Cured film-forming composition, orientation member, and phase difference member

By using polymers of N-alkoxymethyl(meth)acrylamide and N-hydroxyalkyl(meth)acrylamide, combining crosslinking catalysts and adhesion-enhancing components, the liquid crystal orientation in the prior art was solved. The problem of insufficient properties and solvent resistance has achieved efficient formation of phase difference members.

CN113874470BActive Publication Date: 2024-11-19NISSAN CHEM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080038503.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-05-27
Filing Date
2020-05-26
Publication Date
2024-11-19
Estimated Expiration
2040-05-26

AI Technical Summary

Technical Problem

In the prior art, when forming a phase difference member, it is difficult to obtain sufficient liquid crystal orientation and solvent resistance, and a large polarized UV is required when acrylic resin with a side chain has a photodimerization part. The exposure amount leads to a decrease in orientation sensitivity.

Method used

The polymer containing N-alkoxymethyl(meth)acrylamide and N-hydroxyalkyl(meth)acrylamide is used as the liquid crystal alignment agent for photo-oriented, and the crosslinking catalyst and adhesion-enhancing component are combined to form Cured film to improve orientation sensitivity and solvent resistance.

Benefits of technology

It realizes efficient liquid crystal orientation and solvent resistance, reduces the exposure amount of polarized light, and improves the performance of the phase difference member.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003371495130000071
    Figure BDA0003371495130000071
  • Figure BDA0003371495130000111
    Figure BDA0003371495130000111
  • Figure BDA0003371495130000171
    Figure BDA0003371495130000171
Patent Text Reader

Abstract

The object of the present invention is to provide an orientation member and a composition for forming a cured film for obtaining the orientation member, wherein the orientation member not only has excellent orientation sensitivity, but also has excellent orientation uniformity, and even if it is a thin film, it is still resistant to solvents in a liquid crystal solution, and can also function as a protective layer for protecting a film substrate. The composition for forming a cured film of the present invention is characterized by containing: (A) a compound having a photo-orientation group and a substituent selected from a hydroxyl group, a carboxyl group, and an amino group, (B) a polymer obtained by polymerizing a monomer containing at least an N-alkoxymethyl (meth) acrylamide compound, and (C) a polymer obtained by polymerizing a monomer containing at least an N-hydroxyalkyl (meth) acrylamide compound, and may also contain a crosslinking catalyst as a component (D) and a component (E) as required. A cured film can be formed by using the composition for forming a cured film, and an orientation member can be formed by using a photo-orientation technique. A phase difference member can be obtained by coating a polymerizable liquid crystal on the orientation member and curing it.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a cured film-forming composition, an orientation member, and a phase difference member. Background Art

[0002] In the case of a 3D display of circularly polarized glasses, a phase difference component is usually arranged on a display component that forms an image, such as a liquid crystal panel. The phase difference component is a patterned phase difference component formed by regularly arranging a plurality of two phase difference regions with different phase difference characteristics. It should be noted that, hereinafter, in this specification, a phase difference component patterned by arranging a plurality of phase difference regions with different phase difference characteristics is referred to as a patterned phase difference component.

[0003] The patterned phase difference component can be produced by optically patterning the phase difference material containing polymerizable liquid crystal, for example, as disclosed in Patent Document 1. The optical patterning of the phase difference material containing polymerizable liquid crystal utilizes the well-known photo-orientation technology in the formation of the orientation component of the liquid crystal panel. That is, a coating film containing a photo-orientation material is provided on the substrate, and two polarized lights with different polarization directions are irradiated thereto. Subsequently, a photo-orientation film is obtained as an orientation component of two liquid crystal orientation regions with different orientation control directions of liquid crystals. A solution-like phase difference material containing polymerizable liquid crystal is applied to the photo-orientation film to achieve the orientation of the polymerizable liquid crystal. Thereafter, the oriented polymerizable liquid crystal is cured to form a patterned phase difference component.

[0004] The anti-reflection film of the organic EL display is composed of a linear polarizing plate and a 1 / 4 wavelength phase difference plate, and the external light toward the panel surface of the image display panel is converted into linear polarized light by the linear polarizing plate, and then converted into circular polarized light by the 1 / 4 wavelength phase difference plate. Here, although the external light formed by the circularly polarized light is reflected on the surface of the image display panel, the rotation direction of the polarization plane is reversed at the time of the reflection. As a result, the reflected light is converted into linear polarized light in the direction shielded by the linear polarizing plate by the 1 / 4 wavelength phase difference plate in the opposite direction to when it arrives, and then shielded by the linear polarizing plate, and as a result, the outgoing light toward the outside is significantly suppressed.

[0005] Regarding the 1 / 4 wavelength phase difference plate, Patent Document 2 has proposed a method of forming a 1 / 4 wavelength phase difference plate by combining a 1 / 2 wavelength plate and a 1 / 4 wavelength plate, and forming the optical film by anti-dispersion characteristics. In the case of this method, a liquid crystal material using positive dispersion characteristics can be used to form an optical film by anti-dispersion characteristics in a wide wavelength region for color image display.

[0006] In addition, in recent years, as a liquid crystal material suitable for the phase difference layer, a material having anti-dispersion characteristics has been proposed (Patent Documents 3 and 4). If a liquid crystal material having such anti-dispersion characteristics is used, it is possible to replace the combination of a 1 / 2 wavelength plate and a 1 / 4 wavelength plate, and to form a 1 / 4 wavelength phase difference plate by two phase difference layers, and to form a phase difference layer by a single layer and ensure the anti-dispersion characteristics, and thereby to realize an optical film that can ensure the desired phase difference in a wide wavelength region with a simple structure.

[0007] An alignment layer is used to orient liquid crystals. As methods for forming an alignment layer, there are known methods such as a rubbing method and a photo-alignment method. The photo-alignment method does not have the problems of the rubbing method, that is, does not generate static electricity or dust, and is useful in that a quantitative alignment process can be controlled.

[0008] In the formation of the orientation member using the photo-orientation method, as the photo-orientation material that can be used, acrylic resin or polyimide resin having a photo-dimerization site of a cinnamoyl group and a chalcone group in the side chain is known. It has been reported that these resins show the performance of controlling the liquid crystal orientation (hereinafter also referred to as liquid crystal orientation) by polarized UV irradiation (see Patent Documents 5 to 7).

[0009] In addition, the orientation layer is required to have solvent resistance in addition to liquid crystal orientation ability. For example, the orientation layer may be exposed to heat or solvent during the manufacturing process of the phase difference component. If the orientation layer is exposed to a solvent, there is a concern that the liquid crystal orientation ability may be significantly reduced.

[0010] Therefore, for example, in Patent Document 8, in order to obtain stable liquid crystal orientation ability, a liquid crystal orientation agent has been proposed, which contains: a polymer component having a structure that can undergo a cross-linking reaction by light and a structure that can undergo a cross-linking reaction by heat; a liquid crystal orientation agent has also been proposed, which contains: a polymer component having a structure that can undergo a cross-linking reaction by light and a compound having a structure that can undergo a cross-linking reaction by heat.

[0011] [Prior art literature]

[0012] [Patent Document]

[0013] [Patent Document 1] Japanese Patent Application Publication No. 2005-49865

[0014] [Patent Document 2] Japanese Patent Application Laid-Open No. 10-68816

[0015] [Patent Document 3] U.S. Patent No. 8119026

[0016] [Patent Document 4] Japanese Patent Application Publication No. 2009-179563

[0017] [Patent Document 5] Japanese Patent No. 3611342

[0018] [Patent Document 6] Japanese Patent Application Publication No. 2009-058584

[0019] [Patent Document 7] Japanese Patent Publication No. 2001-517719

[0020] [Patent Document 8] Japanese Patent No. 4207430 Summary of the invention

[0021] [Problems to be Solved by the Invention]

[0022] As described above, the phase difference member is composed of a layer of a cured polymerizable liquid crystal laminated on an alignment member, that is, a photo-alignment film. Therefore, it is considered necessary to develop an alignment member that can achieve both excellent liquid crystal alignment and solvent resistance.

