Method for producing positive electrode active material for lithium ion secondary battery
By adding titanium and niobium to lithium-nickel-manganese composite oxide and processing it under specific conditions, the problem of insufficient thermal stability of lithium-ion secondary batteries is solved, and efficient thermal stability and battery capacity improvement are achieved, which is suitable for many applications. kind of electronic equipment.
Patent Information
- Application Number
- CN202080049773.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-05-27
- Filing Date
- 2020-06-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-06-30
AI Technical Summary
Lithium-nickel-manganese composite oxides with high nickel ratios in existing lithium-ion secondary batteries have deficiencies in thermal stability, and the high cost of niobium limits its widespread application, and existing technology cannot effectively combine niobium and titanium as dissimilar elements. to improve thermal stability and battery capacity.
Using a mixture preparation process and a firing process, titanium and niobium are added to the lithium nickel manganese composite oxide and fired under specific temperature and oxygen concentration conditions to form a lithium nickel manganese composite oxide with a hexagonal crystal layered structure. , combined with water washing and drying processes to improve volume resistivity and discharge capacity.
It achieves significant improvement in thermal stability and battery capacity of lithium-ion secondary batteries at low cost, and is suitable for industrial-scale production and suitable for applications such as small portable electronic devices and electric vehicles.
Smart Images

Figure CN114096486B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a positive electrode active material for a lithium ion secondary battery. Background Art
[0002] In recent years, with the popularity of portable electronic devices such as mobile phones and notebook personal computers, there is a strong desire to develop small and lightweight non-aqueous electrolyte secondary batteries with high energy density and durability. In addition, as batteries for power tools and electric vehicles represented by hybrid vehicles, there is a strong desire to develop high-output secondary batteries.
[0003] As secondary batteries that meet such requirements, there are non-aqueous electrolyte secondary batteries such as lithium ion secondary batteries. Lithium ion secondary batteries using lithium metal composite oxides with layered or spinel crystal structures as positive electrode active materials can obtain high voltages of 4V, and are therefore being promoted for practical use as batteries with high energy density.
[0004] As a lithium metal composite oxide, lithium cobalt composite oxide (LiCoO) which is relatively easy to synthesize has been proposed. 2 ), using lithium nickel composite oxide (LiNiO 2 ), lithium nickel cobalt manganese composite oxide (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 ), lithium manganese composite oxide (LiMn 2 O 4 ), lithium nickel manganese composite oxide (LiNi 0.5 Mn 0.5 O 2 )wait.
[0005] In addition, when a lithium ion secondary battery uses a non-aqueous electrolyte as a battery material, high thermal stability is required. For example, when a short circuit occurs inside the lithium ion secondary battery, heat is generated due to a rapid current, so higher thermal stability is required.
[0006] Therefore, attention has been paid to lithium nickel cobalt manganese composite oxides and lithium nickel manganese composite oxides having excellent thermal stability. Lithium nickel cobalt manganese composite oxides are layered compounds like lithium cobalt composite oxides and lithium nickel composite oxides, and materials having a composition ratio of 1:1:1 of nickel, cobalt and manganese at transition metal sites are called ternary positive electrode active materials.
[0007] In particular, in recent years, attention has been paid to ternary positive electrode active materials with the goal of high capacity, and positive electrode active materials with high nickel ratios (Hi-Ni positive electrode materials) that increase the nickel ratio of lithium nickel manganese composite oxides. However, the increase in battery capacity and the decrease in thermal stability caused by the nickel ratio are trade-offs, so positive electrode active materials with high performance (high cycle characteristics, high capacity, high output) as lithium ion secondary batteries and short circuit resistance and thermal stability are required.
[0008] In order to improve thermal stability, some technologies for adding niobium to lithium metal composite oxides have been proposed. For example, Patent Document 1 proposes a positive electrode active material for a non-aqueous secondary battery, which comprises a general formula: Li a Ni 1-x-y-z Co x M y Nb z O b (wherein M is one or more elements selected from the group consisting of Mn, Fe and Al, 1≤a≤1.1, 0.1≤x≤0.3, 0≤y≤0.1, 0.01≤z≤0.05, 2≤b≤2.2) A composition consisting of at least one compound containing lithium, nickel, cobalt, element M, niobium and oxygen. According to Patent Document 1, since the Li-Nb-O series compound present near the surface or inside the particle has high thermal stability, a positive electrode active material with high thermal stability and large discharge capacity can be obtained.
[0009] In addition, Patent Document 2 proposes a positive electrode active material for a non-aqueous electrolyte secondary battery, which comprises a general formula (1): Li d Ni 1-a-b-c Mn a M b Nb c O 2+γ (In the above general formula (1), M is at least one element selected from Co, W, Mo, V, Mg, Ca, Al, Ti, Cr, Zr and Ta, 0.05≤a≤0.60, 0≤b≤0.60, 0.0003≤c≤0.03, 0.95≤d≤1.20, 0≤γ≤0.5.) A lithium nickel manganese composite oxide represented by, at least a portion of niobium in the lithium nickel manganese composite oxide is solid dissolved in the primary particles. According to Patent Document 2, a non-aqueous secondary battery having both high energy density and excellent output characteristics and thermal stability during short circuit due to reduced conductivity can be obtained.
[0010] Prior art literature
[0011] Patent Literature
[0012] Patent Document 1: Japanese Patent Application Publication No. 2002-151071
[0013] Patent Document 2: International Publication No. 2018 / 043669
[0014] Patent Document 3: Japanese Patent Application Publication No. 2008-017729
[0015] Patent Document 4: Japanese Patent No. 4807467
[0016] Patent Document 5: Japanese Patent Application Publication No. 2006-147499
[0017] Patent Document 6: Japanese Patent Application Publication No. 2007-265784
[0018] Patent Document 7: Japanese Patent Application Publication No. 2008-257902 Summary of the invention
[0019] Problems to be solved by the invention
[0020] Although the above-mentioned Patent Documents 1 and 2 state that the positive electrode active material described therein improves thermal stability by including niobium in a specific form, it is required to further improve the thermal stability of lithium nickel manganese composite oxides having a high nickel ratio. In addition, since niobium is expensive, a method for manufacturing a positive electrode active material that can achieve high thermal stability at a lower cost is required.
[0021] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for easily producing a positive electrode active material containing a lithium nickel manganese composite oxide having a high nickel ratio and achieving higher thermal stability at low cost in industrial-scale production.
[0022] In order to obtain a positive electrode active material with high battery characteristics, for example, some technologies of adding titanium to lithium metal composite oxides have been proposed. According to Patent Documents 3 to 7, positive electrode active materials containing lithium nickel cobalt titanium composite oxides have good thermal stability and high battery capacity.
[0023] In addition, when a short circuit occurs inside a lithium-ion secondary battery, as one of the methods to suppress the rapid current caused by the short circuit, for example, as described in the above-mentioned patent document 2, it is believed that reducing the conductivity of the positive electrode active material in a compressed state in the positive electrode, or increasing the volume resistivity is effective.
[0024] However, the above-mentioned Patent Documents 1 to 7 do not describe the effect of combining niobium and titanium as heterogeneous elements in the lithium nickel manganese composite oxide. In addition, the above-mentioned Patent Documents 1 and 3 to 7 do not describe the conductivity or volume resistivity of the positive electrode active material in a compressed state in the positive electrode.
[0025] Methods for solving problems
[0026] In a first aspect of the present invention, a method for producing a positive electrode active material for a lithium ion secondary battery is provided, the method comprising a mixture preparation step and a calcining step, wherein the positive electrode active material for a lithium ion secondary battery comprises a lithium nickel manganese composite oxide having a layered structure of a hexagonal system and composed of secondary particles formed by agglomeration of a plurality of primary particles, wherein in the mixture preparation step, a mixture comprising at least a nickel manganese composite compound and a lithium compound and optionally comprising one or both of a titanium compound and a niobium compound is prepared, and in the calcining step, the mixture is calcined at a temperature of not less than 750° C. and not more than 1000° C. to obtain a lithium nickel manganese composite oxide, wherein the nickel manganese composite compound comprises nickel (Ni) and manganese (Mn), and optionally comprises a metal selected from Co, V, Mg, Mo, Ca, Cr, Ta, Na, W, At least one element selected from the group consisting of nickel, manganese, element M, titanium (Ti) and niobium (Nb), the mass ratio of each element being represented by Ni:Mn:M:Ti:Nb=(1-xy):x:y:z':w' (wherein 0.03≤x≤0.30, 0≤y≤0.30, 0≤z'≤0.05, 0≤w'≤0.03), and in the mixture, the mass ratio (z) of titanium and the mass ratio (w) of niobium relative to the total mass of nickel, manganese, element M, titanium and niobium satisfy 0.005≤z≤0.05, 0.001<w≤0.03, (z+w)≤0.06 and z>w, and at least a portion of niobium in the lithium nickel manganese composite oxide is segregated at the grain boundaries between primary particles.
[0027] In a second aspect of the present invention, a method for producing a positive electrode active material for a lithium ion secondary battery is provided, which comprises a mixture preparation step and a calcination step, wherein the positive electrode active material for a lithium ion secondary battery comprises a lithium nickel manganese composite oxide having a layered structure of a hexagonal system and composed of secondary particles formed by agglomeration of a plurality of primary particles, wherein in the mixture preparation step, at least a nickel manganese composite compound, a titanium compound, a niobium compound and a lithium compound are mixed to prepare a mixture, and in the calcination step, the mixture is calcined at a temperature of not less than 750° C. and not more than 1000° C. to obtain a lithium nickel manganese composite oxide, wherein the nickel manganese composite compound comprises nickel (Ni) and manganese (Mn), and optionally comprises a metal selected from Co, V, At least one element among Mg, Mo, Ca, Cr, Ta, Na, W, Fe, Zn, B, Si, P, Zr and Al, namely element M (M), the mass ratio of each element is represented by Ni:Mn:M=(1-xy):x:y (wherein, 0.03≤x≤0.30, 0≤y≤0.30), in the mixture, the mass ratio of titanium (z) and the mass ratio of niobium (w) relative to the total mass of nickel, manganese, element M, titanium and niobium satisfy 0.005≤z≤0.05, 0.001<w≤0.03, (z+w)≤0.06 and z>w, and at least a part of niobium in the lithium nickel manganese composite oxide is segregated at the grain boundary between primary particles.
[0028] In addition, in the first embodiment or the second embodiment, a water washing step and a drying step may be provided. In the water washing step, water is mixed in a ratio of 50 parts by weight to 200 parts by weight relative to 150 parts by weight of the lithium nickel manganese composite oxide obtained after calcination, and solid-liquid separation is performed after stirring. In the drying step, the lithium nickel manganese composite oxide after water washing is dried. In addition, in the mixture, the mass ratio (z) of titanium and the mass ratio (w) of niobium relative to the total mass of nickel, manganese, element M, titanium and niobium may satisfy 0.005≤z≤0.05, 0.002≤w≤0.03, (z+w)≤0.06 and z>w.
[0029] In addition, in the mixture preparation step, at least a titanium-containing nickel-manganese composite compound, a niobium compound and a lithium compound can be mixed, and the nickel-manganese composite compound contains nickel (Ni), manganese (Mn) and titanium (Ti), and arbitrarily contains at least one element selected from Co, V, Mg, Mo, Ca, Cr, Ta, Na, W, Fe, Zn, B, Si, P, Zr and Al, namely, element M (M), and the mass ratio of each element is represented by Ni:Mn:M:Ti=(1-xy-z'):x:y:z' (wherein 0.03≤x≤0.30, 0≤y≤0.30, 0.005≤z'≤0.05).
[0030] The nickel-manganese composite compound containing titanium can be obtained by crystallization. The nickel-manganese composite compound containing titanium can also be obtained by coating a nickel-manganese composite compound obtained by crystallization with a compound containing titanium.
[0031] In addition, in the mixture preparation step, at least a niobium-containing nickel-manganese composite compound, a lithium compound and a titanium compound can be mixed, and the niobium-containing nickel-manganese composite compound contains nickel (Ni), manganese (Mn) and niobium (Nb), and optionally contains at least one element selected from the group consisting of Co, V, Mg, Mo, Ca, Cr, Ta, Na, W, Fe, Zn, B, Si, P, Zr and Al, namely, an element M (M), and the mass ratio of each of the above elements is expressed by Ni:Mn:M:Nb=(1-xy):x:y:w' (wherein 0.03≤x≤0.30, 0≤y≤0.30, 0.001<w'≤0.03).
[0032] In addition, the nickel-manganese composite compound containing niobium can be obtained by coating the nickel-manganese composite compound obtained by crystallization with a compound containing niobium. In addition, the mass ratio of the above elements in the nickel-manganese composite compound containing niobium is represented by Ni:Mn:M:Nb=(1-xy):x:y:w' (wherein 0.03≤x≤0.30, 0≤y≤0.30, 0.002≤w'≤0.03).
[0033] In addition, the sintering process is preferably carried out in an atmosphere with an oxygen concentration of 80 volume % or more and 100 volume % or less. In addition, the titanium in the lithium nickel manganese composite oxide is preferably present inside the primary particle. In addition, the titanium compound is preferably titanium oxide. In addition, the niobium compound is preferably niobium oxide, niobic acid or a mixture thereof. In addition, the lithium nickel manganese composite oxide obtained after sintering has a compression resistance of 4.0 g / cm2 obtained by measuring the pressed powder resistance. 3 The volume resistivity is preferably 5.0×10 2 Ω·cm or more 1.0×10 5 Ω·cm or less.
[0034] Effects of the Invention
[0035] According to the present invention, a method for producing a positive electrode active material that can achieve very high thermal stability at low cost can be provided. In addition, the present invention can easily produce such a positive electrode active material in industrial-scale production, and can be said to have great industrial value. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] [ Figure 1 ] Figure 1 This is a graph showing the maximum oxygen generation peak temperature of the positive electrode active materials obtained in Comparative Examples 1A, 2A, 3A and Example 2A.
[0037] [ Figure 2 ] Figure 2 This is a graph showing the volume resistivity of the positive electrode active materials obtained in Comparative Examples 1A, 2A, 3A and Example 2A during compression.
[0038] [ Figure 3 ] Figure 3 This is a graph showing the discharge capacity of the positive electrode active materials obtained in Examples 2A and 6A.
[0039] [ Figure 4 ] Figure 4 This is a graph showing the maximum oxygen generation peak temperature of the positive electrode active materials obtained in Comparative Examples 1A, 2A, and 3A, Example 2A, and Example 11A.
[0040] [ Figure 5 ] Figure 5 This is a graph showing the discharge capacity of the positive electrode active materials obtained in Example 2A and Example 11A.
[0041] [ Figure 6 ] Figure 6 This is a diagram showing an example of a method for producing a positive electrode active material according to this embodiment.
[0042] [ Figure 7 ] Figure 7 (A) and Figure 7 (B) is a diagram showing an example of a method for producing a nickel-manganese composite compound according to the present embodiment.
[0043] [ Figure 8 ] Figure 8 This is a diagram showing an example of a method for producing a positive electrode active material according to this embodiment.
[0044] [ Fig. 9 ] Fig. 9 (A) and Fig. 9 (B) is a diagram showing an example of a method for producing a titanium-containing nickel-manganese composite compound according to the present embodiment.
[0045] [ Fig.10 ] Fig.10 This is a diagram showing an example of a method for producing a titanium-containing nickel-manganese composite compound according to the present embodiment.
[0046] [ Fig.11 ] Fig.11 This is a diagram showing an example of a method for producing a positive electrode active material according to this embodiment.
[0047] [ Fig.12 ] Fig.12 This is a diagram showing an example of a method for producing a niobium-containing nickel-manganese composite compound according to the present embodiment.
[0048] [ Fig.13 ] Fig.13 This is a diagram showing an example of a method for producing a positive electrode active material according to the present embodiment (including a water washing step and a drying step).
[0049] [ Fig.14 ] Fig.14 This is a diagram showing an example of a method for producing a positive electrode active material according to the present embodiment (including a water washing step and a drying step).
[0050] [ Fig.15 ] Fig.15 This is a diagram showing an example of a method for producing a positive electrode active material according to the present embodiment (including a water washing step and a drying step).
[0051] [ Fig.16 ] Fig.16 This is a schematic cross-sectional view of a button-type battery used in battery evaluation.
[0052] [ Fig.17 ] Fig.17 (A) is a diagram showing an example of a cross-sectional photograph of a positive electrode active material, Fig.17 (B) and Fig.17 (C) is a diagram showing an example of the STEM-EDX evaluation results of the inside of the primary particles of the positive electrode active materials of Example 2A and Example 2B, respectively.
[0053] [ Fig.18 ] Fig.18 (A) is a diagram showing an example of a cross-sectional photograph of a positive electrode active material, Fig.18 (B) and Fig.18 (C) is a diagram showing an example of the STEM-EDX evaluation results of the primary particle boundaries of the positive electrode active materials of Example 2A and Example 2B, respectively. DETAILED DESCRIPTION
[0054] Hereinafter, first, a positive electrode active material for a lithium ion secondary battery obtained by the manufacturing method of this embodiment is described, and then a manufacturing method of the positive electrode active material for a lithium ion secondary battery of this embodiment and a lithium ion secondary battery using the positive electrode active material are described.
