Amino acid derivative-based electrolytes and their applications in flow batteries
By developing new phenazine, quinone, phenothiazine and thionine amino acid derivative electrolytes as aqueous flow battery energy storage materials, the geographical limitations and low efficiency problems of existing energy storage technology have been solved, and high efficiency has been achieved. , environmentally friendly energy storage effect.
Patent Information
- Application Number
- CN202110185442.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-02-10
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-02-10
AI Technical Summary
Existing large-scale energy storage technologies such as pumped hydro energy storage, compressed air energy storage and non-aqueous flow batteries have geographical limitations, low efficiency, environmental pollution and safety hazards, making it difficult to meet the storage needs of clean energy.
Develop a new type of phenazine, quinone, phenothiazine and thionine amino acid derivative electrolyte as an energy storage material for aqueous flow batteries. It is prepared through a specific synthesis method and used in flow battery energy storage systems. .
It achieves high cycle stability and excellent energy efficiency of flow battery energy storage materials, which is suitable for large-scale energy storage power stations and reduces environmental pollution and resource waste.
Smart Images

Figure CN114105893B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of liquid flow battery energy storage, and specifically relates to a synthesis method of several phenazine, quinone, phenothiazine and thione electrolytes of amino acid derivatives with redox activity, and their application in aqueous liquid flow battery energy storage systems. Background Art
[0002] The rapid consumption of traditional energy (such as oil and coal) and the serious environmental pollution it brings urgently require us to use cleaner energy to reduce pollution to the environment. With the development of science and technology, the cost of clean energy such as solar energy and wind energy is lower than that of traditional energy. However, these two clean energy sources have strong volatility and intermittency, and have high requirements for the surrounding environment. However, the demand for electricity in human daily production activities is very regular, so the intermittency and volatility of clean energy hinder their large-scale application in the power grid. This contradiction between supply and demand requires us to develop a large-scale energy storage technology to regulate the peak and trough of electricity consumption, that is, to store energy when electricity consumption is low and output energy when it is peak, to provide support and guarantee for the stability of the power grid. Through such regulation, the waste of resources is reduced, clean energy is properly stored and utilized, and it is transformed from low-value, unplanned energy to high-value, reliable products.
[0003] Existing large-scale energy storage technologies include pumped storage, compressed air storage, electrochemical storage (secondary batteries), supercapacitor storage, and flywheel storage. Among all the above energy storage technologies, the first three have a long enough discharge time and a large enough capacity range to be used to store solar and wind energy. Pumped storage requires the construction of two huge reservoirs at different altitudes. It is a large-scale project restricted by special geographical conditions and may be accompanied by ecological problems, making it difficult to promote in many places. Compressed air storage is a storage method that uses electricity to compress air, seals the compressed high-pressure air in a gas storage facility, and releases the compressed air to generate electricity when needed. Therefore, special geographical conditions such as rock caves and abandoned mines are also required as large gas storage chambers. In addition, part of the energy is converted into heat energy during the air compression and release process, resulting in low efficiency of this technology. In contrast, electrochemical energy storage has attracted widespread attention due to its advantages such as environmental friendliness, high energy efficiency, low maintenance cost, adjustable properties, and no geographical restrictions. Among them, flow batteries are one of the most promising energy storage methods in flow batteries due to their rich electrolyte reserve options.
[0004] According to the type of solvent used in the electrolyte, flow batteries are divided into aqueous flow batteries and non-aqueous (organic solvent) flow batteries. The organic solvents used in non-aqueous flow batteries are toxic to a certain extent, their cost is much higher than water, and they may cause pollution to the environment; the safety hazards caused by the flammability and explosiveness of organic solvents also make non-aqueous flow batteries unsuitable for large-scale energy storage power stations. It can be seen that aqueous flow batteries have greater application prospects and application potential worthy of large-scale promotion. Among them, aqueous flow batteries that use organic matter as energy storage materials are the current research hotspot because of their wide sources of energy storage materials and the ability to modify and functionalize organic molecules using chemical means.
[0005] In summary, there is an urgent need to develop new organic energy storage materials in this field. Summary of the invention
[0006] The purpose of the invention is to develop a novel organic energy storage material.
[0007] The first aspect of the present invention provides a compound represented by the following formula (I):
[0008]
[0009] wherein Y and Z are each independently selected from the group consisting of N, NH, C═O or S;
[0010] Dashed lines are chemical bonds or do not exist;
[0011] m1 and m2 are selected from the following group: 0, 1, 2, 3 or 4;
[0012] p1 and p2 are selected from the following group: 0, 1, 2, 3 or 4;
[0013] Each R is independently selected from the following group: halogen, substituted or unsubstituted C1-C10 alkyl, cycloalkyl, heterocycloalkyl, substituted or unsubstituted C6-C10 aryl, hydroxyl, thiol group, amine group, carboxyl group, phosphoric acid group, sulfonic acid group or the following groups:
[0014]
[0015] R 0 Selected from the following group: -COOX, -SO3X, -PO3H2, -NH2, -NHCH3, -N(CH3)2, -N + (CH3)3M - ; wherein X is selected from the following group: H + NH4 + , Li + 、Na + , K + Mg 2+ 、Al 3+, Ca 2+ ; M is selected from the group consisting of F, Cl, Br or I; each Rg is independently a functional group; wherein the functional group is in:
[0016] Ra and Rb are each independently selected from the following group: H, substituted or unsubstituted C1-C10 alkyl, cycloalkyl, heterocycloalkyl, substituted or unsubstituted C6-C10 aryl, or Ra and Rb together form a substituted or unsubstituted 3-8-membered nitrogen-containing heterocyclic ring or nitrogen-containing heteroaromatic ring; and the Rg includes at least one R 0 Substituents;
[0017] Unless otherwise specified, the substitution refers to that one or more hydrogen atoms on the group are replaced by a substituent selected from the following group: halogen, C1-C10 alkyl, cycloalkyl, heterocycloalkyl, C6-C10 aryl, hydroxyl, thiol group, amine group, carboxyl group, phosphate group, sulfonic acid group.