[0023] However, according to the research of the inventors, it is known that acrylic resins having photodimerization sites such as cinnamoyl or chalcone groups in the side chains cannot obtain sufficient properties when used to form phase difference components. In particular, in order to irradiate these resins with polarized UV to form an orientation component, and use the orientation component to manufacture a phase difference component containing polymerizable liquid crystal, it becomes necessary to have a huge polarized UV exposure. This polarized UV exposure is greater than the sufficient polarized UV exposure required to orient the liquid crystal for a conventional liquid crystal panel (for example, 30 mJ / cm 2 degree. ) and become more.

[0024] The reason why the polarized UV exposure amount increases is that, when forming the phase difference member, unlike the liquid crystal for liquid crystal panels, the polymerizable liquid crystal is used in the state of a solution and is applied on the alignment member.

[0025] In the case of attempting to use an acrylic resin having a photodimerization site of a cinnamoyl group or the like in the side chain to form an orientation member and orienting a polymerizable liquid crystal, photocrosslinking will be performed in the acrylic resin or the like due to the photodimerization reaction. And until the tolerance to the polymerizable liquid crystal solution is demonstrated, it is necessary to irradiate with polarized light with a huge exposure amount. In order to orient the liquid crystal of the liquid crystal panel, it is usually sufficient to dimerize only the surface of the photo-oriented orientation member. However, when attempting to use the above-mentioned acrylic resin or the like to make the orientation member exhibit solvent resistance, it is necessary to allow the reaction to proceed to the interior of the orientation member, and more exposure is required. As a result, there will be a problem that the orientation sensitivity of the previous material becomes very small.

[0026] In addition, in order to make the resin of the above-mentioned conventional materials exhibit such solvent resistance, a technique of adding a crosslinking agent is known. However, it is known that after a thermal curing reaction using a crosslinking agent is performed, a three-dimensional structure is formed inside the formed coating film, and the photoreactivity decreases. In other words, the orientation sensitivity is greatly reduced, and even if a crosslinking agent is added to the conventional material and used, the desired effect cannot be obtained.

[0027] Furthermore, various organic solvents are used in liquid crystal inks, and a film having low resistance to organic solvents may be used as a substrate. Therefore, an alignment film having high solvent resistance is required for the purpose of protecting the film.

[0028] In view of the above, a photo-alignment technology capable of improving the alignment sensitivity of an alignment member and reducing the exposure amount of polarized UV light, and a cured film-forming composition that can be used as a liquid crystal alignment agent for photo-alignment to form the alignment member are required. In addition, a technology capable of efficiently providing a phase difference member is required.

[0029] The object of the present invention is achieved based on the above knowledge and research results. That is, the object of the present invention is to provide a composition for forming a cured film, which can be used as a liquid crystal orientation agent for photo-orientation, and the liquid crystal orientation agent for photo-orientation is used to provide an orientation member, which has excellent orientation sensitivity and orientation uniformity, and is resistant to solvents in a liquid crystal solution even in the form of a thin film, and can also function as a protective layer for protecting a film substrate.

[0030] Other objects and advantages of the present invention will become apparent from the following description.

[0031] [Methods to solve the problem]

[0032] A first aspect of the present invention relates to a cured film-forming composition, comprising:

[0033] (A) a compound having a photo-alignment group and one substituent selected from a hydroxyl group, a carboxyl group and an amino group,

[0034] (B) a polymer obtained by polymerizing a monomer containing at least an N-alkoxymethyl (meth)acrylamide compound, and

[0035] (C) A polymer obtained by polymerizing a monomer containing at least an N-hydroxyalkyl (meth)acrylamide compound.

[0036] In the first aspect of the present invention, the photo-alignment group of the component (A) is preferably a functional group of a structure that undergoes photodimerization or photoisomerization.

[0037] In the first aspect of the present invention, the photo-alignment group of the component (A) is preferably a cinnamoyl group.

[0038] In the first aspect of the present invention, the photo-alignment group of the component (A) is preferably a group having an azobenzene structure.

[0039] In the first aspect of the present invention, it is preferred that a cross-linking catalyst is further contained as the component (D).

[0040] In the first aspect of the present invention, it is preferred that an adhesion-improving component is further contained as the component (E).

[0041] In the first aspect of the present invention, the total amount of the component (B) and the component (C) is preferably 100 to 3000 parts by mass based on 100 parts by mass of the component (A).

[0042] In the first aspect of the present invention, the mass ratio of the component (B) to the component (C) is preferably 1:99 to 99:1.

[0043] In the first aspect of the present invention, it is preferred that 0.01 to 10 parts by mass of the component (D) is contained based on 100 parts by mass of the total amount of the component (B) and the component (C).

[0044] A second aspect of the present invention relates to an orientation member characterized by being obtained by using the cured film-forming composition of the first aspect of the present invention.

[0045] A third aspect of the present invention relates to a phase difference member characterized by being formed using a cured film obtained from the cured film-forming composition of the first aspect of the present invention.

[0046] [Effects of the invention]

[0047] According to the first embodiment of the present invention, a composition for forming a cured film can be provided, which is used to provide an orientation component, which not only has excellent orientation sensitivity but also excellent orientation uniformity, and even in the form of a thin film, is resistant to solvents in a liquid crystal solution and can also function as a protective layer for protecting a film substrate.

[0048] According to the second aspect of the present invention, there can be provided an orientation member which has excellent orientation sensitivity and orientation uniformity, is resistant to solvents in a liquid crystal solution even in the form of a thin film, and can function as a protective layer for protecting a film substrate.

[0049] According to the third aspect of the present invention, it is possible to provide a phase difference member that can be formed efficiently even on a film substrate and can be optically patterned. DETAILED DESCRIPTION

[0050] <Cured film-forming composition>

[0051] The cured film-forming composition of the present invention contains: (A) component, (B) component and (C) component, wherein the (A) component is a compound having a photo-alignment group and one substituent selected from a hydroxyl group, a carboxyl group and an amino group (hereinafter also described as "low-molecular photo-alignment component"), the (B) component is a polymer obtained by polymerizing a monomer containing at least an N-alkoxymethyl (meth) acrylamide compound, and the (C) component is a polymer obtained by polymerizing a monomer containing at least an N-hydroxyalkyl (meth) acrylamide compound. In addition to the (A) component, the (B) component and the (C) component, the cured film-forming composition of the present invention may also contain a crosslinking catalyst as a component (D) and a component for improving the adhesion of the cured film as a component (E). Other additives may also be contained as long as the effects of the present invention are not impaired.

[0052] Hereinafter, the details of each component will be described.

[0053] <(A)Component>

[0054] The (A) component contained in the cured film-forming composition of the present invention is a low-molecular photo-alignment component as described above.

[0055] Furthermore, the low molecular weight photo-alignment component as component (A) is a compound having a photo-alignment group and one substituent selected from hydroxyl, carboxyl and amino groups. In the compound having a photo-alignment group and one substituent selected from hydroxyl, carboxyl and amino groups, as described above, the photo-alignment group reacts with light to form a hydrophobic photo-alignment part, and the hydroxyl group and the like form a hydrophilic thermal reaction part.

[0056] In addition, in this invention, a photo-alignment group refers to the functional group of the structural part which performs photodimerization or photoisomerization.

[0057] The structural part that undergoes photodimerization refers to a part that can form a dimer by light irradiation, and as a specific example thereof, cinnamoyl, chalcone, coumarin, anthracene, etc. can be cited. Among these, cinnamoyl having high transparency and photodimerization reactivity in the visible light field is preferred. In addition, the structural part that undergoes photoisomerization refers to a structural part that can be converted into a cis-isomer and a trans-isomer by light irradiation, and as a specific example thereof, a part including an azobenzene structure, a stilbene structure, etc. can be cited. Among these, from the perspective of the height of reactivity, an azobenzene structure is preferred. The compound having a photo-orientation group and a hydroxyl group is, for example, as shown in the following formula.

