Low density polyethylene with enhanced aluminum foil adhesion by incorporation of an acid copolymer resin
By adding acid copolymers to LDPE and using high-pressure radical polymerization method, a macromolecular structure with improved adhesion was prepared, which solved the problem of insufficient adhesion between LDPE and polar substrates, and enhanced the barrier properties of food packaging , suitable for medium to high extrusion coating linear speeds.
Patent Information
- Application Number
- CN202080055564.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-07-31
- Filing Date
- 2020-07-27
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-07-27
AI Technical Summary
The lack of adhesion between low-density polyethylene (LDPE) and polar substrates leads to a decrease in barrier properties of food packaging and food is prone to deterioration, especially at medium to high extrusion coating linear speeds, LDPE coating is used to the electrodes. The adhesion of the elastic substrate is low.
Using polymer blends containing at least 90% low density polyethylene (LDPE) and 1% to 10% acid copolymer, prepared by high pressure radical polymerization, chain transfer agents and initiators are added to control molecular weight and The melt index forms a macromolecular structure with improved adhesion.
It significantly improves the adhesion strength of LDPE coating to polar substrates, enhances the barrier properties of food packaging, ensures food safety and packaging stability, and is suitable for processing at medium to high extrusion coating linear speeds.
Smart Images

Figure BDA0003493741640000091 
Figure BDA0003493741640000092 
Figure BDA0003493741640000101
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to International Patent Application No. PCT / CN2018 / 098558 filed on July 31, 2019, the entire disclosure of which is hereby incorporated by reference. Technical Field
[0003] Embodiments of the present disclosure generally relate to polymer blends for extrusion coating or lamination and improved metal adhesion; and to films and coated substrates including the polymer blends. Background Art
[0004] Low-density polyethylene (LDPE) is widely used in extrusion coating to make food packaging, such as condiment bags, potato chip bags, and many flexible packaging. However, the low adhesion strength of LDPE to polar substrates (such as aluminum foil and metallized films) can lead to packaging failure, thereby compromising barrier properties and causing food spoilage. Adhesion to polar substrates is driven by polar functional groups (such as carbonyl groups). LDPE is non-polar and therefore generally has low adhesion to foils and metallized films. To enhance adhesion, LDPE can be extruded and coated at high temperatures (typically 280°C-330°C). High-temperature extrusion coating promotes oxidation of the polymer surface, which can produce carbonyl groups, resulting in better adhesion. In addition to temperature, the degree of oxidation is also related to the time the hot polymer is exposed to air before contacting the substrate to be coated. Extrusion coating lines operate at line speeds of 100 to 800 meters per minute (m / min). Fast line speeds can reduce oxidation. When less oxidation occurs, fewer carbonyl groups are formed, thereby reducing the ability of the LDPE coating to adhere to polar substrates. Summary of the invention
[0005] There is a continuing need for polymers or polymer blends that can be processed at medium to high extrusion coating line speeds (eg, 200 m / min to 800 m / min) and adhere well to polar substrates (eg, aluminum foil).
[0006] Embodiments of the present disclosure include polymer blends. Based on the total weight of the polymer blend, the polymer blend comprises at least 90% by weight of a low density polyethylene (LDPE) polymer and 1% to 10% by weight of an acid copolymer. In the polymer blend, the LDPE polymer has a melt index (I2) of 2g / 10min to 8g / 10min as measured according to ASTM D1238 (190°C, 2.16kg) and a molecular weight distribution (MWD) of 5 to 10.5 as measured by conventional gel permeation chromatography. In the polymer blend, the acid copolymer is a polymerization product of at least 60% by weight of ethylene monomers based on the total weight of monomers present in the ethylene acid copolymer; 1% to 20% by weight of monocarboxylic acid monomers based on the total weight of monomers present in the ethylene acid copolymer; and 0% to 20% by weight of alkyl acrylate monomers based on the total weight of monomers present in the ethylene acid copolymer.
[0007] Embodiments of the present disclosure include coated metal substrates.The coated metal substrate includes a metal substrate and a film of a polymer blend comprising any of the polymer blends of the present disclosure adhered to the metal substrate. DETAILED DESCRIPTION
[0008] Embodiments of the present disclosure include polymer blends. The polymer blends include at least 90 wt% of a low density polyethylene (LDPE) polymer and 1 wt% to 10 wt% of an acid copolymer, based on the total weight of the polymer blend.
[0009] In some embodiments of the polymer blend, the LDPE polymer has a melt index (I2) of 2 g / 10 min to 8 g / 10 min as measured according to ASTM D1238 (190° C., 2.16 kg). In various embodiments, the LDPE homopolymer has a melt index (I2) of 2 g / 10 mins to 7.7 g / 10 mins, 2 g / 10 mins to 6 g / 10 mins, 2 g / 10 mins to 5 g / 10 mins, or 2 g / 10 mins to 4.5 g / 10 mins.
[0010] In one or more embodiments of the polymer blend, the LDPE polymer has a molecular weight distribution (MWD = Mw / Mn) of 5 to 11, 8 to 10.5, or 8.5 to 11 as determined by conventional gel permeation chromatography (GPC) methods.
