the present invention, the situation where "the crystal phase is not a single phase" refers to the situation where multiple types of magnetoplumbite-type hexagonal ferrites of arbitrary compositions are mixed and more than two diffraction patterns are observed, or the situation where the diffraction pattern of a crystal other than magnetoplumbite-type hexagonal ferrite is observed.

[0113] When the crystal phase is not a single phase, a diffraction pattern having a main peak and other peaks can be obtained. Here, "main peak" refers to the peak with the highest diffraction intensity value in the observed diffraction pattern.

[0114] When the radio wave absorbing layer comprises magnetoplumbite hexagonal ferrite powder as a magnetic powder, for example, from the viewpoint of being able to produce a radio wave absorber having better radio wave absorption performance, the ratio (Is / Im) of the diffraction intensity value of other peaks (hereinafter referred to as "Is") obtained by powder X-ray diffraction (XRD) measurement of magnetoplumbite hexagonal ferrite powder to the diffraction intensity value of the main peak (hereinafter referred to as "Im") is preferably 1 / 2 or less, and more preferably 1 / 5 or less.

[0115] In addition, when two or more diffraction patterns overlap and the peak of each diffraction pattern has a maximum value, each maximum value is defined as Im and Is, and their ratio is obtained. In addition, when two or more diffraction patterns overlap and other peaks are observed as the shoulder of the main peak, the maximum intensity value of the shoulder is defined as Is, and their ratio is obtained.

[0116] Furthermore, when there are two or more other peaks, the total value of each diffraction intensity is defined as Is, and the ratio between them is calculated.

[0117] The assignment of diffraction patterns can be referred to, for example, the database of the International Center for Diffraction Data (ICDD: International Centrefor Diffraction Data, registered trademark).

[0118] For example, the diffraction pattern of magnetoplumbite hexagonal ferrite containing Sr can be referred to "00-033-1340" of the International Center for Diffraction Data (ICDD). However, for a specific magnetoplumbite hexagonal ferrite, if part of the iron is replaced by aluminum, the peak position shifts.

[0119] As described above, the fact that the crystal phase of magnetoplumbite-type hexagonal ferrite is a single phase was confirmed by powder X-ray diffraction (XRD) measurement.

[0120] Specifically, the measurement was performed using a powder X-ray diffraction (XRD) apparatus under the following conditions.

[0121] As a powder X-ray diffraction (XRD) apparatus, for example, X'Pert Pro (product name) manufactured by PANalytical Inc. can be suitably used. However, the powder X-ray diffraction (XRD) apparatus is not limited thereto.

[0122] -condition-

[0123] X-ray source: CuKα line

[0124] 〔wavelength: (0.154nm), output: 40mA, 45kV〕

[0125] Scanning range: 20°<2θ<70°

[0126] Scanning interval: 0.05°

[0127] Scanning speed: 0.75° / min

[0128] For example, it can be confirmed by the following method that the radio wave absorbing layer contains magnetoplumbite-type hexagonal ferrite powder.

[0129] After the radio wave absorbing layer is cut into pieces, it is immersed in a solvent (eg, acetone) for 1 to 2 days and then dried. The structure can be confirmed by further grinding the dried radio wave absorbing layer and performing powder X-ray diffraction (XRD) measurement.

[0130] Then, after cutting out a cross section of the radio wave absorbing layer, the composition can be confirmed by using, for example, an energy dispersive X-ray analyzer.

[0131] The shape of the particles constituting the magnetic powder is not particularly limited, and examples thereof include spherical, rod-shaped, needle-shaped, flat-plate-shaped, and irregular shapes.

[0132] The shape of particles constituting the magnetoplumbite hexagonal ferrite powder may be, for example, a flat plate shape or an irregular shape.

[0133] The size of the particles constituting the magnetic powder is not particularly limited.

[0134] In the particle size distribution of the magnetic powder (preferably magnetoplumbite hexagonal ferrite powder, more preferably specific magnetoplumbite hexagonal ferrite powder; the same shall apply hereinafter) measured by the laser diffraction scattering method, the mode value is defined as the mode diameter and the cumulative 10% diameter is defined as D 10 , and the cumulative 90% diameter is set to D 90 When the mode diameter is preferably 5 μm or more and less than 10 μm, and (D 90 -D 10 ) / mode diameter ≤ 3.0, more preferably the mode diameter is 5 μm or more and less than 10 μm, and (D 90 -D 10 ) / mode diameter ≤ 2.5, more preferably the mode diameter is 5 μm or more and less than 10 μm, and (D 90 -D 10 ) / mode diameter ≤ 2.0, and it is particularly preferred that the mode diameter is not less than 5 μm and less than 10 μm, and (D 90 -D 10 ) / mode diameter ≤ 1.5, most preferably the mode diameter is 5 μm or more and less than 10 μm, and (D 90 -D 10 ) / mode diameter ≤1.0.

[0135] According to the mode diameter of 5 μm or more and (D 90 -D 10 ) / mode diameter ≤3.0, since the number of fine particles with poor magnetic properties is relatively small, there is a tendency for the production of radio wave absorbers with better radio wave absorption performance.

[0136] According to the mode diameter less than 10μm and (D 90 -D 10 ) / mode diameter ≤3.0, since the number of coarse particles is relatively small, there is a tendency for the magnetic powder to be able to produce a radio wave absorber with better strength.

[0137] The particle size of magnetic powder (i.e., mode diameter, D 10 and D 90 ) can be controlled by classification using a sieve, a centrifugal separator, etc., or by pulverization using a mortar and pestle, an ultrasonic disperser, etc. For example, when the particle size of the magnetic powder is controlled by pulverization, it can be adjusted to a target value by selecting a pulverization mechanism, pulverization time, medium material, medium diameter, etc.

[0138] For example, the particle size of the magnetic powder tends to become smaller by pulverizing using a medium. Also, for example, the longer the pulverizing time, the smaller the particle size of the magnetic powder tends to become. Also, for example, the smaller the medium diameter, the smaller the particle size of the magnetic powder tends to become.

[0139] “(D 90 -D 10 The value of "( ) / mode diameter" can be adjusted to a target value by classifying the particles after pulverization, for example, by using a sieve, a centrifuge, or the like.

[0140] The mode value, cumulative 10% diameter, and cumulative 90% diameter of the magnetic powder are values ​​obtained from a number-based particle size distribution measured by a laser diffraction scattering method. Specifically, they are values ​​measured by the following method.

[0141] After adding 500 mL of cyclohexanone to 10 mg of magnetic powder for dilution, the mixture was stirred for 30 seconds using an oscillator, and the resulting liquid was used as a sample for particle size distribution measurement. Next, the particle size distribution was measured using the sample for particle size distribution measurement by a laser diffraction scattering method. A laser diffraction / scattering particle size distribution measuring device was used in the measuring device.

[0142] As a laser diffraction / scattering type particle size distribution measuring apparatus, for example, Partica LA-960 (product name) manufactured by HORIBA, Ltd. can be suitably used. However, the laser diffraction / scattering type particle size distribution measuring apparatus is not limited thereto.