[0058]

[0059] In the above formulas [A1] to [A5], A 1 With A 2 Each independently represents a hydrogen atom or a methyl group, X 1represents a divalent group bonded to one to three groups selected from an alkylene group having 1 to 18 carbon atoms, a phenylene group, a biphenylene group, or a combination thereof, via one or more bonds selected from a single bond, an ether bond, an ester bond, an amide bond, a carbamate bond, an amino bond, or a combination thereof. 2 represents a hydrogen atom, a halogen atom, a cyano group, an alkyl group having 1 to 18 carbon atoms, a phenyl group, a biphenyl group, or a cyclohexyl group. In this case, the alkyl group having 1 to 18 carbon atoms, the phenyl group, the biphenyl group, and the cyclohexyl group may be bonded to the benzene ring via a covalent bond, an ether bond, an ester bond, an amide bond, or a urea bond. 5 represents a hydroxyl group, a carboxyl group, an amino group or an alkoxysilyl group. X represents a single bond, an oxygen atom or a sulfur atom. 6 X represents a hydroxyl group, a mercapto group, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, a phenyl group, a phenoxy group or a biphenyloxy group. 7 represents a single bond, an alkylene group having 1 to 20 carbon atoms, a divalent group formed by removing two hydrogen atoms from an aromatic ring, or a divalent group formed by removing two hydrogen atoms from an aliphatic ring. Here, the alkylene group having 1 to 20 carbon atoms may be branched or linear.

[0060] It should be noted that among these substituents, phenylene, phenylene, biphenylene, biphenylyl, phenoxy and biphenyloxy groups may also be substituted by one or more substituents that are the same or different and are selected from alkyl groups having 1 to 4 carbon atoms, alkoxy groups having 1 to 4 carbon atoms, halogen atoms, trifluoromethyl groups and cyano groups.

[0061] In the above formula, R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 and R 8 Each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a halogen atom, a trifluoromethyl group or a cyano group.

[0062] Examples of the alkyl group having 1 to 18 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, 1-methyl-n-butyl, 2-methyl-n-butyl, 3-methyl-n-butyl, 1,1-dimethyl-n-propyl, 1,2-dimethyl-n-propyl, 2,2-dimethyl-n-propyl, 1-ethyl-n-propyl, n-hexyl, 1-methyl-n-pentyl, 2-methyl-n-pentyl, 3-methyl-n-pentyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-butyl, 1,2-dimethyl-n-propyl ... 3-Dimethyl-n-butyl, 2,2-dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl, 1-ethyl-2-methyl-n-propyl, n-heptyl, 1-methyl-n-hexyl, 2-methyl-n-hexyl, 3-methyl-n-hexyl, 1,1-dimethyl-n-pentyl, 1,2-dimethyl-n-pentyl, 1,3-dimethyl-n-pentyl, 2,2-dimethyl -n-pentyl, 2,3-dimethyl-n-pentyl, 3,3-dimethyl-n-pentyl, 1-ethyl-n-pentyl, 2-ethyl-n-pentyl, 3-ethyl-n-pentyl, 1-methyl-1-ethyl-n-butyl, 1-methyl-2-ethyl-n-butyl, 1-ethyl-2-methyl-n-butyl, 2-methyl-2-ethyl-n-butyl, 2-ethyl-3-methyl-n-butyl, n-octyl, 1-methyl-n-heptyl, 2-methyl-n-heptyl, 3-methyl-n-heptyl, 1,1-dimethyl-n-hexyl, 1,2-dimethyl-n-hexyl, 1,3-dimethyl-n-hexyl, 2 ,2-dimethyl-n-hexyl, 2,3-dimethyl-n-hexyl, 3,3-dimethyl-n-hexyl, 1-ethyl-n-hexyl, 2-ethyl-n-hexyl, 3-ethyl-n-hexyl, 1-methyl-1-ethyl-n-pentyl, 1-methyl-2-ethyl-n-pentyl, 1-methyl-3-ethyl-n-pentyl, 2-methyl-2-ethyl-n-pentyl, 2-methyl-3-ethyl-n-pentyl, 3-methyl-3-ethyl-n-pentyl, nonyl, n-decyl, n-undecyl, n-dodecyl, n-thirteendecyl, n-tetradecyl, n-pentadecyl, n-hexadecyl, n-heptadecyl and n-octadecyl, etc.

[0063] Examples of the alkylene group having 1 to 18 carbon atoms include divalent groups obtained by removing one hydrogen atom from the alkyl groups listed above.

[0064] Examples of the alkyl group having 1 to 4 carbon atoms include those listed above having corresponding numbers of carbon atoms.

[0065] Examples of the alkoxy group having 1 to 10 carbon atoms, the alkoxy group having 1 to 4 carbon atoms, and the alkylthio group having 1 to 10 carbon atoms include groups obtained by oxylating or thiolating the alkyl groups listed above and having a corresponding number of carbon atoms.

[0066] Examples of the alkylene group having 1 to 20 carbon atoms include divalent groups obtained by removing one hydrogen atom from the above alkyl groups and alkyl groups having 1 to 20 carbon atoms such as n-nonadecanyl and n-eicosyl.

[0067] Specific examples of the compound having a photo-alignment group and a hydroxyl group as the component (A) include, for example,4-(8-hydroxyoctyloxy)cinnamic acid methyl ester, 4-(6-hydroxyhexyloxy)cinnamic acid methyl ester, 4-(4-hydroxybutoxy)cinnamic acid methyl ester, 4-(3-hydroxypropoxy)cinnamic acid methyl ester, 4-(2-hydroxyethoxy)cinnamic acid methyl ester, 4-hydroxymethoxycinnamic acid methyl ester, 4-hydroxycinnamic acid methyl ester, 4-(8-hydroxyoctyloxy)cinnamic acid ethyl ester, 4-(6-hydroxyhexyloxy)cinnamic acid ethyl ester, 4-(4-hydroxybutoxy)cinnamic acid ethyl ester, 4-(3-hydroxypropoxy)cinnamic acid ethyl ester, 4-(2-hydroxyethoxy)cinnamic acid ethyl ester, 4-hydroxymethoxycinnamic acid ethyl ester, 4-hydroxycinnamic acid ethyl ester, 4-(8-hydroxyoctyloxy)cinnamic acid phenyl ester, 4- (6-Hydroxyhexyloxy) phenyl cinnamate, 4-(4-hydroxybutoxy) phenyl cinnamate, 4-(3-hydroxypropoxy) phenyl cinnamate, 4-(2-hydroxyethoxy) phenyl cinnamate, 4-hydroxymethoxy phenyl cinnamate, 4-hydroxy cinnamate, 4-(8-hydroxyoctyloxy) biphenyl cinnamate, 4-(6-hydroxyhexyloxy) biphenyl cinnamate, 4-(4-hydroxybutoxy) biphenyl cinnamate, 4-(3-hydroxypropoxy) biphenyl cinnamate, 4-(2-hydroxyethoxy) biphenyl cinnamate, 4-hydroxymethoxy biphenyl cinnamate, 4-hydroxy biphenyl cinnamate, 8-hydroxyoctyl cinnamate, 6-hydroxyhexyl cinnamate, 4-hydroxybutyl cinnamate, 3-Hydroxypropyl cinnamate, 2-hydroxyethyl cinnamate, hydroxymethyl cinnamate, 4-(8-hydroxyoctyloxy)azobenzene, 4-(6-hydroxyhexyloxy)azobenzene, 4-(4-hydroxybutoxy)azobenzene, 4-(3-hydroxypropoxy)azobenzene, 4-(2-hydroxyethoxy)azobenzene, 4-hydroxymethoxyazobenzene, 4-hydroxyazobenzene, 4-(8-hydroxyoctyloxy)chalcone, 4-(6-hydroxyhexyloxy)chalcone, 4-(4-hydroxybutoxy)chalcone, 4-(3-hydroxypropoxy)chalcone, 4-(2-hydroxyethoxy)chalcone, 4-hydroxymethoxychalcone, 4-hydroxychalcone, 4'-(8-hydroxyoctyloxy)chalcone, 4'-(6-hydroxyhexyloxy)chalcone 、4'-(4-hydroxybutoxy) chalcone, 4'-(3-hydroxypropoxy) chalcone, 4'-(2-hydroxyethoxy) chalcone, 4'-hydroxymethoxy chalcone, 4'-hydroxy chalcone, 7-(8-hydroxyoctyloxy) coumarin, 7-(6-hydroxyhexyloxy) coumarin, 7-(4-hydroxybutoxy) coumarin, 7-(3-hydroxypropoxy) coumarin, 7-(2-hydroxyethoxy) coumarin, 7-hydroxymethoxy coumarin, 7-hydroxycoumarin, 6-hydroxyoctyloxy coumarin, 6-hydroxyhexyloxy coumarin, 6-(4-hydroxybutoxy) coumarin, 6-(3-hydroxypropoxy) coumarin, 6-(2-hydroxyethoxy) coumarin, 6-hydroxymethoxy coumarin, 6-hydroxycoumarin. 、

[0068] Specific examples of the compound having a photo-alignment group and a carboxyl group include cinnamic acid, ferulic acid, 4-nitrocinnamic acid, 4-methoxycinnamic acid, 3,4-dimethoxycinnamic acid, coumarin-3-carboxylic acid, and 4-(dimethylamino)cinnamic acid.