[0018] In another preferred embodiment, the compound has a structure shown by the following formula (Ia), formula (Ib), formula (Ic) or formula (Id):
[0019]
[0020] Among them, R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 Each is independently selected from the following group: H, halogen, substituted or unsubstituted C1-C10 alkyl, cycloalkyl, heterocycloalkyl, substituted or unsubstituted C6-C10 aryl, hydroxyl, thiol group, amine group, carboxyl group, phosphate group, sulfonic acid group, or functional group;
[0021] The limiting condition is that R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 The compound comprises at least one functional group.
[0022] In another preferred embodiment, R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R8 Each is independently selected from the following group: H, substituted or unsubstituted C1-C10 alkyl, cycloalkyl, heterocycloalkyl, or functionalized group; wherein the functionalized group is a group selected from the following group:
[0023]
[0024] Among them, each X, X 1 and X 2 Each independently selected from the following group: H, NH4 + , Li + 、Na + , K + Mg 2+ 、Al 3+ , Ca 2+ ;
[0025] R 9 , R 10 and R 11 Each is independently selected from the following group: H, substituted or unsubstituted C1-C10 alkyl, cycloalkyl, heterocycloalkyl, or substituted or unsubstituted C6-C10 aryl;
[0026] n is 1, 2, 3, 4, 5, 6, 7 or 8;
[0027] C1 is a substituted or unsubstituted 3-8 membered heterocyclic ring (including partially unsaturated or saturated ring), or a substituted or unsubstituted 5-8 membered heteroaromatic ring.
[0028] In another preferred embodiment, the Ra and Rb are independently selected from the following group: H, substituted or unsubstituted C1-C10 alkyl, cycloalkyl, heterocycloalkyl, and the Rg includes at least one R 0 Substituent.
[0029] In another preferred embodiment, the R 9 , R 10 and R 11 Each is independently selected from the following group: H, substituted or unsubstituted C1-C10 alkyl, cycloalkyl, heterocycloalkyl.
[0030] In another preferred embodiment, the compound is selected from the following group:
[0031]
[0032] The second aspect of the present invention provides a method for preparing the compound according to the first aspect of the present invention, wherein the method comprises the steps of:
[0033]
[0034] (i) reacting a compound of formula (II) with RgH in an inert solvent to obtain a compound of formula (I);
[0035] Or the method comprises the steps of:
[0036]
[0037] (1) reacting a compound of formula (III) with CH2=CHCOOEt in an inert solvent to obtain a compound of formula (IIIa);
[0038]
[0039] (2) reducing the compound of formula (IIIa) under a hydrogen atmosphere to obtain a compound of formula (IIIb);
[0040]
[0041] (3) hydrolyzing and deprotecting the compound of formula (IIIb) to obtain a compound of formula (I-1);
[0042] Wherein, M is F, Cl, Br or I.
[0043] In another preferred embodiment, in the step (i), the method is carried out in the presence of a palladium catalyst, a ligand and a base; preferably, the palladium catalyst is Pd2(dba)3, and the base is t BuOK or Cs2CO3, and the ligand is selected from the group consisting of BrettPhos, RuPhos, XPhos or Pd2(dba)3;
[0044] In another preferred embodiment, in the step (1), the reaction is carried out in the presence of a palladium catalyst, a ligand, a base and a catalyst; preferably, the palladium catalyst is PdCl2, the base is potassium carbonate, the ligand is P(o-Tol)3, and the catalyst is Bu4NBr.
[0045] In another preferred embodiment, in the step (2), the reaction is carried out in the presence of palladium / carbon.
[0046] In another preferred embodiment, in the step (3), the reaction is carried out in the presence of a base; preferably, the base is NaOH.
[0047] In another preferred embodiment, in the step (i), the inert solvent is selected from the group consisting of tert-butanol, n-butanol, toluene, or a combination thereof.
[0048] In another preferred embodiment, in the step (1), the inert solvent is selected from the following group: DMF, water, or a combination thereof.
[0049] In another preferred embodiment, in the step (2), the inert solvent is selected from the following group: ethyl acetate.
[0050] In another preferred embodiment, in the step (2), the inert solvent is selected from the following group: methanol, water, or a combination thereof.
[0051] In another preferred embodiment, the method further comprises: after the reaction is completed, filtering and collecting the filter cake, dissolving the filter cake with deionized water and filtering again to remove insoluble impurities in the water, collecting the filtrate, acidifying the filtrate with HCl to pH=3-4, and filtering after the solid precipitates.
[0052] In another preferred embodiment, the method further comprises: after the reaction is completed, purifying the product using a reverse phase column.
[0053] The third aspect of the present invention provides a liquid flow battery energy storage material, characterized in that the liquid flow battery energy storage material is prepared using the compound described in the first aspect of the present invention as an active ingredient.