[0011] The density of the LDPE polymer may be from 0.910 g / cc to 0.930 g / cc. In some embodiments, the density of the LDPE polymer may be from 0.910 g / cc to 0.920 g / cc, from 0.916 g / cc to 0.930 g / cc, from 0.918 g / cc to 0.926 g / cc, or from 0.915 g / cc to 0.920 g / cc.
[0012] In some embodiments of the polymer blend, the LDPE polymer has a molecular weight of 0.910 g / cm 3 Up to 0.930g / cm 3 density and MWD of 8.5 to 10.5.
[0013] In one or more embodiments, the polymer blend comprises 1 wt % to 10 wt % of the acid copolymer. In some embodiments, the polymer blend comprises 2 wt % to 8 wt %, 3 wt % to 6 wt %, or 3 wt % to 5 wt % of the acid copolymer.
[0014] In various embodiments of the polymer blend, the acid copolymer is the polymerization reaction product of: at least 60 weight percent ethylene, based on the total weight of monomers present in the ethylene acid copolymer; from 1 weight percent to 20 weight percent monocarboxylic acid monomer, based on the total weight of monomers present in the ethylene acid copolymer; and from 0 weight percent to 20 weight percent alkyl acrylate monomer, based on the total weight of monomers present in the ethylene acid copolymer.
[0015] In one or more embodiments, the monocarboxylic acid monomer of the acid copolymer may be present in the acid copolymer in an amount of 1 wt % to 15 wt %, based on the total weight of monomers present in the vinyl copolymer. In some embodiments, the monocarboxylic acid monomer may be present in an amount of 2 wt % to 20 wt %, 2 wt % to 10 wt %, or 2 wt % to 5 wt %, based on the total weight of monomers present in the acid copolymer.
[0016] In some embodiments of the polymer blend, the ethylene acid copolymer comprises at least 65 weight percent ethylene monomer, based on the total weight of the monomers in the ethylene acid copolymer; 1 weight percent to 15 weight percent monocarboxylic acid monomer, based on the total weight of the monomers in the ethylene acid copolymer; and 0 weight percent to 15 weight percent alkyl acrylate, based on the total weight of the monomers in the ethylene acid copolymer.
[0017] In one or more embodiments, the ethylene acid copolymer comprises at least 75 wt % ethylene; 2 to 6 wt % monocarboxylic acid monomer, based on the total weight of monomers in the ethylene acid copolymer; and 1 to 15 wt % alkyl acrylate, based on the total weight of monomers in the ethylene acid copolymer.
[0018] In various embodiments of the polymer blend, the monocarboxylic acid monomer includes acrylic acid, methacrylic acid, or a combination thereof.
[0019] In some embodiments of the polymer blend, the alkyl acrylate of the acid copolymer can be, for example, but not limited to, methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, or a combination thereof. In various embodiments, the alkyl acrylate is a C2-C8-alkyl acrylate, i.e., an alkyl acrylate having an alkyl group of 1 to 8 carbons.
[0020] In one or more embodiments of the polymer blend, the acid copolymer has a melt index (I2) of 2 g / 10 min to 30 g / 10 min as measured according to ASTM D1238 (190° C., 2.16 kg). In some embodiments, the acid copolymer has a melt index (I2) of 10 g / 10 mins to 30 g / 10 mins.
[0021] In one or more embodiments of the present disclosure, the polymer blend comprises a linear low density polyethylene (LLDPE) polymer in addition to the LDPE polymer and the acid copolymer. In one or more embodiments, the LLDPE polymer has a melt index (I2) of 0.5 g / 10 min to 30 g / 10 min as measured according to ASTM D1238 (190° C., 2.16 kg) and a viscosity of 0.910 g / cm 3 Up to 0.925g / cm 3 density.
[0022] In one or more embodiments of the polymer blend, the ethylene acid copolymer has a melt index (I2) of 2 to 12 g / 10 min as measured according to ASTM D1238 (190° C., 2.16 kg).
[0023] Embodiments of the present disclosure include coatings, wherein the coating comprises the polymer blend of the present disclosure.
[0024] Embodiments of the present disclosure include coated substrates. In some embodiments, the coated substrate is a coated polymer substrate. The coated polymer substrate includes a polymer substrate and a coating on the polymer substrate, the coating comprising any polymer blend of the present disclosure.
[0025] In one or more embodiments of the coated polymeric substrate, the polymeric substrate comprises polyethylene, polypropylene, polyethylene terephthalate, or polyamide. In some embodiments, the polymeric substrate is uniaxially or biaxially oriented.
[0026] In some embodiments, the coated substrate includes a coated metal substrate. The coated metal substrate includes a metal substrate and a coating on the metal substrate. The coating comprises any polymer blend of the present disclosure.
[0027] In some embodiments, the metal substrate comprises aluminum or a metallized polymer substrate, wherein the coating is adhered to the metallized surface of the metallized polymer substrate. In one or more embodiments, the polymer substrate is polyethylene terephthalate (PET), polyethylene, polypropylene, or polyamide.