[0069] Specific examples of the compound having a photo-alignment group and an amino group include methyl 4-aminocinnamate, ethyl 4-aminocinnamate, methyl 3-aminocinnamate, and ethyl 3-aminocinnamate.

[0070] (A) The low-molecular-weight photo-alignment component as the component may be exemplified by the above-mentioned specific examples, but is not limited thereto.

[0071] In addition, in the case where the low molecular weight photo-alignment component as component (A) is a compound having a photo-alignment group and a hydroxyl group, as component (A), a compound having two or more photo-alignment groups and / or two or more hydroxyl groups in the molecule can be used. Specifically, as component (A), a compound having one hydroxyl group and two or more photo-alignment groups in the molecule, or a compound having one photo-alignment group and two or more hydroxyl groups in the molecule, or a compound having two or more photo-alignment groups and hydroxyl groups in the molecule, respectively. For example, with respect to a compound having two or more photo-alignment groups and hydroxyl groups in the molecule, respectively, as an example thereof, a compound as shown in the following formula can be exemplified.

[0072]

[0073] By appropriately selecting such a compound, it becomes possible to control and increase the molecular weight of the low molecular weight photo-alignment component of component (A). As a result, as described later, when the low molecular weight photo-alignment component of component (A) and the polymer of component (B) and the polymer of component (C) undergo a thermal reaction, the sublimation of the low molecular weight photo-alignment component of component (A) can be suppressed. In addition, the cured film-forming composition of the present invention can form an alignment member with high photoreaction efficiency as a cured film.

[0074] Moreover, as (A) component compound in the cured film formation composition of this invention, you may be a mixture of several compounds which have a photo-alignment group and 1 type of substituent selected from a hydroxyl group, a carboxyl group, and an amino group.

[0075] <(B) Ingredient>

[0076] The component (B) contained in the cured film-forming composition of the present invention is a polymer obtained by polymerizing a monomer containing at least an N-alkoxymethyl (meth) acrylamide compound. In addition, N-alkoxymethyl (meth) acrylamide means both N-alkoxymethyl-acrylamide and N-alkoxymethyl-methacrylamide.

[0077] Examples of such polymers include polymers obtained by polymerizing N-alkoxymethyl (meth) acrylamide compounds alone or by copolymerizing them with copolymerizable monomers. Examples of such polymers include poly(N-butoxymethyl-acrylamide), poly(N-ethoxymethyl-acrylamide), poly(N-methoxymethyl-acrylamide), copolymers of N-butoxymethyl-acrylamide and styrene, copolymers of N-butoxymethyl-acrylamide and methyl methacrylate, copolymers of N-ethoxymethyl-methacrylamide and benzyl methacrylate, and copolymers of N-butoxymethyl-acrylamide, benzyl methacrylate, and 2-hydroxypropyl methacrylate.

[0078] The method for obtaining the polymer of the component (B) used in the present invention is not particularly limited. For example, it can be obtained by polymerizing the polymer at a temperature of 50 to 110° C. in a solvent in which an N-alkoxymethyl (meth) acrylamide compound and a copolymerizable monomer and a polymerization initiator are coexistent. In this case, the solvent used is not particularly limited as long as it can dissolve the N-alkoxymethyl (meth) acrylamide compound, the copolymerizable monomer and the polymerization initiator added as desired. Specific examples are described in the <Solvent> described later.

[0079] The polymer obtained by the above method is usually in the state of a solution dissolved in a solvent.

[0080] In addition, the solution of the polymer obtained by the above method is put into diethyl ether or water under stirring to precipitate it, and the precipitate that has been generated is filtered and washed, and then dried at room temperature or heated under normal pressure or reduced pressure to obtain a powder of the polymer. Through the above operation, the polymerization initiator and unreacted monomers coexisting with the polymer can be removed, and as a result, a purified powder of the polymer can be obtained. In the case where it cannot be fully purified in one operation, the obtained powder is dissolved in a solvent again, and the above operation can be repeated.

[0081] In the present invention, the polymer of the component (B) may be used in the form of a powder, or may be used in the form of a solution obtained by re-dissolving a purified powder in a solvent described below.

[0082] Furthermore, in the present invention, the component (B) polymer may be a mixture of a plurality of types of polymers.

[0083] In the present invention, when the above-mentioned copolymerizable monomer is used in the production of the component (B) polymer, the amount of the copolymerizable monomer used is preferably 1 mol % to 200 mol %, more preferably 10 mol % to 100 mol %, relative to the total number of moles of the monomers used in the production of the component (B) polymer.

[0084] The weight average molecular weight of the component (B) polymer is 1,000 to 500,000, preferably 2,000 to 200,000, more preferably 3,000 to 150,000, and even more preferably 3,000 to 50,000. The weight average molecular weight is a value obtained by gel permeation chromatography (GPC) using polystyrene as a standard sample.

[0085] These (B) component polymers may be used alone or in combination of two or more.

[0086] <(C) Ingredients>

[0087] (C) Component is a polymer obtained by polymerizing monomers containing at least an N-hydroxyalkyl (meth) acrylamide compound. In addition, N-hydroxyalkyl (meth) acrylamide means both N-hydroxyalkyl acrylamide and N-hydroxyalkyl methacrylamide.

[0088] When the composition of the present invention is formed into a coating film and thermally cured, the N-alkoxymethyl group of the component (B) reacts with the hydroxyl group of the component (C) to form a bond, thereby making the coating film strong and firm and providing solvent resistance.

[0089] Examples of the N-hydroxyalkyl (meth)acrylamide compound include N-(2-hydroxyethyl)acrylamide, N-(2-hydroxyethyl)methacrylamide, N-(2-hydroxypropyl)acrylamide, N-(2-hydroxypropyl)methacrylamide, N-(4-hydroxybutyl)acrylamide, N-(4-hydroxybutyl)methacrylamide, N-(2,3-dihydroxypropyl)acrylamide, and N-(2,3-dihydroxypropyl)methacrylamide.

[0090] In the present invention, when producing the component (C) polymer, a monomer other than the above-mentioned N-hydroxyalkyl (meth)acrylamide compound (hereinafter also referred to as "other monomer") may be copolymerized.

[0091] In the present invention, when other monomers are used to produce the component (C) polymer, the amount of the other monomers used is preferably 30 to 90 mol%, more preferably 30 to 70 mol%, based on the total molar number of the monomers used to produce the component (C) polymer.

[0092] Examples of other monomers include industrially available monomers capable of undergoing radical polymerization.

[0093] Specific examples of other monomers include unsaturated carboxylic acids, acrylate compounds, methacrylate compounds, amide group-containing monomers, maleimide compounds, acrylonitrile, maleic anhydride, styrene compounds, and vinyl compounds.

[0094] Specific examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, and the like.