[0054] A fourth aspect of the present invention provides a liquid flow battery, wherein the liquid flow battery comprises the compound as described in the first aspect of the present invention as an energy storage material.
[0055] In another preferred embodiment, in the liquid flow battery, the compound as described in the first aspect of the present invention is used as the negative electrode or positive electrode solution.
[0056] It should be understood that within the scope of the present invention, the above-mentioned technical features of the present invention and the technical features specifically described below (such as embodiments) can be combined with each other to form a new or preferred technical solution. Due to space limitations, they will not be described one by one here. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Figure 1 For compound 3 1 H NMR spectra;
[0058] Figure 2 For compound 3 13 C NMR spectra;
[0059] Figure 3 For compound 5 1 H NMR spectra;
[0060] Figure 4 For compound 5 13 C NMR spectra;
[0061] Figure 5 For compound 7 1 H NMR spectra;
[0062] Figure 6 For compound 7 13 C NMR spectra;
[0063] Figure 7 For compound 9 1 H NMR spectra;
[0064] Figure 8 For compound 9 13 C NMR spectra;
[0065] Fig. 9 For compound 11 1 H NMR spectra;
[0066] Fig.10 For compound 11 13 C NMR spectra;
[0067] Fig.11 For compound 13 1 H NMR spectra;
[0068] Fig.12 For compound 13 13 C NMR spectra;
[0069] Fig.13 For compound 14 1 H NMR spectra;
[0070] Fig.14 For compound 14 13 C NMR spectra;
[0071] Fig.15 For compound 15 1 H NMR spectra;
[0072] Fig.16 For compound 15 13 C NMR spectra;
[0073] Fig.17 For compound 16 1 H NMR spectra;
[0074] Fig.18 For compound 16 13 C NMR spectra;
[0075] Fig.19 For compound 19 1 H NMR spectra;
[0076] Fig. 20 For compound 20 1 H NMR spectra;
[0077] Fig.21For compound 21 1 H NMR spectra;
[0078] Fig. 22 For compound 22 1 H NMR spectra;
[0079] Fig.23 is the cyclic voltammogram of compound 15 in 1 M KCl solution;
[0080] Fig.24 The main parameters and schematic diagram of the flow battery device are shown below;
[0081] Fig.25 Schematic diagram showing the changes in battery capacity, current efficiency, and energy efficiency of compound 15 as an energy storage material with the number of battery cycles;
[0082] Fig.26 A schematic diagram showing the relationship between battery capacity and voltage change at different battery cycle times when compound 15 is used as an energy storage material;
[0083] Fig. 27 is the cyclic voltammogram of compound 3 in 1 M KCl solution;
[0084] Fig.28 is the cyclic voltammogram of compound 5 in 1 M KCl solution;
[0085] Fig.29 is the cyclic voltammogram of compound 7 in 1 M KCl solution;
[0086] Fig.30 is the cyclic voltammogram of compound 9 in 1 M KCl solution;
[0087] Fig.31 is the cyclic voltammogram of compound 11 in 1 M KCl solution;
[0088] Fig.32 is the cyclic voltammogram of compound 13 in 1 M KCl solution;
[0089] Fig.33 is the cyclic voltammogram of compound 14 in 1 M KCl solution;
[0090] Fig.34 is the cyclic voltammogram of compound 16 in 1 M KCl solution;
[0091] Fig.35 For compound 22 1 H NMR spectra;
[0092] Fig.36 For compound 23 1H NMR spectra;
[0093] Fig.37 For compound 24 1 H NMR spectra;
[0094] Fig.38 For compound 25 1 H NMR diagram
[0095] Fig.39 For compound 26 1 H NMR spectra;
[0096] Fig.40 is the cyclic voltammogram of compound 21 in 1M KCl solution;
[0097] Fig.41 is the cyclic voltammogram of compound 22 in 1M KCl solution;
[0098] Fig.42 is the cyclic voltammogram of compound 23 in 1M KCl solution;
[0099] Fig.43 is the cyclic voltammogram of compound 24 in 1M KCl solution;
[0100] Fig.44 is the cyclic voltammogram of compound 25 in 1M KCl solution;
[0101] Fig.45 is the cyclic voltammogram of compound 26 in 1M KCl solution;
[0102] Fig.46 and 47 The charge-discharge cycle test results of compound 22 in 1M KCl solution;
[0103] Fig.48 and 49 The charge-discharge cycle test results of compound 24 in 1M KCl solution;
[0104] Fig.50 and 51 The charge-discharge cycle test results of compound 25 in 1M KCl solution;
[0105] Fig.52 and 53 The charge-discharge cycle test results of compound 26 in 1M KCl solution. DETAILED DESCRIPTION
[0106] After long-term and in-depth research, the inventors have developed a compound that can be used as an energy storage material for aqueous liquid flow batteries. The preparation method of the compound is simple, and the prepared battery energy storage material has good cycle stability and energy efficiency. Based on the above findings, the inventors have completed the present invention.
[0107] the term
[0108] In the present invention, the halogen is F, Cl, Br or I.
[0109] In the present invention, the term "C1-C10" refers to having 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 carbon atoms, "C3-C6" refers to having 3, 4, 5 or 6 carbon atoms, and so on.
[0110] In the present invention, the term "alkyl" refers to a saturated linear or branched hydrocarbon moiety. For example, the term "C1-C10 alkyl" refers to a straight or branched alkyl group having 1 to 10 carbon atoms, including but not limited to methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl and hexyl, etc.; preferably ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl and tert-butyl.
