Secondary battery and device containing the same

By using a combination of negative electrode plates of silicon-based materials and carbon materials, special-thickness separators, and electrolytes in secondary batteries, the problem of existing secondary batteries being unable to balance high energy density and high-temperature performance is solved, and high performance is achieved. Comprehensive improvements in energy density, good high-temperature cycling and storage performance, and low-temperature DC impedance.

CN114245943BActive Publication Date: 2024-10-18CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN201980098827.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-12-24
Publication Date
2024-10-18
Estimated Expiration
2039-12-24

AI Technical Summary

Technical Problem

It is difficult for existing secondary batteries to balance high energy density, good high-temperature cycle performance, high-temperature storage performance and low-temperature DC impedance, and cannot meet actual use needs.

Method used

It uses a combination of negative electrode piece, isolation film and electrolyte. The negative electrode piece includes silicon-based material and carbon material. The base material thickness of the isolation film is 7 μm ~ 12 μm. The electrolyte contains organic solvents such as ethylene carbonate (EC) and carbonic acid. The content of vinyl ester is ≤20%, and the concentration of lithium bisfluorosulfonyl imide (LiFSI) and lithium hexafluorophosphate (LiPF6) in the electrolyte is within a specific range to ensure that the conductivity and viscosity of the electrolyte are within the appropriate range.

Benefits of technology

It is realized that under the premise of high energy density, the secondary battery has better high-temperature cycle performance, high-temperature storage performance and low-temperature DC impedance, which improves the overall performance and safety of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114245943B_ABST
    Figure CN114245943B_ABST
Patent Text Reader

Abstract

The present application provides a secondary battery and a device containing the secondary battery, the secondary battery comprising: a negative electrode plate, the negative electrode plate comprising a negative electrode active material; a separator, the separator comprising a substrate and a coating disposed on at least one surface of the substrate; and an electrolyte, the electrolyte comprising an organic solvent; wherein the negative electrode active material comprises a silicon-based material and a carbon material; the thickness of the substrate of the separator is 7 μm to 12 μm; the organic solvent comprises ethylene carbonate, and the weight proportion of the ethylene carbonate content in the organic solvent is ≤20%. The secondary battery of the present application and the device containing the secondary battery can not only have high energy density, but also have good high temperature cycle performance, high temperature storage performance and low low temperature DC impedance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a secondary battery and a device containing the secondary battery. Background Art

[0002] The large-scale consumption of fossil resources has led to increasingly serious resource depletion. At the same time, the serious environmental problems caused by the use of fossil resources have also made the development of new clean and environmentally friendly new energy sources more urgent. Although wind energy, hydropower, solar energy and other existing new energy sources have been developed and applied to varying degrees, they cannot be supplied continuously and stably due to factors such as seasons and regions, and suitable energy storage equipment is needed to store and release electrical energy. Secondary batteries have developed rapidly due to their advantages such as relatively easy access to raw materials and environmental friendliness, and have been widely used in the new energy industry.

[0003] However, currently commercialized secondary batteries often cannot meet actual usage needs, so there is an urgent need to develop a secondary battery that can simultaneously take into account higher energy density and better electrochemical performance. Summary of the invention

[0004] In view of the problems existing in the background technology, the purpose of the present application is to provide a secondary battery and a device containing the secondary battery, which can not only have high energy density, but also have good high-temperature cycle performance, high-temperature storage performance and low low-temperature DC impedance.

[0005] In order to achieve the above-mentioned purpose, the first aspect of the present application provides a secondary battery, comprising: a negative electrode plate, the negative electrode plate comprising a negative electrode collector and a negative electrode membrane arranged on at least one surface of the negative electrode collector and comprising a negative electrode active material; a separator, the separator comprising a substrate and a coating arranged on at least one surface of the substrate; and an electrolyte, the electrolyte comprising an organic solvent; wherein the negative electrode active material comprises a silicon-based material and a carbon material; the thickness of the substrate of the separator is 7μm to 12μm; the organic solvent comprises ethylene carbonate (EC), and the weight content of the ethylene carbonate (EC) in the organic solvent is ≤20%.

[0006] The secondary battery of the present application includes: a negative electrode including a specific active material, a substrate of an isolation membrane of a specific thickness, and an electrolyte including a specific organic solvent. Under the joint action of the negative electrode, the secondary battery of the present application can have high energy density while also having good high-temperature cycle performance, high-temperature storage performance and low low-temperature DC impedance.

[0007] In any embodiment of the first aspect of the present application, the weight proportion of ethylene carbonate EC in the organic solvent is ≤15%.