[0143] The particle size of the magnetic powder contained in the radio wave absorbing layer can be confirmed by the following method, for example.

[0144] After the radio wave absorbing layer is cut into small pieces, it is dispersed in a solvent (eg, acetone) by ultrasonic wave, and the obtained dispersion is used as a sample and measured by laser diffraction scattering method to confirm the particle size of the magnetic powder.

[0145] The coercive force (Hc) of the magnetic powder is not particularly limited, but is, for example, preferably 2.5 kOe or more, more preferably 4.0 kOe or more, and further preferably 5.0 kOe or more.

[0146] When the coercive force (Hc) of the magnetic powder is 2.5 kOe or more, a radio wave absorber excellent in radio wave absorption performance can be produced.

[0147] The upper limit of the coercive force (Hc) of the magnetic powder is not particularly limited, but is preferably 18 kOe or less, for example.

[0148] The saturation magnetization (δs) per unit mass of the magnetic powder is not particularly limited, but is, for example, preferably 10 emu / g or more, more preferably 20 emu / g or more, and further preferably 30 emu / g or more.

[0149] When the saturation magnetization (δs) per unit mass of the magnetic powder is 10 emu / g or more, a radio wave absorber having excellent radio wave absorption performance can be produced.

[0150] The upper limit of the saturation magnetization (δs) per unit mass of the magnetic powder is not particularly limited, but is preferably 60 emu / g or less, for example.

[0151] The coercive force (Hc) and saturation magnetization per unit mass (δs) of the magnetic powder are values ​​measured using a vibrating sample magnetometer at an ambient temperature of 23°C, under the conditions of a maximum applied magnetic field of 50 kOe and a magnetic field scanning speed of 25 Oe / s (seconds).

[0152] As the vibration test type magnetometer, for example, TM-TRVSM5050-SMSL type (model number) manufactured by TAMAKAWA CO., LTD. can be suitably used. However, the vibration test type magnetometer is not limited to this.

[0153] The radio wave absorbing layer may contain only one type of magnetic powder, or may contain two or more types of binders.

[0154] The mass-based content of the magnetic powder in the radio wave absorbing layer is not particularly limited as long as the filling rate of the magnetic powder in the radio wave absorbing layer is 35 volume % or less.

[0155] - Method for producing specific magnetoplumbite-type hexagonal ferrite powder -

[0156] The method for producing the specific magnetoplumbite hexagonal ferrite powder is not particularly limited.

[0157] The specific magnetoplumbite hexagonal ferrite powder can be produced by either a solid phase method or a liquid phase method.

[0158] As a method for manufacturing a specific magnetoplumbite type hexagonal ferrite powder by a solid phase method, for example, a method using SrCO3, Al2O3, α-Fe2O3, etc. as raw materials can be cited. For a general method for manufacturing a specific magnetoplumbite type hexagonal ferrite powder by a solid phase method, paragraphs

[0023] to

[0025] of Japanese Patent Gazette No. 4674380 can be appropriately referred to.

[0159] As a method for producing specific magnetoplumbite hexagonal ferrite powder, the method described below (hereinafter referred to as "production method A") is preferred from the viewpoint of easily obtaining specific magnetoplumbite hexagonal ferrite powder having more excellent magnetic properties.

[0160] Manufacturing method A includes: step A, obtaining a reaction product containing Fe, Al and at least one metal element selected from the group consisting of Sr, Ba, Ca and Pb (hereinafter also referred to as "specific metal element") by a liquid phase method; step B, obtaining a dried product by drying the reaction product obtained in step A; step C, which is either a step of calcining the dried product obtained in step B to obtain a calcined product, and then crushing the obtained calcined product (hereinafter also referred to as "c1 step") or a step of crushing the obtained dried product obtained in step B to obtain a crushed product, and then calcining the obtained crushed product (hereinafter also referred to as "c2 step") .

[0161] Each of step A, step B and step C can be divided into two or more stages.

[0162] Furthermore, the manufacturing method A may include steps other than step A, step B, and step C as necessary.

[0163] Hereinafter, each step will be described in detail.

[0164] (Process A)

[0165] Step A is a step of obtaining a reaction product containing Fe, Al, and at least one metal element selected from the group consisting of Sr, Ba, Ca, and Pb (ie, a specific metal element) by a liquid phase method.

[0166] In step A, a reaction product that is a precursor of a specific magnetoplumbite type hexagonal ferrite powder can be obtained. The reaction product obtained in step A is estimated to be iron hydroxide, aluminum hydroxide, a composite hydroxide of iron and aluminum with a specific metal element, or the like.

[0167] Step A preferably includes a step of obtaining a reaction product by mixing an aqueous solution containing an Fe salt, an Al salt and a salt of a specific metal element (hereinafter also referred to as “raw material aqueous solution”) with an alkali aqueous solution (hereinafter also referred to as “step A1”).

[0168] In step A1, a reaction product precipitate is generated by mixing the raw material aqueous solution and the alkaline aqueous solution. In step A1, a liquid containing a reaction product that is a precursor of a specific magnetoplumbite-type hexagonal ferrite powder (so-called precursor-containing liquid) can be obtained.

[0169] Furthermore, step A preferably includes a step of solid-liquid separation of the reaction product obtained in step A1 (hereinafter also referred to as "step A2").

[0170] In step A2, a reaction product that is a precursor of a specific magnetoplumbite-type hexagonal ferrite powder (that is, a reaction product in step A) can be obtained.

[0171] -Process A1-

[0172] Step A1 is a step of obtaining a reaction product by mixing an aqueous solution containing an Fe salt, an Al salt, and a salt of a specific metal element (ie, a raw material aqueous solution) with an alkali aqueous solution.

[0173] The salt among the Fe salt, the Al salt and the salt of the specific metal element is not particularly limited, but water-soluble inorganic acid salts such as nitrates, sulfates and chlorides are preferred from the viewpoint of availability and cost.

[0174] Specific examples of the Fe salt include iron (III) chloride hexahydrate [FeCl 3 ·6H 2 O], iron (III) nitrate nonahydrate [Fe(NO 3 ) 3 ·9H 2 O], and the like.

[0175] Specific examples of Al salts include aluminum chloride hexahydrate [AlCl 3 ·6H 2 O], aluminum nitrate nonahydrate [Al(NO 3 ) 3 ·9H 2 O], and the like.

[0176] Specific examples of Sr salts include strontium chloride hexahydrate [SrCl2.6H2O], strontium nitrate [Sr(NO3)2], and strontium acetate 0.5 hydrate [Sr(CH3COO)2.0.5H2O].

[0177] Specific examples of the Ba salt include barium chloride dihydrate [BaCl2.2H2O], barium nitrate [Ba(NO3)2], and barium acetate [(CH3COO)2Ba].

[0178] Specific examples of the Ca salt include calcium chloride dihydrate [CaCl2.2H2O], calcium nitrate tetrahydrate [Ca(NO3)2.4H2O], and calcium acetate monohydrate [(CH3COO)2Ca.H2O].