[0055] 1. Positive electrode active material for lithium-ion secondary batteries
[0056] The positive electrode active material for lithium ion secondary battery of the present embodiment (hereinafter also referred to as "positive electrode active material") preferably includes a lithium nickel manganese composite oxide having a hexagonal layered structure and composed of secondary particles formed by agglomeration of a plurality of primary particles. The lithium nickel manganese composite oxide contains lithium (Li), nickel (Ni), manganese (Mn), titanium (Ti) and niobium (Nb) as elements other than oxygen, and optionally contains at least one element selected from Co, V, Mg, Mo, Ca, Cr, Ta, Na, W, Fe, Zn, B, Si, P, Zr and Al, that is, element M (M).
[0057] In particular, when a flammable non-aqueous electrolyte is used as a constituent material of a lithium-ion secondary battery, a high thermal stability is required for the lithium-ion secondary battery. In addition, in a lithium-ion secondary battery, when a short circuit occurs between the positive electrode and the negative electrode in a charged state, the following chain reaction sometimes occurs: the positive electrode active material decomposes due to a large amount of heat generated by the rapid flow of current, and then generates heat. Therefore, by using a positive electrode active material with a high volume resistivity under the condition of being compressed in the positive electrode, the sharp increase in current caused by the short circuit can be suppressed, and the thermal stability during the short circuit can be further improved.
[0058] The inventors of the present invention conducted intensive research and found that by containing specific amounts of titanium (Ti) and niobium (Nb) in a specific distribution in a lithium nickel manganese composite oxide used as a positive electrode active material, the positive electrode active material can have a very high volume resistivity and can achieve high thermal stability by suppressing oxygen release during overcharging, thereby completing the present invention.
[0059] Below, refer to Figures 1 to 5 The effect of including titanium (Ti) and niobium (Nb) in the lithium nickel manganese composite oxide of this embodiment is described below. Figures 1 to 5 The positive electrode active materials and secondary batteries obtained in the examples and comparative examples described below were prepared based on the evaluation results.
[0060] Figure 1 This is a graph showing the maximum oxygen generation peak temperature (° C.) obtained by measuring the amount of oxygen when the temperature of a lithium nickel manganese composite oxide (positive electrode active material) was increased from room temperature to 450° C. in an overcharged state.
[0061] Figure 1 In the chart, from left to right, the maximum oxygen generation peak temperatures of Comparative Example 1A containing no titanium and niobium, Comparative Example 2A containing only titanium (Ti: 2.6 atomic %), Comparative Example 3 containing only niobium (Nb: 1 atomic %), and Example 2 containing titanium and niobium (Ti: 2.2 atomic %, Nb: 0.5 atomic %) are shown.
[0062] like Figure 1 As shown, the maximum oxygen generation peak temperature is higher in Comparative Example 2A (Ti: 2.6 atomic %) containing only titanium and Comparative Example 3 (Nb: 1 atomic %) containing only niobium than in Comparative Example 1A containing neither titanium nor niobium. Furthermore, in Example 2A (Ti: 2.2 atomic %, Nb: 0.5 atomic %) containing both titanium and niobium, the maximum oxygen generation peak temperature is further higher than in Comparative Examples 2A and 3A.
[0063] In addition, in Example 2A, only by containing 0.5 atomic % of Nb together with Ti, a higher maximum oxygen generation peak temperature than that of Comparative Example 3A (Nb: 1 atomic %) was shown. Therefore, the positive electrode active material of this embodiment can suppress oxygen generation during overcharge at a higher level while reducing the amount of expensive niobium used.
[0064] Figure 2 The lithium nickel manganese composite oxide (positive electrode active material) is compressed to 4.0 g / cm 3 Graph of volume resistivity (Ω·cm) at .
[0065] like Figure 2 As shown, compared with Comparative Example 1A without titanium and niobium, the volume resistivity of Comparative Example 2A (Ti: 2.6 atomic %) containing only titanium and Comparative Example 3A (Nb: 1 atomic %) containing only niobium increases to a certain extent. However, in Example 2A (Ti: 2.2 atomic %, Nb: 0.5 atomic %) containing both titanium and niobium, the volume resistivity increases significantly even compared with Comparative Examples 2A and 3A. Therefore, the positive electrode active material of this embodiment significantly increases the volume resistivity during compression by containing titanium and niobium, and thus has excellent thermal stability during short circuit.
[0066] also, Figure 3 : is a graph showing the discharge capacity (mAh / g) of Example 2A and Example 6A (Ti: 2.2 atomic %, Nb: 0.5 atomic %) manufactured under the same conditions except that the oxygen concentration of the atmosphere in the firing step was changed. Figure 3 As shown, in Example 2A (oxygen concentration: 90 volume %) in which the oxygen concentration during firing was 80 volume % or more, the discharge capacity was improved compared with Example 6A in which the oxygen concentration during firing was 60 volume %.
[0067] Therefore, although it is generally considered difficult to have both high volume resistivity and high battery capacity, the positive electrode active material of this embodiment can achieve high volume resistivity even with a very high volume resistivity (4.0 g / cm 3 When compressed), it can also have a high battery capacity, and can have both high thermal stability and high battery capacity at a low cost.
[0068] From the above content, it is clear that the positive electrode active material of this embodiment (i) contains titanium and niobium through a lithium nickel manganese composite oxide combination, so that high thermal stability during overcharge and very high volume resistivity during compression can be achieved at low cost, and thermal stability during short circuit is excellent. In addition, (ii) by adjusting the manufacturing conditions, it is possible to have both high battery capacity and high thermal stability.
[0069] As a result of further studies, the present inventors have found that, in a lithium nickel manganese composite oxide used as a positive electrode active material, iii) the lithium nickel manganese composite oxide can have high thermal stability and further improve the battery capacity by washing and drying the lithium nickel manganese composite oxide.
[0070] Below, refer to Figure 4 , 5 The effects of washing with water and drying in the lithium nickel manganese composite oxide of the present embodiment will be described.
[0071] Figure 4 This is a graph showing the maximum oxygen generation peak temperature (° C.) obtained by measuring the amount of oxygen when the temperature of a lithium nickel manganese composite oxide (positive electrode active material) was increased from room temperature to 450° C. in an overcharged state.
[0072] Figure 4 The chart shows, from left to right, the maximum oxygen generation peak temperatures of Comparative Example 1A containing no titanium and niobium, Comparative Example 2A containing only titanium (Ti: 2.6 atomic %), Comparative Example 3A containing only niobium (Nb: 1 atomic %), Example 2A containing titanium and niobium (Ti: 2.2 atomic %, Nb: 0.5 atomic %), and Example 11A obtained by washing and drying Example 2A (Ti: 2.2 atomic %, Nb: 0.5 atomic %).
[0073] like Figure 4 As shown, the maximum oxygen generation peak temperature is higher in Comparative Example 2A (Ti: 2.6 atomic %) containing only titanium and Comparative Example 3 (Nb: 1 atomic %) containing only niobium than in Comparative Example 1A containing neither titanium nor niobium. In addition, in Example 2A and Example 11A (Ti: 2.2 atomic %, Nb: 0.5 atomic %) containing both titanium and niobium, the maximum oxygen generation peak temperature is higher than that of Comparative Example 2A, and the maximum oxygen generation peak temperature is equal to or higher than that of Comparative Example 3A.
[0074] In addition, in Example 11A and Example 2A, only by containing 0.5 atomic % of Nb together with Ti, a maximum exothermic peak temperature higher than that of Comparative Example 2A (Ti: 2.6 atomic %) and Comparative Example 3A (Nb: 1 atomic %) was shown. Therefore, it is clear that the positive electrode active material of this embodiment can suppress the generation of oxygen during overcharge at a higher level while reducing the amount of expensive niobium used.
[0075] Figure 5 : is a graph showing the battery capacity (initial discharge capacity) of Example 2A containing titanium and niobium (Ti: 2.2 atomic %, Nb: 0.5 atomic %) and Example 11 obtained by washing and drying Example 2A. Figure 5 As shown, the battery capacity of Example 11A which was washed with water was improved compared with that of Example 2A which was not washed with water.
[0076] Therefore, although the battery capacity of the lithium nickel manganese composite oxide is slightly reduced due to the inclusion of titanium and niobium as heterogeneous elements, the positive electrode active material of the present embodiment can have both high thermal stability and higher battery capacity by washing and drying after calcination as described later. The preferred configuration of the positive electrode active material of the present embodiment is described in detail below.
[0077] [Lithium Nickel Manganese Composite Oxide]
[0078] The lithium nickel manganese composite oxide contained in the positive electrode active material is composed of secondary particles formed by agglomeration of a plurality of primary particles. In addition, the lithium nickel manganese composite oxide preferably has a hexagonal layered structure.
[0079] The lithium nickel manganese composite oxide contains lithium (Li), nickel (Ni), manganese (Mn), titanium (Ti) and niobium (Nb) as elements other than oxygen, and optionally contains at least one element selected from Co, V, Mg, Mo, Ca, Cr, Ta, Na, W, Fe, Zn, B, Si, P, Zr and Al, i.e., element M (M).
[0080] The ratio (molar ratio) of the amounts of the above elements contained in the lithium nickel manganese composite oxide is not particularly limited. From the viewpoint of high battery capacity, it is preferably represented by Li:Ni:Mn:M:Ti:Nb=a:(1-xyzw):x:y:z:w (wherein 0.97≤a≤1.25, 0.03≤x≤0.30, 0≤y≤0.30, 0.005≤z≤0.05, 0.001<w≤0.03). In addition, in the above amount ratio, z representing the amount ratio of titanium (Ti) and w representing the amount ratio of niobium (Nb) satisfy the relationship of (z+w)≤0.06 and z>w. The preferred composition of each element is described below.
[0081] (lithium)
[0082] In the above-mentioned amount ratio, the total amount ratio of the above-mentioned elements other than Li becomes 1, so a representing the amount ratio of Li corresponds to the amount ratio of lithium to the above-mentioned element (Me) other than lithium (hereinafter also referred to as "Li / Me".). In addition, the range of a is 0.97≤a≤1.25, preferably 1.00≤a≤1.15. When the value of a is in the above-mentioned range, the reaction resistance of the positive electrode is reduced and the output of the battery can be increased. In addition, the range of a can be 1.00≤a≤1.05.
[0083] (manganese)
[0084] In the above-mentioned amount ratio, the range of x representing the amount ratio of Mn is 0.03≤x≤0.30, preferably 0.05≤x≤0.15, and more preferably 0.05≤x≤0.10. When the value of x is in the above-mentioned range, it is possible to have a high battery capacity and high thermal stability. On the other hand, when the value of x is less than 0.03, the improvement effect of thermal stability cannot be obtained. In addition, when the value of x is greater than 0.30, the battery capacity is reduced. In addition, by including manganese in the above-mentioned range, the sintering temperature can be increased in the sintering step (S20) described later, and the dispersion of titanium and the like can be promoted.
[0085] (Element M)
[0086] In the above-mentioned amount ratio, element M is at least one element selected from Co, V, Mg, Mo, Ca, Cr, Ta, Na, W, Fe, Zn, B, Si, P, Zr and Al. In addition, the range of y representing the amount ratio of element M is 0≤y≤0.30, preferably 0≤y≤0.15. When y is greater than 0, thermal stability, storage characteristics and battery characteristics can be improved. On the other hand, when y is greater than 0.30, there is a situation where the crystal structure becomes unstable and a compound with a layered crystal structure cannot be formed, and the battery capacity is reduced due to the relative decrease in the ratio of Ni and Mn. For example, when M contains Co, the battery capacity and output characteristics are more excellent. When M is Co, it is preferably 0≤y≤0.10. In addition, when the amount ratio of Co contained in element M is set to y1, it is preferably 0<y1≤0.10, and more preferably 0.01≤y1≤0.10.
[0087] (titanium)
[0088] In the above-mentioned amount ratio, the range of z representing the amount ratio of Ti is 0.005≤z≤0.05. As described above, when titanium is included in the above-mentioned range together with niobium, the volume resistivity of the lithium nickel manganese composite oxide during compression can be significantly increased, and oxygen release can be suppressed when used in the positive electrode of a secondary battery, thereby obtaining high thermal stability. On the other hand, when the value of z is less than 0.005, the effect of improving thermal stability is not sufficient. In addition, when the value of z is greater than 0.05, the ratio of Ni to Mn is relatively reduced, or the crystal structure is unstable and cation mixing is prone to occur, so the battery capacity is sometimes greatly reduced.
[0089] (niobium)
[0090] In the above-mentioned amount ratio, the range of w representing the amount ratio of Nb is 0.001<w≤0.03, preferably 0.002≤w≤0.03, more preferably 0.002≤w≤0.02, and further preferably 0.002≤w≤0.01. As described above, by including niobium in the above-mentioned range together with titanium, the volume resistivity of the lithium nickel manganese composite oxide during compression can be significantly increased even if the niobium content is small, and oxygen release can be suppressed when used in the positive electrode of a secondary battery, and it has high thermal stability.
[0091] In addition, in the above-mentioned amount ratio, the total amount ratio (z) of titanium and the amount ratio (w) of niobium (z+w) is 0.06 or less, preferably 0.05 or less, and more preferably 0.03 or less. When z+w is within the above-mentioned range, high thermal stability can be achieved while obtaining a higher battery capacity.
[0092] In addition, in the above-mentioned amount ratio, the amount ratio of niobium (w) is less than the amount ratio of titanium (z) (z>w), preferably z≥2w, more preferably z≥3w, and further preferably z≥4w. Niobium is an element more expensive than titanium, so by making its content less than titanium, the manufacturing cost can be reduced, and by combining with titanium, high thermal stability can be achieved.
[0093] (nickel)
[0094] In the above-mentioned amount ratio, (1-xyzw) representing the amount ratio of Ni is 0.34 or more, preferably 0.5 or more, more preferably 0.65 or more, more preferably 0.70 or more, further preferably 0.80 or more, and can be 0.90 or more. When the amount ratio of nickel is within the above-mentioned range, a secondary battery with a high battery capacity can be obtained. When the amount ratio of nickel is high, although the battery capacity is improved, the thermal stability sometimes decreases. However, the lithium nickel manganese composite oxide of the present embodiment has the above composition, so that even if the nickel ratio is high, it can have high thermal stability.
[0095] The composition of the lithium nickel manganese composite oxide can be measured by quantitative analysis using inductively coupled plasma (ICP) emission spectrometry.
[0096] (Distribution of Niobium)
[0097] At least a portion of niobium (Nb) contained in the lithium nickel manganese composite oxide of the present embodiment is preferably segregated at the grain boundaries between primary particles. The segregation of niobium can be confirmed, for example, by performing surface analysis / line analysis of the composition of the primary particle cross section using energy dispersive X-ray spectroscopy (EDX) of a scanning transmission electron microscope (S-TEM) to detect the concentration of niobium in at least a portion of the grain boundaries between primary particles. It should be noted that at least a portion of niobium may be present inside the primary particles.
[0098] The niobium concentration at the grain boundary between primary particles determined by STEM-EDX is preferably 1.3 times or more, more preferably 1.5 times or more, the niobium concentration inside the primary particles. The upper limit of the niobium concentration is not particularly limited, and is, for example, 5 times or less.
[0099] The concentration of niobium inside the primary particles or at the grain boundaries can be confirmed by performing surface analysis, line analysis, and point analysis on the composition of the cross sections of a plurality of secondary particles using EDX measurement using a scanning transmission electron microscope (S-TEM).
[0100] For example, the niobium concentration at the grain boundaries between primary particles can be obtained as follows: 20 regions including the grain boundaries between primary particles are randomly selected from the cross sections of a plurality of secondary particles (e.g., Fig.18 The composition of each region is confirmed by point analysis, and the average value is calculated. In addition, the niobium concentration in the primary particles can be obtained by randomly selecting the internal regions of 20 primary particles (for example, the 130 nm × 130 nm region without grain boundaries: refer to Fig.17 ), analyze the composition of each region and calculate its average value.
[0101] (Distribution of Titanium)
[0102] The distribution of titanium (Ti) contained in the lithium nickel manganese composite oxide of the present embodiment is not particularly limited, and may be present on at least one of the surface and grain boundary of the primary particle, or may be solid-dissolved in the interior of the primary particle. From the viewpoint of increasing the battery capacity in the secondary battery, it is preferred that titanium is solid-dissolved. Here, titanium is solid-dissolved means, for example, that titanium is detected inside the primary particle by performing surface analysis of the cross section of the secondary particle using EDX in S-TEM, and no concentration of titanium at the interface of the primary particle is confirmed, and titanium is preferably detected on the entire surface inside the primary particle.
[0103] For example, the titanium concentration at the grain boundary between primary particles obtained by STEM-EDX is preferably less than 1.3 times, preferably less than 1.2 times, preferably less than 1.1 times, and may be less than 1.0 times relative to the titanium concentration inside the primary particles. In addition, the lower limit of the titanium concentration at the grain boundary between primary particles relative to the titanium concentration inside the primary particles may be more than 0.6 times, may be more than 0.7 times, for example, may be more than 0.8 times and less than 1.2 times, and may be more than 0.9 times and less than 1.1 times. It should be noted that the titanium concentration, like the above-mentioned niobium concentration, can be measured by surface analysis of EDX of S-TEM, etc.