[0008] Optionally, the weight percentage of ethylene carbonate EC in the organic solvent is ≤10%.

[0009] The use of a specific content of ethylene carbonate EC together with a specific thickness of the separator substrate can enable the electrolyte to infiltrate the separator well, thereby effectively improving the power performance and cycle performance of the battery.

[0010] In any embodiment of the first aspect of the present application, the thickness of the substrate of the isolation membrane is 7 μm to 10 μm.

[0011] In any embodiment of the first aspect of the present application, the porosity of the separator is 25% to 50%. Optionally, the porosity of the separator is 30% to 48%. If the porosity of the separator is too low, the path of lithium ions passing through the separator is longer, which will affect the dynamic performance of the secondary battery; if the porosity of the separator is too high, the mechanical strength of the separator will deteriorate, thereby causing a greater safety hazard to the secondary battery.

[0012] In any embodiment of the first aspect of the present application, the organic solvent further comprises one or more of ethyl methyl carbonate EMC, diethyl carbonate DEC, and dimethyl carbonate DMC.

[0013] In any embodiment of the first aspect of the present application, the weight percentage of ethyl methyl carbonate EMC in the organic solvent is 60% to 95%.

[0014] Optionally, the weight percentage of ethyl methyl carbonate EMC in the organic solvent is 75% to 95%.

[0015] In any embodiment of the first aspect of the present application, the weight percentage of diethyl carbonate DEC in the organic solvent is ≤30%.

[0016] Optionally, the content of diethyl carbonate DEC in the organic solvent accounts for ≤20% by weight.

[0017] In any embodiment of the first aspect of the present application, the weight proportion of dimethyl carbonate DMC in the organic solvent is ≤15%.

[0018] Optionally, the content of dimethyl carbonate DMC in the organic solvent is ≤10% by weight.

[0019] In any embodiment of the first aspect of the present application, the electrolyte further comprises an electrolyte salt, and the electrolyte salt comprises lithium bis(fluorosulfonyl)imide LiFSI and lithium hexafluorophosphate LiPF6;

[0020] The volume molar concentration of lithium bis(fluorosulfonyl)imide LiFSI in the electrolyte is 0.8 mol / L to 1.3 mol / L, and the volume molar concentration of lithium hexafluorophosphate LiPF6 in the electrolyte is 0.15 mol / L to 0.4 mol / L.

[0021] When the contents of lithium bis(fluorosulfonyl)imide LiFSI and lithium hexafluorophosphate LiPF6 are within the above range, it can not only alleviate the oxidation of lithium bis(fluorosulfonyl)imide LiFSI at the positive electrode and improve the cycle performance of the battery, but also effectively improve the low-temperature power performance of the battery.

[0022] In any embodiment of the first aspect of the present application, the volume molar concentration of lithium bis(fluorosulfonyl)imide LiFSI in the electrolyte is 0.9 mol / L to 1.2 mol / L, and the volume molar concentration of lithium hexafluorophosphate LiPF6 in the electrolyte is 0.15 mol / L to 0.3 mol / L.

[0023] In any embodiment of the first aspect of the present application, the conductivity of the electrolyte at 25° C. is 6.5 mS / cm to 9.5 mS / cm. Optionally, the conductivity of the electrolyte at 25° C. is 7 mS / cm to 9 mS / cm.

[0024] In any embodiment of the first aspect of the present application, the viscosity of the electrolyte at 25° C. is 3.5 mPa·s to 5.5 mPa·s. Optionally, the viscosity of the electrolyte at 25° C. is 4 mPa·s to 5 mPa·s.

[0025] In any embodiment of the first aspect of the present application, the silicon-based material includes one or more of silicon, silicon alloy, silicon-oxygen compound, silicon-carbon compound, and silicon-nitrogen compound. Optionally, the silicon-based material includes silicon-oxygen compound.

[0026] In any embodiment of the first aspect of the present application, the carbon material includes one or more of graphite, soft carbon, and hard carbon. Optionally, the carbon material includes graphite, and the graphite is selected from one or more of artificial graphite and natural graphite.

[0027] In any embodiment of the first aspect of the present application, the mass proportion of the silicon-based material in the negative electrode active material is ≤50%, and can be optionally 15% to 30%.

[0028] In any embodiment of the first aspect of the present application, the thickness of the isolation film is 11 μm to 16 μm. Optionally, the thickness of the isolation film is 12 μm to 14 μm.