[0111] In the present invention, the term "aryl" or "aromatic ring" refers to a hydrocarbon moiety containing one or more aromatic rings. Examples of aryl groups include, but are not limited to, phenyl (Ph), naphthyl, pyrenyl, fluorenyl, anthracenyl, and phenanthrenyl.
[0112] In the present invention, the term "heteroaryl" refers to a moiety containing one or more aromatic rings having at least one heteroatom, such as N, O or S. Examples of heteroaryl groups include furanyl, pyrrolyl, thienyl, oxazolyl, imidazolyl, thiazolyl, pyridyl, pyrimidinyl, quinazolinyl, quinolyl, isoquinolyl and indolyl, etc.
[0113] Flow Battery
[0114] In a flow battery, the positive and negative electrolytes are stored in external storage tanks respectively and transported to the battery stack through a peristaltic pump. The active substances undergo redox reactions on the electrode surface to achieve energy storage and release. Compared with traditional chemical batteries such as lithium-ion batteries, flow batteries have the advantage that energy and power are independent of each other, that is, the energy depends on the concentration and volume of the energy storage material, while the power depends on the electrode area. When the scale of energy storage is larger, the cost of this technology is closer to the cost of the energy storage material, so although lithium-ion batteries have a higher energy density, flow batteries are more suitable for large-scale energy storage power stations. According to the type of solvent used in the electrolyte, flow batteries are divided into aqueous flow batteries and non-aqueous (organic solvent) flow batteries.
[0115] Aqueous flow batteries are divided into aqueous inorganic flow batteries and aqueous organic flow batteries according to whether the energy storage materials used are inorganic or organic. At present, the most studied and widely used energy storage materials are all inorganic materials. However, the high cost and limited resources of inorganic materials, the easy formation of dendrites during use, and the slow electrochemical reaction rate limit the large-scale application of inorganic flow batteries. Using organic matter as an energy storage material, its source is more extensive than the limited metals stored in the earth's crust, the cost of use is lower, and it can reduce the pollution of heavy metals to the environment. Compared with inorganic materials, organic materials have the advantages of light weight, low price, ductility and plasticity; the electrochemical reaction rate of organic materials is faster, usually 1-2 orders of magnitude higher than that of inorganic metals, without the use of catalysts, and will not form dendrites to damage the diaphragm; at the same time, synthetic chemists can modify and functionalize them at the molecular level, and optimize the solubility and redox potential of organic materials by introducing functional groups, thereby adjusting the energy density and open circuit voltage of the battery. Therefore, studying the structural characteristics, electrochemical properties and possible degradation mechanisms of organic energy storage materials to improve the performance, energy density and life of aqueous organic flow batteries while reducing their costs is of great significance for promoting the application of flow batteries in the field of energy storage, reducing environmental pollution and energy waste, and meeting the demand for electricity in human production activities.
[0116] Flow battery energy storage materials
[0117] The present invention provides a compound that can be used as an organic energy storage material for an aqueous liquid flow battery. Specifically, the compound has a structure shown in the following formula (I):
[0118]
[0119] wherein Y and Z are each independently selected from the group consisting of N, NH, C═O or S;
[0120] Dashed lines are chemical bonds or do not exist;
[0121] m1 and m2 are selected from the following group: 0, 1, 2, 3 or 4;
[0122] p1 and p2 are selected from the following group: 0, 1, 2, 3 or 4;
[0123] Each R is independently selected from the following group: halogen, substituted or unsubstituted C1-C10 alkyl, cycloalkyl, heterocycloalkyl, substituted or unsubstituted C6-C10 aryl, hydroxyl, thiol group, amine group, carboxyl group, phosphoric acid group, sulfonic acid group or the following groups:
[0124]
[0125] R 0Selected from the following group: -COOX, -SO3X, -PO3H2, -NH2, -NHCH3, -N(CH3)2, -N + (CH3)3M - ; wherein X is selected from the following group: H + NH4 + , Li + 、Na + , K + Mg 2+ 、Al 3+ , Ca 2+ ; M is selected from the group consisting of F, Cl, Br or I; each Rg is independently a functional group; wherein the functional group is in:
[0126] Ra and Rb are each independently selected from the following group: H, substituted or unsubstituted C1-C10 alkyl, cycloalkyl, heterocycloalkyl, substituted or unsubstituted C6-C10 aryl, or Ra and Rb together form a substituted or unsubstituted 3-8-membered nitrogen-containing heterocyclic ring or nitrogen-containing heteroaromatic ring; and the Rg includes at least one R 0 Substituent.
[0127] In a preferred embodiment, the compound has the structure shown as each compound prepared in the Examples.
[0128] The compound is dissolved in a solvent and used as a negative electrode or positive electrode solution for assembling a liquid flow battery.
[0129] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually based on conventional conditions or the conditions recommended by the manufacturer. Unless otherwise stated, percentages and parts are calculated by weight.