[0104] It should be noted that in the lithium nickel manganese composite oxide of this embodiment, the distribution of metal elements other than the above-mentioned niobium (Nb) and titanium (Ti) is not particularly limited. For example, in the case of containing Ni, Mn and Co as the element M, these metal elements are preferably detected on the entire surface inside the multiple primary particles constituting the secondary particles.
[0105] [Volume average particle size (Mv)]
[0106] The volume average particle size (Mv) of the positive electrode active material of this embodiment is preferably 8 μm or more and 20 μm or less, and more preferably 10 μm or more and 17 μm or less. When the volume average particle size (Mv) is within the above range, when the positive electrode active material is used for the positive electrode of a secondary battery, it can have both high output characteristics and battery capacity, as well as high filling property in the positive electrode.
[0107] On the other hand, when the volume average particle size (Mv) is less than 8 μm, high filling property in the positive electrode cannot be obtained sometimes. In addition, if the volume average particle size (Mv) is greater than 20 μm, high output characteristics and battery capacity cannot be obtained sometimes. It should be noted that the volume average particle size (Mv) can be obtained, for example, by the volume integral value measured by a laser diffraction scattering particle size distribution meter.
[0108] [(D90-D10) / Mv] (Dispersion Index)
[0109] [(D90-D10) / Mv] of the positive electrode active material of this embodiment is preferably 0.80 or more and 1.20 or less. It should be noted that [(D90-D10) / Mv] represents the discrete index of the particle size of the particles constituting the positive electrode active material calculated from D90 and D10 in the particle size distribution obtained by laser diffraction scattering method (the particle size at 90% and the particle size at 10% based on the volume integral of the particle amount in the particle size distribution curve) and the volume average particle size (Mv).
[0110] When the particle size distribution of the particles constituting the positive electrode active material is wide, there are many small particles having a particle size less than the volume average particle size (Mv) and coarse particles having a particle size greater than the average particle size. When the discrete index is within the above range, small particles and coarse particles are appropriately mixed together and the packing density becomes high, which can increase the energy density per unit volume. In addition, from the viewpoint of increasing the energy density per unit volume, [(D90-D10) / Mv] can be 0.90 or more, and can be 0.95 or more.
[0111] On the other hand, when the discrete index of the positive electrode active material is less than 0.80, the volume energy density sometimes decreases. In addition, in the case of using the method for manufacturing the positive electrode active material of the present embodiment, the upper limit is about 1.20. It should be noted that in the calcining step (S20) described later, if the calcining temperature is greater than 1000°C, the discrete index of the particle size may sometimes be greater than 1.20. In this case, sometimes when the positive electrode active material is formed, the specific surface area decreases and the resistance of the positive electrode increases, thereby reducing the battery capacity.
[0112] [Compressed to 4.0g / cm 3 Volume resistivity at ]
[0113] The positive electrode active material obtained after the calcination step (S20) has a powder resistance of 4.0 g / cm2 obtained by measuring the pressed powder resistance. 3 The volume resistivity is 5.0×10 2 Ω·cm or more 1.0×10 5 Ω·cm or less, preferably 1.0×10 3 Ω·cm or more 1.0×10 4 Ω·cm or less, more preferably 2.0×10 3 Ω·cm or more 1.0×10 4 Ω·cm or less. When the volume resistivity of the positive electrode active material is within the above range, high thermal stability during short circuit can be obtained. Generally, the higher the conductivity of the positive electrode active material, the lower the resistance in the electrochemical reaction is considered to be. Excellent active material, but in the case of considering the thermal stability during short circuit, the volume resistivity is moderately high, thereby being able to suppress the generation of sharp current during short circuit.
[0114] The volume resistivity can be determined, for example, by weighing the positive electrode active material in a range of 4.5 g to 5.5 g so as to be 4.0 g / cm 3 The resistivity was measured in a pressurized state by a four-probe method according to JIS K 7194:1994 after being press-molded into a cylindrical shape with a diameter of 20 mm.
[0115] [Maximum oxygen production peak temperature]
[0116] The maximum oxygen generation peak temperature of the positive electrode active material obtained after the calcination step (S20) in the overcharged state is preferably 250°C or higher, more preferably 260°C or higher. The upper limit of the maximum oxygen generation peak temperature during heating is not particularly limited, but is about 300°C or lower.
[0117] Furthermore, the maximum oxygen generation peak temperature of the positive electrode active material obtained after the water washing step ( S30 ) and the drying step ( S40 ) in the overcharged state when the temperature is increased is preferably 250° C. or higher.
[0118] The upper limit of the maximum oxygen generation peak temperature during temperature increase is not particularly limited, but is about 300° C. or less. It should be noted that the maximum oxygen generation peak temperature can be measured by the method described in the examples. In addition, the maximum oxygen generation peak temperature refers to the temperature at which the oxygen generated during temperature increase reaches a maximum and largest peak.
[0119] [Amount of dissolved lithium]
[0120] The amount of lithium dissolved in water (dissolved lithium amount) of the positive electrode active material of this embodiment when immersed in water is preferably less than the amount of dissolved lithium of the positive electrode active material manufactured under the same conditions except that the washing step (S30) and the drying step (S40) described later are not performed. By reducing the amount of dissolved lithium to a specific amount, the crystallinity of the positive electrode active material can be improved, the discharge capacity can be increased, and the gelation of the positive electrode composite paste when making the electrode plate of the secondary battery can be suppressed.
[0121] The amount of lithium dissolved in water (dissolved lithium amount) of the positive electrode active material obtained after the washing step (S30) and the drying step (S40) when immersed in water is preferably 0.20% by mass or less relative to the positive electrode active material as a whole, more preferably 0.10% by mass or less, can be 0.08% by mass or less, can be 0.06% by mass or less. In addition, the lower limit of the amount of dissolved lithium is not particularly limited, for example, it is 0.01% by mass or more. When the amount of dissolved lithium is within the above range, the remaining lithium in the lithium nickel manganese composite oxide can be drawn out to suppress the occurrence of gelation of the positive electrode mixture paste, etc. It should be noted that when the amount of dissolved lithium is less than 0.01% by mass, lithium is sometimes excessively drawn out of the lithium nickel manganese composite oxide during water washing, in which case the battery characteristics will decrease.
[0122] It should be noted that the amount of dissolved lithium can be measured as follows: 2 g of positive electrode active material is taken and put into 125 ml of pure water at room temperature stirred by a stirrer, and immediately after the active material is put in, it is titrated with an aqueous solution of HCl. The titration is evaluated by the Warder method to calculate the amount of lithium hydroxide (LiOH) and lithium carbonate (LiCO). 2 CO 3 ) amount, and the sum of these lithium amounts is calculated as the eluted lithium.
[0123] It should be noted that the lithium nickel manganese composite oxide of the present embodiment may contain a small amount of elements other than the above-mentioned metal elements (Li, Ni, Mn, element M, Nb, Ti) and oxygen within a range that does not impair the effect of the present invention. In addition, the lithium nickel manganese composite oxide contained in the positive electrode active material may contain a small amount of separate primary particles in addition to secondary particles. In addition, the positive electrode active material may contain compounds other than the above-mentioned lithium nickel manganese composite oxide.
[0124] 2. Method for producing positive electrode active material for lithium ion secondary battery
[0125] Figure 6 to Figure 15 This is a diagram showing an example of a method for producing a positive electrode active material for a lithium ion secondary battery according to the present embodiment (hereinafter also referred to as a "method for producing a positive electrode active material"). By the production method of the present embodiment, a positive electrode active material comprising the above-mentioned lithium nickel manganese composite oxide can be easily obtained on an industrial scale.
[0126] The method for producing a positive electrode active material of the present embodiment comprises a mixture preparation step (S10) and a calcination step (S20), wherein in the mixture preparation step (S10), a mixture containing at least a nickel-manganese composite compound and a lithium compound and optionally containing one or both of a titanium compound and a niobium compound is prepared, and in the calcination step (S20), the mixture is calcined to obtain a lithium nickel-manganese composite oxide, wherein the nickel-manganese composite compound contains nickel (Ni) and manganese (Mn) and optionally contains an element M (M), titanium (Ti) and niobium (Nb), wherein the element M (M) is selected from Co, V, Mg, Mo, Ca, Cr, Ta, Na, W, Fe, Zn, , at least one element from the group consisting of nickel, manganese, element M, titanium and niobium, the mass ratio of each of the above elements is represented by Ni:Mn:M:Ti:Nb=(1-xy):x:y:z':w' (wherein 0.03≤x≤0.30, 0≤y≤0.30, 0≤z'≤0.05, 0≤w'≤0.03), and in the mixture prepared in the mixture preparation step, the mass ratio of titanium (z) and the mass ratio of niobium (w) relative to the total mass of nickel, manganese, element M, titanium and niobium satisfy 0.005≤z≤0.05, 0.001<w≤0.03, (z+w)≤0.06 and z>w.
[0127] The manufacturing method of this embodiment is, for example, Figure 6 The method may include: a mixture preparation step (S10A) of mixing a nickel-manganese composite compound, a titanium compound, a niobium compound and a lithium compound to prepare a mixture; and a calcination step (S20) of calcining the mixture to obtain a lithium-nickel-manganese composite oxide.
[0128] In addition, the manufacturing method of this embodiment is as follows, for example Figure 8 The method may include: a mixture preparation step (S10B) of mixing at least a titanium-containing nickel-manganese composite compound, a niobium compound and a lithium compound to prepare a mixture; and a calcination step (S20) of calcining the mixture to obtain a lithium nickel-manganese composite oxide.
[0129] In addition, the manufacturing method of this embodiment is as follows, for example Fig.11 The method may include: a mixture preparation step (S10C) of mixing at least a nickel-manganese composite compound containing niobium, a titanium compound and a lithium compound to prepare a mixture; and a calcination step (S20) of calcining the mixture to obtain a lithium nickel-manganese composite oxide.
[0130] In the mixture preparation step ( S10D), the mixture may be prepared by mixing at least a nickel-manganese composite compound containing titanium and niobium and a lithium compound.
[0131] In addition, the manufacturing method of this embodiment is as follows, for example Fig.13The method may include: a mixture preparation step (S10A) of mixing at least a nickel-manganese composite compound, a titanium compound, a niobium compound and a lithium compound to prepare a mixture; a calcining step (S20) of calcining the mixture to obtain the above-mentioned lithium nickel-manganese composite oxide; a water washing step (S30) of mixing the obtained lithium nickel-manganese composite oxide with water and stirring and then performing solid-liquid separation; and a drying step (S40) of drying the lithium nickel-manganese composite oxide (precipitate) after water washing.
[0132] In addition, the manufacturing method of this embodiment is, for example, Fig.14 The method may include: a mixture preparation step (S10B) of mixing at least a titanium-containing nickel-manganese composite compound, a niobium compound and a lithium compound to prepare a mixture; a calcination step (S20) of calcining the mixture to obtain a lithium nickel-manganese composite oxide; a water washing step (S30) of mixing the obtained lithium nickel-manganese composite oxide with water and stirring it to perform solid-liquid separation; and a drying step (S40) of drying the lithium nickel-manganese composite oxide (precipitate) after washing.
[0133] In addition, the manufacturing method of this embodiment is, for example, Fig.15 The method may include: a mixture preparation step (S10C) of mixing at least a niobium-containing nickel-manganese composite compound, a titanium compound and a lithium compound to prepare a mixture; a calcination step (S20) of calcining the mixture to obtain a lithium nickel-manganese composite oxide; a water washing step (S30) of mixing the obtained lithium nickel-manganese composite oxide with water and stirring and then performing solid-liquid separation; and a drying step (S40) of drying the lithium nickel-manganese composite oxide (precipitate) after water washing.
[0134] Hereinafter, the manufacturing method of this embodiment will be described in detail for each step. It should be noted that the following description is an example of the manufacturing method of this embodiment and does not limit the manufacturing method.
[0135] [Crystallization Steps (S1A, S1B)]
[0136] The nickel-manganese composite compound used in the mixture preparation step (S10A) is, for example, Figure 7 (A) and Figure 7 As shown in (B), it is preferably obtained by a method including a crystallization step (S1A) and / or a heat treatment step (S2).
[0137] In addition, the titanium-containing nickel-manganese composite compound used in the mixture preparation step (S10B) is, for example, Fig. 9 (A) Fig. 9 As shown in (B), it is preferably obtained by a method including a crystallization step (S1B) and / or a heat treatment step (S2).
[0138] In addition, the nickel-manganese composite compound containing niobium used in the mixture preparation step (S10C) can be prepared by, for example, Fig. 9 The titanium salt shown in (A) can be replaced with a niobium salt. In addition, the nickel-manganese composite compound containing titanium and niobium used in the mixture preparation step (S10D) can be prepared, for example, by mixing with Fig. 9 The titanium salt shown in (A) is obtained by adding a niobium salt together.
[0139] The nickel-manganese composite hydroxide obtained in the crystallization step (S1A) contains nickel (Ni) and manganese (Mn) as elements other than hydroxyl group (OH), and optionally contains at least one element selected from Co, V, Mg, Mo, Ca, Cr, Ta, Na, W, Fe, Zn, B, Si, P, Zr and Al, i.e., element M (M), and the ratio (A) of the respective amounts is preferably represented by Ni:Mn:M=(1-xy):x:y (wherein 0.03≤x≤0.30, 0≤y≤0.30).
[0140] The nickel-manganese composite hydroxide obtained in the crystallization step (S1B) contains nickel (Ni), manganese (Mn) and titanium (Ti) as elements other than hydroxyl (OH), and optionally contains at least one element selected from Co, V, Mg, Mo, Ca, Cr, Ta, Na, W, Fe, Zn, B, Si, P, Zr and Al, that is, element M (M), and the ratio of the amount of each element (B) is preferably represented by Ni: Mn: M: Ti = (1-xy-z'): x: y: z' (wherein 0.03 ≤ x ≤ 0.30, 0 ≤ y ≤ 0.30, 0.005 ≤ z' ≤ 0.05). It should be noted that in the crystallization step (S1B), except that a titanium-containing salt (titanium salt) is added as a raw material to obtain a titanium-containing nickel-manganese composite hydroxide, it can be carried out under the same conditions as the crystallization step (S1A).
[0141] In addition, the niobium-containing nickel-manganese composite hydroxide contains nickel (Ni), manganese (Mn) and niobium (Nb) as elements other than hydroxyl (OH), and optionally contains at least one element selected from Co, V, Mg, Mo, Ca, Cr, Ta, Na, W, Fe, Zn, B, Si, P, Zr and Al, that is, element M (M), and the ratio of the amounts of each element (C) is preferably represented by Ni:Mn:M:Nb=(1-xy-w'):x:y:w' (wherein 0.03≤x≤0.30, 0≤y≤0.30, 0.001<w'≤0.03). It should be noted that, in the crystallization step (S1B), the niobium-containing nickel-manganese composite hydroxide can be obtained under the same conditions as the crystallization step (S1B) except that a niobium-containing salt (niobium salt) is added as a raw material instead of a titanium salt to obtain the niobium-containing nickel-manganese composite hydroxide.
[0142] The crystallization steps (S1A) and (S1B) can be performed by a known crystallization method as long as a nickel-manganese composite hydroxide having the above-mentioned amount ratio (molar ratio) can be obtained. An example of a crystallization step for obtaining a nickel-manganese composite hydroxide by crystallization is described below.
[0143] For example, in a reaction tank, a mixed aqueous solution containing at least nickel and manganese is stirred at a constant speed while a neutralizer is added to form a reaction aqueous solution, and the pH of the reaction aqueous solution is controlled by neutralization to generate nickel-manganese composite hydroxide by coprecipitation (crystallization).
[0144] The mixed aqueous solution containing nickel and manganese can use an aqueous solution containing nickel salt and manganese salt, such as a sulfate solution, nitrate solution, chloride solution, etc. of nickel and manganese. It should be noted that the mixed aqueous solution containing nickel and manganese can be prepared by separately preparing an aqueous solution containing nickel and an aqueous solution containing manganese and then supplying them to a reaction tank.
[0145] In addition, the mixed aqueous solution may contain element M as described later. In addition, in the case of obtaining a nickel-manganese composite hydroxide containing titanium and / or niobium, the mixed aqueous solution may contain titanium and / or niobium. The composition of each metal element contained in the mixed aqueous solution is substantially consistent with the composition of each metal element contained in the obtained nickel-manganese composite hydroxide. Therefore, the composition of the metal elements of the mixed aqueous solution can be modulated in a manner that is the same as the composition of each metal element of the target nickel-manganese composite hydroxide.
[0146] As the neutralizing agent, an alkaline aqueous solution can be used, for example, sodium hydroxide, potassium hydroxide, etc. can be used.
[0147] In addition, preferably, a complexing agent is added to the reaction aqueous solution together with a neutralizing agent. The complexing agent is not particularly limited as long as it can be combined with nickel ions and other metal ions in the reaction aqueous solution in the reaction tank to form a complex, and known substances can be used, for example, an ammonium ion donor can be used. As the ammonium ion donor, it is not particularly limited, for example, ammonia, ammonium sulfate, ammonium chloride, ammonium carbonate, ammonium fluoride, etc. can be used. By adding a complexing agent, the solubility of the metal ions in the reaction aqueous solution can be adjusted.