[0179] Specific examples of Pb salts include lead (II) chloride [PbCl 2 ], lead (II) nitrate [Pb(NO 3 ) 2 ], and the like.

[0180] The aqueous alkali solution is not particularly limited, and examples thereof include an aqueous sodium hydroxide solution and an aqueous potassium hydroxide solution.

[0181] The concentration of the aqueous alkali solution is not particularly limited, and can be, for example, 0.1 mol / L to 10 mol / L.

[0182] The raw material aqueous solution and the alkaline aqueous solution may be mixed.

[0183] The raw material aqueous solution and the alkaline aqueous solution may be mixed in total at once, or the raw material aqueous solution and the alkaline aqueous solution may be slowly mixed little by little. Furthermore, the raw material aqueous solution and the alkaline aqueous solution may be added little by little to one of the other and mixed.

[0184] For example, from the viewpoint of reproducibility of radio wave absorption performance, it is preferred to gradually mix the raw material aqueous solution and the alkaline aqueous solution little by little.

[0185] The method of mixing the raw material aqueous solution and the alkaline aqueous solution is not particularly limited, and an example thereof includes a method of mixing by stirring.

[0186] The stirring mechanism is not particularly limited, and a general stirrer or stirring device can be used.

[0187] The stirring time is not particularly limited as long as the reaction of the mixed components is completed, and can be appropriately set according to the composition of the raw material aqueous solution, the type of the stirrer or stirring device, and the like.

[0188] The temperature when mixing the raw material aqueous solution and the alkaline aqueous solution is preferably 100° C. or lower from the viewpoint of preventing sudden boiling, more preferably 95° C. or lower, and further preferably 15° C. or higher and 92° C. or lower from the viewpoint of obtaining a good reaction product.

[0189] The temperature adjustment mechanism is not particularly limited, and a general heating device, cooling device, etc. can be used.

[0190] The pH of the aqueous solution obtained by mixing the raw material aqueous solution and the alkaline aqueous solution at 25° C. is preferably 5 to 13, and more preferably 6 to 12, for example, from the viewpoint of more easily obtaining a reaction product.

[0191] The mixing ratio of the raw material aqueous solution and the alkaline aqueous solution is not particularly limited, and for example, the alkaline aqueous solution can be set to 0.1 to 10.0 parts by mass relative to 1 part by mass of the raw material aqueous solution.

[0192] -Process A2-

[0193] Step A2 is a step of subjecting the reaction product obtained in step A1 to solid-liquid separation.

[0194] The method for solid-liquid separation is not particularly limited, and examples thereof include decantation, centrifugal separation, filtration (suction filtration, pressure filtration, etc.), and the like.

[0195] When the solid-liquid separation method is centrifugal separation, the conditions for centrifugal separation are not particularly limited. For example, it is preferred to centrifuge at a rotation speed of 2000 rpm (revolutions per minute; the same applies hereinafter) or more for 3 to 30 minutes. Furthermore, centrifugal separation may be performed multiple times.

[0196] (Process B)

[0197] Step B is a step of drying the reaction product obtained in step A to obtain a dry product (so-called precursor powder).

[0198] The reaction product obtained in the pre-calcination drying step A can improve the reproducibility of the radio wave absorption performance of the manufactured radio wave absorber. In addition, the reaction product obtained in the pre-crushing drying step A can easily control the particle size distribution of the specific magnetoplumbite hexagonal ferrite powder by crushing.

[0199] The drying mechanism is not particularly limited, and examples thereof include drying machines such as ovens.

[0200] The drying temperature is not particularly limited, but is preferably 50°C to 200°C, and more preferably 70°C to 150°C, for example.

[0201] The drying time is not particularly limited, but is preferably, for example, 2 hours to 50 hours, and more preferably 5 hours to 30 hours.

[0202] (Process C)

[0203] Step C is a step of calcining the dried product obtained in step B to obtain a calcined product, and then pulverizing the calcined product (i.e., step c1), or pulverizing the dried product obtained in step B to obtain a pulverized product, and then calcining the pulverized product (i.e., step c2).

[0204] The dried product obtained in step B is calcined to obtain a calcined product, and then the calcined product is crushed, or the dried product obtained in step B is crushed to obtain a crushed product, and then the crushed product is calcined, thereby obtaining a specific magnetoplumbite-type hexagonal ferrite powder with a target particle size.

[0205] Step C may be step c1 or step c2.

[0206] For example, from the viewpoint of making the magnetic properties after calcination more uniform, step C is preferably step c2.

[0207] When step C is step c2, the calcined pulverized product may be further pulverized.

[0208] Calcination can be performed using a heating device.

[0209] The heating device is not particularly limited as long as it can heat to the target temperature, and any known heating device can be used. As the heating device, in addition to an electric furnace, for example, a calcining device individually manufactured according to a production line can be used.

[0210] Calcination is preferably carried out under atmospheric conditions.

[0211] The calcination temperature is not particularly limited, but is, for example, preferably 900°C or higher, more preferably 900°C to 1400°C, and further preferably 1000°C to 1200°C.

[0212] The calcination time is not particularly limited, but is preferably, for example, 1 to 10 hours, and more preferably 2 to 6 hours.

[0213] The pulverizing mechanism is not particularly limited as long as the specific magnetoplumbite hexagonal ferrite powder having a target particle size can be obtained.

[0214] Examples of the pulverizing mechanism include a mortar and pestle, a pulverizer (a cutter mill, a ball mill, a bead mill, a roller mill, a jet mill, a hammer mill, an attritor, etc.), and the like.

[0215] When the pulverization is performed using a medium, the particle size of the medium (so-called medium diameter) is not particularly limited, but is preferably, for example, 0.1 mm to 5.0 mm, and more preferably 0.5 mm to 3.0 mm.

[0216] In the present invention, when the "medium diameter" refers to a spherical medium (such as spherical beads), it means the diameter of the medium (such as beads); when it refers to a non-spherical medium (such as non-spherical beads), it means the diameter obtained by measuring the equivalent circular diameters of multiple media (such as beads) from observation images using a transmission electron microscope (TEM) or a scanning electron microscope (SEM), and arithmetically averaging the measured values.

[0217] The material of the medium is not particularly limited, and for example, a medium made of glass, alumina, steel, zirconia, ceramics, or the like can be preferably used.

[0218] <Adhesive>

[0219] The radio wave absorbing layer contains a binder.

[0220] Examples of the binder include thermoplastic resins and thermosetting resins.

[0221] Examples of the thermoplastic resin include acrylic resin, polyacetal, polyamide, polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polycarbonate, polystyrene, polyphenylene sulfide, polyvinyl chloride, ABS (acrylonitrile butadiene styrene) resin obtained by copolymerizing acrylonitrile, butadiene and styrene, and AS (acrylonitrile styrene) resin obtained by copolymerizing acrylonitrile and styrene.

[0222] Examples of the thermosetting resin include phenol resin, epoxy resin, melamine resin, urea resin, unsaturated polyester, diallyl phthalate resin, polyurethane resin, and silicone resin.

[0223] As the binder, for example, rubber can be mentioned.