[0130] Example 1-9 Synthesis of Phenazine Amino Acid Derivatives
[0131]
[0132] Under nitrogen atmosphere, weigh 2,7-dibromophenazine (3mmol, 1.014g), glycine (7.2mmol, 0.54g), Pd2(dba)3 (5mol%, 137.4mg), BrettPhos (10mol%, 161mg), potassium tert-butoxide (15mmol, 1.68g), and 30mL of tert-butanol in a thick-walled pressure-resistant reaction tube. Stir thoroughly and heat to 100°C, react for 12h, and cool to room temperature. Filter and collect the filter cake, dissolve the filter cake in deionized water and filter again to remove insoluble impurities in water. Collect the filtrate, acidify the filtrate with HCl to pH=3-4, filter after solid precipitation, collect the filter cake, wash the filter cake with deionized water (2×5mL), and dry to obtain the target compound 3. Further, purify by reverse phase column (C18) (MeOH:H2O=15:85), with a yield of 92%.
[0133] By using the above general method 1 and replacing the reaction starting materials, the following compound 5-16 was obtained:
[0134]
[0135] The NMR spectra (including hydrogen and carbon spectra) of the above compounds are as follows: Figure 1-Figure 18 shown.
[0136] Example 10 Synthesis of Phenazine Alanine Derivatives
[0137]
[0138] The synthesis steps are as follows:
[0139] Under nitrogen atmosphere, weigh 2,7-dibromophenazine (3mmol, 1.014g), 3,3'-imidodipropionitrile (12mmol, 1.48g), Pd2(dba)3 (5mol%, 137.4mg), BrettPhos (10mol%, 161mg), cesium carbonate (21mmol, 6.842g), 10mL of tert-butanol in a reaction tube. Stir well and heat to 100℃, react for 12h, filter while hot. The solid is washed with deionized water and EtOH in turn and dried in a vacuum oven to obtain compound 18. Weigh compound 18 (1mmol, 422mg) and add it to a thick-walled pressure bottle, add NaOH (4mmol, 160mg), 4mL of deionized water, stir well and heat to 150℃, react for 12h, cool and filter, and collect the solid. Further, the product was purified by reverse phase column (C18) (MeOH:H2O=5:95) to obtain compound 19 with a yield of 90%.
[0140] Example 11-13 Synthesis of Anthraquinone Amino Acid Derivatives
[0141]
[0142] Under nitrogen atmosphere, weigh 2,6-diiodoanthraquinone (3mmol, 1.38g), glycine (9mmol, 0.68g), Pd2(dba)3 (5mol%, 137.4mg), BrettPhos (10mol%, 161mg), potassium tert-butoxide (15mmol, 1.68g), and 30mL of tert-butanol in a thick-walled pressure-resistant reaction tube. Stir thoroughly and heat to 120°C, react for 12h, and then cool to room temperature. Filter and collect the filter cake, dissolve the filter cake in deionized water and filter again to remove insoluble impurities in water. Collect the filtrate, acidify the filtrate with HCl to pH=3~4, filter after solid precipitation, collect the filter cake, wash the filter cake with deionized water (2*5mL), and dry to obtain the target compound 21.
[0143] Compound 20-22 was obtained by the above method, and its NMR spectrum is as follows Figure 20-22 shown.
[0144]
[0145] Example 14-17 Synthesis of Phenazine Derivatives
[0146]
[0147] Under nitrogen atmosphere, 1,8-dibromophenazine (10 g, 29.8 mmol), ethyl acrylate (17.9 g, 178.8 mmol), palladium chloride (106 mg, 0.596 mmol), tri(o-methylphenyl)phosphine (726 mg, 2.384 mmol), tetrabutylammonium bromide (1.92 g, 5.96 mmol), potassium carbonate (16.4 g, 119.2 mmol), N,N-dimethylformamide (8 mL), and water (80 mL) were weighed in a thick-walled pressure-resistant reaction tube, stirred thoroughly, and heated to 100 °C for 12 h. After the reaction, the system was cooled to room temperature, and the dark insoluble solid in the system was filtered under reduced pressure, washed with distilled water and petroleum ether, and then redissolved in dichloromethane, and washed with distilled water and saturated brine. The organic phase was then separated, dried over anhydrous sodium sulfate, filtered, and concentrated under reduced pressure before being subjected to flash silica gel column chromatography (developing solvent: dichloromethane / ethyl acetate / triethylamine = 500 / 20 / 3) to obtain a large amount of dark green solid. The dark green solid was washed with ethyl acetate and filtered to obtain a pure yellow-green product 27 (11.9 g) with a yield of 70.8%.
[0148] Weigh the yellow-green solid 27 (4.6 g, 12.23 mmol) and palladium / carbon (460 mg) into a reaction flask, and replace the air in the reaction flask with nitrogen, and then replace it with hydrogen. Then 150 mL of ethyl acetate was added to the above system, and the reaction was stirred at 85 degrees for 12 hours under a hydrogen atmosphere. After the reaction was completed and cooled to room temperature, the system was filtered through diatomaceous earth, concentrated under reduced pressure, and chromatographed on a silica gel column (developing solvent: petroleum ether / ethyl acetate / triethylamine = 400 / 100 / 3) to obtain the pure target compound 28 (4.4 g), with a yield of 94.6%.
[0149] Finally, the pure compound 28 (4.4 g, 11.6 mmol) prepared in the previous step was dissolved in 25 mL of methanol, and an aqueous sodium hydroxide solution [sodium hydroxide (9.28 g, 232 mmol) dissolved in 25 mL of water] was added thereto, the system was fully stirred and heated to 65 ° C for reaction. After reacting for 12 hours, it was cooled to room temperature, and the reaction system was acidified with hydrochloric acid until a large amount of yellow-green solid precipitated. The filter cake was then collected by filtration and fully washed with distilled water, and the target compound 24 (3.72 g) was obtained after drying, with a yield of 99%.