[0148] In the crystallization step (S1A) or (S1B), when a complexing agent is not used, the temperature of the reaction aqueous solution is preferably set to a range of greater than 60°C and less than 80°C, and the pH of the reaction aqueous solution at the above temperature is preferably greater than 10 and less than 12 (25°C reference). When the pH of the reaction aqueous solution is greater than 12, the obtained nickel-manganese composite hydroxide may form fine particles, and the filterability is also deteriorated, and spherical particles cannot be obtained. On the other hand, when the pH of the reaction aqueous solution is less than 10, the generation rate of the nickel-manganese composite hydroxide is significantly slowed down, Ni remains in the filtrate, and the amount of Ni precipitation deviates from the target composition, and the target ratio of nickel-manganese composite hydroxide may not be obtained.
[0149] In addition, when the temperature of the reaction aqueous solution is greater than 60°C, the solubility of Ni is increased, and the amount of Ni precipitation can be prevented from deviating from the target composition without forming a co-precipitation phenomenon. On the other hand, if the temperature of the reaction aqueous solution is greater than 80°C, the slurry concentration (concentration of the reaction aqueous solution) may increase due to the evaporation of water, the solubility of Ni may decrease, and crystals of sodium sulfate or the like may be generated in the filtrate, the impurity concentration may increase, and the charge and discharge capacity of the positive electrode active material may decrease.
[0150] In the crystallization step (S1A) or (S1B), when a complexing agent such as an ammonium ion donor is used, in order to increase the solubility of Ni in the reaction aqueous solution, the temperature of the reaction aqueous solution is preferably from 30°C to 60°C, and the pH of the reaction aqueous solution is preferably from 10 to 13 (based on 25°C), more preferably from 12 to 13.
[0151] In addition, the ammonia concentration in the reaction aqueous solution is preferably maintained at a constant value within a range of more than 3g / L and less than 25g / L. When the ammonia concentration is less than 3g / L, the solubility of the metal ion cannot be constantly maintained, so the primary particles of the composite hydroxide with neat shape and particle size may not be formed. In addition, since a gel-like core is easily generated, the particle size distribution of the obtained nickel-manganese composite hydroxide is also easily widened. On the other hand, if the ammonia concentration is greater than 25g / L, the solubility of the metal ion becomes too large, and the amount of metal ions remaining in the reaction aqueous solution increases, which easily causes the deviation of the composition of the obtained nickel-manganese composite hydroxide. It should be noted that if the ammonia concentration changes, the solubility of the metal ion changes, and uniform hydroxide particles will not be formed, so it is preferably maintained at a constant value. For example, with regard to the ammonia concentration, it is preferred that the amplitude of the upper limit and the lower limit is set to about 5g / L and maintained at the desired concentration.
[0152] In addition, when the nickel-manganese composite hydroxide obtained by crystallization contains at least one element selected from Co, V, Mg, Mo, Ca, Cr, Ta, Na, W, Fe, Zn, B, Si, P, Zr and Al, i.e., element M, there is no particular limitation on the method of adding element M to the nickel-manganese composite hydroxide, and a known method can be used. For example, from the viewpoint of improving productivity, it is preferred to add an aqueous solution containing element M to a mixed aqueous solution containing nickel and manganese in a reaction tank to coprecipitate the nickel-manganese composite hydroxide containing element M.
[0153] In addition, when the nickel-manganese composite hydroxide obtained by crystallization contains titanium and / or niobium, the method of coordinating titanium and / or niobium in the nickel-manganese composite hydroxide is not particularly limited, and a known method can be used. For example, from the viewpoint of improving productivity, it is preferred to add an aqueous solution containing titanium and / or niobium to a mixed aqueous solution containing nickel and manganese in a reaction tank, and coprecipitate the nickel-manganese composite hydroxide containing titanium and / or niobium.
[0154] As the aqueous solution containing the element M, for example, an aqueous solution containing cobalt sulfate, vanadium oxychloride, vanadium oxysulfate, magnesium sulfate, magnesium chloride, molybdenum chloride, calcium chloride, chromium chloride, sodium tantalate, sodium hydroxide, sodium tungstate, tungsten oxide, iron sulfate, zinc chloride, zinc sulfate, boric acid, ammonium borate, silicon bromide, phosphoric acid, zirconium sulfate, zirconium nitrate, aluminum sulfate, sodium aluminate, etc. can be used. In addition, as the aqueous solution containing titanium, an aqueous solution containing titanium salts, for example, an aqueous solution containing titanium sulfate, etc. can be used. In addition, as the aqueous solution containing niobium, an aqueous solution containing niobium salts, for example, an aqueous solution obtained by dissolving niobium hydroxide, niobium pentachloride, niobic acid, etc. in potassium hydroxide or hydrochloric acid, etc. can be used.
[0155] In addition, from the viewpoint of optimizing the crystallization conditions and facilitating the control of the composition ratio, after obtaining the nickel-manganese composite hydroxide by the crystallization step (S1A), a step of coating the obtained nickel-manganese composite hydroxide with the element M may be further provided. The coating method of the element M is not particularly limited, and a known method may be used.
[0156] Furthermore, in the case of obtaining a nickel-manganese composite hydroxide containing titanium and / or niobium, as Fig.10 and Fig.12 As shown, after obtaining the nickel-manganese composite hydroxide by the crystallization step (S1A) or (S1B), a coating step (S3) of coating with a compound containing titanium and / or niobium may be provided. The coating method of titanium and / or niobium is not particularly limited, and a known method can be used. The coating method of titanium and / or niobium is also the same as the coating method of the element M, and is not particularly limited, and a known method can be used.
[0157] Hereinafter, an example of a coating method for at least one element among titanium, niobium and element M (hereinafter collectively referred to as "additive element") is described. First, the nickel-manganese composite hydroxide obtained by crystallization is dispersed in pure water to form a slurry. Then, an aqueous solution containing the additive element corresponding to the target coating amount is mixed with the above-mentioned slurry, and a neutralizer (acid or alkali) is added dropwise to adjust the pH to a predetermined pH. As an acid, for example, sulfuric acid, hydrochloric acid, nitric acid, etc. can be used. As an alkali, for example, sodium hydroxide, potassium hydroxide, etc. can be used. Then, after the slurry is mixed for a predetermined time, the slurry is filtered and dried, so that a nickel-manganese composite hydroxide coated with the additive element can be obtained. It should be noted that, as other coating methods, a spray drying method in which a solution containing a compound containing the additive element is sprayed on the nickel-manganese composite hydroxide and then dried, a method in which a solution containing a compound containing the element M is impregnated in the nickel-manganese composite hydroxide, etc. can be cited.
[0158] It should be noted that the method of combining the additive element with the nickel-manganese composite hydroxide may include one or both of mixing the additive element into the mixed aqueous solution and coating the nickel-manganese composite hydroxide with the additive element.
[0159] For example, 1) an aqueous alkali solution can be added to a mixed aqueous solution containing nickel and manganese (which does not contain the additive element) to perform crystallization to obtain a nickel-manganese composite hydroxide, and the additive element can be coated on the nickel-manganese composite hydroxide; 2) a mixed aqueous solution containing nickel, manganese and a part of the additive element can be prepared, and the nickel-manganese composite hydroxide (containing the additive element) can be co-precipitated, and the additive element can be coated on the co-precipitate to adjust the content of the additive element.
[0160] For example, as a method for producing a titanium-containing nickel-manganese composite hydroxide, Fig.10 As shown, for example, 1) may include adding an alkaline aqueous solution to a mixed aqueous solution containing nickel and manganese (which does not contain titanium) for crystallization to obtain a nickel-manganese composite hydroxide (S1A), and coating the obtained nickel-manganese composite hydroxide with titanium (S3); 2) may also include preparing a mixed aqueous solution containing nickel, manganese and titanium, adding an alkaline aqueous solution for crystallization, coprecipitating to obtain a nickel-manganese composite hydroxide containing titanium (S1B), and coating the obtained nickel-manganese composite hydroxide containing titanium (coprecipitate) (S3). In the case of including a crystallization step (S1B) and a coating step (S3), the titanium content may be adjusted in such a way that the total amount of titanium added in these steps reaches the range of the above-mentioned mass ratio (B).
[0161] It should be noted that as a method for producing a nickel-manganese composite hydroxide containing niobium, Fig.12 As shown, in addition to Fig.10Except that the titanium shown is replaced by niobium, the same method as the above-mentioned method for producing the nickel-manganese composite hydroxide containing titanium can be used.
[0162] It should be noted that the crystallization steps (S1A) and (S1B) can be prepared by 1) using a batch crystallization method (batch crystallization method), or by 2) using a continuous crystallization method (continuous crystallization method). For example, in the case of the batch crystallization method, the precipitate can be collected after the reaction aqueous solution in the reaction tank becomes a stable state, filtered, and washed with water to obtain a nickel-manganese composite hydroxide. In addition, in the case of the continuous crystallization method, the precipitate can be collected by continuously supplying a mixed aqueous solution and an alkaline aqueous solution, or, as the case may be, continuously supplying an aqueous solution containing an ammonium ion donor, and overflowing the reaction tank to collect the precipitate, filter, and wash with water to obtain a nickel-manganese composite hydroxide.
[0163] In the manufacturing method of the positive electrode active material of the present embodiment, from the viewpoint of obtaining a positive electrode active material showing a high volume energy density when used in a secondary battery, a continuous crystallization method is preferably used. In the manufacture using continuous crystallization, a positive electrode active material with a high discrete index, a wide range of particle size distribution, and high filling properties can be easily obtained. In addition, the continuous crystallization method is also more productive than the batch crystallization method and is more suitable for industrial-scale production.
[0164] [Heat treatment step (S2)]
[0165] like Figure 7 (B) and Fig. 9 As shown in (B), the nickel-manganese composite compound can be obtained by a method that includes a heat treatment step (S2) after the crystallization step (S1A) or (S1B). Fig.10 and Fig.12 The method can be obtained by carrying out the above-mentioned heat treatment step (S2) after the coating step (S3) shown.
[0166] The heat treatment step (S2) is a step of removing at least a portion of the water contained in the nickel-manganese composite hydroxide by heat treatment. In the case of the heat treatment step (S2), by removing at least a portion of the water remaining in the nickel-manganese composite hydroxide, it is possible to prevent the Li / Me of the positive electrode active material obtained in the calcination step (step S20) described later from being biased.
[0167] The heat treatment step (S2) can remove the water in the nickel-manganese composite hydroxide to the extent that the Li / Me of the positive electrode active material does not have a deviation. From the perspective of further reducing the deviation of Li / Me, it is preferred to fully oxidize the nickel-manganese composite hydroxide and convert it into a nickel-manganese composite oxide. It should be noted that it is not necessary to convert all nickel-manganese composite hydroxides into nickel-manganese composite oxides.
[0168] In addition, when the heat treatment step (S2) is provided, at least one of the nickel-manganese composite hydroxide and the nickel-manganese composite oxide obtained by the heat treatment step (S2) can be used as the nickel-manganese composite compound in the mixture preparation step (S10). In addition, when the nickel-manganese composite hydroxide is coated with an additive element (at least one element among titanium, niobium and element M), the heat treatment step (S2) can be performed after the compound containing the additive element is coated on the nickel-manganese composite hydroxide, or the compound containing the additive element can be coated on at least one of the nickel-manganese composite hydroxide and the nickel-manganese composite oxide obtained by the heat treatment step (S2).
[0169] The heat treatment can be performed by heating under the condition of removing the residual moisture in the nickel-manganese composite hydroxide. For example, the temperature of the heat treatment is preferably above 105°C and below 700°C. When the nickel-manganese composite hydroxide is heated at above 105°C, at least a portion of the residual moisture can be easily removed. It should be noted that when the temperature of the heat treatment is less than 105°C, it takes a long time to remove the residual moisture, which is not suitable in industry. On the other hand, when the temperature of the heat treatment is greater than 700°C, the particles converted into nickel-manganese composite oxides are sometimes sintered and agglomerated. For example, when most of the nickel-manganese composite hydroxide is converted into nickel-manganese composite oxides, the temperature of the heat treatment is preferably above 350°C and below 700°C.
[0170] The atmosphere of heat treatment is not particularly limited, for example, from the viewpoint of being easy to operate, it is preferably in air flow. In addition, the time of heat treatment is not particularly limited, for example, it can be set to more than 1 hour. When the time of heat treatment is less than 1 hour, it is sometimes impossible to fully remove the residual moisture in the particles of nickel manganese composite hydroxide. In addition, the time of heat treatment is preferably more than 5 hours and less than 15 hours. In addition, the equipment used in heat treatment is not particularly limited, as long as nickel manganese composite hydroxide can be heated in air flow, for example, air drier, electric furnace that does not produce gas, etc. can be suitably used.
[0171] It should be noted that Figure 7 In (B), the nickel-manganese composite hydroxide after the crystallization step (S1) is heat-treated, but the nickel-manganese composite hydroxide obtained in a step other than the crystallization step (S1) may also be heat-treated. In this case, the above-mentioned effect can also be obtained by removing at least a portion of the water in the nickel-manganese composite hydroxide.
[0172] [Mixture preparation step (S10)]
[0173] The mixture preparation step (S10) is a step of preparing a mixture containing at least a nickel-manganese composite compound and a lithium compound, and optionally containing one or both of a titanium compound and a niobium compound. An example of the mixture preparation step (S10) is described below. It should be noted that the following description is an example of the mixture preparation step (S10), and the mixture preparation step (S10) can also prepare the mixture by a method other than the method described below.
[0174] like Figure 6 As shown, the mixture preparation step (S10A) is a step of preparing a mixture by mixing at least a nickel-manganese composite compound, a titanium compound, a niobium compound, and a lithium compound. In addition, in the mixture preparation step (S10), compounds other than the above compounds may be mixed, for example, a compound containing the element M may be mixed.
[0175] In addition, if Figure 8 As shown, the mixture preparation step (S10B) is a step of preparing a mixture by mixing at least a nickel-manganese composite compound containing titanium, a niobium compound, and a lithium compound. It should be noted that in the mixture preparation step (S10B), compounds other than the above compounds may be mixed, for example, a titanium compound may be further mixed, and a compound containing the element M may also be mixed.
[0176] In addition, if Fig.11 As shown, the mixture preparation step (S10C) is a step of preparing a mixture by mixing at least a nickel-manganese composite compound containing niobium, a titanium compound, and a lithium compound. It should be noted that in the mixture preparation step (S10C), compounds other than the above compounds may be mixed, for example, a niobium compound may be further mixed, and a compound containing the element M may also be mixed.
[0177] In the mixture preparation step (S10), each compound may be added and mixed in the form of, for example, powder (solid phase). Hereinafter, each material used in the mixture preparation step (S10) will be described.
[0178] (Nickel-manganese complex compound)
[0179] The nickel-manganese composite compound used in the mixture preparation step (S10A) contains nickel (Ni) and manganese (Mn) as elements other than hydrogen (H) and oxygen (O), and optionally contains an element M (M) as at least one element selected from Co, V, Mg, Mo, Ca, Cr, Ta, Na, W, Fe, Zn, B, Si, P, Zr and Al. In addition, the ratio of the amount of the above elements contained is preferably represented by Ni:Mn:M=(1-xy):x:y (wherein 0≤x≤0.30, 0≤y≤0.30). In addition, the nickel-manganese composite compound may be at least one of a hydroxide and an oxide.
[0180] The titanium-containing nickel-manganese composite compound used in the mixture preparation step (S10B) contains nickel (Ni), manganese (Mn) and titanium (Ti) as elements other than hydrogen (H) and oxygen (O), and optionally contains an element M (M) as at least one element selected from Co, V, Mg, Mo, Ca, Cr, Zr, Ta, Na, W, Fe, Zn, B, Si, P and Al. In addition, the ratio of the amount of the above elements contained is preferably represented by Ni:Mn:M:Ti=(1-xy-z'):x:y:z' (wherein 0≤x≤0.30, 0≤y≤0.30, 0.005≤z'≤0.05). In addition, the titanium-containing nickel-manganese composite compound may be at least one of a hydroxide and an oxide.
[0181] The niobium-containing nickel-manganese composite hydroxide used in the mixture preparation step (S10C) contains nickel (Ni), manganese (Mn) and niobium (Nb) as elements other than hydroxyl (OH), and optionally contains an element M (M) which is at least one element selected from Co, V, Mg, Mo, Ca, Cr, Ta, Na, W, Fe, Zn, B, Si, P, Zr and Al. In addition, the ratio of the amounts of the above elements contained is preferably represented by Ni:Mn:M:Nb=(1-xy-w'):x:y:w' (wherein 0.03≤x≤0.30, 0≤y≤0.30, 0.001<w'≤0.03). In addition, the niobium-containing nickel-manganese composite compound may be at least one of a hydroxide and an oxide.
[0182] The content (composition) of each element (Ni, Mn, M) in the nickel-manganese composite compound is also substantially maintained in the particles of the lithium-nickel-manganese composite oxide, so the content of each element (Ni, Mn, M) is preferably in the same range as that in the above-mentioned lithium-nickel-manganese composite oxide. It should be noted that the nickel-manganese composite compound used in this embodiment may contain a small amount of elements other than the above-mentioned elements (Ni, Mn, M), hydrogen and oxygen within a range that does not impair the effects of the present invention.