[0028] Embodiments of the present disclosure include multi-layer structures.In embodiments, the multi-layer structure includes a second substrate in contact with the coating layer of the coated substrate.
[0029] In one or more embodiments, the coating has a peel strength of at least 0.6 N / in, at least 0.7 N / in, at least 1 N / in, or at least 2 N / in as measured by ASTM F904.
[0030] polymerization
[0031] For high pressure, free radical initiated polymerization processes, two basic types of reactors are known. The first type is a stirred autoclave vessel with one or more reaction zones (autoclave reactor). The second type is a jacketed tube with one or more reaction zones (tubular reactor).
[0032] The pressure in each autoclave and tubular reactor zone of the process is typically from 100 MPa to 400 MPa, from 120 MPa to 360 MPa, or from 150 MPa to 320 MPa.
[0033] The polymerization temperature in each tubular reactor zone of the process is typically from 100°C to 400°C, from 130°C to 360°C, or from 140°C to 330°C.
[0034] The polymerization temperature in each autoclave reactor zone of the process is typically from 150°C to 300°C, from 165°C to 290°C, or from 180°C to 280°C.
[0035] A tubular reactor having at least three reaction zones can be used to produce LDPE of polymer blends.
[0036] In order to produce LDPE, a high pressure, free radical initiated polymerization process is usually used. Typically, a jacketed tube is used as a reactor, which has one or more reaction zones. Suitable (but not limiting) reactor lengths may be from 100 meters to 3000 meters (m) or from 1000 meters to 2000 meters. The beginning of the reaction zone of the reactor is usually defined by the side injection of the initiator, ethylene, chain transfer agent (or telomer) and any combination thereof of the reaction. The high pressure process can be carried out in one or more tubular reactors having one or more reaction zones or in a combination of an autoclave and a tubular reactor each comprising one or more reaction zones.
[0037] Chain transfer agents can be used to control molecular weight. In a preferred embodiment, one or more chain transfer agents (CTAs) are added to the process of the present invention. Typical CTAs that can be used include, but are not limited to, propylene, n-butane, 1-butene, isobutane, propionaldehyde, and methyl ethyl ketone. In one embodiment, the amount of CTA used in the process is 0.03 wt % to 10 wt % of the total reaction mixture. The ethylene used to produce LDPE can be purified ethylene, which is obtained by removing polar components from a loop recycle stream, or by using a certain reaction system configuration so that only newly made ethylene is used to make the polymer of the present invention. It is not typical to require that only purified ethylene be used to make ethylene-based polymers. In such cases, ethylene from a recycle loop can be used. In one embodiment, the ethylene-based polymer is LDPE.
[0038] Ethylene acid copolymers can be prepared by standard free radical copolymerization methods, using high pressure, operating in a continuous manner. Monomers are fed into the reaction mixture in a ratio relevant to monomer activity and the required monomer amount incorporated into the copolymer. In this way, the monomer units are uniformly and nearly randomly distributed along the chain. Unreacted monomers are recyclable. Additional information about the preparation of ethylene acid copolymers can be found in U.S. Patent No. 3,264,272 and U.S. Patent No. 4,766,174, each of which is incorporated by reference in its entirety.
[0039] Initiator
[0040] The method for producing the LDPE of the polymer blend of the present disclosure is a free radical polymerization method. The type of free radical initiator used in the present method is not important, but one of the initiators preferably used should allow high temperature operation in the range of 300° C. to 350° C. Examples of suitable free radical initiators include organic peroxides such as peresters, perketals, peroxyketones, percarbonates and cyclic multifunctional peroxides. These organic peroxy initiators are added to the reactor in an amount of 0.005 wt % to 0.2 wt % based on the total weight of polymerizable monomers in the reactor. The peroxide is typically injected in the form of a dilute solution in a suitable solvent, such as a hydrocarbon solvent.
[0041] Other suitable initiators include azodicarboxylates, azodicarboxylic acid dinitriles, and 1,1,2,2-tetramethylethane derivatives, as well as other components capable of forming free radicals within the desired operating temperature range.
[0042] In one embodiment, the initiator is added to at least one reaction zone of the polymerization reactor. In other embodiments, the initiator is added to the reactor or polymerization process at a peak polymerization temperature of 320° C. to 350° C. In other embodiments, the initiator comprises at least one peroxide group incorporated into a ring structure.
[0043] Examples of initiators suitable for polymerizing polyethylene include, but are not limited to, TRIGONOX 301 (3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane) and TRIGONOX 311 (3,3,5,7,7-pentamethyl-1,2,4-trioxepane), both available from Akzo Nobel; and HMCH-4-AL (3,3,6,6,9,9-hexamethyl-1,2,4,5-tetraoxacyclononane), available from United Initiators. Additional initiators are disclosed in International Publications WO 02 / 14379 and WO 01 / 68723, both of which are incorporated herein by reference.