[0224] As rubber, for example, from the viewpoint of being able to produce a radio wave absorber that has good miscibility with magnetic powder and is more excellent in durability, weather resistance and impact resistance, preferred are: butadiene rubber; isoprene rubber; chloroprene rubber; halogenated butyl rubber; fluororubber; polyurethane rubber; acrylic rubber (ACM) obtained by copolymerizing acrylates (for example, ethyl acrylate, butyl acrylate and 2-ethylhexyl acrylate) and other monomers; ethylene-propylene rubber obtained by coordination polymerization of ethylene and propylene using a Ziegler catalyst; butyl rubber (IIR) obtained by copolymerizing isobutylene and isoprene; styrene butadiene rubber (SBR) obtained by copolymerizing butadiene and styrene; acrylonitrile butadiene rubber (NBR) obtained by copolymerizing acrylonitrile and butadiene; and synthetic rubbers such as silicone rubber.

[0225] As the binder, for example, thermoplastic elastomer (TPE) can also be mentioned.

[0226] Examples of the thermoplastic elastomer include olefin-based thermoplastic elastomers (TPO), styrene-based thermoplastic elastomers (TPS), amide-based thermoplastic elastomers (TPA), and polyester-based thermoplastic elastomers (TPC).

[0227] When the radio wave absorbing layer contains rubber as a binder, it may contain various additives such as a vulcanizing agent, a vulcanizing accelerator, a softener, and a plasticizer in addition to the rubber.

[0228] Examples of the vulcanizing agent include sulfur, organic sulfur compounds, and metal oxides.

[0229] The melt flow rate (hereinafter also referred to as "MFR") of the binder is not particularly limited, and is, for example, preferably 1 g / 10 min to 200 g / 10 min, more preferably 3 g / 10 min to 100 g / 10 min, further preferably 5 g / 10 min to 80 g / 10 min, and particularly preferably 10 g / 10 min to 50 g / 10 min.

[0230] When the MFR of the adhesive is 1 g / 10 min or more, the fluidity is sufficiently high and appearance defects are less likely to occur.

[0231] When the MFR of the binder is 200 g / 10 min or less, it is easier to improve mechanical properties such as strength of the molded product.

[0232] The MFR of the adhesive is a value measured under the conditions of a measurement temperature of 230° C. and a load of 10 kg in accordance with JIS K 7210:1999.

[0233] The hardness of the binder is not particularly limited, but is preferably 5 g to 150 g, more preferably 10 g to 120 g, further preferably 30 g to 100 g, and particularly preferably 40 g to 90 g, from the viewpoint of molding suitability.

[0234] The hardness of the adhesive is an instantaneous value measured in accordance with JIS K 6253-3:2012.

[0235] The density of the binder is not particularly limited, but is preferably 600 kg / m 3 ~1100kg / m 3 , more preferably 700kg / m 3 ~1000kg / m 3 , more preferably 750kg / m 3 ~1050kg / m 3 , especially preferably 800kg / m3 ~950kg / m 3 .

[0236] The density of the adhesive is a value measured in accordance with JIS K 0061:2001.

[0237] The 100% tensile stress of the adhesive is not particularly limited, but is preferably 0.2 MPa to 20 MPa, more preferably 0.5 MPa to 10 MPa, further preferably 1 MPa to 5 MPa, and particularly preferably 1.5 MPa to 3 MPa, from the viewpoint of molding suitability.

[0238] The tensile strength of the adhesive is not particularly limited, but is preferably 1 MPa to 20 MPa, more preferably 2 MPa to 15 MPa, further preferably 3 MPa to 10 MPa, and particularly preferably 5 MPa to 8 MPa, from the viewpoint of molding suitability.

[0239] The elongation of the adhesive during cutting is not particularly limited, but is preferably 110% to 1500%, more preferably 150% to 1000%, further preferably 200% to 900%, and particularly preferably 400% to 800%, from the viewpoint of molding suitability.

[0240] The above tensile properties are values ​​measured in accordance with JIS K 6251: 2010. The measurement was performed using a JIS No. 3 dumbbell as a test piece at a tensile speed of 500 mm / min.

[0241] The radio wave absorbing layer may contain only one type of binder, or may contain two or more types of binders.

[0242] The filling rate of the binder in the radio wave absorbing layer is not particularly limited, but is, for example, preferably 65 volume % or more, more preferably 65 volume % or more and 92 volume % or less, and further preferably 65 volume % or more and 85 volume % or less.

[0243] <Other additives>

[0244] The radio wave absorbing layer may contain various additives (so-called other additives) as necessary, in addition to the magnetic powder and the binder, within a range that does not impair the effect of the radio wave absorber of the present invention.

[0245] Examples of other additives include dispersants, dispersing aids, mildew preventers, antistatic agents, antioxidants, etc. Other additives may be additives in which one component performs two or more functions.

[0246] [Method for producing radio wave absorber]

[0247] The method for producing the radio wave absorber of the present invention is not particularly limited.

[0248] The radio wave absorber of the present invention can be produced by a known method using magnetic powder, a binder, a solvent as needed, other additives, and the like.

[0249] The radio wave absorber of the present invention can be produced by, for example, the following method X.

[0250] The mixture containing the magnetic powder, the binder, and other additives as needed is kneaded using a kneading machine while being heated to obtain a composite material. Then, the obtained composite material is molded to produce a radio wave absorber including a radio wave absorbing layer.

[0251] The magnetic powder in method X has the same meaning as the magnetic powder described in the section of "radio wave absorber" and the preferred embodiment is also the same, so the description is omitted here.

[0252] The content of the magnetic powder in the mixture may be adjusted so that the filling rate of the magnetic powder in the radio wave absorbing layer finally obtained becomes 35 volume % or less.

[0253] The adhesive in method X has the same meaning as the adhesive described in the section of "radio wave absorber" and the preferred embodiment is also the same, so the description thereof is omitted here.

[0254] The content of the binder in the mixture is not particularly limited. For example, the filling rate of the binder in the finally obtained radio wave absorbing layer is preferably adjusted to the filling rate of the binder in the radio wave absorbing layer described above.

[0255] The other additives in method X have the same meanings as those of the other additives described in the section "Radio wave absorber" and the same preferred embodiments, so their description is omitted here.

[0256] In the mixture, the magnetic powder and the binder only need to be mixed.

[0257] The method of mixing the magnetic powder and the binder is not particularly limited, and an example thereof includes a method of mixing by stirring.

[0258] The stirring mechanism is not particularly limited, and a general stirring device can be used.

[0259] Examples of the stirring device include stirrers such as a paddle stirrer and an impeller stirrer.

[0260] The stirring time is not particularly limited, and can be appropriately set according to, for example, the type of stirring device, the composition of the mixture, and the like.

[0261] The heating temperature of the mixture is not particularly limited, and can be appropriately set according to the type of the binder, for example.

[0262] The heating temperature is preferably a temperature at which the adhesive can be melted, and can be set to 170°C to 300°C, for example.

[0263] The kneading mechanism is not particularly limited, and a general kneading device can be used.