[0150] By using the above general method and replacing the reaction starting materials, the following compounds 25 and 26 were obtained:
[0151]
[0152] Test Example
[0153] Test Example 1 Cyclic Voltammetry Test (Compound 15)
[0154] The cyclic voltammetry test uses a three-electrode system. The working electrode is a 5mm glassy carbon electrode, the reference electrode is aqueous Ag / AgCl, and the counter electrode is a platinum wire electrode. The voltage scanning range during the test is: -1.1V~-0.3V, and the scanning rate is 20mV / s.
[0155] Cyclic voltammogram of test compound 15 in 1 M KCl solution, as shown in Fig.23 The results show that the compound can exhibit good redox performance under neutral (KCl) conditions. And it has a high negative potential, E 1 / 2 =-0.56V,ΔE=341mV.
[0156] Test Example 2 Current Cycle Test
[0157] The main parameters and schematic diagram of the flow battery device are as follows: Fig.24As shown in . Constant current charge and discharge cycle test was performed using an electrochemical workstation. The battery was assembled with compound 15, using Nafion117 cation exchange membrane and SGL39AA carbon paper as electrode materials. The charge and discharge current was 100 mA and the current density was 20 mA / cm 2 .
[0158] During the battery cycle, the negative electrode solution was 6.9 mL of 0.1 M compound 15 dissolved in 1 M KCl solution; the positive electrode solution was 40 mL of 0.1 M K4FeCN6 and 0.02 M K3FeCN6 dissolved in 1 M KCl solution. The cycle process adopted constant current circulation, and its current density was 20 mA / cm 2 .
[0159] The test results of compound 15 in 1M KCl solution are as follows Fig.25 , 26 As shown. The test results show that the compound has excellent battery cycle stability. The constant current uninterrupted charge and discharge test lasts for 6 days. During the process, it has maintained a stable charge and discharge platform, the battery capacity has not decayed, the actual capacity accounts for 91% of the theoretical capacity, and the energy efficiency is 73%. The research results fully show that this type of compound is an ideal energy storage material for aqueous liquid flow batteries.
[0160] Test Example 3 Cyclic Voltammetry Test (Compound 3)
[0161] Cyclic voltammogram of test compound 3 in 1M KCl solution, as shown in Fig. 27 The results show that the compound can exhibit good redox performance under neutral (KCl) conditions. And it has a high negative potential, E 1 / 2 =-0.52V,ΔE=95mV.
[0162] Test Example 4 Cyclic Voltammetry Test (Compound 5)
[0163] Cyclic voltammogram of test compound 5 in 1M KCl solution, as shown in Fig.28 The results show that the compound can exhibit good redox performance under neutral (KCl) conditions. And it has a high negative potential, E 1 / 2 =-0.54V,ΔE=276mV.
[0164] Test Example 5 Cyclic Voltammetry Test (Compound 7)
[0165] Cyclic voltammogram of test compound 7 in 1 M KCl solution, as shown in Fig.29 The results show that the compound can exhibit good redox performance under neutral (KCl) conditions. And it has a high negative potential, E 1 / 2 =-0.52V,ΔE=115mV.
[0166] Test Example 6 Cyclic Voltammetry Test (Compound 9)
[0167] Cyclic voltammogram of test compound 9 in 1M KCl solution, as shown in Fig.30 The results show that the compound can exhibit good redox performance under neutral (KCl) conditions. And it has a high negative potential, E 1 / 2 =-0.53V,ΔE=95mV.
[0168] Test Example 7 Cyclic Voltammetry Test (Compound 11)
[0169] The cyclic voltammogram of the test compound 11 in 1M KCl solution is shown in Fig.31 The results show that the compound can exhibit good redox performance under neutral (KCl) conditions. And it has a high negative potential, E 1 / 2 =-0.57V,ΔE=205mV.
[0170] Test Example 8 Cyclic Voltammetry Test (Compound 13)
[0171] The cyclic voltammogram of the test compound 13 in 1M KCl solution is shown in Fig.32 The results show that the compound can exhibit good redox performance under neutral (KCl) conditions. And it has a high negative potential, E 1 / 2 =-0.52V,ΔE=376mV.
[0172] Test Example 9 Cyclic Voltammetry Test (Compound 14)
[0173] The cyclic voltammogram of the test compound 14 in 1M KCl solution is shown in Fig.33 The results show that the compound can exhibit good redox performance under neutral (KCl) conditions. And it has a high negative potential, E 1 / 2 =-0.51V,ΔE=425mV.
[0174] Test Example 10 Cyclic Voltammetry Test (Compound 16)
[0175] The cyclic voltammogram of the test compound 16 in 1M KCl solution is shown in Fig.34 The results show that the compound can exhibit good redox performance under neutral (KCl) conditions. And it has a high negative potential, E 1 / 2 =-0.51V,ΔE=425mV.
[0176] Test Example 11 Cyclic Voltammetry Test (Compound 21)
[0177] The cyclic voltammogram of the test compound 21 in 1M KCl solution is shown in Fig.40 The results show that the compound can exhibit good redox performance under neutral (KCl) conditions. And it has a high negative potential, E 1 / 2 =-0.56V,ΔE=44mV.
[0178] Test Example 12 Cyclic Voltammetry Test (Compound 22)
[0179] The cyclic voltammogram of the test compound 22 in 1M KCl solution is shown in Fig.41 The results show that the compound can exhibit good redox performance under neutral (KCl) conditions. And it has a high negative potential, E 1 / 2 =-0.60V,ΔE=59mV.