[0183] As the nickel-manganese composite compound, as described above, the nickel-manganese composite hydroxide obtained by the crystallization step (S1A) or (S1B) can be used, and the nickel-manganese composite hydroxide obtained by the coating step (S3) can also be used. In addition, at least one of the nickel-manganese composite hydroxide and the nickel-manganese composite oxide obtained after the heat treatment step (S2) can be used. It should be noted that the nickel-manganese composite compound can be obtained by the above-mentioned crystallization step (S1A, S1B) and / or the heat treatment step (S2), etc., but can also be obtained by other methods.
[0184] In addition, the nickel-manganese composite compound preferably contains nickel and manganese uniformly in its particles. For example, when using a mixture of nickel hydroxide particles and manganese compounds, nickel hydroxide particles coated with manganese compounds, etc. as raw materials, the distribution of manganese in the obtained positive electrode active material is sometimes uneven and the effect obtained by containing manganese cannot be fully obtained.
[0185] (Titanium compounds)
[0186] As the titanium compound, a known titanium-containing compound can be used, for example, titanium oxide, titanium sulfate, titanium tetrabromide, titanium tetrachloride, titanium silicide, etc. The titanium compound may be used alone or in combination of two or more.
[0187] Among them, titanium oxide is preferred from the viewpoint of easy availability and avoiding impurities from being mixed into the lithium nickel manganese composite oxide. It should be noted that when impurities are mixed into the lithium nickel manganese composite oxide, the thermal stability, battery capacity and cycle characteristics of the obtained secondary battery may be reduced.
[0188] The titanium compound is preferably mixed in particles (solid phase). When titanium is added in the solid phase, the reactivity in the calcining process (S20) will change due to the particle size of the titanium compound, so the particle size of the titanium compound used is one of the important factors. The average particle size of the titanium compound is preferably 0.01 μm to 5 μm, more preferably 0.05 μm to 3 μm, and further preferably 0.08 μm to 1 μm. In the case where the average particle size is less than 0.01 μm, the operation of the powder may become very difficult, and the titanium compound may scatter in the mixture modulation process (S10) and the calcining process (S20) and the target composition cannot be added to the active material. On the other hand, in the case where the average particle size is greater than 5 μm, it is possible that titanium is unevenly distributed in the calcined lithium nickel manganese composite oxide and the battery capacity is reduced. It should be noted that the average particle size is a volume average particle size (Mv), for example, it can be obtained from the volume integral value measured by a laser diffraction scattering particle size distribution meter.
[0189] The titanium compound can be crushed into the particle size within the above range in advance using various pulverizers such as a ball mill, a planetary ball mill, a jet mill / nano jet mill, a bead mill, and a spiked disc mill. In addition, the titanium compound can be classified by a dry classifier or sieving as needed. For example, a dry classifier can be used to obtain particles close to 1 μm.
[0190] (Niobium compounds)
[0191] As the niobium compound, a known compound containing niobium can be used, for example, niobic acid, niobium oxide, niobium nitrate, niobium pentachloride, niobium nitrate, etc. can be used. Among them, from the viewpoint of easy acquisition and avoiding impurities from being mixed into the lithium nickel manganese composite oxide, the niobium compound is preferably niobium oxide, niobic acid or a mixture thereof. It should be noted that when impurities are mixed into the lithium nickel manganese composite oxide, the thermal stability, battery capacity and cycle characteristics of the obtained secondary battery may be reduced.
[0192] The niobium compound is preferably mixed in the form of particles (solid phase). When niobium is added in the solid phase, the reactivity in the subsequent sintering process (step S20) will change due to the particle size of the niobium compound, so the particle size of the niobium compound used is one of the important factors. The average particle size of the niobium compound is preferably 0.01 μm to 20 μm, more preferably 0.08 μm to 5 μm, and further preferably 0.10 μm to 3 μm. In the case where the average particle size is less than 0.01 μm, problems such as the handling of the powder becomes very difficult, and the niobium compound scatters in the mixture preparation process (S10) and the sintering process (S20) and the target composition cannot be added to the active material may occur. On the other hand, in the case where the average particle size is greater than 10 μm, it is possible that Nb is unevenly distributed in the sintered lithium nickel manganese composite oxide and thermal stability cannot be ensured. It should be noted that the average particle size is a volume average particle size (Mv), which can be obtained, for example, from the volume integral value measured by a laser diffraction scattering particle size distribution meter.
[0193] The niobium compound may be pulverized in advance into a particle size within the above range using various pulverizers such as a ball mill, a planetary ball mill, a jet mill / nano jet mill, a bead mill, and a pin-disc mill. In addition, the niobium compound may be classified by a dry classifier or sieving as needed. For example, a dry classifier may be used to obtain particles having an average particle size of approximately 0.05 μm.
[0194] (Compound containing element M)
[0195] As the compound containing element M, a known compound containing element M can be used, for example, cobalt oxide, vanadium pentoxide, magnesium oxide, molybdenum oxide, calcium oxide, calcium carbonate, chromium oxide, tantalum pentoxide, sodium carbonate, tungsten trioxide, iron oxide, zinc oxide, boric acid, boron oxide, silicon oxide, phosphoric acid, zirconium oxide, etc. It should be noted that when impurities are mixed into the lithium nickel manganese composite oxide, the thermal stability, battery capacity, and cycle characteristics of the obtained secondary battery may be reduced.
[0196] The element M can be mixed with a compound containing the element M in the form of particles (solid phase), or can be contained in the nickel-manganese composite hydroxide by the aforementioned method. In the case where the compound containing the element M is added in the solid phase, the reactivity in the subsequent calcination process (step S20) will change due to the particle size of the compound containing the element M, so it is preferred to appropriately adjust the particle size of the compound containing the element M used. In addition, in the case of mixing a compound containing the element M in the mixture modulation process (S10), it is preferred to mix the compound containing the element M in such a manner that the total amount of the element M contained in the nickel-manganese composite compound and the compound containing the element M becomes the range of the ratio of the amount of the element M in the above-mentioned lithium-nickel-manganese composite compound.
[0197] The compound containing element M can be pulverized into the particle size within the above range in advance using various pulverizers such as ball mill, planetary ball mill, jet mill / nano jet mill, bead mill, and pin-disc mill. In addition, the compound containing element M can be classified by dry classifier or sieving as needed.
[0198] (Lithium compounds)
[0199] The lithium compound is not particularly limited, and known compounds containing lithium can be used, for example, lithium carbonate, lithium hydroxide, lithium nitrate or a mixture thereof can be used. Among them, lithium carbonate, lithium hydroxide or a mixture thereof is preferably used from the viewpoint that the influence of residual impurities is small and the mixture is dissolved at the calcination temperature.
[0200] (Hybrid Method)
[0201] The mixing method of the above-mentioned compounds is not particularly limited, as long as the particles are fully mixed to such an extent that the skeletons of the particles are not destroyed. As a mixing method, for example, a general mixer can be used for mixing, for example, a vibration mixer, a Lodige mixer, a Julia mixer, a V-type blender, etc. can be used for mixing. It should be noted that the titanium mixture is preferably fully mixed before the sintering step described later. In the case of insufficient mixing, sometimes the mass ratio (atomic % ratio) of Li and metal elements other than Li (Me: Me=Ni+Mn+element M+Ti+Nb in this embodiment) between each particle of the positive electrode active material, i.e., Li / Me, deviates, and problems such as failure to obtain sufficient battery characteristics may occur.
[0202] Without performing the water washing step (S30) described later, the lithium compound is mixed in such a way that the Li / Me in the mixture becomes 0.97 or more and 1.25 or less. That is, the mixture is mixed in such a way that the Li / Me in the mixture becomes the same as the Li / Me in the positive electrode active material to be obtained. This is because the molar ratio of Li / Me and each metal element does not change before and after the calcining step (S20), so the Li / Me of the mixture in the mixture preparation step (S10) is the Li / Me of the positive electrode active material.
[0203] In addition, when the water washing step (S30) is performed, part of the remaining lithium components present on the surface of the lithium nickel composite oxide is dissolved in water, so the Li / Me ratio may be reduced compared to the lithium nickel composite oxide after the calcination step (S20). The reduction in the Li / Me ratio varies depending on the composition, physical properties, and water washing conditions of the lithium nickel composite oxide, and in one example of the manufacturing method of this embodiment, the ratio is reduced by about 0.02 due to the water washing step (S30).
[0204] In addition, in the mixture, the amount of the titanium compound and the niobium compound mixed is adjusted so that the ratio (z) of the amount of titanium and the ratio (w) of the amount of niobium relative to the total amount of the above-mentioned metal elements (Ni, Mn, element M, Ti and Nb) except lithium satisfies 0.005≤z≤0.05, 0.001<w≤0.03, (z+w)≤0.06 and z>w. In addition, in the mixture, the ratio (c) of the amount of niobium can be 0.002≤c≤0.03.
[0205] It should be noted that the content (ratio) of niobium (Nb) and titanium (Ti) in the mixture is also substantially maintained in the lithium nickel manganese composite oxide. Therefore, the mixing amount of the niobium compound and the titanium compound in the mixture preparation step (S10A) is preferably in the same range as the content of niobium and titanium in the above-mentioned lithium nickel manganese composite oxide.
[0206] In addition, the amount of titanium contained in the entire mixture in the mixture preparation step (S10B) may be the same as the amount of titanium contained in the titanium-containing nickel-manganese composite compound. In addition, when a titanium compound is further mixed in the mixture preparation step (S10B), it may be the same as the sum of the amounts of titanium contained in the titanium-containing nickel-manganese composite compound and the mixed titanium compound.
[0207] In addition, the amount of niobium contained in the entire mixture in the mixture preparation step (S10C) may be the same as the amount of niobium contained in the nickel-manganese composite compound containing niobium. In addition, when a niobium compound is further mixed in the mixture preparation step (S10C), it may be the same as the total amount of niobium contained in the nickel-manganese composite compound containing niobium and the mixed niobium compound.
[0208] [Firing step (S20)]
[0209] The calcining step ( S20 ) is a step of calcining the mixture obtained in the mixture preparation step ( S10 ) to obtain a lithium nickel manganese composite oxide.
[0210] If the mixture is fired, the lithium in the lithium compound diffuses in the nickel-manganese composite compound, thereby forming a lithium-nickel-manganese composite oxide composed of particles of a polycrystalline structure. The lithium compound melts at the temperature during firing, penetrates into the nickel-manganese composite compound to form a lithium-nickel-manganese composite oxide. The lithium compound melts at the temperature during firing, penetrates into the nickel-manganese composite compound to form a lithium-nickel-manganese composite oxide. At this time, the niobium and titanium contained in the lithium mixture also penetrate into the secondary particles together with the molten lithium compound, and if there are grain boundaries in the primary particles, penetration is also considered to occur.
[0211] The calcining atmosphere preferably has an oxygen concentration of 80% by volume or more and 100% by volume or less, and more preferably has an oxygen concentration of 90% by volume or more and 100% by volume or less. In lithium nickel manganese composite oxides with a high nickel ratio, transition metal elements such as Ni are easily arranged at the Li site in the layered compound, so-called cation mixing. In addition, the crystallinity of the layered compound is reduced, and the atomic distribution is easily disordered. Due to the disorder of this structure, it is believed that titanium and the like cannot be uniformly dissolved at the Me site (transition metal element site), and the battery capacity is reduced. On the other hand, when calcining is performed in the above-mentioned oxygen concentration range, it is possible to obtain a positive electrode active material having both high battery capacity and thermal stability while maintaining high battery capacity.
[0212] The firing temperature is 750°C to 1000°C in an oxidizing atmosphere, preferably 750°C to 950°C. When firing at the above temperature, melting of the lithium compound occurs, promoting the penetration and diffusion of titanium. In addition, the mixture can increase the firing temperature by containing manganese. The firing temperature can be appropriately adjusted within the above range, and by increasing the firing temperature, the diffusion of titanium and niobium can be promoted. Furthermore, the crystallinity of the lithium nickel manganese composite oxide becomes higher, which can further increase the battery capacity.
[0213] On the other hand, when the calcination temperature is less than 750°C, the diffusion of lithium, titanium, and manganese into the nickel-manganese composite compound will not proceed sufficiently, and the remaining lithium and unreacted particles will remain, or the crystal structure will not be neat enough, resulting in the problem that sufficient battery characteristics cannot be obtained. In addition, when the calcination temperature is greater than 1000°C, sintering occurs violently between the particles of the formed lithium-nickel-manganese composite oxide, and abnormal particle growth may occur. If abnormal particle growth occurs, the following problems will arise: the particles after calcination will become coarse, and the filling property will be reduced when the positive electrode active material is formed. In addition, the reaction resistance will increase due to the disorder of the crystal structure, and the discharge capacity will decrease.
[0214] The firing time is preferably set to at least 3 hours, more preferably 6 hours or more and 24 hours or less. When the firing time is less than 3 hours, it is possible not to fully generate the lithium nickel manganese composite oxide. In addition, the furnace used in the firing is not particularly limited, as long as the titanium mixture can be fired in an oxygen stream, preferably an electric furnace that does not generate gas, and any of a batch or continuous furnace can be used.
[0215] [Compressed to 4.0g / cm 3 Volume resistivity at ]
[0216] The compression of the lithium nickel manganese composite oxide obtained after sintering was 4.0 g / cm 3 The volume resistivity is 5.0×10 2 Ω·cm or more 1.0×10 5 Ω·cm or less, preferably 1.0×10 3 Ω·cm or more 1.0×10 4 Ω·cm or less, more preferably 2.0×10 3 Ω·cm or more 1.0×10 4 When the volume resistivity of the lithium nickel manganese composite oxide is within the above range, high thermal stability during short circuit can be obtained.
[0217] Regarding the volume resistivity, for example, the positive electrode active material may be weighed in a range of 4.5 g to 5.5 g so as to have a volume resistivity of 4.0 g / cm 3 The resistivity was determined by press-molding the product into a cylindrical shape having a diameter of 20 mm in a pressurized state by a four-probe method in accordance with JIS K 7194:1994.
[0218] [Pre-burn]
[0219] It should be noted that in the calcining process (S20), before calcining at a temperature of 750°C to 1000°C, a pre-calcining process at a temperature lower than the above-mentioned calcining temperature may be further included. Pre-calcining is preferably carried out at a temperature at which the lithium compound in the mixture melts and can react with the nickel-manganese composite compound. The pre-calcining temperature can be set to a temperature of 350°C or more and lower than the calcining temperature, for example. In addition, the lower limit of the pre-calcining temperature is preferably above 400°C. By maintaining (pre-calcining) the mixture in the above-mentioned temperature range, the lithium compound can penetrate into the nickel-manganese composite compound, the lithium is fully diffused, and a uniform lithium-nickel-manganese composite oxide is obtained. For example, when lithium hydroxide is used as the lithium compound, the pre-calcining is preferably carried out by maintaining it at a temperature of 400°C to 550°C for more than 1 hour to about 10 hours.
[0220] [broken]
[0221] It should be noted that although the lithium nickel manganese composite oxide obtained after the calcining step (S20) suppresses sintering between particles, it may form coarse particles due to weak sintering and aggregation. In such a case, the sintering and aggregation can be eliminated by crushing to adjust the particle size distribution.
[0222] In addition, the manufacturing method of this embodiment may include a water washing step (S30) and a drying step (S40) after the sintering step (S20) as described below. By including these steps, the discharge capacity can be increased, thereby achieving both high thermal stability and higher battery capacity. Each step is described below.
[0223] [Water washing step (S30)]
[0224] The water washing step ( S30 ) is a step of mixing the lithium nickel manganese composite oxide obtained in the calcining step ( S20 ) with water and stirring (hereinafter referred to as “water stirring”), followed by solid-liquid separation.
[0225] The manufacturing method of this embodiment is provided with a water washing step (S30) and a drying step (S40) described later, so that the crystallinity of the positive electrode active material is improved and the discharge capacity is improved. Although the details are not clear, it is believed that, for example, when lithium in the positive electrode active material is extracted by water stirring, the disorder of the atomic arrangement is alleviated and the crystallinity of the positive electrode active material is improved, showing a high discharge capacity. In addition, by dissolving the remaining lithium component on the surface in water and removing it by utilizing the water washing step (S30), the gelation of the positive electrode composite paste when making the plate of the secondary battery can be suppressed.
[0226] The amount of water mixed in the water washing process (S30) is preferably 50 parts by mass or more and 200 parts by mass or less relative to 150 parts by mass of the lithium nickel manganese composite oxide. When the mixing ratio of water is more than 200 parts by mass, excessive lithium will be drawn out from the positive electrode active material, which may cause a decrease in battery capacity and an increase in reaction resistance. On the other hand, when the mixing ratio of water is less than 50 parts by mass, the effect of improving crystallinity and the removal of residual lithium components will be insufficient, which may cause a decrease in battery capacity and gelation of the positive electrode composite paste. In addition, the amount of water mixed in the water washing process (S30) can be 50 parts by mass or more and 200 parts by mass or less relative to 100 parts by mass of the lithium nickel manganese composite oxide.
[0227] The time for washing with water is not particularly limited, and is, for example, about 1 minute to 2 hours, and may be 5 minutes to 50 minutes.
[0228] After the lithium nickel manganese composite oxide is stirred with water, solid-liquid separation is performed to obtain the lithium nickel manganese composite oxide (precipitate). The method of solid-liquid separation is not particularly limited, and a known method can be used. For example, solid-liquid separation can be performed using one or more of a suction filter selected from a Nutsche filter (Buchner funnel), a filter press, a centrifuge, and the like.