[0264] Examples of the kneading device include a stirrer, a twin roll, a kneader and the like.

[0265] The kneading conditions are not particularly limited, and can be appropriately set according to, for example, the type of kneading apparatus, the composition of the mixture, and the like.

[0266] Examples of the molding process include press molding, extrusion molding, injection molding, in-mold molding, and molding using a three-dimensional molding machine.

[0267] The molding conditions are not particularly limited, and can be appropriately set according to, for example, the type of molding apparatus, the composition of the mixture, the thickness of the radio wave absorbing layer, and the like.

[0268] When the filling rate of the magnetic powder in the radio wave absorbing layer is P volume % and the thickness of the radio wave absorbing layer is Q mm, the thickness of the radio wave absorbing layer is not particularly limited as long as the relationship of 0.65≤(P / 100)×Q is satisfied.

[0269] The thickness of the radio wave absorbing layer can be adjusted by, for example, molding the composite.

[0270] Furthermore, the radio wave absorber of the present invention can be produced by, for example, the following method Y.

[0271] A composition for forming a radio wave absorbing layer, which includes a magnetic powder, a binder, and, if necessary, a solvent, other additives, etc., is applied to a dummy support to form a coating film of the composition for forming a radio wave absorbing layer. Then, the coating film of the composition for forming a radio wave absorbing layer is dried to form a radio wave absorbing layer. Then, the dummy support can be peeled off from the radio wave absorbing layer to produce a radio wave absorber composed of the radio wave absorbing layer.

[0272] The magnetic powder in method Y has the same meaning as the magnetic powder described in the section of "radio wave absorber" and the preferred method is also the same, so the description is omitted here.

[0273] The content of the magnetic powder in the composition for forming a radio wave absorbing layer is adjusted so that the filling rate of the magnetic powder in the radio wave absorbing layer finally obtained becomes 35 volume % or less.

[0274] The adhesive in method Y has the same meaning as the adhesive described in the section of "radio wave absorber" and the preferred embodiment is also the same, so the description thereof is omitted here.

[0275] The content of the binder in the composition for forming a radio wave absorbing layer is not particularly limited. For example, the filling rate of the binder in the finally obtained radio wave absorbing layer is preferably adjusted to the filling rate of the binder in the radio wave absorbing layer described above.

[0276] The solvent in the method Y is not particularly limited, and examples thereof include water, an organic solvent, and a mixed solvent of water and an organic solvent.

[0277] Examples of the organic solvent include alcohols such as methanol, ethanol, n-propanol, isopropanol, and methoxypropanol; ketones such as acetone, methyl ethyl ketone, cyclohexane, and cyclohexanone; tetrahydrofuran, acetonitrile, ethyl acetate, and toluene.

[0278] When the composition for forming a radio wave absorbing layer contains a solvent, the content of the solvent in the composition for forming a radio wave absorbing layer is not particularly limited and can be appropriately set according to the types and amounts of components blended in the composition for forming a radio wave absorbing layer.

[0279] The other additives in method Y have the same meanings as the other additives described in the section "Radio wave absorber" and the same preferred embodiments, so their description is omitted here.

[0280] In the composition for forming a radio wave absorbing layer, the magnetic powder and the binder may be mixed.

[0281] The method of mixing the magnetic powder and the binder is not particularly limited, and an example thereof includes a method of mixing by stirring.

[0282] The stirring mechanism is not particularly limited, and a general stirring device can be used.

[0283] Examples of the stirring device include stirrers such as a paddle stirrer and an impeller stirrer.

[0284] The stirring time is not particularly limited, and can be appropriately set according to, for example, the type of stirring device, the composition of the composition for forming the radio wave absorbing layer, and the like.

[0285] The dummy support is not particularly limited.

[0286] As pseudo supports, metal plates (aluminum, zinc, copper and other metal plates), glass plates, plastic sheets [polyester (polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, etc.), polyethylene (linear low-density polyethylene, low-density polyethylene, high-density polyethylene, etc.), polypropylene, polystyrene, polycarbonate, polyimide, polyamide, polyamideimide, polysulfone, polyvinyl chloride, polyacrylonitrile, polyphenylene sulfide, polyetherimide, polyethersulfone, polyvinyl acetal, acrylic resin and other sheets] and the like can be listed.

[0287] The plastic sheet is preferably subjected to a mold release treatment on its surface.

[0288] The size of the dummy support is not particularly limited, and can be appropriately set according to the size of the radio wave absorbing layer, for example.

[0289] The thickness of the dummy support is not particularly limited, but is generally about 0.01 mm to 0.5 mm, and preferably 0.05 mm to 0.2 mm, for example, from the viewpoint of handleability.

[0290] The method for coating the radio wave absorbing layer-forming composition on the dummy support is not particularly limited, and examples thereof include methods using a film coater, a knife coater, an applicator, and the like.

[0291] The method of drying the coating film of the composition for forming a radio wave absorbing layer is not particularly limited, and examples thereof include a method using a heating device such as an oven.

[0292] The drying temperature and the drying time are not particularly limited as long as the solvent contained in the coating film of the composition for forming a radio wave absorbing layer can be volatilized.

[0293] For example, heating is performed at 70°C to 90°C for 1 hour to 3 hours.

[0294] When the filling rate of the magnetic powder in the radio wave absorbing layer is P volume % and the thickness of the radio wave absorbing layer is Q mm, the thickness of the radio wave absorbing layer is not particularly limited as long as the relationship of 0.65≤(P / 100)×Q is satisfied.

[0295] The thickness of the radio wave absorbing layer can be adjusted by, for example, the coating amount of the composition for forming the radio wave absorbing layer.

[0296] [Compound]

[0297] The composite of the present invention is a composite for producing the radio wave absorber of the present invention, and contains magnetic powder and a binder, wherein the filling rate of the magnetic powder is 35 volume % or less.

[0298] The magnetic powder in the composite of the present invention has the same meaning as the magnetic powder described in the section of "radio wave absorber" and the preferred embodiment is also the same, so the description thereof is omitted here.

[0299] The filling rate of the magnetic powder in the composite of the present invention is 35 volume % or less, preferably 8 volume % or more and 35 volume % or less, more preferably 15 volume % or more and 35 volume % or less, and further preferably 20 volume % or more and 35 volume % or less.

[0300] The filling rate of the magnetic powder in the composite of the present invention is a value measured by the following method.

[0301] A radio wave absorbing layer was prepared using the composite of the present invention. The prepared radio wave absorbing layer was used to measure the filling rate of the magnetic powder in the radio wave absorbing layer by the same method as described in the section of "Radio wave absorber".

[0302] The binder in the composite of the present invention has the same meaning as the binder described in the section of "radio wave absorber" and the preferred embodiments are also the same, so the description thereof is omitted here.

[0303] The filling rate of the binder in the composite of the present invention is not particularly limited, but is, for example, preferably 65 volume % or more, more preferably 65 volume % or more and 92 volume % or less, and further preferably 65 volume % or more and 85 volume % or less.

[0304] The composite of the present invention may be in the form of particles.