[0044] Polymer Manufacturing
[0045] The polymer blends of the present disclosure may be used in a variety of thermoplastic manufacturing processes to produce useful articles, including extrusion coating and extrusion lamination.
[0046] definition
[0047] Unless stated to the contrary, implicit from the context, or customary in the art, all parts and percentages are by weight and all test methods are current as of the filing date of this disclosure.
[0048] The term "blend" or "polymer blend" as used in this disclosure refers to an intimate physical mixture of two or more polymers without chemical reactions between the polymers. The blend may be miscible and not phase separated at the molecular level, or may be immiscible and exhibit a certain degree of phase separation at the molecular level. The blend may or may not include one or more domain configurations that may be determined by transmission electron spectroscopy, light scattering, x-ray scattering, and other methods known in the art. The blend may be affected by physically mixing two or more polymers at the macroscopic or microscopic level. Examples of physical mixing at the macroscopic level include melt blending or compounding of resins. Examples of physical mixing at the microscopic level include forming two or more polymers simultaneously in the same reactor.
[0049] The term "polymer" refers to a polymeric compound prepared by polymerizing monomers of the same or a different type. The generic term polymer thus encompasses the terms "homopolymer" and "copolymer." The term "homopolymer" refers to a polymer prepared from only one type of monomer; the term "copolymer" refers to a polymer prepared from two or more different monomers.
[0050] The term "ethylene-based polymer" or "ethylene polymer" refers to a polymer that contains at least 50 weight percent polymerized ethylene (based on the total weight of the polymer). Ethylene-based polymers and ethylene polymers can be ethylene homopolymers or can include one or more than one comonomer, provided that ethylene has the largest polymer weight fraction among all monomers in the polymer.
[0051] The term "monocarboxylic acid monomer" means a molecule having a reactive moiety (such as a vinyl or vinylidene group) that can bond to other monomers to form a polymer and a carboxylic acid (-C(O)OH) moiety not included in the reactive moiety.
[0052] Test Method
[0053] Density: Samples for density measurement were prepared according to ASTM D 1928. Polymer samples were pressed at 190°C and 30,000 psi for three minutes and then at 21°C and 207 MPa for one minute. Measurements were made using ASTM D792, Method B within one hour of sample pressing.
[0054] Melt Index: Melt index or I2 (grams / 10 minutes or dg / min) is measured according to ASTM D 1238, Condition 190°C / 2.16 kg, Procedure B.
[0055] Triple Detector Gel Permeation Chromatography (3D-GPC)
[0056] The chromatographic system includes a PolymerChar GPC-IR (Valencia, Spain) high temperature GPC chromatograph equipped with an internal IR5 infrared detector (IR5) connected to a precision detector (Now Agilent Technologies) 2-angle laser scattering (LS) detector model 2040. For all light scattering measurements, a 15 degree angle is used for measurement purposes. The autosampler oven is set to 160°C, and the column chamber is set to 150°C. The columns that can be used are 4 Agilent "Mixed A" 30cm 20 micron linear mixed bed columns. The chromatographic solvents that can be used include 1,2,4-trichlorobenzene and contain 200ppm of butylated hydroxytoluene (BHT). The solvent source is nitrogen bubbling. The injection volume that can be used includes 200 microliters (μL) and a flow rate of 1.0 ml / min.
[0057] The GPC column set is calibrated with at least 20 narrow molecular weight distribution polystyrene standards ranging in molecular weight from 580 to 8,400,000, arranged in a cocktail of 6 with at least a decade of spacing, meaning that
[0058] There is an order of magnitude of about 10 times between the individual molecular weights. These standards are purchased from Agilent Technologies. Polystyrene standards are prepared at 0.025 grams in 50 milliliters of solvent for molecular weights equal to or greater than 1,000,000, and at 0.05 grams in 50 milliliters of solvent for molecular weights less than 1,000,000. Dissolve the polystyrene standards at 80 degrees Celsius for 30 minutes under gentle agitation. Use equation 1 to convert the polystyrene standard peak molecular weight to polyethylene molecular weight (as described in Williams and Ward, J. Polym. Sci., Polym. Let., 6, 621 (1968)):
[0059] M 聚乙烯 =A×(M 聚苯乙烯 ) B (Equation 1)
[0060] Where M is the molecular weight, A has a value of 0.4315 and B equals 1.0.
[0061] A fifth order polynomial was used to fit the calibration points to the corresponding polyethylene equivalents. A minor adjustment (approximately 0.415 to 0.44) was made to A to correct for column resolution and band broadening effects such that the NIST standard NBS 1475 was obtained at 52,000 g / mol Mw.
[0062] Total plate counts for the GPC column set were performed using eicosane (prepared at 0.04 g in 50 mL TCB and dissolved for 20 minutes with gentle agitation). Plate counts (Equation 2) and symmetry (Equation 3) were measured with a 200 μL injection volume according to the following equations:
[0063]
[0064] Where RV is the retention volume in milliliters, peak width is in milliliters, peak maximum is the maximum height of the peak, and 1 / 2 height is 1 / 2 the height of peak maximum.