[0029] In any embodiment of the first aspect of the present application, the secondary battery further comprises a positive electrode sheet, the positive electrode sheet comprises a positive current collector and a positive electrode film disposed on at least one surface of the positive current collector and comprising a positive electrode active material, the positive electrode active material comprising one or more of lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide. As positive electrode active materials of secondary batteries, lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide have the advantages of high specific capacity and long cycle life, and are used in combination with negative electrode active materials comprising silicon-based materials to further improve the electrochemical performance of the battery.

[0030] Optionally, the positive electrode active material includes Li a Ni b Co c M d M' e O f A g or a Li having a coating layer disposed on at least a portion of the surface a Ni b Co c M d M' e O f A g One or more of, wherein, 0.8≤a≤1.2, 0.5≤b<1, 0<c<1, 0<d<1, 0.e≤0.1, 1.f≤2, 0.g≤1, M is selected from one or two of Mn and Al, M' is selected from one or more of Zr, Al, Zn, Cu, Cr, Mg, Fe, V, Ti, B, and A is selected from one or more of N, F, S, and Cl. The cycle performance of the secondary battery can be further improved by coating and modifying the surface of the positive electrode active material.

[0031] A second aspect of the present application provides a device, which includes the secondary battery described in the first aspect of the present application.

[0032] The device described in the second aspect of the present application includes the secondary battery described in the first aspect of the present application, and thus has at least the same advantages as the secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic diagram of a secondary battery provided in an embodiment of the present application.

[0034] Figure 2 It is a schematic diagram of a battery module provided in an embodiment of the present application.

[0035] Figure 3 It is a schematic diagram of a battery pack provided in an embodiment of the present application.

[0036] Figure 4 yes Figure 3 Exploded diagram of .

[0037] Figure 5 It is a schematic diagram of a device provided in an embodiment of the present application.

[0038] The reference numerals are described as follows:

[0039] 1. Battery box;

[0040] 2. Upper box;

[0041] 3. Lower box;

[0042] 4. Battery module;

[0043] 5. Secondary battery. DETAILED DESCRIPTION

[0044] The secondary battery and the device including the secondary battery according to the present application are described in detail below.

[0045] First, a secondary battery according to the first aspect of the present application will be described.

[0046] The secondary battery according to the first aspect of the present application includes a negative electrode plate, a separator and an electrolyte. The negative electrode plate includes a negative electrode current collector and a negative electrode membrane disposed on at least one surface of the negative electrode current collector and including a negative electrode active material; the separator includes a substrate and a coating disposed on at least one surface of the substrate; the electrolyte includes an organic solvent. Among them, the negative electrode active material includes a silicon-based material and a carbon material, the thickness of the substrate of the separator is 7μm to 12μm, the organic solvent includes ethylene carbonate (EC), and the weight content of the ethylene carbonate (EC) in the organic solvent is ≤20%.

[0047] In the secondary battery described in the present application, the silicon-based material has a large theoretical specific capacity, and when used as the negative electrode active material of the secondary battery, the capacity of the secondary battery can be significantly increased. However, the volume of the silicon-based material will seriously expand during the charging and discharging process, thereby affecting the performance of the secondary battery. The silicon-based material and the carbon material are used together as the negative electrode active material. On the one hand, it can increase the capacity of the secondary battery. On the other hand, the addition of the carbon material can also alleviate the effect of the volume expansion of the silicon-based material on the performance of the secondary battery to a certain extent. At the same time, in the secondary battery of the present application, the organic solvent in the electrolyte includes ethylene carbonate (EC), and the weight proportion of the ethylene carbonate (EC) in the organic solvent is ≤20%, which can effectively reduce the risk of gas production in the battery. At the same time, the inventors have found that the use of a specific content of ethylene carbonate (EC) and a specific thickness of the isolation membrane substrate together can make the electrolyte well infiltrated in the isolation membrane, thereby effectively improving the power performance and cycle performance of the battery.

[0048] In the secondary battery according to the first aspect of the present application, optionally, the thickness of the substrate of the isolation film is 7 μm to 10 μm.

[0049] In the secondary battery according to the first aspect of the present application, optionally, the porosity of the separator is 25% to 50%. If the porosity of the separator is too low, the path of lithium ions passing through the separator is longer, which will affect the dynamic performance of the secondary battery; if the porosity of the separator is too high, the mechanical strength of the separator will deteriorate, which will cause a greater safety hazard to the secondary battery. More optionally, the porosity of the separator is 30% to 48%.

[0050] In the secondary battery according to the first aspect of the present application, in the isolation film, the substrate can be selected from one or more of polyethylene film, polypropylene film, polyvinylidene fluoride film and multilayer composite films thereof.