[0305] The size (diameter) of the granular composite is not particularly limited, but is, for example, preferably 0.5 mm to 20 mm, more preferably 1 mm to 10 mm, further preferably 2 mm to 8 mm, and particularly preferably 3 mm to 6 mm.

[0306] The density of the granular composite is not particularly limited, but is preferably 500 kg / m 3 ~5000kg / m 3 , more preferably 800kg / m 3 ~4000kg / m 3 , more preferably 1000kg / m 3 ~3500kg / m 3 , especially preferably 1200kg / m 3 ~3000kg / m 3 .

[0307] The density of the composite is a value measured in accordance with JIS K 0061:2001.

[0308] The composite of the present invention may contain various additives (so-called other additives) as necessary in addition to the magnetic powder and the binder.

[0309] The other additives in the composite of the present invention have the same meanings as the other additives described in the section of "radio wave absorber" and the same preferred embodiments, so the description thereof is omitted here.

[0310] Example

[0311] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to the following Examples unless the scope of the invention exceeds the scope of the invention.

[0312] [Production of magnetic powder]

[0313] 〔Magnetic powder 1〕

[0314] 400.0 g of water was stirred and maintained at 35° C., and all amounts of a raw aqueous solution prepared by dissolving 57.0 g of iron (III) chloride hexahydrate [FeCl3·6H2O], 27.8 g of strontium chloride hexahydrate [SrCl2·6H2O] and 10.2 g of aluminum chloride hexahydrate [AlCl3·6H2O] in 216.0 g of water and a solution prepared by adding 113.0 g of water to 181.3 g of a 5 mol / L sodium hydroxide aqueous solution were added to the stirred water at a flow rate of 10 mL / min at the same addition timing to obtain a first liquid.

[0315] Next, after the temperature of the first liquid was changed to 25° C., 39.8 g of a 1 mol / L sodium hydroxide aqueous solution was added while maintaining the temperature to obtain a second liquid. The pH of the obtained second liquid was 10.5. The pH of the second liquid was measured using a tabletop pH meter F-71 (product name) from HORIBA, Ltd. (the same shall apply hereinafter).

[0316] Next, the second liquid was stirred for 15 minutes to complete the reaction, thereby obtaining a liquid containing a reaction product of a precursor of magnetoplumbite-type hexagonal ferrite powder (ie, a precursor-containing liquid).

[0317] Next, the liquid containing the precursor was subjected to centrifugal separation treatment three times (rotation speed: 3000 rpm, rotation time: 10 minutes), and the obtained precipitate was recovered.

[0318] Next, the recovered precipitate was dried in an oven at an internal ambient temperature of 95° C. for 12 hours to obtain an aggregate of particles consisting of the precursor (ie, precursor powder).

[0319] Next, the precursor powder was placed in a muffle furnace and calcined for 4 hours under an atmospheric environment with the temperature in the furnace set to 1100° C., thereby obtaining a calcined body.

[0320] Next, the calcined body was pulverized for 90 seconds using Wonder Crusher WC-3 (product name) from OSAKA CHEMICAL Co., Ltd. by setting the speed dial to “5” to obtain a magnetic powder 1 .

[0321] 〔Magnetic powder 2〕

[0322] 400.0 g of water was stirred and maintained at 35° C., and all amounts of a raw aqueous solution prepared by dissolving 57.0 g of iron (III) chloride hexahydrate [FeCl3·6H2O], 27.8 g of strontium chloride hexahydrate [SrCl2·6H2O] and 10.2 g of aluminum chloride hexahydrate [AlCl3·6H2O] in 216.0 g of water and a solution prepared by adding 113.0 g of water to 181.3 g of a 5 mol / L sodium hydroxide aqueous solution were added to the stirred water at a flow rate of 10 mL / min at the same addition timing to obtain a first liquid.

[0323] Next, after the temperature of the first liquid was changed to 25° C., 30.2 g of a 1 mol / L sodium hydroxide aqueous solution was added while maintaining the temperature to obtain a second liquid. The pH of the obtained second liquid was measured to be 9.5.

[0324] Next, the second liquid was stirred for 15 minutes to complete the reaction, thereby obtaining a liquid containing a reaction product of a precursor of magnetoplumbite-type hexagonal ferrite powder (ie, a precursor-containing liquid).

[0325] Next, the liquid containing the precursor was subjected to centrifugal separation treatment three times (rotation speed: 3000 rpm, rotation time: 10 minutes), and the obtained precipitate was recovered.

[0326] Next, the recovered precipitate was dried in an oven at an internal ambient temperature of 95° C. for 12 hours to obtain an aggregate of particles consisting of the precursor (ie, precursor powder).

[0327] Next, the precursor powder was placed in a muffle furnace and calcined for 4 hours under an atmospheric environment with the temperature in the furnace set to 1100° C., thereby obtaining a calcined body.

[0328] Next, the calcined body was pulverized for 60 seconds using Wonder Crusher WC-3 (product name) manufactured by OSAKA CHEMICAL Co., Ltd. by setting the speed dial to “5” to obtain a magnetic powder 2.

[0329] <Confirmation of Crystal Structure>

[0330] The crystal structure of the magnetic substance forming each of the magnetic powders 1 and 2 (hereinafter, also referred to as “magnetic substance 1 and magnetic substance 2 ”, respectively) was confirmed by X-ray diffraction (XRD) method.

[0331] Specifically, it is confirmed whether or not the material has a magnetoplumbite type crystal structure, and whether it is a single phase or has two or more different crystal phases.

[0332] The measurement apparatus used was X'Pert Pro (product name) of PANalytical, which is a powder X-ray diffraction apparatus. The measurement conditions are shown below.

[0333] -Measurement conditions-

[0334] X-ray source: CuKα line

[0335] 〔wavelength: (0.154nm), output: 40mA, 45kV〕

[0336] Scanning range: 20°<2θ<70°

[0337] Scanning interval: 0.05°

[0338] Scanning speed: 0.75° / min

[0339] As a result, it was confirmed that both the magnetic substance 1 and the magnetic substance 2 had a magnetoplumbite type crystal structure and were single-phase magnetoplumbite type hexagonal ferrites that did not include a crystal structure other than the magnetoplumbite type.

[0340] <Confirmation of composition>

[0341] The composition of each magnetic substance of Magnetic Substance 1 and Magnetic Substance 2 was confirmed by high-frequency inductively coupled plasma (ICP) emission spectrometry.

[0342] Specifically, the confirmation was performed by the following method.

[0343] A beaker (pressure-resistant container) containing 12 mg of magnetic powder and 10 mL of 4 mol / L hydrochloric acid aqueous solution was kept in an oven set at 120°C for 12 hours to obtain a solution. After adding 30 mL of pure water to the obtained solution, it was filtered using a 0.1 μm membrane filter. The elemental analysis of the filtrate obtained in this way was performed using a high-frequency inductively coupled plasma (ICP) emission spectrometer [Model: ICPS-8100, Shimadzu Corporation].

[0344] Based on the obtained elemental analysis results, the content of each metal atom relative to 100 atomic % of iron atoms was determined. Then, the composition of the magnetic substance was confirmed based on the obtained content. The composition of each magnetic substance is shown below.