[0065]
[0066] Where RV is the retention volume in milliliters, and peak width is in milliliters, peak maximum is the maximum peak position, tenth height is 1 / 10 the height of the peak maximum, and where post-peak refers to the tail of the peak at a later retention volume than the peak maximum, and where pre-peak refers to the front of the peak at an earlier retention volume than the peak maximum. The plate count of the chromatographic system should be greater than 24,000, and the symmetry should be between 0.98 and 1.22.
[0067] The samples were prepared semi-automatically using the PolymerChar "Instrument Control" software, where the target weight of the sample was set to 2 mg / mL and the solvent (containing 200 ppm BHT) was added to a septum-capped vial previously sparged with nitrogen by the PolymerChar high temperature autosampler. The samples were dissolved at 160°C for 2 hours with "low speed" shaking.
[0068] Based on the GPC results, the internal IR5 detector (measurement channel) of the PolymerCharGPC-IR spectrometer was used, according to Equations 4-6, using the PolymerChar GPCOne TM The software was used to calculate the Mn of the baseline-subtracted IR chromatogram at each equidistant data collection point (i) and the polyethylene equivalent molecular weight obtained from the narrow standard calibration curve at point (i) according to Equation 1. (GPC) 、Mw (GPC) and Mz (GPC) Calculation.
[0069]
[0070]
[0071]
[0072] To monitor deviations over time, a flow rate marker (decane) was introduced into each sample via a micropump controlled by the PolymerChar GPC-IR system. This flow rate marker (FM) was used to linearly correct the pump flow rate (flow rate (nominal)) for each sample by comparing the RV of the corresponding decane peak in the sample (RV (FM sample)) with the retention volume of the decane peak in the narrow standard calibration (RV (FM calibration)). It is assumed that any change in the decane marker peak time is related to a linear change in the flow rate (flow rate (effective)) throughout the run. In order to facilitate the highest accuracy in the RV measurement of the flow marker peak, a least squares fitting procedure was used to fit the peak of the flow marker concentration chromatogram to a quadratic equation. The first derivative of the quadratic equation was used to solve for the true peak position. After calibrating the system based on the flow marker peak, the effective flow rate (relative to the narrow standard calibration) was calculated as Equation 7. By PolymerCharGPCOne TM The software completes the processing of the flow marker peak. An acceptable flow rate correction is such that the effective flow rate should be within + / - 2% of the nominal flow rate. Flow Rate (Effective) = Flow Rate (Nominal) * (RV (FM Calibration) / RV (FM Sample)) (Equation 7)
[0073] The systematic method for determining multi-detector bias was performed in a manner consistent with that published by Balke, Mourey et al. (Mourey and Balke, Chromatography Polym. Chapter 12, (1992)) (Balke, Thitiratsakul, Lew, Cheung, Mourey, Chromatography Polym. Chapter 13, (1992)) using the PolymerChar GPCOne TM The software optimizes the triple detector log (MW and IV) results from broad homopolymer polyethylene standards (Mw / Mn>3) with the narrow standards column calibration results from the narrow standards calibration curve.
[0074] Extrusion Coating: Extrusion coating trials were conducted using a Black–Clawson line following a standard coating procedure. Briefly, a 3-layer extrusion coating (EC) line was used with only the main 3.5-inch diameter extruder (30:1 L / D) powered by a 150HP Eurotherm drive extruding a single layer of coating. The primary barrel had six heating zones with a temperature profile of 179°C, 230°C, 286°C, 316°C, 317°C, 318°C (354°F, 446°F, 546°F, 601°F, 603°F, 605°F). A Nordson EDI 36-inch Autoflex TMThe die is set with a die gap of 0.5mm-0.6mm (0.020") and an air gap of 153mm (6 inches). The line is equipped with a 30-inch cooling roll, a nip roll, a backup roll and a shear slitter.
[0075] Extrusion coating was conducted at 25 gsm at 600°F (315°C), 90 RPM screw speed and 250 lbs / hr, 24 inch die width, 20 mil die gap, which translated to a coating thickness of 1.2 mils (30 microns) at 440 ft / min.
[0076] Peel strength measured by peel test
[0077] The polymer or polymer blend was extrusion coated on an aluminum plate (aluminum foil laminated with LDPE and white paper, with a total thickness of 5.2 mils to 5.5 mils) by an extrusion coating process. The coating was applied to the aluminum side and had a thickness of 1.2 mils. Before the polymer or polymer blend was extruded and coated on the aluminum plate, a masking tape was placed on a portion of the aluminum plate. Since the adhesion between the masking tape and the coating was weak, the masking tape could be peeled off from the coating before the peel test. Then, the peel test was used to obtain the peel strength between the coating and the aluminum plate.
[0078] Prior to testing peel strength, the samples were conditioned at 23° C. (± 2° C.) and 50% (± 10%) relative humidity (RH) for a minimum of 40 hours.