[0229] [Drying step (S40)]
[0230] The drying step ( S40 ) is a step of drying the lithium nickel manganese composite oxide (precipitate) obtained in the water washing step ( S30 ) to obtain a powder of the lithium metal composite oxide (dried powder).
[0231] The drying conditions are preferably heat treatment at a temperature of 100° C. to 250° C. in an oxidizing atmosphere or a vacuum atmosphere. When the drying temperature is 100° C. or higher, the water in the precipitate can be fully evaporated. In addition, when the drying temperature is 250° C. or lower, a compact drying device can be used, which is suitable for industrial-scale implementation.
[0232] The atmosphere during drying is preferably an atmosphere that does not contain water vapor or carbon dioxide to avoid the reaction of moisture, carbonic acid and the obtained positive electrode active material in the atmosphere, and is specifically preferably an oxidizing atmosphere or a vacuum atmosphere such as an oxygen atmosphere. In addition, from the viewpoint that the water vapor generated by drying can be quickly discharged, it is preferred to add an exhaust mechanism to the drying device.
[0233] The drying time is not particularly limited, but is preferably set to 0.5 hours or more at the highest temperature reached during drying in order to fully evaporate the water content of the raw material mixture. In addition, from the viewpoint of productivity, the upper limit of the drying time is preferably set to 48 hours or less.
[0234] 3. Lithium-ion secondary battery
[0235] The lithium-ion secondary battery of the present embodiment (hereinafter also referred to as "secondary battery") comprises a positive electrode, a negative electrode and a non-aqueous electrolyte containing the above-mentioned positive electrode active material. The secondary battery, for example, comprises a positive electrode, a negative electrode and a non-aqueous electrolyte. In addition, the secondary battery, for example, may comprise a positive electrode, a negative electrode and a solid electrolyte. In addition, any secondary battery is a secondary battery that is charged and discharged by the separation and insertion of lithium ions, for example, it may be a non-aqueous electrolyte secondary battery, or it may be an all-solid-state lithium secondary battery. It should be noted that the embodiments described below are merely illustrative, and the secondary battery of the present embodiment may also be applicable to various modified and improved forms based on the embodiments described in this specification.
[0236] [positive electrode]
[0237] The positive electrode of the secondary battery is produced using the positive electrode active material. An example of a method for producing the positive electrode is described below.
[0238] First, the above-mentioned positive electrode active material, conductive material and binder are mixed, and activated carbon, a solvent for the purpose of viscosity adjustment, etc. are added as needed, and they are kneaded to make a positive electrode composite paste. At this time, the respective mixing ratios in the positive electrode composite paste can be appropriately adjusted according to the performance of the secondary battery as the target. For example, when the solid content of the positive electrode composite material other than the solvent is set to 100 parts by mass, the content of the positive electrode active material can be set to more than 60 parts by mass and less than 95 parts by mass, the content of the conductive material can be set to more than 1 part by mass and less than 20 parts by mass, and the content of the binder can be set to more than 1 part by mass and less than 20 parts by mass.
[0239] The obtained positive electrode composite material paste is applied to the surface of a collector made of aluminum foil, for example, and dried to disperse the solvent to produce a sheet-like positive electrode. As needed, a roller press is sometimes used to pressurize the electrode to increase the electrode density. The sheet-like positive electrode thus obtained can be cut to an appropriate size according to the target battery and provided for the production of the battery. However, the production method of the positive electrode is not limited to the above-mentioned examples, and can also be based on other methods.
[0240] As the conductive material, for example, graphite (natural graphite, artificial graphite, expanded graphite, etc.), carbon black materials such as acetylene black and Ketjen black, etc. can be used.
[0241] The binder (adhesive) plays the role of linking the active material particles together, and for example, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluororubber, ethylene propylene diene rubber, styrene butadiene, cellulose resin, polyacrylic acid, etc. can be used.
[0242] As required, a solvent is added to the positive electrode composite material to disperse the positive electrode active material, the conductive material, and the activated carbon and dissolve the binder. As the solvent, an organic solvent such as N-methyl-2-pyrrolidone can be used. In addition, activated carbon can be added to the positive electrode composite material to increase the double electric layer capacity.
[0243] [negative electrode]
[0244] As the negative electrode, metallic lithium, lithium alloy, etc. can be used. In addition, as the negative electrode, a negative electrode formed as follows can be used, that is, a negative electrode active material capable of absorbing and releasing lithium ions is mixed with a binder, and a suitable solvent is added to form a paste-like negative electrode composite material, and the negative electrode composite material is applied to the surface of a metal foil collector such as copper, dried, and compressed as needed to increase the electrode density, thereby forming a negative electrode.
[0245] As the negative electrode active material, for example, a sintered body of an organic compound such as natural graphite, artificial graphite and phenolic resin, and a powder of a carbon material such as coke can be used. In this case, as the negative electrode binder, a fluorine-containing resin such as PVDF can be used, as the solvent for dispersing these active materials and the binder, an organic solvent such as N-methyl-2-pyrrolidone can be used.
[0246] [Diaphragm]
[0247] The positive electrode and the negative electrode are arranged with a separator sandwiched therebetween. The separator is used to separate the positive electrode from the negative electrode and to retain the electrolyte, and a known material can be used, for example, a thin film such as polyethylene or polypropylene having a large number of minute pores can be used.
[0248] [Non-aqueous electrolytes]
[0249] As the non-aqueous electrolyte, for example, a non-aqueous electrolyte can be used. The non-aqueous electrolyte is a solution obtained by dissolving a lithium salt as a supporting salt in an organic solvent. In addition, as the non-aqueous electrolyte, a solution in which a lithium salt is dissolved in an ionic liquid can be used. It should be noted that an ionic liquid refers to a salt that is composed of cations and anions other than lithium ions and is also liquid at room temperature.
[0250] As the organic solvent, one selected from cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate and trifluoropropylene carbonate, chain carbonates such as diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate and dipropyl carbonate, ether compounds such as tetrahydrofuran, 2-methyltetrahydrofuran and dimethoxyethane, sulfur compounds such as methyl ethyl sulfone and butane sultone, phosphorus compounds such as triethyl phosphate and trioctyl phosphate, etc. can be used alone, or two or more thereof can be used in combination.
[0251] As supporting salt, LiPF can be used 6 , LiBF4 、LiClO 4 、LiAsF 6 、LiN(CF 3 SO 2 ) 2 and composite salts thereof. Furthermore, the non-aqueous electrolyte may also contain a radical scavenger, a surfactant, a flame retardant, and the like.
[0252] In addition, as a non-aqueous electrolyte, a solid electrolyte can also be used. Solid electrolytes have the property of being able to withstand high voltages. Examples of solid electrolytes include inorganic solid electrolytes and organic solid electrolytes.
[0253] Examples of the inorganic solid electrolyte include oxide-based solid electrolytes and sulfide-based solid electrolytes.
[0254] The oxide-based solid electrolyte is not particularly limited, and an electrolyte containing oxygen (O) and having lithium ion conductivity and electronic insulation can be suitably used. For example, an oxide-based solid electrolyte selected from lithium phosphate (Li 3 PO 4 )、Li 3 PO 4 N X 、LiBO 2 N X 、LiNbO 3 、LiTaO 3 , Li 2 SiO 3 , Li 4 SiO 4 -Li 3 PO 4 , Li 4 SiO 4 -Li 3 VO 4 , Li 2 OB 2 O 3 -P 2 O 5 , Li 2 O-SiO 2 , Li 2 OB 2 O 3 -ZnO, Li 1+X Al X Ti 2-X (PO 4 ) 3 (0≤X≤1), Li 1+X Al X Ge 2-X (PO4 ) 3 (0≤X≤1), LiTi 2 (PO 4 ) 3 , Li 3X La 2 / 3-X TiO 3 (0≤X≤2 / 3), Li 5 La 3 Ta 2 O 12 , Li 7 La 3 Zr 2 O 12 , Li 6 BaLa 2 Ta 2 O 12 , Li 3.6 Si 0.6 P 0.4 O 4 One or more of the following.
[0255] The sulfide-based solid electrolyte is not particularly limited, and for example, an electrolyte containing sulfur (S) and having lithium ion conductivity and electronic insulation can be suitably used. As the sulfide-based solid electrolyte, for example, a sulfide-based solid electrolyte selected from Li 2 SP 2 S 5 , Li 2 S-SiS 2 、LiI-Li 2 S-SiS 2 、LiI-Li 2 SP 2 S 5 、LiI-Li 2 SB 2 S 3 , Li 3 PO 4 -Li 2 S-Si 2 S. Li 3 PO 4 -Li 2 S-SiS 2 、LiPO 4 -Li 2 S-SiS、LiI-Li 2 SP 2 O 5 、LiI-Li 3 PO 4 -P 2 S 5 One or more of the following.
[0256] It should be noted that as the inorganic solid electrolyte, substances other than those mentioned above may also be used, for example, Li 3 N, LiI, Li 3 N-LiI-LiOH, etc. As the organic solid electrolyte, there is no particular limitation as long as it is a polymer compound showing ion conductivity, for example, polyethylene oxide, polypropylene oxide, copolymers thereof, etc. can be used. In addition, the organic solid electrolyte may also contain a supporting salt (lithium salt).
[0257] It should be noted that a solid electrolyte can also be used instead of a non-aqueous electrolyte to form a secondary battery. The solid electrolyte will not decompose even at a high potential, so it will not cause gas generation and thermal runaway due to the decomposition of the electrolyte during charging as seen in a non-aqueous electrolyte, so it has high thermal stability. Therefore, in the case of a lithium ion secondary battery using the positive electrode active material of the present invention, a secondary battery with higher thermal stability can be obtained.
[0258] [Shape and structure of secondary battery]
[0259] The composition of the secondary battery is not particularly limited, and as mentioned above, it can be composed of a positive electrode, a negative electrode, a separator, a non-aqueous electrolyte, etc., or it can be composed of a positive electrode, a negative electrode, a solid electrolyte, etc. In addition, the shape of the secondary battery is not particularly limited, and it can be made into various shapes such as a cylindrical shape and a stacked shape.
[0260] For example, in the case where the secondary battery is a non-aqueous electrolyte secondary battery, the positive electrode and the negative electrode are stacked with a separator to form an electrode body, the non-aqueous electrolyte is impregnated into the obtained electrode body, and the positive electrode collector and the positive terminal leading to the outside and the negative electrode collector and the negative terminal leading to the outside are connected using a collecting lead, etc., and then sealed in a battery box to complete the secondary battery.
[0261] It should be noted that the secondary battery of this embodiment is not limited to the form of using a non-aqueous electrolyte as a non-aqueous electrolyte, and can also be made into a secondary battery using, for example, a solid non-aqueous electrolyte, that is, an all-solid-state battery. In the case of making an all-solid-state battery, the composition other than the positive electrode active material can be changed as needed.
[0262] The secondary battery of the present embodiment can achieve high thermal stability at low cost. In addition, the positive electrode active material for the secondary battery can be obtained by the above-mentioned industrial manufacturing method. In addition, the secondary battery is suitable for the power supply of small portable electronic devices (notebook personal computers, mobile phone terminals, etc.) that always require high capacity. In addition, compared with the batteries using lithium cobalt oxides or lithium nickel oxides as positive electrode active materials in the past, the secondary battery is not only excellent in capacity, but also excellent in durability and thermal stability during overcharge. Therefore, since it can be miniaturized and high-capacity, it is suitable as a power supply for electric vehicles with restricted carrying space. It should be noted that the secondary battery can be used not only as a power supply for electric vehicles driven purely by electric energy, but also as a so-called hybrid vehicle power supply used in conjunction with combustion mechanisms such as gasoline engines and diesel engines.
[0263] Example
[0264] Hereinafter, the present invention will be further described in detail using the embodiments and comparative examples of the present invention, but the present invention is not limited to these embodiments. It should be noted that the analysis method of the metal contained in the positive electrode active material in the embodiments and comparative examples and the various evaluation methods of the positive electrode active material are as follows.
[0265] (1) Composition analysis: Measured by ICP emission analysis.
[0266] (2) Volume average particle size (Mv) and particle size dispersion index [(D90-D10) / average volume particle size]: The particle size distribution was measured on a volume basis using a laser diffraction scattering particle size analyzer (MICROTRAC HRA, manufactured by Nikkiso Co., Ltd.).
[0267] (3) Concentration of each element
[0268] The positive electrode active material was processed so that the cross-section analysis of the primary particles could be performed using S-TEM. 20 primary particles were randomly selected from the multiple secondary particles contained in the positive electrode active material, and the composition of the internal and grain boundary regions (130nm×130nm) of each primary particle cross section was analyzed using EDX of S-TEM.
[0269] (4) Volume resistivity: 5 g of positive electrode active material is 4.0 g / cm 3 The resistivity was determined by press-molding the product into a cylindrical shape having a diameter of 20 mm in a pressurized state by a four-probe method in accordance with JIS K 7194:1994.
[0270] (5) Amount of dissolved lithium:
[0271] 2 g of the positive electrode active material was added to 125 ml of pure water at room temperature stirred by a stirrer, and titrated with a 1 mol / L HCl aqueous solution immediately after the active material was added. The titration was performed using an automatic titrator COM-1750 (manufactured by Hiranuma Sangyo Co., Ltd.) under the following conditions.
[0272] End point detection method: inflection point detection
[0273] Detection sensitivity: 2500
[0274] Dropper Model: H-1700
[0275] Dropper speed: 2
[0276] Minimum drop volume: 0.013mL
[0277] The titration results were evaluated by the Warder method to calculate the lithium hydroxide (LiOH) and lithium carbonate (Li 2 CO 3 ), and the sum of these lithium amounts is calculated as the dissolved lithium.
[0278] (6) Initial discharge capacity:
[0279] The initial charge capacity and initial discharge capacity were prepared as follows: Fig.16 The button-type battery CBA shown in the figure is placed for about 24 hours. After the open circuit voltage OCV (open circuit voltage) stabilizes, the current density at the positive electrode is 0.1 mA / cm 2 The battery was charged to a cutoff voltage of 4.3 V and the initial charge capacity was set. After a 1-hour pause, the initial discharge capacity was set at a capacity when the battery was discharged to a cutoff voltage of 3.0 V. A multi-channel voltage / current generator (R6741A manufactured by Advantest Co., Ltd.) was used for the measurement of the discharge capacity.
[0280] (Production of button-type batteries)
[0281] 52.5 mg of the obtained positive electrode active material, 15 mg of acetylene black and 7.5 mg of polytetrafluoroethylene resin (PTFE) were mixed and press-formed at a pressure of 100 MPa into a diameter of 11 mm and a thickness of 100 μm to prepare Fig.16 The positive electrode (electrode for evaluation) PE shown in the figure. The prepared positive electrode PE was dried in a vacuum dryer at 120°C for 12 hours, and then the positive electrode PE was used to make a 2032-type button-type battery CBA in a glove box with an Ar atmosphere whose dew point was controlled at -80°C. As the negative electrode NE, lithium (Li) metal with a diameter of 17 mm and a thickness of 1 mm was used, and as the electrolyte, 1M LiClO 4An equal amount of a mixed solution of ethylene carbonate (EC) and diethyl carbonate (DEC) (manufactured by Toyama Pharmaceutical Industry Co., Ltd.) was used as a supporting electrolyte. A polyethylene porous membrane with a thickness of 25 μm was used as a separator SE. In addition, the button-type battery CBA was assembled into a button-type battery by configuring a gasket GA and a corrugated gasket WW, and using a positive electrode case PC and a negative electrode case NC.
[0282] (7) Maximum oxygen generation peak temperature
[0283] The thermal stability of the positive electrode is evaluated as follows: the positive electrode active material is made into an overcharged state and heated, and the amount of oxygen released thereby is quantified. A button-type battery is made in the same manner as (6), and CC charging (constant current-constant voltage charging) is performed at a rate of 0.05C to a cut-off voltage of 4.3V. Then, the button battery is disassembled, and only the positive electrode is carefully removed to avoid short circuit, and it is cleaned with DMC (dimethyl carbonate) and dried. About 2 mg of the dried positive electrode is measured, and a gas chromatograph-mass spectrometer (GCMS, Shimadzu Corporation, QP-2010plus) is used to heat the sample from room temperature to 450°C at a heating rate of 10°C / min. Helium is used as a carrier gas. The generation behavior of oxygen (m / z=32) generated during heating is measured to obtain the maximum oxygen generation peak temperature.
[0284] (Example 1A)
[0285] [Crystallization process]
[0286] A predetermined amount of pure water was added to the reaction tank (60 L), and the temperature in the tank was set at 49°C while stirring. At this time, N 2 Gas was added to make the dissolved oxygen concentration in the reaction tank liquid 0.8 mg / L. Into the reaction tank, a 2.0 M mixed aqueous solution of nickel sulfate, manganese sulfate, and cobalt sulfate in a molar ratio of nickel:manganese:cobalt of 85:10:5, a 25 mass % sodium hydroxide solution as an alkaline solution, and a 25 mass % ammonia water as a complexing agent were simultaneously and continuously added to the reaction tank, and crystallization was performed by a continuous crystallization method.