[0345] Magnetic body 1: SrFe (10.00) Al (2.00) O 19

[0346] Magnetic body 2: SrFe (9.70) Al (2.30) O 19

[0347] As a result, it was confirmed that both the magnetic powder 1 and the magnetic powder 2 were powders of magnetoplumbite-type hexagonal ferrite represented by the formula (1) (that is, specific magnetoplumbite-type hexagonal ferrite powders).

[0348] <Measurement of Particle Size Distribution>

[0349] The particle size distribution of each of the magnetic powders 1 and 2 was measured based on the number of particles by a laser diffraction scattering method, and the mode value (so-called mode diameter), the cumulative 10% diameter, and the cumulative 90% diameter were obtained.

[0350] Specifically, 500 mL of cyclohexanone was added to 10 mg of the magnetic powder for dilution, and then the mixture was stirred for 30 seconds using a shaker, and the obtained liquid was used as a sample for particle size distribution measurement.

[0351] Next, the particle size distribution of the sample for particle size distribution measurement was measured using a laser diffraction / scattering particle size distribution measuring apparatus [product name: Partica LA-960, HORIBA, Ltd.].

[0352] Then, based on the obtained number-based particle size distribution, the mode diameter (unit: μm) as the mode value and the cumulative 10% diameter D 10 (Unit: μm) and D as the cumulative 90% diameter 90 (Unit: μm). And, the "(D 90 -D 10 ) / mode diameter” value.

[0353] As a result, the mode diameter of magnetic powder 1 was 6.7 μm, and D 10 4.1μm, D 90 9.5μm, (D 90 -D 10 ) / mode diameter" is 0.81. In addition, in magnetic powder 2, the mode diameter is 8.8 μm, D 10 5.5μm, D 90 12.5μm, (D 90 -D 10 ) / mode diameter” is 0.80.

[0354] <Measurement of Magnetic Properties>

[0355] For each of the magnetic powders 1 and 2, the coercive force (Hc) and the saturation magnetization (δs) were measured as magnetic properties.

[0356] Specifically, the measurement was performed by the following method.

[0357] As a measuring device, a vibrating sample magnetometer [Model: TM-TRVSM5050-SMSL, TAMAKAWA CO., LTD] was used. Under the conditions of a maximum applied magnetic field of 50 kOe and a magnetic field scanning speed of 25 Oe / s (seconds) at an ambient temperature of 23°C, the magnetization intensity of the magnetic powder relative to the applied magnetic field was measured. From the measurement results, a magnetic field (H)-magnetization (M) curve of the magnetic powder was obtained. Based on the obtained magnetic field (H)-magnetization (M) curve, the coercive force (Hc) (unit: kOe) and saturation magnetization (δs) (unit: emu / g) of the magnetic powder were calculated.

[0358] As a result, the coercive force (Hc) of magnetic powder 1 was 10.5 kOe and the saturation magnetization (δs) was 43.2 emu / g, and the coercive force (Hc) of magnetic powder 2 was 10.0 kOe and the saturation magnetization (δs) was 40.2 emu / g.

[0359] [Production of Radio Wave Absorber (1)]

[0360] [Example 1]

[0361] 1. Preparation of the composite

[0362] A composite was prepared using the magnetic powder 1 and a binder [trade name: Mirastomer (registered trademark) 7030NS, olefin-based thermoplastic elastomer (TPO), Mitsui Chemicals, Inc.] Specifically, the composite was prepared as follows.

[0363] The magnetic powder 1 and the above-mentioned binder were mixed to obtain a mixture. The mixing amounts of the magnetic powder 1 and the above-mentioned binder were set to an amount such that the filling rate of the magnetic powder 1 in the final composite material was 15 volume %. Next, the obtained mixture was kneaded for 20 minutes at a set temperature of 200° C. and a rotation speed of 50 rpm using LABOPLASTOMILL (product name, Toyo Seiki Seisaku-sho, Ltd.) to obtain a composite material.

[0364] 2. Fabrication of radio wave absorbers

[0365] The obtained compound was molded using a hot press device under the conditions of molding pressure: 20 MPa, pressing temperature: 200°C and pressing time: 10 minutes to obtain a sheet-shaped radio wave absorber (size: 100 mm×100 mm). The amount of the compound used was set to an amount that the thickness of the final radio wave absorber was 4.5 mm.

[0366] [Example 2]

[0367] The same operations as in Example 1 were performed, except that the amounts of the magnetic powder 1 and the binder were changed so that the filling rate of the magnetic powder 1 in the final composite material became 30 volume %, and the amount of the composite material was changed so that the thickness of the final radio wave absorber became 3 mm. Thus, a sheet-shaped radio wave absorber (size: 100 mm × 100 mm) was obtained.

[0368] [Comparative Example 1]

[0369] A sheet-shaped radio wave absorber (size: 100 mm×100 mm) was obtained by performing the same operation as in Example 1 except that the amount of the composite used was changed so that the thickness of the radio wave absorber finally obtained would be 3 mm.

[0370] [Comparative Example 2]

[0371] A sheet-shaped radio wave absorber (size: 100 mm × 100 mm) was obtained by performing the same operations as in Example 1, except that the amounts of the magnetic powder 1 and the binder were changed so that the filling rate of the magnetic powder 1 in the final composite material became 30 volume %, and the amount of the composite material was changed so that the thickness of the final radio wave absorber became 2 mm.

[0372] [Comparative Example 3]

[0373] A sheet-shaped radio wave absorber (size: 100 mm × 100 mm) was obtained by performing the same operations as in Example 1, except that the amounts of the magnetic powder 1 and the binder were changed so that the filling rate of the magnetic powder 1 in the final composite material became 40 volume %, and the amount of the composite material was changed so that the thickness of the final radio wave absorber became 2 mm.

[0374] [Comparative Example 4]

[0375] A sheet-shaped radio wave absorber (size: 100 mm × 100 mm) was obtained by performing the same operations as in Example 1, except that the amounts of the magnetic powder 1 and the binder were changed so that the filling rate of the magnetic powder 1 in the final composite material became 40 volume %, and the amount of the composite material was changed so that the thickness of the final radio wave absorber became 3 mm.

[0376] [Comparative Example 5]

[0377] A sheet-shaped radio wave absorber (size: 100 mm × 100 mm) was obtained by performing the same operations as in Example 1, except that the amounts of the magnetic powder 1 and the binder were changed so that the filling rate of the magnetic powder 1 in the final composite material became 50 volume %, and the amount of the composite material was changed so that the thickness of the final radio wave absorber became 2 mm.

[0378] Table 1 shows “the filling rate of the magnetic powder in the radio wave absorbing layer (unit: volume %)”, “the thickness of the radio wave absorbing layer (unit: mm)” and “(P / 100)×Q” of each radio wave absorber of Example 1, Example 2 and Comparative Examples 1 to 5.