[0079] The extrusion coated sheet to be tested is cut into 1 inch wide strips in the machine direction with the longer side oriented in the machine direction. The coating is peeled off the aluminum plate (starting from the location of the masking tape), and then the two jaws of the tensile tester clamp the peeled coating and the ends of the aluminum plate. The entire sample is then slowly pulled at a speed of 1 in / min to eliminate slack. The sample is then tested at a speed of 12 in / min. Five samples are tested and the average peak load and the average load over a range of 3 inches (1 inch to 4 inches) are reported.
[0080] The peel strength improvement rate (%) was obtained from the following equation.
[0081]
[0082] Peel strength is the peak load obtained from the peel test.
[0083] Example
[0084] Twenty-five example compositions were prepared and the polymer properties of each composition were measured. Each example composition was a blend of LDPE homopolymer and acid copolymer. The properties of LDPE homopolymer are listed in Table 1.
[0085] Table 1: Polymer properties of LDPE homopolymer
[0086]
[0087] Example 1 is 95 wt% AGILITY manufactured by Dow, Inc. TM EC 7030 as the LDPE component and 5 wt% of an acid copolymer. The acid copolymer comprises 2 wt% methacrylic acid, 6 wt% isobutyl acrylate and 92 wt% ethylene based on the total weight of the monomers of the acid copolymer and has a melt index of 10 dg / min. Example 2 is a 95 wt% AGILITY TM A polymer blend prepared with EC 7030 as the LDPE component and 5 wt% of an acid copolymer comprising 10 wt% methacrylic acid, 10 wt% isobutyl acrylate and 80 wt% ethylene based on the total weight of the monomers of the acid copolymer and having a melt index of 10 dg / min.
[0088] Example 3 is 95 wt% AGILITY manufactured by Dow, Inc. TM A polymer blend prepared with EC 7030 as the LDPE component and 5 wt% of an acid copolymer comprising 9 wt% methacrylic acid and 91 wt% ethylene based on the total weight of the monomers of the acid copolymer and having a melt index of 10 dg / min.
[0089] Example 4 is 95 wt% AGILITY manufactured by Dow, Inc. TM A polymer blend prepared with EC 7000 as the LDPE component and 5 wt% of an acid copolymer comprising 9 wt% methacrylic acid and 91 wt% ethylene based on the total weight of the monomers of the acid copolymer and having a melt index of 10 dg / min.
[0090] Example 5 is 95 wt% AGILITY manufactured by Dow, Inc. TM A polymer blend prepared with EC 7000 as the LDPE component and 5 wt% of an acid copolymer comprising 2 wt% methacrylic acid and 6 wt% isobutyl acrylate and 92 wt% ethylene based on the total weight of the monomers of the acid copolymer and having a melt index of 10 dg / min.
[0091] Example 6 is a polymer blend prepared from 95 wt% LDPE 5005 manufactured by Dow, Inc. as the LDPE component and 5 wt% of an acid copolymer. The acid copolymer comprises 2 wt% methacrylic acid and 6 wt% isobutyl acrylate and 92 wt% ethylene based on the total weight of the monomers of the acid copolymer and has a melt index of 10 dg / min.
[0092] Example 7 is a polymer blend prepared from 95 wt% LDPE PG 7008 manufactured by Dow, Inc. as the LDPE component and 5 wt% of an acid copolymer. The acid copolymer comprises 2 wt% methacrylic acid and 6 wt% isobutyl acrylate and 92 wt% ethylene based on the total weight of the monomers of the acid copolymer and has a melt index of 10 dg / min.
[0093] Example 8 is a polymer blend prepared from 95 wt% LDPE 4016 manufactured by Dow, Inc. as the LDPE component and 5 wt% of an acid copolymer. The acid copolymer comprises 2 wt% methacrylic acid and 6 wt% isobutyl acrylate and 92 wt% ethylene based on the total weight of the monomers of the acid copolymer and has a melt index of 10 dg / min.
[0094] Example 9 is a polymer blend prepared from 95 wt% LDPE 621I manufactured by Dow, Inc. as the LDPE component and 5 wt% of an acid copolymer. The acid copolymer comprises 2 wt% methacrylic acid and 6 wt% isobutyl acrylate and 92 wt% ethylene based on the total weight of the monomers of the acid copolymer and has a melt index of 10 dg / min.
[0095] Example 10 is a polymer blend prepared from 95 wt% LDPE 722 manufactured by Dow, Inc. as the LDPE component and 5 wt% of an acid copolymer. The acid copolymer comprises 2 wt% methacrylic acid and 6 wt% isobutyl acrylate and 92 wt% ethylene based on the total weight of the monomers of the acid copolymer and has a melt index of 10 dg / min.
[0096] Example 11 is a polymer blend prepared from 95 wt% LDPE 4010 manufactured by Dow, Inc. as the LDPE component and 5 wt% of an acid copolymer. The acid copolymer comprises 2 wt% methacrylic acid and 6 wt% isobutyl acrylate and 92 wt% ethylene based on the total weight of the monomers of the acid copolymer and has a melt index of 10 dg / min.