[0095] Examples of the acrylate compound include methyl acrylate, ethyl acrylate, isopropyl acrylate, benzyl acrylate, naphthyl acrylate, anthracenyl acrylate, anthracenyl methyl acrylate, phenyl acrylate, 2,2,2-trifluoroethyl acrylate, tert-butyl acrylate, cyclohexyl acrylate, isobornyl acrylate, 2-methoxyethyl acrylate, methoxytriethylene glycol acrylate, 2-ethoxyethyl acrylate, tetrahydrofurfuryl acrylate, 3-methoxybutyl acrylate, 2-methyl-2-adamantyl acrylate, Acid ester, 2-propyl-2-adamantyl acrylate, 8-methyl-8-tricyclodecyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, 2,3-dihydroxypropyl acrylate, diethylene glycol monoacrylate, caprolactone 2-(acryloyloxy)ethyl ester, poly(ethylene glycol) ethyl ether acrylate, 5-acryloyloxy-6-hydroxynorbornene-2-carboxylic acid-6-lactone, acryloylethyl isocyanate, and, 8-ethyl-8-tricyclodecyl acrylate, glycidyl acrylate, etc.

[0096] Examples of the methacrylate compound include methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, benzyl methacrylate, naphthyl methacrylate, anthracenyl methacrylate, anthracenyl methyl methacrylate, phenyl methacrylate, 2,2,2-trifluoroethyl methacrylate, tert-butyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, 2-methoxyethyl methacrylate, methoxytriethylene glycol methacrylate, 2-ethoxyethyl methacrylate, tetrahydrofurfuryl methacrylate, 3-methoxybutyl methacrylate, 2-methyl-2-adamantyl methacrylate, acrylate, γ-butyrolactone methacrylate, 2-propyl-2-adamantyl methacrylate, 8-methyl-8-tricyclodecanyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 4-hydroxybutyl methacrylate, 2,3-dihydroxypropyl methacrylate, diethylene glycol monomethacrylate, caprolactone 2-(methacryloyloxy)ethyl ester, poly(ethylene glycol) ethyl ether methacrylate, 5-methacryloyloxy-6-hydroxynorbornene-2-carboxylic acid-6-lactone, methacryloyl ethyl isocyanate, and 8-ethyl-8-tricyclodecanyl methacrylate, glycidyl methacrylate, etc.

[0097] Examples of the amide group-containing monomer include N-vinylpyrrolidone, N-vinylformamide, N-vinylacetamide, N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-propyl(meth)acrylamide, N-butyl(meth)acrylamide, N-isobutyl(meth)acrylamide, N-hexyl(meth)acrylamide, N-octyl(meth)acrylamide, N-(methoxymethyl)(meth)acrylamide, N-(methoxybutyl)(meth)acrylamide, N-(ethoxymethyl)(meth)acrylamide, N-(butoxymethyl)(meth)acrylamide, N-(isobutoxymethyl)(meth)acrylamide, N-(isobutoxyethyl)(meth)acrylamide, N-vinylphthalimide, and N-vinylsuccinimide.

[0098] Examples of the vinyl compound include vinyl ether, methyl vinyl ether, benzyl vinyl ether, vinyl naphthalene, vinyl anthracene, vinyl biphenyl, vinyl carbazole, 2-hydroxyethyl vinyl ether, phenyl vinyl ether, and propyl vinyl ether.

[0099] Examples of the styrene compound include styrene, methylstyrene, chlorostyrene, and bromostyrene.

[0100] Examples of the maleimide compound include maleimide, N-methylmaleimide, N-phenylmaleimide, and N-cyclohexylmaleimide.

[0101] Examples of the acrylonitrile compound include acrylonitrile and the like.

[0102] The method for obtaining the component (C) polymer used in the present invention is not particularly limited, and the N-hydroxyalkyl (meth)acrylamide compound may be used instead of the N-alkoxymethyl (meth)acrylamide compound in the method for producing the component (B) polymer.

[0103] The weight average molecular weight of the component (C) polymer is 1,000 to 500,000, preferably 2,000 to 200,000, more preferably 3,000 to 150,000, and even more preferably 3,000 to 100,000. The weight average molecular weight is a value obtained by gel permeation chromatography (GPC) using polystyrene as a standard sample.

[0104] These (C) component polymers may be used alone or in combination of two or more.

[0105] As the content of the component (B) polymer and the component (C) polymer in the cured film-forming composition of the present invention, the total amount of the component (B) and the component (C) is preferably 100 to 3000 parts by mass, more preferably 200 to 2500 parts by mass, and particularly preferably 300 to 2000 parts by mass, relative to 100 parts by mass of the component (A).

[0106] The mass ratio of the component (B) to the component (C) is preferably 1:99 to 99:1, more preferably 5:95 to 95:5, and particularly preferably 10:90 to 90:10.

[0107] <(D) Ingredient>

[0108] The cured film-forming composition of the present invention may further contain a crosslinking catalyst as a component (D) in addition to the component (A), the component (B) and the component (C).

[0109] As the crosslinking catalyst of the component (D), for example, an acid or a thermal acid generator can be used. The component (D) effectively promotes the thermal curing reaction of the cured film-forming composition of the present invention.

[0110] Examples of the acid include sulfonic acid group-containing compounds, hydrochloric acid or its salts, etc. The thermal acid generator is not particularly limited as long as it is a compound that generates an acid by thermal decomposition during pre-baking or post-baking, that is, a compound that generates an acid by thermal decomposition at a temperature of 80° C. to 250° C.

[0111] Examples of the acid include hydrochloric acid or its salts; sulfonic acids such as methanesulfonic acid, ethanesulfonic acid, propanesulfonic acid, butanesulfonic acid, pentanesulfonic acid, octanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, camphorsulfonic acid, trifluoromethanesulfonic acid, p-hydroxybenzenesulfonic acid, 2-naphthalenesulfonic acid, mesitylenesulfonic acid, p-xylene-2-sulfonic acid, m-xylene-2-sulfonic acid, 4-ethylbenzenesulfonic acid, 1H,1H,2H,2H-perfluorooctanesulfonic acid, perfluoro(2-ethoxyethane)sulfonic acid, pentafluoroethanesulfonic acid, nonafluorobutane-1-sulfonic acid, and dodecylbenzenesulfonic acid, or their hydrates or salts thereof.

[0112] Examples of the compound that generates an acid by heat include bis(toluenesulfonyloxy)ethane, bis(toluenesulfonyloxy)propane, bis(toluenesulfonyloxy)butane, p-nitrobenzyl toluenesulfonate, o-nitrobenzyl toluenesulfonate, 1,2,3-phenylene tris(methyl sulfonate), pyridinium p-toluenesulfonate, Salt, Morpholine p-toluenesulfonate salts, ethyl p-toluenesulfonate, propyl p-toluenesulfonate, butyl p-toluenesulfonate, isobutyl p-toluenesulfonate, methyl p-toluenesulfonate, phenethyl p-toluenesulfonate, cyanomethyl p-toluenesulfonate, 2,2,2-trifluoroethyl p-toluenesulfonate, 2-hydroxybutyl p-toluenesulfonate, N-ethyl-p-toluenesulfonamide, and compounds represented by the following formulas, etc.

[0113]

[0114]

[0115] The content of the component (D) in the cured film-forming composition of the present invention is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 6 parts by mass, and further preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of the total amount of the component (B) polymer and the component (C) polymer. By setting the content of the component (D) to 0.01 parts by mass or more, sufficient thermosetting properties and solvent resistance can be imparted, and high sensitivity to light irradiation can also be imparted. However, when the content exceeds 10 parts by mass, the storage stability of the composition is reduced.

[0116] <(E) Ingredient>

[0117] The cured film-forming composition of the present invention may contain a component for improving the adhesion of the cured film to be formed (hereinafter, also referred to as an adhesion-improving component) as the component (E).

[0118] The adhesion improving component as component (E) can link the polymerizable functional group of the polymerizable liquid crystal and the crosslinking reaction site of the orientation member through a covalent bond, thereby improving the adhesion of the orientation member obtained from the cured film forming composition of the present invention and the layer of the polymerizable liquid crystal. As a result, the phase difference member of the present embodiment, which is formed by laminating the cured polymerizable liquid crystal on the orientation member of the present embodiment, can maintain strong adhesion even under high temperature and high humidity conditions, and can show high durability against peeling, etc.

[0119] As the component (E), a monomer or polymer having a group selected from a hydroxyl group and an N-alkoxymethyl group and a polymerizable group is preferred.