[0379] [Production of Radio Wave Absorber (2)]

[0380] [Example 3]

[0381] 1. Preparation of the composite

[0382] A composite was prepared using the magnetic powder 2 and a binder [trade name: Mirastomer (registered trademark) 7030NS, olefin-based thermoplastic elastomer (TPO), Mitsui Chemicals, Inc.] Specifically, the composite was prepared as follows.

[0383] The magnetic powder 2 and the binder were mixed to obtain a mixture. The amounts of the magnetic powder 2 and the binder were set so that the filling rate of the magnetic powder 2 in the final composite material was 15% by volume. Then, the obtained mixture was kneaded for 20 minutes at a set temperature of 200° C. and a rotation speed of 50 rpm using LABOPLASTOMILL (product name, Toyo Seiki Seisaku-sho, Ltd.) to obtain a composite material.

[0384] 2. Fabrication of radio wave absorbers

[0385] The obtained compound was molded using a hot press device under the conditions of molding pressure: 20 MPa, pressing temperature: 200°C and pressing time: 10 minutes to obtain a sheet-shaped radio wave absorber (size: 100 mm×100 mm). The amount of the compound used was set to an amount that the thickness of the final radio wave absorber was 4.5 mm.

[0386] [Example 4]

[0387] The same operations as in Example 3 were performed, except that the amounts of the magnetic powder 2 and the adhesive were changed so that the filling rate of the magnetic powder 2 in the final composite material became 30 volume %, and the amount of the composite material was changed so that the thickness of the final radio wave absorber became 3 mm. Thus, a sheet-shaped radio wave absorber (size: 100 mm × 100 mm) was obtained.

[0388] [Comparative Example 6]

[0389] The same operations as in Example 3 were performed, except that the amounts of the magnetic powder 2 and the binder were changed so that the filling rate of the magnetic powder 2 in the final composite material became 40 volume %, and the amount of the composite material was changed so that the thickness of the final radio wave absorber became 2 mm. Thus, a sheet-shaped radio wave absorber (size: 100 mm × 100 mm) was obtained.

[0390] Table 2 shows “the filling rate of the magnetic powder in the radio wave absorbing layer (unit: volume %)”, “the thickness of the radio wave absorbing layer (unit: mm)” and “(P / 100)×Q” of each radio wave absorber of Example 3, Example 4 and Comparative Example 6.

[0391] [Measurement]

[0392] 1. Determination of transmission attenuation and reflection attenuation (1)

[0393] The transmission attenuation (unit: dB) and reflection attenuation (unit: dB) of each radio wave absorber of Examples 1 to 4 and Comparative Examples 1 to 6 were measured.

[0394] Specifically, the measurement is performed as follows.

[0395] As a measuring device, a vector network analyzer (product name: N5225B) of Keysight and a horn antenna (product name: RH12S23) of KEYCOM Corporation were used. By the free space method, the incident angle was set to 0°, and the scanning frequency was set to 60 GHz to 90 GHz. The S parameters were measured. For the radio wave absorbers of Example 1, Example 2, and Comparative Examples 1 to Comparative Examples 5, the transmission attenuation and reflection attenuation at 76.5 GHz were obtained. For the radio wave absorbers of Example 3, Example 4, and Comparative Example 6, the transmission attenuation and reflection attenuation at 85.0 GHz were obtained. The results are shown in Tables 1 and 2, respectively.

[0396] [Table 1]

[0397]

[0398] [Table 2]

[0399]

[0400] As shown in Table 1 and Table 2, it was confirmed that the transmission attenuation and reflection attenuation of the radio wave absorbers of Examples 1 to 4 were all 10 dB or more in the millimeter wave band.

[0401] On the other hand, it was confirmed that at least one of the transmission attenuation and the reflection attenuation of the radio wave absorbers of Comparative Examples 1 to 6 was less than 10 dB.

[0402] [Production of Radio Wave Absorber (3)]

[0403] [Example 5]

[0404] 1. Preparation of the composite

[0405] A composite was prepared using the magnetic powder 1 and a binder [trade name: Mirastomer (registered trademark) 7030NS, olefin-based thermoplastic elastomer (TPO), Mitsui Chemicals, Inc.] Specifically, the composite was prepared as follows.

[0406] The magnetic powder 1 and the binder were mixed to obtain a mixture. The amounts of the magnetic powder 1 and the binder were set so that the filling rate of the magnetic powder 1 in the final composite material was 30% by volume. Then, the obtained mixture was kneaded for 20 minutes at a set temperature of 200° C. and a rotation speed of 50 rpm using LABOPLASTOMILL (product name, Toyo Seiki Seisaku-sho, Ltd.) to obtain a composite material.

[0407] 2. Fabrication of radio wave absorbers

[0408] The obtained compound was extruded into a cylindrical shape from a die using a two-screw mixing extruder [Model: KZW15TW, TECHNOVE L CORPORATION] with the screw temperature set to 200°C, thereby obtaining a cylindrical radio wave absorber (inner diameter: 100 mm, height: 150 mm, thickness: 3 mm).

Claims

1. A radio wave absorber having a radio wave absorbing layer comprising magnetic powder and a binder and having no metal layer, wherein: The filling rate of the magnetic powder in the radio wave absorbing layer is 35 volume % or less, When the filling rate of the magnetic powder in the radio wave absorbing layer is set to P volume % and the thickness of the radio wave absorbing layer is set to Q mm, the relationship of 0.65≤(P / 100)×Q is satisfied, The magnetic powder comprises powder of magnetoplumbite hexagonal ferrite, The adhesive is selected from thermoplastic resin, thermosetting resin, rubber and thermoplastic elastomer.

2. The radio wave absorber according to claim 1, wherein: The thickness of the radio wave absorbing layer is 10 mm or less, and the filling rate is 8 volume % or more and 35 volume % or less.

3. The radio wave absorber according to claim 1 or 2, wherein: The thickness of the radio wave absorbing layer is 5 mm or less, and the filling rate is 15 volume % or more and 35 volume % or less.

4. The radio wave absorber according to claim 1 or 2, wherein: The magnetic powder includes a powder of magnetoplumbite hexagonal ferrite represented by the following formula (1): AFe(12-x)AⅠxO19 Formula (1) In formula (1), A represents at least one metal element selected from the group consisting of Sr, Ba, Ca and Pb, and x satisfies 1.5≤x≤8.

0.

5. The radio wave absorber according to claim 4, wherein: A in the formula (1) is Sr.

6. The radio wave absorber according to claim 4, wherein: In the formula (1), x satisfies 1.5≤x≤6.

0.

7. The radio wave absorber according to claim 1 or 2, wherein: In the particle size distribution of the magnetic powder measured by the laser diffraction scattering method, when the mode value is defined as the mode diameter and the cumulative 10% diameter is defined as D 10 , and the cumulative 90% diameter is set to D 90 When the mode diameter is 5 μm or more and less than 10 μm, and (D 90 -D 10 ) / mode diameter ≤3.

0.

8. The radio wave absorber according to claim 1 or 2, wherein: The radio wave absorber has a planar shape.

9. The radio wave absorber according to claim 1 or 2, wherein: The radio wave absorber has a three-dimensional shape.