[0287] At this time, the flow rate is controlled in such a way that the residence time of the mixed aqueous solution becomes 8 hours, the pH in the reaction tank is adjusted to 12.0-12.6, and the ammonia concentration is adjusted to 10-14 g / L. After the reaction tank is stabilized, the slurry containing the nickel-manganese-cobalt composite hydroxide is recovered from the overflow port and filtered to obtain a filter cake of the nickel-manganese-cobalt composite hydroxide. 140 g of the nickel-manganese-cobalt composite hydroxide in the filtered filter cloth (Denver) is passed through 1 L of pure water to clean the impurities. The filtered powder is dried to obtain particles of nickel-manganese-cobalt composite hydroxide represented by the mass ratio of nickel, manganese and cobalt as Ni:Mn:Co=0.85:0.10:0.05.
[0288] [Mixture preparation process]
[0289] The obtained nickel-manganese-cobalt composite hydroxide particles, lithium hydroxide, and titanium oxide (TiO) were weighed so that the mass ratio of lithium: (nickel + manganese + cobalt): titanium: niobium was 1.01:0.973:0.022:0.005. 2 ) and niobate (Nb 2 O 5 ·4H 2 O), and then the mixture was thoroughly mixed using a vibration mixer (TURBULA T2C model manufactured by Willy A Bachofen (WAB)) to obtain a lithium mixture.
[0290] [Firing process]
[0291] The obtained lithium mixture was calcined in an oxygen (oxygen concentration: 90 volume %) gas flow at 850° C. for 10 hours and then crushed to obtain particles of lithium nickel manganese cobalt composite oxide (positive electrode active material).
[0292] [evaluate]
[0293] The manufacturing conditions of the positive electrode active material are shown in Table 1, and the results of evaluating the obtained positive electrode active material by the above-mentioned evaluation method are shown in Table 2. It should be noted that for the amount ratio of each element in the following table, the value obtained by rounding off the fourth decimal place of the measured value is shown, and for the Ti / Nb amount ratio, the value obtained by rounding off the second decimal place of the ratio calculated from the measured value of the amount ratio of Ti and Nb is shown.
[0294] (Example 2A)
[0295] A positive electrode active material was obtained and evaluated in the same manner as in Example 1A except that the calcination temperature was set to 870° C. Tables 1 and 2 show the production conditions and evaluation results of the positive electrode active material.
[0296] (Example 3A)
[0297] A positive electrode active material was obtained and evaluated in the same manner as in Example 1A except that the calcination temperature was set to 890° C. Tables 1 and 2 show the production conditions and evaluation results of the positive electrode active material.
[0298] (Example 4A)
[0299] In the mixture preparation step, the obtained nickel-manganese-cobalt composite hydroxide particles, lithium hydroxide, titanium oxide (TiO2 ) and niobate (Nb 2 O 5 ·4H 2 O), except for this, a positive electrode active material was obtained and evaluated in the same manner as in Example 2A. The production conditions and evaluation results of the positive electrode active material are shown in Tables 1 and 2.
[0300] (Example 5A)
[0301] In the mixture preparation process, niobium oxide (Nb 2 O 5 ) was used as the niobium compound, and a positive electrode active material was obtained and evaluated in the same manner as in Example 2A. The production conditions and evaluation results of the positive electrode active material are shown in Tables 1 and 2.
[0302] (Example 6A)
[0303] A positive electrode active material was obtained and evaluated in the same manner as in Example 2A except that the calcination step was performed in an oxygen (oxygen concentration: 60 volume %) gas flow. Tables 1 and 2 show the production conditions and evaluation results of the positive electrode active material.
[0304] (Comparative Example 1A)
[0305] In the mixture preparation step, the particles of the nickel-manganese-cobalt composite hydroxide and lithium hydroxide obtained were weighed in a manner that the mass ratio of lithium: nickel: manganese: cobalt was 1.02: 0.85: 0.10: 0.05 without preparing the titanium compound and the niobium compound, and in the sintering step, the sintering temperature was set to 800° C., and the positive electrode active material was obtained and evaluated in the same manner as in Example 1A. The manufacturing conditions and evaluation results of the positive electrode active material are shown in Tables 1 and 2.
[0306] (Comparative Example 2A)
[0307] In the mixture preparation step, the obtained nickel-manganese-cobalt composite hydroxide particles, lithium hydroxide and titanium oxide (TiO) were weighed so that the mass ratio of lithium: (nickel + manganese + cobalt): titanium was 1.02:0.974:0.026 without preparing a niobium compound. 2 ) and the calcination temperature was set to 830° C. in the calcination step, a positive electrode active material was obtained and evaluated in the same manner as in Example 1A. The production conditions and evaluation results of the positive electrode active material are shown in Tables 1 and 2.
[0308] (Comparative Example 3A)
[0309] In the mixture preparation step, the obtained nickel-manganese-cobalt composite hydroxide particles, lithium hydroxide and niobic acid (Nb) were weighed so that the mass ratio of lithium: (nickel + manganese + cobalt): niobium was 1.02:0.99:0.010 without preparing a titanium compound. 2 O 5 ·4H 2 O), and in the calcination step, the calcination temperature was set to 850° C. A positive electrode active material was obtained and evaluated in the same manner as in Example 1A. The production conditions and evaluation results of the positive electrode active material are shown in Tables 1 and 2.
[0310] (Comparative Example 4A)
[0311] In the mixture preparation step, the obtained nickel-manganese-cobalt composite hydroxide particles, lithium hydroxide, titanium oxide (TiO 2 ) and niobate (Nb 2 O 5 ·4H 2 O), and in the calcination step, the calcination temperature was set to 840° C. A positive electrode active material was obtained and evaluated in the same manner as in Example 1A. The production conditions and evaluation results of the positive electrode active material are shown in Tables 1 and 2.
[0312] [Table 1]
[0313]
[0314] [Table 2]
[0315]
[0316] (Example 1B)
[0317] [Crystallization process]
[0318] A predetermined amount of pure water was added to the reaction tank (60 L), and the temperature in the tank was set at 49°C while stirring. At this time, N 2 Gas was added to the reaction tank so that the dissolved oxygen concentration in the reaction tank solution became 0.8 mg / L. A 2.0 M mixed aqueous solution of nickel sulfate, manganese sulfate, cobalt sulfate, and titanium sulfate, which was formulated in a molar ratio of nickel:manganese:cobalt:titanium of 0.833:0.095:0.050:0.022, a 25 mass % sodium hydroxide solution as an alkaline solution, and a 25 mass % ammonia water as a complexing agent were simultaneously and continuously added to the reaction tank, and crystallization was performed by a continuous crystallization method.
[0319] At this time, the flow rate is controlled in such a way that the residence time of the mixed aqueous solution becomes 8 hours, the pH in the reaction tank is adjusted to 12.0-12.6, and the ammonia concentration is adjusted to 10-14 g / L. After the reaction tank is stabilized, the slurry containing the nickel-manganese-cobalt-titanium composite hydroxide is recovered from the overflow port and filtered to obtain a filter cake of the nickel-manganese-cobalt-titanium composite hydroxide. 140 g of the nickel-manganese-cobalt-titanium composite hydroxide in the filtered filter cloth is passed through 1 L of pure water to clean the impurities. The filtered powder is dried to obtain particles of nickel-manganese-cobalt-titanium composite hydroxide represented by the mass ratio of nickel, manganese, cobalt and titanium as Ni:Mn:Co:Ti=0.833:0.095:0.050:0.022.
[0320] [Mixture preparation process]
[0321] The obtained nickel-manganese-cobalt-titanium composite hydroxide particles, lithium hydroxide and niobic acid (Nb) were weighed so that the mass ratio of lithium: (nickel + manganese + cobalt + titanium): niobium was 1.01:0.995:0.005. 2 O 5 ·4H 2 O), and then the mixture was thoroughly mixed using a vibration mixer (TURBULA T2C model manufactured by Willy A Bachofen (WAB)) to obtain a lithium mixture.
[0322] [Firing process]
[0323] The obtained lithium mixture was calcined in an oxygen (oxygen concentration: 90 volume %) gas flow at 850° C. for 10 hours and then crushed to obtain particles of lithium nickel manganese cobalt composite oxide (positive electrode active material).
[0324] [evaluate]
[0325] Table 3 shows the production conditions of the positive electrode active material, and Table 4 shows the results of evaluation of the obtained positive electrode active material by the above-mentioned evaluation method.
[0326] (Example 2B)
[0327] A positive electrode active material was obtained and evaluated in the same manner as in Example 1B except that the calcination temperature was 870° C. Tables 3 and 4 show the production conditions and evaluation results of the positive electrode active material.
[0328] (Example 3B)
[0329] A positive electrode active material was obtained and evaluated in the same manner as in Example 1B except that the calcination temperature was 890° C. Tables 3 and 4 show the production conditions and evaluation results of the positive electrode active material.
[0330] (Example 4B)
[0331] In the mixture preparation step, the obtained nickel-manganese-cobalt-titanium composite hydroxide particles, lithium hydroxide and niobic acid (Nb) were weighed so that the mass ratio of lithium: (nickel + manganese + cobalt + titanium): niobium was 1.01:0.997:0.003. 2 O 5 ·4H 2 O), except for this, a positive electrode active material was obtained and evaluated in the same manner as in Example 2B. The production conditions and evaluation results of the positive electrode active material are shown in Tables 3 and 4.
[0332] (Example 5B)
[0333] In the mixture preparation process, niobium oxide (Nb 2 O 5 ) was used as the niobium compound, and a positive electrode active material was obtained and evaluated in the same manner as in Example 2B. The production conditions and evaluation results of the positive electrode active material are shown in Tables 3 and 4.
[0334] (Example 6B)
[0335] The positive electrode active material was obtained and evaluated in the same manner as in Example 2B except that the calcination step was performed in an oxygen (oxygen concentration: 60 volume %) gas flow. Tables 3 and 4 show the production conditions and evaluation results of the positive electrode active material.
[0336] (Example 1C)
[0337] [Crystallization process]
[0338] In the crystallization step, the 2.0 M mixed aqueous solution added to the reaction tank does not contain titanium sulfate, and nickel sulfate, manganese sulfate and cobalt sulfate are combined in a molar ratio of nickel: manganese: cobalt of 0.85:0.10:0.05. Except for this, crystallization is carried out in the same manner as in Example 1B to obtain a filter cake of nickel-manganese-cobalt composite hydroxide obtained after filtration.
[0339] [Coating process]
[0340] The obtained filter cake of nickel-manganese-cobalt composite hydroxide was dispersed in pure water and adjusted to pH 8.2 using sulfuric acid. Niobic acid dissolved in potassium hydroxide solution was then added so that the molar ratio of nickel:manganese:cobalt:niobium became 0.847:0.098:0.050:0.005 to coat the nickel-manganese-cobalt composite hydroxide with niobium compound.
[0341] [Mixture preparation process]
[0342] The obtained nickel-manganese-cobalt-niobium composite hydroxide particles, lithium hydroxide, and titanium oxide (TiO 2 ), except for this, the same mixing as in Example 1B was carried out to obtain a lithium mixture.
[0343] [Firing process]
[0344] The cathode active material was obtained by calcination under the same conditions as in Example 2B and evaluated. Tables 3 and 4 show the production conditions and evaluation results of the cathode active material.
[0345] (Example 2C)
[0346] In the coating step, except that niobic acid dissolved in a potassium hydroxide solution was added so that the molar ratio of nickel:manganese:cobalt:niobium was 0.848:0.097:0.052:0.003, a positive electrode active material was obtained and evaluated in the same manner as in Example 1C. The production conditions and evaluation results of the positive electrode active material are shown in Tables 3 and 4.
[0347] (Comparative Example 1B)
[0348] In the crystallization step, no titanium sulfate aqueous solution was prepared, and in the mixture preparation step, no niobium compound was prepared, and the obtained nickel-manganese-cobalt composite hydroxide particles and lithium hydroxide were weighed so that the mass ratio of lithium: nickel: manganese: cobalt was 1.01:0.85:0.10:0.05, and in the calcination step, the calcination temperature was set to 800° C., and a positive electrode active material was obtained and evaluated in the same manner as in Example 1B. The manufacturing conditions and evaluation results of the positive electrode active material are shown in Tables 3 and 4.
[0349] (Comparative Example 2B)
[0350] In the mixture preparation step, the niobium compound was not prepared, and the obtained nickel-manganese-cobalt-titanium composite hydroxide particles and lithium hydroxide were weighed in a manner such that the mass ratio of lithium: (nickel + manganese + cobalt + titanium) was 1.01:1, and in the sintering step, the sintering temperature was set to 830° C., and the positive electrode active material was obtained and evaluated in the same manner as in Example 1B. The manufacturing conditions and evaluation results of the positive electrode active material are shown in Tables 3 and 4.
[0351] (Comparative Example 3B)
[0352] In the crystallization step, the obtained nickel-manganese-cobalt composite hydroxide particles, lithium hydroxide, and niobic acid (Nb) were weighed so that the mass ratio of lithium: (nickel + manganese + cobalt): niobium was 1.01:0.990:0.010 without preparing a titanium sulfate aqueous solution. 2 O5 ·4H 2 O), and in the calcination step, the calcination temperature was set to 850° C. A positive electrode active material was obtained and evaluated in the same manner as in Example 1B. The production conditions and evaluation results of the positive electrode active material are shown in Tables 3 and 4.
[0353] (Comparative Example 4B)
[0354] In the mixture preparation step, the obtained nickel-manganese-cobalt-titanium composite hydroxide particles, lithium hydroxide and niobic acid (Nb) were weighed so that the mass ratio of lithium: (nickel + manganese + cobalt + titanium): niobium was 1.01:0.999:0.001. 2 O 5 ·4H 2 O), and in the calcination step, the calcination temperature was set to 840° C. A positive electrode active material was obtained and evaluated in the same manner as in Example 1B. The production conditions and evaluation results of the positive electrode active material are shown in Tables 3 and 4.
[0355] [Table 3]
[0356]
[0357] [Table 4]
[0358]
[0359] (Evaluation result 1)
[0360] As shown in Tables 1 to 4 and Figure 1 , 2 As shown in the figure, the volume resistivity of the positive electrode active material obtained in the example when compressed is 5×10 2 Ω·cm or more, and the maximum oxygen generation peak temperature is 250°C or more, indicating that it has high thermal stability and suppresses oxygen release during overcharge.
[0361] In addition, as shown in Tables 1 to 4, Figure 3 As shown, in Examples 1A to 5A, 1B to 5B, 1C, and 2C, which were sintered in an atmosphere with an oxygen concentration of 80 vol %, a positive electrode active material having a high discharge capacity of more than 184 mAh / g and a high battery capacity while having high thermal stability was obtained.
[0362] Fig.17 (A) Fig.18 (A) is a diagram showing a cross-sectional photograph of a positive electrode active material. The portion surrounded by a square in these diagrams shows an example of a position used in the analysis, and the concentration (atomic %) of each element in the portion surrounded by the square is analyzed by point analysis using STEM-EDX. Fig.17 (B) Fig.17 (C) and Fig.18 (B) Fig.18 (C) shows the interior of the primary particles in the cross section of the positive electrode active materials obtained in Examples 2A and 2B by point analysis using STEM-EDX ( Fig.17 (B): Example 2A, Fig.17 (C): Example 2B) and grain boundaries ( Fig.18 (B): Example 2B, Fig.18 (B) is a diagram showing an example of the results of evaluating the composition of Example 2B).
[0363] like Fig.17 (B) Fig.17 (C) and Fig.18 (B) Fig.18 As shown in (C), in the positive electrode active material obtained in the embodiment, niobium segregates at the grain boundaries between the primary particles. In addition, as shown in Tables 2 and 4, the niobium concentration at the grain boundaries between the primary particles is 1.3 times or more relative to the niobium concentration inside the primary particles (niobium concentration at the grain boundaries / niobium concentration inside the particles). In addition, for titanium, no segregation at the grain boundaries between the primary particles was confirmed, and the titanium concentration at the grain boundaries between the primary particles was less than 1.3 times (specifically, 0.8 times or more and 1.1 times or less) relative to the titanium concentration inside the primary particles (titanium concentration at the grain boundaries / titanium concentration inside the particles).
[0364] On the other hand, since the positive electrode active materials of Comparative Examples 1A and 1B did not contain titanium and niobium, the volume resistivity and the maximum oxygen generation peak temperature during compression were low, and the thermal stability was insufficient.
[0365] In addition, since the positive electrode active material of Comparative Examples 2A, 3A and 2B, 3B contains only one of titanium or niobium, the maximum oxygen generation peak temperature and the volume resistivity during compression are slightly higher than those of Comparative Example 1, but lower than those of the embodiment, and it cannot be said that the thermal stability during short circuit is sufficient.
[0366] In addition, in the positive electrode active materials of Comparative Examples 4A and 4B, since the niobium content was 0.001 or less, the volume resistivity and the maximum oxygen generation peak temperature during compression were low, and the thermal stability was insufficient.
[0367] Hereinafter, Examples 11A to 11C in which the water washing step and the drying step were performed will be described.