[0120] Examples of such component (E) include compounds having a hydroxyl group and a (meth)acryloyl group, compounds having an N-alkoxymethyl group and a (meth)acryloyl group, and polymers having an N-alkoxymethyl group and a (meth)acryloyl group. Specific examples of each are shown below.

[0121] (E) As an example of a component, a polyfunctional acrylate containing a hydroxyl group (hereinafter, also referred to as a hydroxyl-containing polyfunctional acrylate) is mentioned.

[0122] (E) As an example of the hydroxyl group-containing multifunctional acrylate of the component, pentaerythritol triacrylate, dipentaerythritol pentaacrylate, etc. are mentioned, for example.

[0123] (E) As an example of a component, a compound which has one (meth)acryloyl group and one or more hydroxyl groups can also be mentioned.

[0124] Examples of the compound of the component (E) include compounds having at least one polymerizable group containing a C═C double bond and at least one N-alkoxymethyl group in one molecule.

[0125] Examples of the polymerizable group containing a C═C double bond include an acryloyl group, a methacryloyl group, a vinyl group, an allyl group, and a maleimido group.

[0126] Preferred examples of the compound having at least one polymerizable group containing a C═C double bond and at least one N-alkoxymethyl group in one molecule include compounds represented by the following formula (X1).

[0127]

[0128] (Where R 31 represents a hydrogen atom or a methyl group, R 32 represents a hydrogen atom, or a linear or branched alkyl group having 1 to 10 carbon atoms).

[0129] Examples of the alkyl group having 1 to 10 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, 1-methyl-n-butyl, 2-methyl-n-butyl, 3-methyl-n-butyl, 1,1-dimethyl-n-propyl, 1,2-dimethyl-n-propyl, 2,2-dimethyl-n-propyl, 1-ethyl-n-propyl, n-hexyl, 1-methyl-n-pentyl, 2-methyl-n-pentyl, 3-methyl-n-pentyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-propyl, 2,2-dimethyl-n-propyl, 1-ethyl-n-propyl, n-hexyl, 1-methyl-n-pentyl, 2-methyl-n-pentyl, 3-methyl-n-pentyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2- Dimethyl-n-butyl, 1,3-dimethyl-n-butyl, 2,2-dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl, 1-ethyl-2-methyl-n-propyl, n-heptyl, 1-methyl-n-hexyl, 2-methyl-n-hexyl, 3-methyl-n-hexyl, 1,1-dimethyl-n-pentyl, 1,2-dimethyl-n-pentyl , 1,3-dimethyl-n-pentyl, 2,2-dimethyl-n-pentyl, 2,3-dimethyl-n-pentyl, 3,3-dimethyl-n-pentyl, 1-ethyl-n-pentyl, 2-ethyl-n-pentyl, 3-ethyl-n-pentyl, 1-methyl-1-ethyl-n-butyl, 1-methyl-2-ethyl-n-butyl, 1-ethyl-2-methyl-n-butyl, 2-methyl-2-ethyl-n-butyl, 2-ethyl-3-methyl-n-butyl, n-octyl, 1-methyl-n-heptyl, 2-methyl-n-heptyl, 3-methyl-n-heptyl, 1,1-dimethyl -n-hexyl, 1,2-dimethyl-n-hexyl, 1,3-dimethyl-n-hexyl, 2,2-dimethyl-n-hexyl, 2,3-dimethyl-n-hexyl, 3,3-dimethyl-n-hexyl, 1-ethyl-n-hexyl, 2-ethyl-n-hexyl, 3-ethyl-n-hexyl, 1-methyl-1-ethyl-n-pentyl, 1-methyl-2-ethyl-n-pentyl, 1-methyl-3-ethyl-n-pentyl, 2-methyl-2-ethyl-n-pentyl, 2-methyl-3-ethyl-n-pentyl, 3-methyl-3-ethyl-n-pentyl, n-nonyl, n-decyl, etc.

[0130] Specific examples of the compound represented by the above formula (X1) include acrylamide compounds or methacrylamide compounds substituted with hydroxymethyl or alkoxymethyl groups, such as N-hydroxymethyl (meth) acrylamide, N-methoxymethyl (meth) acrylamide, N-ethoxymethyl (meth) acrylamide, and N-butoxymethyl (meth) acrylamide. It should be noted that (meth) acrylamide refers to both methacrylamide and acrylamide.

[0131] As another embodiment of the compound having a polymerizable group containing a C═C double bond and an N-alkoxymethyl group as the component (E), the following compounds are more preferably mentioned.

[0132]

[0133] The content of the component (E) in the cured film-forming composition of the present invention is preferably 1 to 100 parts by mass, more preferably 5 to 70 parts by mass, relative to 100 parts by mass of the low-molecular photo-alignment component as the component (A).

[0134] <Solvent>

[0135] The cured film-forming composition of the present invention is mainly used in a solution state dissolved in a solvent. The solvent used in this case is not particularly limited in type and structure as long as it can dissolve the components (A), (B) and (C), and the components (D) and (E) added as necessary and / or other additives described later.

[0136] Specific examples of the solvent include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol propyl ether acetate, toluene, xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-butanone, 3-methyl-2-pentanone, 2-pentanone, 2-heptanone, γ-butyrolactone, 2- Ethyl hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl ethoxylate, ethyl hydroxylate, methyl 2-hydroxy-3-methylbutyrate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone. These solvents may be used alone or in combination of two or more.

[0137] <Other additives>

[0138] Furthermore, the cured film-forming composition of the present invention may contain a sensitizer, a silane coupling agent, a surfactant, a rheology adjuster, a pigment, a dye, a storage stabilizer, a defoamer, an antioxidant, and the like as necessary, unless the effects of the present invention are impaired.

[0139] For example, the sensitizer effectively promotes photoreaction after forming a thermally cured film using the cured film-forming composition of the present invention.

[0140] As an example of other additives, sensitizers include benzophenone, anthracene, anthraquinone, thioxanthone, and derivatives thereof, as well as nitrophenyl compounds. Among these, benzophenone derivatives and nitrophenyl compounds are preferred. As specific examples of more preferred compounds, N, N-diethylaminobenzophenone, 2-nitrofluorene, 2-nitrofluorenone, 5-nitroacenaphthene, 4-nitrobiphenyl, 4-nitrocinnamic acid, 4-nitrostilbene, 4-nitrobenzophenone, 5-nitroindole, and the like can be cited. In particular, N, N-diethylaminobenzophenone, a derivative of benzophenone, is preferred.

[0141] These sensitizers are not limited to the above. In addition, the sensitizer can be used alone or in combination of two or more compounds.

[0142] The usage ratio of the sensitizer in the cured film-forming composition of the present invention is preferably 0.1 to 20 parts by mass, and more preferably 0.2 to 10 parts by mass, relative to 100 parts by mass of the low molecular weight photo-alignment component as component (A). If the ratio is too small, the effect as a sensitizer may not be fully obtained, and if it is too large, the transmittance may be increased and the coating may be roughened.

[0143] <Preparation of Cured Film-Forming Composition>

[0144] The cured film-forming composition of the present embodiment contains a low molecular weight photo-alignment component as component (A), a polymer obtained by polymerizing a monomer containing at least an N-alkoxymethyl (meth) acrylamide compound as component (B), and a polymer obtained by polymerizing a monomer containing at least an N-hydroxyalkyl (meth) acrylamide compound as component (C). In addition, a crosslinking catalyst as component (D), an adhesion-enhancing component as component (E), and / or other additives may be contained as needed.

[0145] The blending ratio, preparation method, and the like when the cured film-forming composition of the present invention is used as a solution will be described in detail below.

[0146] The ratio of the solid content in the cured film-forming composition of the present invention is not particularly limited as long as each component is uniformly dissolved in the solvent, and is 1% to 80% by mass, preferably 3% to 60% by mass, and more preferably 5% to 40% by mass. Here, the solid content refers to the components after removing the solvent from all the components of the cured film-forming composition.

[0147] The method for preparing the cured film-forming composition of the present invention is not particularly limited. Examples of the preparation method include a method in which a solution of component (B) dissolved in a solvent is mixed with component (A), component (C), and component (D) and component (E) added as required in a specified ratio to form a uniform solution, or a method in which other additives are further added and mixed as required at an appropriate stage of the preparation method.