[0097] Example 12 is a polymer blend prepared from 95 wt% LDPE 621I manufactured by Dow, Inc. as the LDPE component and 5 wt% of an acid copolymer. The acid copolymer comprises 9 wt% methacrylic acid and 91 wt% ethylene based on the total weight of the monomers of the acid copolymer and has a melt index of 10 dg / min.
[0098] Example 13 is a polymer blend prepared from 95 wt% LDPE 5005 manufactured by Dow, Inc. as the LDPE component and 5 wt% of an acid copolymer. The acid copolymer comprises 9 wt% methacrylic acid and 91 wt% ethylene based on the total weight of the monomers of the acid copolymer and has a melt index of 10 dg / min.
[0099] Example 14 is a polymer blend prepared from 95 wt% LDPE 722 manufactured by Dow, Inc. as the LDPE component and 5 wt% of an acid copolymer. The acid copolymer comprises 9 wt% methacrylic acid and 91 wt% ethylene based on the total weight of the monomers of the acid copolymer and has a melt index of 10 dg / min.
[0100] Example 15 is a polymer blend prepared from 95 wt% LDPE PG 7008 manufactured by Dow, Inc. as the LDPE component and 5 wt% of an acid copolymer. The acid copolymer comprises 9 wt% methacrylic acid and 91 wt% ethylene based on the total weight of the monomers of the acid copolymer and has a melt index of 10 dg / min.
[0101] Example 16 is a polymer blend prepared from 95 wt% LDPE 4010 manufactured by Dow, Inc. as the LDPE component and 5 wt% of an acid copolymer. The acid copolymer comprises 9 wt% methacrylic acid and 91 wt% ethylene based on the total weight of the monomers of the acid copolymer and has a melt index of 10 dg / min.
[0102] Example 17 is a polymer blend prepared from 95 wt% LDPE 4016 manufactured by Dow, Inc. as the LDPE component and 5 wt% of an acid copolymer. The acid copolymer comprises 9 wt% methacrylic acid and 91 wt% ethylene based on the total weight of the monomers of the acid copolymer and has a melt index of 10 dg / min.
[0103] Example 18 is a polymer blend prepared from 95 wt% LDPE 621I manufactured by Dow, Inc. as the LDPE component and 5 wt% of an acid copolymer. The acid copolymer comprises 10 wt% methacrylic acid and 10 wt% isobutyl acrylate and 80 wt% ethylene based on the total weight of the monomers of the acid copolymer and has a melt index of 10 dg / min.
[0104] Example 19 is a polymer blend prepared from 95 wt% LDPE 5005 manufactured by Dow, Inc. as the LDPE component and 5 wt% of an acid copolymer. The acid copolymer comprises 10 wt% methacrylic acid and 10 wt% isobutyl acrylate and 80 wt% ethylene based on the total weight of the monomers of the acid copolymer and has a melt index of 10 dg / min.
[0105] Example 20 is a polymer blend prepared from 95 wt% LDPE 722 manufactured by Dow, Inc. as the LDPE component and 5 wt% of an acid copolymer. The acid copolymer comprises 10 wt% methacrylic acid and 10 wt% isobutyl acrylate and 80 wt% ethylene based on the total weight of the monomers of the acid copolymer and has a melt index of 10 dg / min.
[0106] Example 21 is a polymer blend prepared from 95 wt% LDPE PG 7008 manufactured by Dow, Inc. as the LDPE component and 5 wt% of an acid copolymer. The acid copolymer comprises 10 wt% methacrylic acid and 10 wt% isobutyl acrylate and 80 wt% ethylene based on the total weight of the monomers of the acid copolymer and has a melt index of 10 dg / min.
[0107] Example 22 is a polymer blend prepared from 95 wt% LDPE 4010 manufactured by Dow, Inc. as the LDPE component and 5 wt% of an acid copolymer. The acid copolymer comprises 10 wt% methacrylic acid and 10 wt% isobutyl acrylate and 80 wt% ethylene based on the total weight of the monomers of the acid copolymer and has a melt index of 10 dg / min.
[0108] Example 23 is a polymer blend prepared from 95 wt% LDPE 4016 manufactured by Dow, Inc. as the LDPE component and 5 wt% of an acid copolymer. The acid copolymer comprises 10 wt% methacrylic acid and 10 wt% isobutyl acrylate and 80 wt% ethylene based on the total weight of the monomers of the acid copolymer and has a melt index of 10 dg / min.
[0109] Example 24 is 97 wt % AGILITY manufactured by Dow, Inc.TM A polymer blend prepared with EC 7030 as the LDPE component and 3 wt% of an acid copolymer comprising 4 wt% methacrylic acid and 15 wt% isobutyl acrylate and 81 wt% ethylene based on the total weight of the monomers of the acid copolymer and having a melt index of 27 dg / min (g / 10 mins).
[0110] Example 25 is 97 wt % AGILITY TM Polymers prepared with EC 7000 as LDPE component and 3 wt% acid copolymer
[0111] Blends. The acid copolymer contained 4 wt% methacrylic acid and 15 wt% isobutyl acrylate and 81 wt% ethylene based on the total weight of the monomers of the acid copolymer and had a melt index of 27 dg / min (g / 10 mins).