[0368] [Example 11A]
[0369] Relative to 150 parts by mass of lithium nickel manganese cobalt titanium composite oxide obtained under the same conditions as in Example 2A, water is mixed in a ratio of 100 parts by mass, and after stirring with water, suction filtration is performed using a Nutsche filter to obtain a precipitate (water washing process). The obtained precipitate is placed in a SUS container, heated to 100°C using a vacuum dryer and left to dry for 12 hours, and heated to 190°C and left to dry for 10 hours to obtain a positive electrode active material (drying process). The manufacturing conditions and evaluation results of the positive electrode active material are shown in Tables 5 to 7. It should be noted that the manufacturing conditions and evaluation results of the positive electrode active materials of Example 2A and Comparative Examples 1A to 4A are shown together as references in Tables 5 to 7.
[0370] [Table 5]
[0371]
[0372] [Table 6]
[0373]
[0374] [Table 7]
[0375]
[0376] (Example 7B)
[0377] [Crystallization process]
[0378] A predetermined amount of pure water was added to the reaction tank (60 L), and the temperature in the tank was set at 49°C while stirring. At this time, N 2 Gas was added to make the dissolved oxygen concentration in the reaction tank liquid 0.8 mg / L. Into the reaction tank, a 2.0 M mixed aqueous solution of nickel sulfate, manganese sulfate, cobalt sulfate, and titanium sulfate in a molar ratio of nickel:manganese:cobalt:titanium of 0.829:0.098:0.050:0.023, a 25 mass % sodium hydroxide solution as an alkaline solution, and a 25 mass % ammonia water as a complexing agent were simultaneously and continuously added to the reaction tank, and crystallization was performed by a continuous crystallization method.
[0379] At this time, the flow rate is controlled in such a way that the residence time of the mixed aqueous solution becomes 8 hours, the pH in the reaction tank is adjusted to 12.0-12.6, and the ammonia concentration is adjusted to 10-14 g / L. After the reaction tank is stabilized, the slurry containing the nickel-manganese-cobalt-titanium composite hydroxide is recovered from the overflow port and filtered to obtain a filter cake of the nickel-manganese-cobalt-titanium composite hydroxide. 140 g of the nickel-manganese-cobalt-titanium composite hydroxide in the filtered filter cloth is passed through 1 L of pure water to clean the impurities. The filtered powder is dried to obtain particles of nickel-manganese-cobalt-titanium composite hydroxide containing titanium, wherein the mass ratio of nickel, manganese, cobalt and titanium is represented by Ni:Mn:Co:Ti=0.829:0.098:0.050:0.023.
[0380] [Mixture preparation process]
[0381] The obtained nickel-manganese-cobalt-titanium composite hydroxide particles containing titanium, lithium hydroxide and niobic acid (Nb) were weighed so that the mass ratio of lithium: (nickel + manganese + cobalt + titanium): niobium was 1.01:0.995:0.005. 2 O 5 ·4H 2 O), and then the mixture was thoroughly mixed using a vibration mixer (TURBULA T2C model manufactured by Willy A Bachofen (WAB)) to obtain a lithium mixture.
[0382] [Firing process]
[0383] The obtained lithium mixture was calcined in a gas flow of oxygen (oxygen concentration: 90 volume %) at 870° C. for 10 hours and then crushed to obtain particles of lithium nickel manganese cobalt composite oxide (positive electrode active material).
[0384] [evaluate]
[0385] The production conditions of the positive electrode active material are shown in Table 8, and the evaluation results of the obtained positive electrode active material are shown in Tables 9 and 10. In addition, the 4.0 g / cm 3 The volume resistivity when compressed is 3.5×10 3 (Ω·cm).
[0386] (Example 11B)
[0387] Relative to 150 parts by mass of lithium nickel manganese cobalt titanium composite oxide obtained under the same conditions as Example 7B, water was mixed in a ratio of 100 parts by mass, and after stirring with water, suction filtration was performed using a Nutsche filter to obtain a precipitate (water washing process). The obtained precipitate was placed in a SUS container, heated to 100°C using a vacuum dryer and left to dry for 12 hours, and heated to 190°C and left to dry for 10 hours, thereby obtaining a positive electrode active material (drying process). The manufacturing conditions and evaluation results of the positive electrode active material are shown in Tables 8 to 10.
[0388] (Example 11C)
[0389] [Crystallization process]
[0390] In the crystallization process, the 2.0M mixed aqueous solution added to the reaction tank does not contain titanium sulfate, and nickel sulfate, manganese sulfate and cobalt sulfate are combined in a molar ratio of nickel:manganese:cobalt of 0.85:0.10:0.05. Except for this, the crystallization process is carried out in the same manner as Example 11B to obtain a filter cake of nickel-manganese-cobalt composite hydroxide obtained after filtration.
[0391] [Coating process]
[0392] The obtained filter cake of nickel-manganese-cobalt composite hydroxide was dispersed in pure water, and after adjusting the pH to 8.2 using sulfuric acid, niobic acid dissolved in a potassium hydroxide solution was added so that the molar ratio of nickel:manganese:cobalt:niobium became 0.845:0.100:0.050:0.005, thereby coating the nickel-manganese-cobalt composite hydroxide with a niobium compound.
[0393] [Mixture preparation process]
[0394] The obtained nickel-manganese-cobalt-niobium composite hydroxide particles, lithium hydroxide, and titanium oxide (TiO 2 ), except for this, the same mixing as in Example 11B was carried out to obtain a lithium mixture.
[0395] [Firing process]
[0396] The cathode active material was obtained by calcination, water washing and drying under the same conditions as in Example 11B and evaluated. The production conditions and evaluation results of the cathode active material are shown in Tables 8 to 10.
[0397] (Comparative Example 5B)
[0398] The positive electrode active material was obtained and evaluated in the same manner as in Example 7B except that the titanium sulfate aqueous solution was not prepared in the crystallization step, the niobium compound was not prepared in the mixture preparation step, and the obtained nickel-manganese-cobalt composite hydroxide particles and lithium hydroxide were weighed in a manner such that the mass ratio of lithium: nickel: manganese: cobalt was 1.02:0.85:0.10:0.05, and the calcination temperature was set to 800°C in the calcination step. The obtained positive electrode active material was compressed to 4.0 g / cm 3 The volume resistivity is 8.5×10 1 Tables 8 and 9 show the production conditions and evaluation results of the positive electrode active material.
[0399] (Comparative Example 6B)
[0400] In the mixture preparation step, the obtained nickel-manganese-cobalt composite hydroxide particles containing titanium and lithium hydroxide were weighed in a manner such that the mass ratio of lithium: (nickel + manganese + cobalt + titanium) was 1.02:1 without preparing a niobium compound, and in the sintering step, the sintering temperature was set to 830° C., and a positive electrode active material was obtained and evaluated in the same manner as in Example 7B. The obtained positive electrode active material was compressed to 4.0 g / cm 3 The volume resistivity is 2.1×10 2 The production conditions and evaluation results of the positive electrode active material are shown in Tables 8 and 9.
[0401] (Comparative Example 7B)
[0402] In the crystallization step, the obtained nickel-manganese-cobalt composite hydroxide particles, lithium hydroxide and niobic acid (Nb) were weighed so that the mass ratio of lithium: (nickel + manganese + cobalt): niobium was 1.01:0.991:0.009 without preparing a titanium sulfate aqueous solution. 2 O 5 ·4H 2 O), and in the calcination step, the calcination temperature was set to 850°C. A positive electrode active material was obtained and evaluated in the same manner as in Example 7B. The obtained positive electrode active material was compressed to 4.0 g / cm 3 The volume resistivity is 3.4×10 2 The production conditions and evaluation results of the positive electrode active material are shown in Tables 8 and 9.
[0403] (Comparative Example 8B)
[0404] In the mixture preparation step, the obtained particles of the nickel-manganese-cobalt composite hydroxide containing titanium, lithium hydroxide and niobic acid (Nb) were weighed so that the mass ratio of lithium: (nickel + manganese + cobalt + titanium): niobium was 1.01:0.999:0.001. 2 O 5·4H 2 O), and in the calcination step, the calcination temperature was set to 840°C. A positive electrode active material was obtained and evaluated in the same manner as in Example 7B. The obtained positive electrode active material was compressed to 4.0 g / cm 3 The volume resistivity is 3.3×10 2 The production conditions and evaluation results of the positive electrode active material are shown in Tables 8 and 9.
[0405] [Table 8]
[0406]
[0407] [Table 9]
[0408]
[0409] [Table 10]
[0410]
[0411] (Evaluation result 2)
[0412] As shown in Tables 6, 9 and Figure 4 As shown, the maximum oxygen generation peak temperature of the positive electrode active materials obtained in Examples 11A to 11C was 250° C. or higher, indicating that they had high thermal stability and could suppress oxygen release during overcharge.
[0413] In addition, as shown in Tables 6, 9 and Figure 5 As shown, compared with Examples 2A and 7B which were not washed and dried, Examples 11A and 11B which were washed and dried had a high discharge capacity and a positive electrode active material having high thermal stability and a higher battery capacity.
[0414] In addition, as shown in Tables 7 and 10, in Examples 2A and 7B where water washing and drying were not performed, the amount of eluted lithium was greater than 0.20 mass %, while in Examples 11A, 11B, and 11C, the amount of eluted lithium was less than 0.20 mass %, indicating a decrease in excess lithium.
[0415] On the other hand, since the positive electrode active materials of Comparative Examples 1A and 5B did not contain titanium and niobium, the maximum oxygen generation peak temperature was low and the thermal stability was insufficient.
[0416] In addition, in the positive electrode active materials of Comparative Examples 4A and 8B, since the niobium content was 0.001 or less, the maximum oxygen generation peak temperature was low and the thermal stability was insufficient.
[0417] Industrial Applicability
[0418] In this embodiment, a positive electrode active material for a lithium ion secondary battery having high thermal stability and excellent battery characteristics can be obtained by an industrial manufacturing method. The lithium ion secondary battery is suitable for power sources of small portable electronic devices (notebook personal computers, mobile terminals, etc.) that always require high capacity.
[0419] In addition, the secondary battery using the positive electrode active material of this embodiment has excellent thermal stability and capacity compared with the battery using the positive electrode active material of the conventional lithium nickel oxide, and is therefore suitable as a power source for electric vehicles with limited mounting space because it can be miniaturized.
[0420] Furthermore, the secondary battery using the positive electrode active material of this embodiment can be used not only as a power source for electric vehicles driven purely by electric energy, but also as a power source for so-called hybrid vehicles used in conjunction with a combustion mechanism such as a gasoline engine or a diesel engine, or as a stationary storage battery.
[0421] It should be noted that the technical scope of the present invention is not limited to the forms described in the above-mentioned embodiments, etc. Sometimes one or more of the elements described in the above-mentioned embodiments, etc. may be omitted. In addition, the elements described in the above-mentioned embodiments, etc. may be appropriately combined. In addition, within the scope permitted by law, Japanese Patent Application Nos. 2019-127259, 2019-236895, 2020-092692, 2019-127258, 2019-236896, 2020-092693, and all the contents of the documents cited in this specification are cited as part of the record of this article.
[0422] Explanation of symbols
[0423] CBA…Button type battery (for evaluation)
[0424] PE…Positive electrode (evaluation electrode)
[0425] NE…Negative electrode
[0426] SE…Diaphragm
[0427] GA...washer
[0428] WW...Wave Washer
[0429] PC…positive electrode shell
[0430] NC…Negative electrode shell
[0431] G…Gap.
Claims
1. A method for producing a positive electrode active material for a lithium ion secondary battery, comprising a mixture preparation step and a calcination step, The positive electrode active material for a lithium ion secondary battery includes a lithium nickel manganese composite oxide having a hexagonal layered structure and composed of secondary particles formed by agglomeration of a plurality of primary particles. In the mixture preparation step, a mixture is prepared that contains at least a nickel-manganese composite compound and a lithium compound and optionally contains one or both of a titanium compound and a niobium compound. In the calcining step, the mixture is calcined at 750° C. to 1000° C. to obtain the lithium nickel manganese composite oxide. The nickel-manganese composite compound contains nickel (Ni) and manganese (Mn), and optionally contains at least one element selected from the group consisting of Co, V, Mg, Mo, Ca, Cr, Ta, Na, W, Fe, Zn, B, Si, P, Zr and Al, namely, element M (M), titanium (Ti) and niobium (Nb), and the amount ratio of each of the elements is represented by Ni:Mn:M:Ti:Nb=(1-xy):x:y:z':w', wherein, 0.03≤x≤0.30, 0≤y≤0.30, 0≤z'≤0.05, 0≤w'≤0.03, In the mixture, the mass ratio z of titanium and the mass ratio w of niobium relative to the total mass of nickel, manganese, element M, titanium and niobium satisfy 0.005≤z≤0.05, 0.001<w≤0.03, (z+w)≤0.06 and z>w, At least a portion of niobium in the lithium nickel manganese composite oxide is segregated at the grain boundaries between the primary particles.
2. A method for producing a positive electrode active material for a lithium ion secondary battery, comprising a mixture preparation step and a calcination step, The positive electrode active material for a lithium ion secondary battery includes a lithium nickel manganese composite oxide having a hexagonal layered structure and composed of secondary particles formed by agglomeration of a plurality of primary particles. In the mixture preparation step, at least a nickel-manganese composite compound, a titanium compound, a niobium compound and a lithium compound are mixed to prepare a mixture. In the calcining step, the mixture is calcined at 750° C. to 1000° C. to obtain the lithium nickel manganese composite oxide. The nickel-manganese composite compound contains nickel (Ni) and manganese (Mn), and optionally contains at least one element selected from the group consisting of Co, V, Mg, Mo, Ca, Cr, Ta, Na, W, Fe, Zn, B, Si, P, Zr and Al, i.e., element M (M), wherein the amount ratio of each of the elements is represented by Ni:Mn:M=(1-xy):x:y, wherein: 0.03≤x≤0.30, 0≤y≤0.30, In the mixture, the mass ratio z of titanium and the mass ratio w of niobium relative to the total mass of nickel, manganese, element M, titanium and niobium satisfy 0.005≤z≤0.05, 0.001<w≤0.03, (z+w)≤0.06 and z>w, At least a portion of niobium in the lithium nickel manganese composite oxide is segregated at the grain boundaries between the primary particles.
3. The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 1 or 2, comprising a water washing step and a drying step. In the water washing step, water is mixed in a ratio of 50 parts by weight to 200 parts by weight relative to 150 parts by weight of the lithium nickel manganese composite oxide obtained after calcination, and the mixture is stirred and then solid-liquid separation is performed. In the drying step, the lithium nickel manganese composite oxide after washing is dried.
4. The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 1 or 2, wherein in the mixture, the mass ratio z of titanium and the mass ratio w of niobium relative to the total mass of nickel, manganese, element M, titanium and niobium satisfy 0.005≤z≤0.05, 0.002≤w≤0.03, (z+w)≤0.06 and z>w.
5. The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 1, wherein in the mixture preparation step, at least a titanium-containing nickel-manganese composite compound, a niobium compound and a lithium compound are mixed, The titanium-containing nickel-manganese composite compound contains nickel (Ni), manganese (Mn) and titanium (Ti), and optionally contains at least one element selected from the group consisting of Co, V, Mg, Mo, Ca, Cr, Ta, Na, W, Fe, Zn, B, Si, P, Zr and Al, that is, element M (M), and the amount ratio of each of the elements is represented by Ni:Mn:M:Ti=(1-xy-z'):x:y:z', wherein, 0.03≤x≤0.30, 0≤y≤0.30, 0.005≤z'≤0.
05. 6 . The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 5 , wherein the titanium-containing nickel-manganese composite compound is obtained by crystallization. 7 . The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 5 , wherein the titanium-containing nickel-manganese composite compound is obtained by coating a titanium-containing compound on a nickel-manganese composite compound obtained by crystallization.
8. The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 1, wherein in the mixture preparation step, at least a nickel-manganese composite compound containing niobium, a lithium compound and a titanium compound are mixed, The niobium-containing nickel-manganese composite compound contains nickel (Ni), manganese (Mn) and niobium (Nb), and optionally contains at least one element selected from the group consisting of Co, V, Mg, Mo, Ca, Cr, Ta, Na, W, Fe, Zn, B, Si, P, Zr and Al, that is, an element M (M), and the amount ratio of each of the elements is represented by Ni:Mn:M:Nb=(1-xy):x:y:w', wherein, 0.03≤x≤0.30, 0≤y≤0.30, 0.001<w'≤0.
03. 9 . The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 8 , wherein the niobium-containing nickel-manganese composite compound is obtained by coating a niobium-containing compound on a nickel-manganese composite compound obtained by crystallization.
10. The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 8, wherein the amount ratio of the elements in the niobium-containing nickel-manganese composite compound is represented by Ni:Mn:M:Nb=(1-xy):x:y:w', wherein: 0.03≤x≤0.30, 0≤y≤0.30, 0.002≤w'≤0.
03. 11 . The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 1 , wherein the calcination step is performed in an atmosphere having an oxygen concentration of 80% by volume or more and 100% by volume or less. 12 . The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 1 , wherein the titanium in the lithium nickel manganese composite oxide is present inside the primary particles. 13 . The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 1 , wherein the titanium compound is titanium oxide. 14 . The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 1 , wherein the niobium compound is niobium oxide, niobic acid or a mixture thereof.
15. The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 1 or 2, wherein the lithium nickel manganese composite oxide obtained after sintering has a compression resistance of 4.0 g / cm2 as determined by powder resistance measurement. 3 The volume resistivity is 5.0×10 2 Ω·cm or more 1.0×10 5 Ω·cm or less.