[0051] In the secondary battery according to the first aspect of the present application, in the isolation film, the coating disposed on at least one surface of the substrate may include one or more of an inorganic particle coating or a polymer coating, and the types of the inorganic particle coating and the polymer coating are not particularly limited and can be selected according to actual needs. Specifically, the inorganic particle coating may include one or more of aluminum oxide particles and zirconium oxide particles, and the polymer coating may include one or more of polyvinylidene fluoride polymers and polyimide polymers.

[0052] In the secondary battery according to the first aspect of the present application, optionally, the thickness of the isolation membrane (ie, the sum of the thickness of the substrate and the thickness of the coating in the isolation membrane) is 10 μm to 16 μm; further optionally, the thickness of the isolation membrane is 12 μm to 14 μm.

[0053] In the secondary battery according to the first aspect of the present application, optionally, the weight percentage of the ethylene carbonate (EC) in the organic solvent is ≤15%; more optionally, the weight percentage of the ethylene carbonate (EC) in the organic solvent is ≤10%.

[0054] In the secondary battery according to the first aspect of the present application, the organic solvent further comprises one or more of ethyl methyl carbonate (EMC), diethyl carbonate (DEC), and dimethyl carbonate (DMC).

[0055] In the secondary battery according to the first aspect of the present application, when the organic solvent further includes EMC, optionally, the weight content of the EMC in the organic solvent is 60% to 95%, and more optionally, the weight content of the EMC in the organic solvent is 75% to 95%.

[0056] In the secondary battery according to the first aspect of the present application, when the organic solvent further includes DEC, optionally, the weight content of DEC in the organic solvent is ≤30%, and more optionally, the weight content of DEC in the organic solvent is ≤20%.

[0057] In the secondary battery according to the first aspect of the present application, when the organic solvent further includes DMC, optionally, the weight ratio of the DMC content in the total weight of the organic solvent is ≤15%, and more optionally, the weight ratio of the DMC content in the total weight of the organic solvent is ≤10%.

[0058] In the secondary battery according to the first aspect of the present application, the organic solvent may also include methyl formate, ethyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, butyl propionate, isobutyl propionate, pentyl propionate, isoamyl propionate, ethyl isopropionate, ethyl butyrate, ethyl isobutyrate, butyl butyrate, butyl isobutyrate, pentyl butyrate, isoamyl butyrate, ethyl valerate, ethyl isovalerate, propyl valerate, propyl isovalerate, and one or more of the compounds in which the above compounds are partially or completely substituted with one or more of the halogen atoms.

[0059] In the secondary battery according to the first aspect of the present application, the electrolyte further includes an electrolyte salt, and the electrolyte salt may include one or more of lithium bis(fluorosulfonyl)imide (LiFSI) and lithium hexafluorophosphate (LiPF6); optionally, the electrolyte salt includes lithium bis(fluorosulfonyl)imide (LiFSI) and lithium hexafluorophosphate (LiPF6), and the volume molar concentration of the lithium bis(fluorosulfonyl)imide (LiFSI) in the electrolyte is 0.8 mol / L to 1.3 mol / L, and the volume molar concentration of the lithium hexafluorophosphate (LiPF6) in the electrolyte is 0.15 mol / L to 0.4 mol / L.

[0060] When the contents of lithium bis(fluorosulfonyl)imide (LiFSI) and lithium hexafluorophosphate (LiPF6) are within the above range, it can not only alleviate the oxidation of lithium bis(fluorosulfonyl)imide (LiFSI) at the positive electrode and improve the cycle performance of the battery, but also effectively improve the low-temperature power performance of the battery.

[0061] In the secondary battery according to the first aspect of the present application, further optionally, the volume molar concentration of lithium bis(fluorosulfonyl)imide (LiFSI) in the electrolyte is 0.9 mol / L to 1.2 mol / L.

[0062] In the secondary battery according to the first aspect of the present application, further optionally, the volume molar concentration of the lithium hexafluorophosphate (LiPF6) in the electrolyte is 0.15 mol / L to 0.3 mol / L.

[0063] In the secondary battery according to the first aspect of the present application, the conductivity of the electrolyte at 25° C. is 6.5 mS / cm to 9.5 mS / cm; optionally, the conductivity of the electrolyte at 25° C. is 7 mS / cm to 9 mS / cm.

[0064] In the secondary battery described in the present application, the viscosity of the electrolyte at 25° C. is 3.5 mPa·s to 5.5 mPa·s; optionally, the viscosity of the electrolyte at 25° C. is 4 mPa·s to 5 mPa·s.

[0065] The conductivity of the electrolyte at 25° C. can be tested by a method known in the art, and the testing instrument used can be a thunder-magnetic conductivity instrument.