[0112] The properties of each polymer blend and comparative polymer are summarized in Table 2.
[0113] Table 2: Peel strength of polymer blends
[0114]
[0115]
[0116] *Peel bond strength is reported as the average peel strength from 1 inch extension to 4 inches extension or until sample failure if less than 4 inches; and the bonded substrate is aluminum foil laminate.
[0117] ** Improved peel strength calculated from the difference between the peel strength of pure LDPE and the peel strength of LDPE and acid copolymer.
[0118] ***The improved peel strength (%) is calculated by the following formula:
[0119]
[0120] ****Blends should not be run on extrusion coating lines with line speeds greater than 440 ft / min (134 m / min).
[0121] Adding 5 weight percent of the acid copolymer to the LDPE polymer produces a polymer blend having a greater peel strength than the LDPE polymer.
Claims
1. A polymer blend, comprising: at least 90 wt. % of a low density polyethylene, LDPE polymer, based on the total weight of the polymer blend, the LDPE polymer having a melt index I2 of 2 to 5.8 g / 10 min as measured at 190° C. and 2.16 kg according to ASTM D1238 and a molecular weight distribution MWD of 5 to 10.5 as measured by conventional gel permeation chromatography; and 2 to 6 wt % of an ethylene acid copolymer, based on the total weight of the polymer blend, wherein the ethylene acid copolymer is the polymerization reaction product of: at least 60 weight percent ethylene, based on the total weight of monomers present in the ethylene acid copolymer; 1 to 20 wt % of a monocarboxylic acid monomer, based on the total weight of the monomers present in the ethylene acid copolymer; and 0 wt % to 20 wt % alkyl acrylate monomers based on the total weight of the monomers present in the ethylene acid copolymer.
2. The polymer blend of claim 1, wherein the LDPE polymer has a 3 Up to 0.935g / cm 3 density and MWD of 8.5 to 10.
5.
3. The polymer blend of claim 1, wherein the LDPE polymer has a melt index of 2 to 4.5 g / 10 min as measured according to ASTM D1238 at 190°C and 2.16 kg.
4. The polymer blend according to claim 1, further comprising a melt index I2 of 0.5 g / 10 min to 30 g / 10 min and a viscosity of 0.910 g / cm2 as measured at 190°C and 2.16 kg according to ASTM D1238. 3 Up to 0.935g / cm 3 Linear low density polyethylene LLDPE polymer with a density of .
5. The polymer blend of claim 1, further comprising an ethylene copolymer having a melt index I2 of 0.5 g / 10 min to 30 g / 10 min as measured at 190° C. and 2.16 kg according to ASTM D1238, wherein the ethylene copolymer comprises the reaction product of: at least 50 weight percent ethylene, based on the total weight of said monomers present in said ethylene acid copolymer; and 0.1 wt% to 40 wt% of a comonomer selected from vinyl acetate, acrylate or carboxylic acid comonomers, based on the total weight of the monomers present in the ethylene copolymer.
6. The polymer blend of claim 1, wherein the ethylene acid copolymer has a melt index I2 of 2 to 30 g / 10 min as measured at 190°C and 2.16 kg according to ASTM D1238.
7. The polymer blend of claim 1, wherein the alkyl acrylate monomer comprises methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, or a combination thereof, and the monocarboxylic acid monomer comprises acrylic acid, methacrylic acid, or a combination thereof.
8. The polymer blend of claim 1, wherein the ethylene acid copolymer comprises at least 65 wt% ethylene monomer, based on the total weight of the monomers in the ethylene acid copolymer; 1 wt% to 15 wt% monocarboxylic acid monomer, based on the total weight of the monomers in the ethylene acid copolymer; and 0 wt% to 15 wt% alkyl acrylate, based on the total weight of the monomers in the ethylene acid copolymer.
9. The polymer blend of claim 1, wherein the ethylene acid copolymer comprises at least 75 weight percent ethylene monomer, based on the total weight of the monomers in the ethylene acid copolymer; 2 weight percent to 6 weight percent monocarboxylic acid monomer, based on the total weight of the monomers in the ethylene acid copolymer; and 1 weight percent to 15 weight percent alkyl acrylate, based on the total weight of the monomers in the ethylene acid copolymer.
10. A coated metal substrate, comprising: Metal substrate; as well as A coating comprising a polymer blend according to any preceding claim adhered to the metal substrate.
11. The coated metal substrate of claim 10, wherein the metal substrate comprises aluminum.
12. The coated metal substrate of claim 10, wherein the coating has a peel strength of at least 0.6 N / in as measured by ASTM F904.
13. The coated metal substrate of claim 10, wherein the coating has a peel strength of at least 1 N / in as measured by ASTM F904.
14. The coated metal substrate of claim 10, wherein the coating has a peel strength of at least 2 N / in as measured by ASTM F904.
15. An extruded article comprising the polymer blend of claim 1.