[0148] In the preparation of the composition for forming a cured film of the present invention, a polymer solution obtained by a polymerization reaction in a solvent can be directly used. In this case, for example, a solution of component (C) is added with component (A), component (B), and component (D) and component (E) added as needed to form a uniform solution. At this time, additional solvent may be added for the purpose of adjusting the concentration. In this case, the solvent used in the production process of component (C) and the solvent used for adjusting the concentration of the composition for forming a cured film may be the same or different.

[0149] In addition, it is preferable to use after filtering the prepared solution of the cured film-forming composition using a filter having a pore size of about 0.2 μm or the like.

[0150] <Cured film, orientation member, and phase difference member>

[0151] The solution of the cured film-forming composition of the present invention can be applied to a substrate (e.g., a silicon / silicon dioxide coated substrate, a silicon nitride substrate, a substrate coated with a metal such as aluminum, molybdenum, chromium, etc., a glass substrate, a quartz substrate, an ITO substrate, etc.) or a film (e.g., a resin film such as a triacetyl cellulose (TAC) film, a cycloolefin polymer film, a polyethylene terephthalate film, an acrylic film, etc.), and the coating can be formed by a bar coating method, a spin coating method, a cast coating method, a roll coating method, a slit coating method, a slit coating method followed by a spin coating method, an inkjet coating method, a printing method, etc., and then, the cured film can be formed by heating and drying using a hot plate or an oven, etc.

[0152] As the conditions for heating and drying, the components of the orientation member formed by the cured film will not precipitate to the extent of the polymerizable liquid crystal solution coated thereon, and the cross-linking reaction using the cross-linking agent will proceed. For example, the heating temperature and heating time can be appropriately selected from the range of 60°C to 200°C and the time of 0.4 minutes to 60 minutes. The heating temperature and heating time are preferably 70°C to 160°C and 0.5 minutes to 10 minutes.

[0153] The film thickness of the cured film formed using the cured film-forming composition of the present invention is, for example, 0.05 μm to 5 μm, and can be appropriately selected in consideration of the height difference of the substrate used and the optical and electrical properties.

[0154] The cured film thus formed can function as an alignment member, that is, a member for orienting a compound having liquid crystal properties such as liquid crystal, by being irradiated with polarized UV light.

[0155] The polarized UV irradiation method is generally performed by using ultraviolet light or visible light with a wavelength of 150 nm to 450 nm, and irradiating linearly polarized light from a vertical or oblique direction at room temperature or in a heated state.

[0156] Since the orientation member formed by the cured film-forming composition of the present invention has solvent resistance and heat resistance, after the phase difference material containing the polymerizable liquid crystal solution is applied to the orientation member, the phase difference material is formed into a liquid crystal state by heating to the phase transition temperature of the liquid crystal, and is oriented on the orientation member. In addition, by directly curing the phase difference material in the oriented state, the phase difference member can be formed as a layer having optical anisotropy.

[0157] As the phase difference material, for example, a liquid crystal monomer having a polymerizable group and a composition containing the same can be used. In addition, when the substrate forming the orientation member is a film, the film having the phase difference member of the present invention can be used as a phase difference film. The phase difference material forming such a phase difference member becomes a liquid crystal state, and there are orientation states such as horizontal orientation, cholesterol orientation, vertical orientation, and mixed orientation on the orientation member, and it can be used differently according to the required phase difference.

[0158] In addition, in the case of manufacturing a patterned phase difference component used in a 3D display, on a cured film formed by the composition for forming a cured film of the present invention and the above method, a mask of a line width and line spacing pattern is separated, based on a specified reference, for example, in the direction of +45 degrees, polarized light UV is exposed, and then the mask is removed, and then, polarized light UV is exposed in the direction of -45 degrees, and an orientation component is obtained in which two liquid crystal orientation regions with different orientation control directions of liquid crystals are formed. Thereafter, after applying a phase difference material containing a polymerizable liquid crystal solution, the phase difference material is formed into a liquid crystal state by heating to the phase transition temperature of the liquid crystal, and oriented on the orientation component. In addition, the phase difference material that has become an oriented state can be directly cured, and a patterned phase difference component in which two phase difference regions with different phase difference characteristics are respectively regularly arranged is obtained.

[0159] In addition, two substrates having the orientation components of the present invention formed by the above operation can be used, and after being bonded together with a spacer in between so that the orientation components on the two substrates face each other, liquid crystal can be injected between these substrates to form a liquid crystal display component with oriented liquid crystal.

[0160] Therefore, the cured film-forming composition of the present invention can be suitably used for producing various phase difference members (phase difference films) or liquid crystal display elements.

[0161] Example

[0162] Hereinafter, the present invention will be described in detail with reference to Examples of the present invention, but the present invention is not to be construed as being limited thereto.

[0163] [Omission Symbols Used in Examples]

[0164] The meanings of the abbreviation symbols used in the following examples are as follows.

[0165] <Raw materials>

[0166] BMAA: N-Butoxymethyl-acrylamide

[0167] AIBN: α,α'-azobisisobutyronitrile

[0168] MMA: Methyl Methacrylate

[0169] HEAA: N-(2-hydroxyethyl)acrylamide

[0170] MAIB: dimethyl 2,2-azodiisobutyrate

[0171] <Component A>

[0172] MCA: 4-Methoxycinnamic acid

[0173]

[0174] <Ingredient B>

[0175] PB-1: The structural formula is shown below.

[0176]

[0177] <Ingredient C>

[0178] PC-1: The structural formula is shown below.

[0179]

[0180] PC-2: The structural formula is shown below.

[0181]

[0182] <Ingredient D>

[0183] PTSA: p-Toluenesulfonic acid monohydrate

[0184] <Ingredient E>

[0185] E-1: A compound having an N-alkoxymethyl group and an acryloyl group represented by the following structural formula

[0186]

[0187] <Solvent>

[0188] Each resin composition of the examples and comparative examples contained a solvent, and propylene glycol monomethyl ether (PM) and butyl acetate (BA) were used as the solvent.

[0189] <Measurement of polymer molecular weight>

[0190] The molecular weight of the acrylic copolymer in the polymerization example was measured by the following operation using a gel permeation chromatography (GPC) apparatus (HLC-8320) manufactured by Tosoh Corporation and columns (TSKgel ALPHA4000 and TSKgel ALPHA3000) manufactured by Tosoh Corporation.

[0191] In addition, the number average molecular weight (hereinafter referred to as Mn) and the weight average molecular weight (hereinafter referred to as Mw) described below are expressed as polystyrene-equivalent values.

[0192] Column temperature: 40℃

[0193] Eluent: Tetrahydrofuran

[0194] Flow rate: 1.0mL / min

[0195] Standard samples for making standard lines: Standard polystyrene manufactured by Tosoh Corporation (molecular weight 427,000, 190,000, 37,900, 18,100, 5,970, 2,420, 1,010)

[0196] <Synthesis of component B>

[0197] <Polymerization Example-1>

[0198] An acrylic polymer solution was obtained by dissolving 100.0 g of BMAA and 1.0 g of a polymerization catalyst AIBN in 193.5 g of PM and reacting them at 80° C. for 20 hours. The obtained acrylic polymer had an Mn of 10,000 and an Mw of 23,000. The acrylic polymer solution was slowly dropped into 2000.0 g of hexane to precipitate a solid, which was filtered and dried under reduced pressure to obtain a polymer (PB-1).

[0199] <Synthesis of component C>

[0200] <Polymerization Example-2>

[0201] 7.0 g of MMA, 5.8 g of HEAA, and 0.23 g of polymerization catalyst MAIB were dissolved in 13.0 g of PM. 6.50 g of PM was added to a four-necked flask in advance and the dissolved solution was dripped into a dripping tank preheated to 85° C. over 3 hours, and the acrylic polymer solution was obtained by reacting it under reflux for 3 hours. The Mn of the obtained acrylic polymer was 12,600 and the Mw was 43,100. The target polymer (PC-1) 40% PM solution was obtained.