[0066] The viscosity of the electrolyte at 25° C. can be tested by a method known in the art, and the testing instrument used can be a viscometer.

[0067] In the secondary battery according to the first aspect of the present application, the electrolyte further includes an additive, and the additive may include one or more of vinylene carbonate, fluoroethylene carbonate (FEC), 1,3-propane sultone, 1,3-propanedisulfonic anhydride (PDSA), vinyl sulfate, succinic anhydride (SA), tris(trimethylsilyl) phosphate (TMSP), trifluoromethanesulfonic anhydride, tetrafluorosuccinic anhydride, and adiponitrile.

[0068] In the secondary battery according to the first aspect of the present application, optionally, the silicon-based material includes one or more of silicon element, silicon alloy, silicon oxide compound, silicon carbon compound, silicon nitrogen compound; more optionally, the silicon-based material includes silicon oxide compound.

[0069] In the secondary battery according to the first aspect of the present application, optionally, the mass proportion of the silicon-based material in the negative electrode active material is ≤50%, and more optionally 15% to 30%.

[0070] In the secondary battery according to the first aspect of the present application, optionally, the carbon material includes one or more of graphite, soft carbon, and hard carbon; more optionally, the carbon material includes graphite, and the graphite is selected from one or more of artificial graphite and natural graphite.

[0071] In the secondary battery described in the first aspect of the present application, it also includes a positive electrode plate, which includes a positive electrode collector and a positive electrode membrane arranged on at least one surface of the positive electrode collector and including a positive electrode active material; the positive electrode membrane can be arranged on one surface of the positive electrode collector, or on both surfaces of the positive electrode collector at the same time; the negative electrode membrane can be arranged on one surface of the negative electrode collector, or on both surfaces of the negative electrode collector at the same time.

[0072] In the secondary battery according to the first aspect of the present application, optionally, the positive electrode active material includes one or more of lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide. As positive electrode active materials of secondary batteries, lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide have the advantages of high specific capacity and long cycle life, and are used in combination with negative electrode active materials including silicon-based materials to further improve the electrochemical performance of the battery.

[0073] In the secondary battery according to the first aspect of the present application, optionally, the positive electrode active material includes a general formula of Li a Ni b Co c M d M' e O f A g or a Li having a coating layer disposed on at least a portion of the surface a Ni b Co c M d M' e O f A g One or more of the materials, wherein 0.8≤a≤1.2, 0.5≤b<1, 0<c<1, 0<d<1, 0≤e≤0.1, 1≤f≤2, 0≤g≤1, M is selected from one or more of Mn and Al, M' is selected from one or more of Zr, Al, Zn, Cu, Cr, Mg, Fe, V, Ti, and B, and A is selected from one or more of N, F, S, and Cl.

[0074] The coating layer on the surface of the positive electrode active material can be a carbon layer, an oxide layer, an inorganic salt layer or a conductive polymer layer. The cycle performance of the secondary battery can be further improved by coating and modifying the surface of the positive electrode active material.

[0075] In the secondary battery according to the first aspect of the present application, further, the positive electrode active material may also include one or more of lithium nickel oxide (e.g., lithium nickelate), lithium manganese oxide (e.g., spinel lithium manganese oxide, layered structure lithium manganese oxide), lithium iron phosphate, lithium manganese phosphate, lithium manganese iron phosphate, lithium cobalt oxide, and modified compounds thereof.

[0076] In the secondary battery according to the first aspect of the present application, the type of the positive electrode current collector is not specifically limited and can be selected according to actual needs. Specifically, the positive electrode current collector can be selected from metal foil, such as aluminum foil.

[0077] In the secondary battery described in the first aspect of the present application, the type of the negative electrode current collector is not particularly limited and can be selected according to actual needs. Specifically, the negative electrode current collector can be selected from metal foil, such as copper foil.

[0078] In some embodiments, the secondary battery may include an outer package for packaging the positive electrode sheet, the negative electrode sheet and the electrolyte. As an example, the positive electrode sheet, the negative electrode sheet and the separator may be laminated or wound to form an electrode assembly of a laminate structure or an electrode assembly of a wound structure, and the electrode assembly is packaged in the outer package; the electrolyte is infiltrated in the electrode assembly. The number of electrode assemblies in the secondary battery may be one or more, which can be adjusted according to demand.

[0079] In some embodiments, the outer packaging of the secondary battery may be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, such as one or more of polypropylene PP, polybutylene terephthalate PBT, polybutylene succinate PBS, etc. The outer packaging of the secondary battery may also be a hard shell, such as an aluminum shell, etc.

[0080] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 1 The secondary battery 5 is a square structure as an example.