[0180] Test Example 13 Cyclic Voltammetry Test (Compound 23)
[0181] The cyclic voltammogram of the test compound 23 in 1M KCl solution is shown in Fig.42 The results show that the compound can exhibit good redox performance under neutral (KCl) conditions. And it has a high negative potential, E 1 / 2 =-0.60V,ΔE=48mV.
[0182] Test Example 14 Cyclic Voltammetry Test (Compound 24)
[0183] The cyclic voltammogram of the test compound 24 in 1 M KOH solution is shown in Fig.43 The results show that the compound can exhibit good redox performance under alkaline (KOH) conditions. And it has a high negative potential, E 1 / 2 =-0.59V,ΔE=163mV.
[0184] Test Example 15 Cyclic Voltammetry Test (Compound 25)
[0185] The cyclic voltammogram of the test compound 25 in 1 M KOH solution is shown in Fig.44 The results show that the compound can exhibit good redox performance under alkaline (KOH) conditions. And it has a high negative potential, E 1 / 2 =-0.56V,ΔE=195mV.
[0186] Test Example 16 Cyclic Voltammetry Test (Compound 26)
[0187] The cyclic voltammogram of the test compound 25 in 1 M KOH solution is shown in Fig.45The results show that the compound can exhibit good redox performance under alkaline (KOH) conditions. And it has a high negative potential, E 1 / 2 =-0.61V,ΔE=91mV.
[0188] Test Example 17 Current Cycling Test (Compound 22)
[0189]
[0190] The main parameters and schematic diagram of the flow battery device are as follows: Fig.24 As shown in . Constant current charge and discharge cycle test was performed using an electrochemical workstation. The battery was assembled with compound 22, using Nafion117 cation exchange membrane and SGL39AA carbon paper as electrode materials. The charge and discharge current was 100 mA and the current density was 20 mA / cm 2 .
[0191] During the battery cycle, the negative electrode solution was 7.0 mL of 0.1 M compound 22 dissolved in a 1 M KCl solution at pH = 12; the positive electrode solution was 40 mL of 0.1 M K4FeCN6 and 0.02 M K3FeCN6 dissolved in a 1 M KCl solution at pH = 12. The cycle process was performed using a constant current cycle with a current density of 20 mA / cm 2 .
[0192] The test results of compound 22 in 1M KCl (pH=12) solution are as follows: Fig.46 , 47 As shown. The test results show that the compound has excellent battery cycle stability. The constant current uninterrupted charge and discharge test lasted for a total of 10 days. During the process, it maintained a stable charge and discharge platform. The battery capacity decayed by 0.61% / day, the actual capacity accounted for 88% of the theoretical capacity, and the energy efficiency reached 68%. The research results fully show that this type of compound is an ideal energy storage material for aqueous liquid flow batteries.
[0193] Test Example 18 Current Cycling Test (Compound 24)
[0194]
[0195] The main parameters and schematic diagram of the flow battery device are as follows: Fig.24 As shown in . Constant current and constant voltage charge-discharge cycle tests were performed using an electrochemical workstation. The battery was assembled with compound 24, using Nafion117 cation exchange membrane and SGL39AA carbon paper as electrode materials. The charge and discharge current was 100 mA and the current density was 20 mA / cm 2 .
[0196] During the battery cycle, the negative electrode solution was 7.0 mL of 0.1 M compound 24 dissolved in a 1 M KCl solution at pH = 12; the positive electrode solution was 40 mL of 0.1 M K4FeCN6 and 0.02 M K3FeCN6 dissolved in a 1 M KCl solution at pH = 12. The cycle process adopted constant current and constant voltage cycles, and the current density was 20 mA / cm 2 .
[0197] The test results of compound 24 in 1M KCl (pH=12) solution are as follows: Fig.48 , 49 As shown. The test results show that the compound has excellent battery cycle stability. The constant current and constant voltage uninterrupted charge and discharge test lasted for a total of 20 days. During the process, it maintained a stable charge and discharge platform. The battery capacity decayed by 0.0033% / day, the actual capacity accounted for 96% of the theoretical capacity, and the energy efficiency reached 66%. The research results fully show that this type of compound is an ideal energy storage material for aqueous liquid flow batteries.
[0198] Test Example 19 Current Cycling Test (Compound 25)
[0199]
[0200] The main parameters and schematic diagram of the flow battery device are as follows: Fig.24 As shown in . Constant current and constant voltage charge-discharge cycle tests were performed using an electrochemical workstation. The battery was assembled with compound 25, using Nafion117 cation exchange membrane and SGL39AA carbon paper as electrode materials. The charge-discharge current was 100 mA and the current density was 20 mA / cm 2 .
[0201] During the battery cycle, the negative electrode solution was 7.0 mL of 0.1 M compound 25 dissolved in a 1 M KCl solution at pH = 12; the positive electrode solution was 40 mL of 0.1 M K4FeCN6 and 0.02 M K3FeCN6 dissolved in a 1 M KCl solution at pH = 12. The cycle process adopted constant current and constant voltage cycles, and the current density was 20 mA / cm 2 .