[0202] <Synthesis of component C>

[0203] <Polymerization Example-3>

[0204] 47.10 g of BMAA, 34.5 g of HEAA, and 0.829 g of polymerization catalyst MAIB were dissolved in 82.50 g of PM. 41.25 g of PM was added to a four-necked flask in advance and the dissolved solution was dripped into a drip tank preheated to 85°C for 3 hours. After the dripping, the acrylic polymer solution was obtained by reacting it for 5 hours. The Mn of the obtained acrylic polymer was 6,500 and the Mw was 17,000. The target polymer (PC-2) 40% PM solution was obtained.

[0205] <Preparation of Liquid Crystal Alignment Agent (Cured Film Forming Composition)>

[0206] <Preparation Example 1>

[0207] MCA 0.079g as component (A), PB-1 0.66g obtained in polymerization example-1 as component (B), 40% PM solution 0.26g of polymer (PC-1) obtained in polymerization example-2 as component (C), E-1 0.056g (94.6% BA solution manufactured by Junsei Chemical Co., Ltd.) as component (E), PTSA 0.021g as component (D), and PM 6.65g and BA 1.62g as solvents were added to the mixture and stirred for 1 hour, and the solution was obtained by visually confirming that the mixture was dissolved. Next, the obtained solution was filtered using a filter having a pore size of 0.2μm to prepare a liquid crystal aligning agent (A-1).

[0208] <Preparation Examples 2 to 6>

[0209] Except having used each component of the kind and the blending amount shown in the following Table 1, it carried out similarly to Preparation Example 1, and prepared each liquid crystal aligning agent (A-2) - (A-4), (B-1), (B-2).

[0210]

[0211] APEPO-1: RFK-505 (manufactured by Kawasaki Chemical Industries, Ltd.)

[0212] PEPO-1: Polylite 8651 (manufactured by DIC Co., Ltd.)

[0213] <Preparation of polymerizable liquid crystal solution for horizontal alignment>

[0214] <Preparation example 1>

[0215] 1.57 g of polymerizable liquid crystal LC-242 for horizontal alignment (manufactured by BASF), 0.047 g of photoradical initiator Irgacure 907 (manufactured by BASF), and 0.008 g of leveling agent BYK-361N were added, and then 6.55 g of N-methylpyrrolidone (NMP) and 9.83 g of cyclopentanone were added as solvents. The mixture was stirred for 2 hours and dissolved by visual confirmation to obtain a 9% by mass polymerizable liquid crystal solution LC-1.

[0216] <Formation of liquid crystal alignment film and preparation of retardation film>

[0217] <Example 1>

[0218] On a triacetyl cellulose (TAC) film as a substrate, the liquid crystal aligning agent (A-1) prepared in Preparation Example 1 was applied to a wet film thickness of 6 μm using a bar coater. Heat drying was performed at 130°C for 2 minutes in a thermal cycle oven to form a cured film on the film. Next, a 10 mJ / cm 2 The surface of the cured film was irradiated with 313 nm linear polarized light vertically at an exposure amount of 1000 nm to form a liquid crystal alignment film. On the above liquid crystal alignment film, a polymerizable liquid crystal solution LC-1 for horizontal alignment was applied to a wet film thickness of 34 μm using a bar coater. Next, after heating and drying at 120°C for 2 minutes in an oven, the film was heated at 300 mJ / cm 2 The phase difference film is produced by vertically irradiating 365nm non-polarized light with an exposure amount of to cure the polymerizable liquid crystal.

[0219] <Examples 2 to 4>

[0220] A retardation film was produced by the same operation as in Example 1 using (A-2) to (A-4) as a liquid crystal aligning agent.

[0221] <Comparative Example 1>

[0222] On the TAC film as the substrate, the liquid crystal aligning agent (B-1) prepared in Preparation Example 1 was applied to a wet film thickness of 4 μm using a bar coater. The film was heated and dried at 130°C for 2 minutes in a heat circulation oven to form a cured film on the film. Next, the film was heated and dried at 10 mJ / cm 2The surface of the cured film was irradiated with linear polarized light of 313 nm vertically with an exposure amount of 1.5 % to form a liquid crystal alignment film. On the above liquid crystal alignment film, a polymerizable liquid crystal solution LC-1 for horizontal alignment was applied to a wet film thickness of 34 μm using a bar coater. Next, after heating and drying at 120°C for 2 minutes in an oven, the film was heated at 300 mJ / cm 2 The polymerizable liquid crystal was cured by vertically irradiating non-polarized light of 365 nm with an exposure amount of 100 nm to produce a phase difference film.

[0223] <Comparative Example 2>

[0224] (B-1) was used as a liquid crystal aligning agent, and a retardation film was produced in the same manner as in Comparative Example 1.

[0225] The retardation films prepared above were evaluated by the following methods. Table 2 shows the evaluation results.

[0226] <Evaluation of Orientation>

[0227] The phase difference film on the produced substrate was sandwiched between a pair of polarizing plates, and the phase difference characteristics were visually observed under crossed Nicol prisms. The film that showed no phase difference was rated as ○, and the film that did not show phase difference was rated as ×, and recorded in the "Orientation" column.

[0228] <TAC protection>

[0229] The produced retardation film including the TAC film was rated as ○ if it was not curled, and was rated as × if it was curled, and the result was recorded in the column of "protective property".

[0230] Table 2

[0231]

[0232] As is clear from the results in Table 2, by using a polymer obtained by polymerizing a monomer containing an N-hydroxyalkyl (meth)acrylamide compound as the component (C), it is possible to obtain alignment with a liquid crystal solution containing NMP and prevent damage to the TAC film by NMP.

[0233] Industrial Applicability

[0234] The composition for forming a cured film of the present invention is very useful as a liquid crystal alignment film of a liquid crystal display component or an alignment member for forming an optical anisotropic film provided inside or outside a liquid crystal display component, and is particularly suitable as a material for forming a patterned phase difference member of a 3D display. In addition, it is suitable as a material for forming a cured film such as a protective film, a planarization film, and an insulating film in various displays such as a thin film transistor (TFT) type liquid crystal display component or an organic EL component, and is particularly suitable as a material for forming an interlayer insulating film of a TFT type liquid crystal component, a protective film of a color filter, or an insulating film of an organic EL component.

Claims

1. A cured film-forming composition, characterized in that: Containing component (A), component (B), component (C) and component (E), The component (A) is a compound having a photo-alignment group and one substituent selected from a hydroxyl group, a carboxyl group and an amino group, The component (B) is a polymer obtained by polymerizing a monomer containing at least an N-alkoxymethyl (meth)acrylamide compound. The component (C) is a polymer obtained by polymerizing a monomer containing at least an N-hydroxyalkyl (meth)acrylamide compound. The component (E) is a compound having at least one polymerizable group containing a C=C double bond and at least one N-alkoxymethyl group in one molecule, wherein the polymerizable group containing a C=C double bond is selected from an acryloyl group, a methacryloyl group, a vinyl group, an allyl group and a maleimido group. 2 . The cured film-forming composition according to claim 1 , wherein the photo-alignment group of the component (A) is a functional group having a structure that undergoes photodimerization or photoisomerization. The cured film-forming composition according to claim 1 or 2, wherein the photo-alignment group of the component (A) is a cinnamoyl group. The cured film-forming composition according to claim 1 or 2, wherein the photo-alignment group of the component (A) is a group of an azobenzene structure. The cured film-forming composition according to claim 1 or 2, further comprising a crosslinking catalyst as component (D). The cured film-forming composition according to claim 1 or 2, wherein the total amount of the component (B) and the component (C) is 100 to 3000 parts by mass based on 100 parts by mass of the component (A). 7 . The cured film-forming composition according to claim 1 , wherein a mass ratio of the component (B) to the component (C) is 1:99 to 99:

1. 8 . The cured film-forming composition according to claim 5 , comprising 0.01 to 10 parts by mass of the component (D) based on 100 parts by mass of the total amount of the component (B) and the component (C).

9. An orientation member, characterized in that: The cured film-forming composition according to any one of claims 1 to 8 is used.

10. A phase difference component, characterized in that: The cured film is formed using the cured film obtained from the cured film-forming composition according to any one of claims 1 to 8.