[0081] In some embodiments, secondary batteries may be assembled into a battery module. The battery module may contain multiple secondary batteries, and the specific number may be adjusted according to the application and capacity of the battery module.

[0082] Figure 2 4 is an example of a battery module. Figure 2 In the battery module 4, the plurality of secondary batteries 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of secondary batteries 5 may be fixed by fasteners.

[0083] Optionally, the battery module 4 may further include a housing having a housing space, and the plurality of secondary batteries 5 are housed in the housing space.

[0084] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0085] Figure 3 and Figure 41 is a battery pack 1 as an example. Figure 3 and Figure 4 The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.

[0086] Next, the device according to the second aspect of the present application is described.

[0087] The second aspect of the present application provides a device, the device includes the secondary battery of the first aspect of the present application, the secondary battery can be used as the power source of the device, and can also be used as the energy storage unit of the device. The device includes but is not limited to mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.

[0088] The device can select a secondary battery, a battery module or a battery pack according to its usage requirements.

[0089] Figure 5 The device is used as an example. The device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the device's requirements for high power and high energy density of secondary batteries, a battery pack or a battery module can be used.

[0090] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a secondary battery may be used as a power source.

[0091] The present application is further described below in conjunction with the examples. It should be understood that these examples are only used to illustrate the present application and are not used to limit the scope of the present application.

[0092] The secondary batteries of Examples 1-19 and Comparative Examples 1-6 were prepared according to the following method:

[0093] (1) Preparation of positive electrode sheet:

[0094] The positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1 O2, binder polyvinylidene fluoride, and conductive agent conductive carbon black are mixed in a weight ratio of 97:1:2, N-methylpyrrolidone (NMP) is added, and stirred in a vacuum mixer until the system becomes uniform and transparent to obtain a positive electrode slurry; the aluminum foil is dried at room temperature and then transferred to an oven for drying, and then cold pressed and cut to obtain a positive electrode sheet.

[0095] (2) Preparation of negative electrode sheet:

[0096] The negative electrode active materials silicon oxide and artificial graphite are mixed in a mass ratio of 2:8, and then mixed with a conductive agent Super P, a thickener sodium carboxymethyl cellulose (CMC-Na), and a binder styrene-butadiene rubber (SBR) in a mass ratio of 92:2:2:4. Deionized water is added and stirred in a vacuum mixer to obtain a uniformly dispersed negative electrode slurry; the copper foil is dried at room temperature and then transferred to an oven for drying, and then cold pressed and cut to obtain a negative electrode sheet.

[0097] (3) Preparation of electrolyte

[0098] In a high-purity nitrogen glove box, organic solvents are mixed to obtain a mixed solvent, and then the fully dried electrolyte salt is dissolved in the mixed solvent, and then additives are added to the mixed solvent, mixed evenly, to obtain an electrolyte. Wherein, the composition of the additive is: 8% FEC + 0.5% SA + 0.5% TMSP, and the content of each additive is the weight percentage calculated based on the total weight of the electrolyte; of course, those skilled in the art may also use additives of other compositions instead, which will not affect the overall performance test results of this application. Wherein, the types and concentrations of electrolyte salts used in the electrolyte, and the specific types and contents of organic solvents are shown in Table 1. The content of each organic solvent is the weight percentage calculated based on the total weight of the organic solvent; the concentration of each electrolyte salt is the volume molar concentration in the electrolyte.

[0099] (4) Preparation of isolation membrane

[0100] The specific settings of the substrate and substrate thickness in the isolation film are shown in Table 1.

[0101] (5) Preparation of secondary batteries:

[0102] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, so that the separator is placed between the positive and negative electrode sheets to play an isolating role, and then they are wound to obtain an electrode assembly; the electrode assembly is placed in an outer package, and the prepared electrolyte is injected into the dried battery. After vacuum packaging, standing, formation, shaping and other processes, a secondary battery is obtained.

[0103] Table 1 Parameters of Examples 1-19 and Comparative Examples 1-6

[0104]

[0105] Next, the test process of the secondary battery is described.

[0106] (1) High temperature cycle performance test

[0107] At 45°C, the secondary battery was charged to 4.25V at a constant current of 1C, then charged to a current of 0.05C at a constant voltage of 4.25V, allowed to stand for 5 minutes, and then discharged to 2.5V at a constant current of 1C. This was the first charge / discharge cycle of the secondary battery. The discharge capacity was recorded as the discharge capacity of the first cycle of the secondary battery. The secondary battery was charged / discharged for 800 cycles according to the above method to obtain the discharge capacity of the secondary battery after 800 cycles.