[0202] The test results of compound 25 in 1M KCl (pH=12) solution are as follows: Fig.50 , 51 As shown. The test results show that the compound has excellent battery cycle stability. The constant current and constant voltage uninterrupted charge and discharge test lasted for a total of 20 days. During the process, it maintained a stable charge and discharge platform. The battery capacity decayed by 0.0044% / day, the actual capacity accounted for 99% of the theoretical capacity, and the energy efficiency reached 65%. The research results fully show that this type of compound is an ideal energy storage material for aqueous liquid flow batteries.
[0203] Test Example 20 Current Cycling Test (Compound 26)
[0204]
[0205] The main parameters and schematic diagram of the flow battery device are as follows: Fig.24 As shown in . Constant current and constant voltage charge-discharge cycle tests were performed using an electrochemical workstation. The battery was assembled with compound 26, using Nafion117 cation exchange membrane and SGL39AA carbon paper as electrode materials. The charge-discharge current was 100 mA and the current density was 20 mA / cm 2 .
[0206] During the battery cycle, the negative electrode solution was 7.0 mL of 0.1 M compound 26 dissolved in a 1 M KCl solution at pH = 12; the positive electrode solution was 40 mL of 0.1 M K4FeCN6 and 0.02 M K3FeCN6 dissolved in a 1 M KCl solution at pH = 12. The cycle process adopted constant current and constant voltage cycles, and the current density was 20 mA / cm 2 .
[0207] The test results of compound 26 in 1M KCl (pH=12) solution are as follows: Fig.52 , 53 As shown. The test results show that the compound has excellent battery cycle stability. The constant current and constant voltage uninterrupted charge and discharge test lasted for a total of 18 days. During the process, it maintained a stable charge and discharge platform. The battery capacity decayed by 0.1110% / day, the actual capacity accounted for 96% of the theoretical capacity, and the energy efficiency reached 70%. The research results fully show that this type of compound is an ideal energy storage material for aqueous liquid flow batteries.
[0208] The results of the above-mentioned embodiments show that the compound of the present invention has a higher negative potential and better redox performance when used as an energy storage material for a liquid flow battery, and is therefore an ideal energy storage material for an aqueous liquid flow battery.
[0209] All documents mentioned in the present invention are cited as references in this application, just as each document is cited as reference individually. In addition, it should be understood that after reading the above teachings of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.
Claims
1. A compound represented by the following formula (I): in, Y and Z are each independently N; the dotted lines are chemical bonds; m1 and m2 are selected from the following group: 0, 1 or 2; p1 and p2 are selected from the following groups: 1 or 2; Each R is independently selected from the following group: halogen, substituted or unsubstituted C1-C4 alkyl, hydroxyl, thiol; Each Rg is independently a functional group; wherein the functional group is in: Ra and Rb are each independently selected from the following group: H, substituted or unsubstituted C1-C10 alkyl; and the Rg includes at least one R 0 Substituent; R 0 Selected from the following group: -COOX; wherein X is selected from the following group: H + NH4 + , Li + 、Na + , K + Mg 2+ 、Al 3+ , Ca 2+ ; or p1 and p2 are 0; m1 and m2 are 1 or 2; each R is independently a C1-C4 alkyl substituted with a carboxyl group; The substitution refers to that one or more hydrogen atoms on the group are replaced by a substituent selected from the group consisting of halogen, C1-C4 alkyl, hydroxyl, mercapto, sulfonic acid, and carboxyl.
2. The compound according to claim 1, characterized in that The functional groups are the following groups: Where X is H, NH4 + , Li + 、Na + , K + ; R 9 , R 10 Each is independently selected from the following group: H, substituted or unsubstituted C1-C4 alkyl; R 11 Selected from the following group: H, substituted or unsubstituted C1-C10 alkyl; n is 1, 2, 3, 4, 5, 6, 7 or 8; The substitution refers to that one or more hydrogen atoms on the group are replaced by a substituent selected from the following group: C1-C4 alkyl, hydroxyl, sulfonic acid, carboxyl.
3. The compound according to claim 1, characterized in that The compound is selected from the following group:
4. The method for preparing the compound according to claim 1, characterized in that: Includes steps: (i) reacting a compound of formula (II) with RgH in an inert solvent to obtain a compound of formula (I); wherein M is F, Cl, Br or I.
5. The method according to claim 4, characterized in that In the step (i), the method is carried out in the presence of a palladium catalyst, a ligand and a base.
6. The method according to claim 5, characterized in that In the step (i), the palladium catalyst is Pd2(dba)3, and the base is t BuOK or Cs2CO3, and the ligand is selected from the group consisting of BrettPhos, RuPhos, XPhos or Pd2(dba)3.
7. The method according to claim 5, characterized in that In the step (i), the inert solvent is selected from the group consisting of tert-butyl alcohol, n-butyl alcohol, toluene, or a combination thereof.
8. A liquid flow battery energy storage material, characterized in that: The liquid flow battery energy storage material comprises the compound as described in any one of claims 1-3.
9. A liquid flow battery, characterized in that: The liquid flow battery comprises the compound as described in any one of claims 1 to 3 as an energy storage material.
10. The flow battery according to claim 9, characterized in that In the liquid flow battery, the compound described in any one of claims 1 to 3 is used as the negative electrode or positive electrode solution.
Citation Information
Patent Citations
Synthesis method, derivative and battery system of anthraquinone derivative containing carboxyl group
CN110526826A
Redox flow battery with electrolyte balancing and compatibility enabling features
EP3605696A2
Quinones having high capacity retention for use as electrolytes in aqueous redox flow batteries
WO2019157437A1