[0108] Capacity retention rate (%) of the secondary battery after 800 cycles at 45° C.=(discharge capacity of the secondary battery after 800 cycles / discharge capacity of the secondary battery at the first cycle)×100%.

[0109] (2) High temperature storage performance test

[0110] At 25°C, the secondary battery was charged at a constant current of 0.5C to 4.25V, and then charged at a constant voltage of 4.25V to a current of 0.05C. The volume of the secondary battery at this time was tested by the drainage method and recorded as V1. The secondary battery was then placed in a constant temperature box at 60°C, taken out after storage for 30 days, and the volume of the secondary battery at this time was tested and recorded as V2.

[0111] Volume expansion ratio of secondary battery after storage at 60°C for 30 days (%) = [(V2-V1) / V1] × 100%

[0112] (3) Low temperature DC impedance test

[0113] At -20°C, charge the secondary battery to 4.25V at a constant current of 1C, then charge to 0.05C at a constant voltage of 4.25V, let stand for 5 minutes, then discharge at a constant current of 1C (I1) for 30 minutes, measure the voltage of the secondary battery after discharge and record it as U1; adjust the temperature to -20°C, let stand for 2 hours, then discharge at a constant current of 0.36C (I2) for 30 seconds, measure the voltage of the secondary battery after discharge and record it as U2;

[0114] The low temperature DC resistance DCR of the secondary battery is (U1–U2) / (I1-I2).

[0115] Table 2 Performance test results of Examples 1-19 and Comparative Examples 1-6

[0116]

[0117] It can be seen from the test results in Table 2 that the secondary battery of the embodiment of the present application can simultaneously take into account good high-temperature cycle performance, high-temperature storage performance and low low-temperature DC impedance.

[0118] In Examples 1-14, the content of ethylene carbonate (EC) in the secondary battery and the thickness of the substrate of the separator are within the range given in this application, and the secondary battery can simultaneously take into account good high-temperature cycle performance, high-temperature storage performance and low low-temperature DC impedance. In Examples 15-19, when the electrolyte salt of the secondary battery contains both lithium bis(fluorosulfonyl)imide (LiFSI) and lithium hexafluorophosphate (LiPF6), and the volume molar concentration of lithium bis(fluorosulfonyl)imide (LiFSI) in the electrolyte is 0.8 mol / L to 1.3 mol / L, and the volume molar concentration of lithium hexafluorophosphate (LiPF6) in the electrolyte is 0.15 mol / L to 0.4 mol / L, the performance of the secondary battery is further improved, especially the high-temperature cycle performance and low-temperature DC impedance of the secondary battery.

[0119] Compared with Examples 1-19, the high temperature cycle performance of the secondary batteries of Comparative Examples 1-6 is relatively poor. In the secondary batteries of Comparative Examples 1-2, the content of ethylene carbonate (EC) is higher than 20%, and the high temperature cycle and high temperature storage performance of the secondary batteries are deteriorated; the substrate thickness of the separator of the secondary batteries of Comparative Examples 3-6 is greater than 12 μm or less than 7 μm, and the high temperature cycle performance of the secondary batteries is deteriorated, and the high temperature storage performance and / or low temperature DC impedance are partially deteriorated.

[0120] In summary, the present invention effectively overcomes various shortcomings of the prior art and has high industrial utilization value.

[0121] The above embodiments are merely illustrative of the principles and effects of the present application and are not intended to limit the present application. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present application. Therefore, all equivalent modifications or changes made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed in the present application shall still be covered by the claims of the present application.

Claims

1. A secondary battery, include: A negative electrode sheet, comprising a negative electrode current collector and a negative electrode membrane sheet disposed on at least one surface of the negative electrode current collector and comprising a negative electrode active material; A separator, comprising a substrate and a coating disposed on at least one surface of the substrate; and Electrolytes, including organic solvents; in, The negative electrode active material includes silicon-based materials and carbon materials; The thickness of the substrate of the isolation film is 7 μm to 12 μm; The organic solvent includes ethylene carbonate EC, and the weight percentage of the ethylene carbonate EC in the organic solvent is ≤20%. The electrolyte solution also includes an electrolyte salt, wherein the electrolyte salt includes lithium bis(fluorosulfonyl)imide LiFSI and lithium hexafluorophosphate LiPF 6 ; The volume molar concentration of the lithium bis(fluorosulfonyl)imide LiFSI in the electrolyte is 0.8 mol / L to 1.3 mol / L, and the lithium hexafluorophosphate LiPF 6 The volume molar concentration in the electrolyte is 0.15 mol / L~0.4 mol / L.

2. The secondary battery according to claim 1, in, The weight percentage of the ethylene carbonate EC in the organic solvent is ≤15%.

3. The secondary battery according to claim 1, in, The weight percentage of the ethylene carbonate EC in the organic solvent is ≤10%.

4. The secondary battery according to any one of claims 1 to 3, in, The thickness of the substrate of the isolation film is 7 μm-10 μm.

5. The secondary battery according to any one of claims 1 to 3, in, The porosity of the isolation membrane is 25% to 50%.

6. The secondary battery according to claim 5, in, The porosity of the isolation membrane is 30% to 48%.

7. The secondary battery according to any one of claims 1 to 3, in, The organic solvent also includes one or more of ethyl methyl carbonate EMC, diethyl carbonate DEC, and dimethyl carbonate DMC.

8. The secondary battery according to claim 7, in, The weight percentage of the ethyl methyl carbonate EMC in the organic solvent is 60% to 95%.

9. The secondary battery according to claim 8, in, The weight percentage of the ethyl methyl carbonate EMC in the organic solvent is 75% to 95%.

10. The secondary battery according to claim 7, in, The content of diethyl carbonate DEC in the organic solvent accounts for ≤30% by weight.

11. The secondary battery according to claim 10, in, The content of diethyl carbonate DEC in the organic solvent accounts for ≤20% by weight.

12. The secondary battery according to claim 7, in, The content of dimethyl carbonate DMC in the organic solvent accounts for ≤15% by weight.

13. The secondary battery according to claim 12, in, The content of dimethyl carbonate DMC in the organic solvent accounts for ≤10% by weight.

14. The secondary battery according to claim 1, in, The volume molar concentration of the lithium bis(fluorosulfonyl)imide LiFSI in the electrolyte is 0.9 mol / L to 1.2 mol / L, and the lithium hexafluorophosphate LiPF 6 The volume molar concentration in the electrolyte is 0.15 mol / L~0.3 mol / L.

15. The secondary battery according to any one of claims 1 to 3, in, The conductivity of the electrolyte at 25° C. is 6.5 mS / cm to 9.5 mS / cm; and / or, The viscosity of the electrolyte at 25° C. is 3.5 mPa·s to 5.5 mPa·s.

16. The secondary battery according to claim 15, in, The conductivity of the electrolyte at 25° C. is 7 mS / cm to 9 mS / cm.

17. The secondary battery according to claim 15, in, The viscosity of the electrolyte at 25° C. is 4 mPa·s to 5 mPa·s.

18. The secondary battery according to any one of claims 1 to 3, in, The silicon-based material includes one or more of silicon, silicon alloy, silicon-oxygen compound, silicon-carbon compound, and silicon-nitrogen compound; and / or, The carbon material includes one or more of graphite, soft carbon and hard carbon.

19. The secondary battery according to claim 18, in, The silicon-based material includes a silicon-oxygen compound.

20. The secondary battery according to claim 18, in, The carbon material includes graphite, and the graphite is selected from one or more of artificial graphite and natural graphite.

21. The secondary battery according to any one of claims 1 to 3, in, The mass proportion of the silicon-based material in the negative electrode active material is ≤50%.

22. The secondary battery according to claim 21, in, The mass proportion of the silicon-based material in the negative electrode active material is 15% to 30%.

23. The secondary battery according to any one of claims 1 to 3, in, The thickness of the isolation film is 11 μm to 16 μm.

24. The secondary battery according to claim 23, in, The thickness of the isolation film is 12 μm to 14 μm.

25. The secondary battery according to any one of claims 1 to 3, in, The secondary battery also includes a positive electrode plate, which includes a positive electrode collector and a positive electrode membrane arranged on at least one surface of the positive electrode collector and including a positive electrode active material, wherein the positive electrode active material includes one or more of lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide.

26. The secondary battery according to claim 25, in, The positive electrode active material includes Li a Ni b Co c M d M' e O f A g or a Li having a coating layer disposed on at least a portion of the surface a Ni b Co c M d M' e O f A g One or more of the following: 0.8≤a≤1.2, 0.5≤b<1, 0<c<1, 0<d<1, 0≤e≤0.1, 1≤f≤2, 0≤g≤1, M is selected from one or two of Mn and Al, M' is selected from one or more of Zr, Al, Zn, Cu, Cr, Mg, Fe, V, Ti, and B, and A is selected from one or more of N, F, S, and Cl.

27. An electrical device comprising the secondary battery according to any one of claims 1 to 26.

Citation Information

Patent Citations

  • High energy density polymer lithium ion battery and preparation method thereof

    CN110391414A