Recording tape with elastic substrate

By using polyetheretherketone (PEEK) substrate and radiation-induced grafting technology, the problem of tape material being sensitive to humidity and temperature is solved, achieving higher dimensional stability and mechanical properties, improving data density and reading and writing reliability. sex.

CN114365220BActive Publication Date: 2024-10-01INTERNATIONAL BUSINESS MACHINE CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080063423.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-09-17
Filing Date
2020-09-16
Publication Date
2024-10-01
Estimated Expiration
2040-09-16

AI Technical Summary

Technical Problem

Existing tape backing materials are sensitive to humidity and temperature, causing tape size instability and affecting data density and reliability of read and write operations.

Method used

Polyetheretherketone (PEEK) is used as the substrate material, and the bottom layer and recording layer are connected to the substrate through radiation-induced grafting technology to improve the interlayer bonding strength and dimensional stability.

Benefits of technology

PEEK substrate material shows stable creep and recovery in the range of 0 to 60℃, low water absorption, and tensile storage modulus in the range of 4GPa to 20GPa, which significantly improves the mechanical properties and dimensional stability of the tape and reduces Sensitivity to humidity and temperature.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114365220B_ABST
    Figure CN114365220B_ABST
Patent Text Reader

Abstract

The present invention relates to a recording tape. According to one method, the recording tape comprises a substrate (604) comprising polyetheretherketone (PEEK). A bottom layer (606) is located on the substrate (604). A recording layer (608) is located on the bottom layer (606).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to magnetic recording media, and more particularly to various configurations of substrates for recording magnetic tape media. Background Art

[0002] In a magnetic storage system, a magnetic transducer reads data from and writes data to a magnetic recording medium. Data is written to a magnetic recording medium by moving the magnetic recording transducer to the location on the medium where the data is to be stored. The magnetic recording transducer then generates a magnetic field that encodes the data into the magnetic medium. Data is read from the medium by similarly positioning a magnetic reading transducer and then sensing the magnetic field of the magnetic medium. The read and write operations can be independently synchronized with the media movement to ensure that data can be read from and written to the desired location on the medium.

[0003] An important and ever-present goal in the data storage industry is to increase the density of data stored on the media. For magnetic tape storage systems, this goal has resulted in an increase in the track and linear bit density on the recording tapes and a decrease in the thickness of the tape media. However, developing higher performance tape drive systems in a smaller footprint has created various challenges ranging from the design of the tape head assemblies used in such systems to coping with tape dimensional instabilities.

[0004] One increasingly limiting format issue that has emerged as track and data densities have increased is tape dimensional stability, particularly lateral dimensional stability. Lateral shrinkage and expansion of tape is a well-known phenomenon that occurs due to a variety of effects including water absorption, thermal expansion and contraction, etc. Variations in bandwidth can result in a number of adverse events, such as overwriting of previously written data tracks when shingled writing is performed, the inability to read data tracks that are no longer aligned with the reader (especially primarily toward the outer ends of the reader array), etc.

[0005] More permanent changes in the lateral dimensions of the media may also occur, such as long-term media creep (also known in the art as "aging"), which tends to occur over time as the tape is wound around the hub of a cassette. Long-term media creep is particularly problematic when dealing with tape dimensional stability issues because the two ends of the tape exhibit creep in different ways. The inner turns of tape located closest to the cassette hub tend to expand laterally over time due to the compressive stresses imposed on them by the turns of tape wound around them. The turns located toward the outer diameter of the tape reel are under less compressive stress but under higher tensile stress, which tends to result in lateral contraction of the tape, i.e., the tape becomes narrower over time. Thus, the ends of the tape tend to exhibit oppositely oriented lateral dimensional changes.

[0006] When the dimensions of the tape change, various problems arise. During a write, the likelihood of overwriting a shingled track increases. The overwritten data is generally unrecoverable. Also, in the event that the tape width has changed since the desired data was written, the reader may no longer be positioned on the track to be read, increasing read errors.

[0007] The substrate is usually the thickest layer in the recording tape and therefore tends to have the greatest impact on the lateral stability of the tape. In other words, the substrate tends to dominate the dimensional variations of the entire laminated tape structure.

[0008] Current recording tape substrate materials, such as polyethylene naphthalate (PEN) and aramid, suffer from a variety of problems, such as poor tape dimensional stability (TDS), sensitivity to moisture, poor creep recovery, and / or other disadvantages, making them unsatisfactory for use in recording tapes having higher data densities than those currently on the market.

[0009] Existing substrates have reached the limits of possible improvements to improve their sensitivity to water and temperature and to overcome the above-mentioned problems.

[0010] Therefore, there is a need in the art to solve the above problems. Summary of the invention

[0011] Viewed from a first aspect, the present invention provides a recording magnetic tape comprising: a substrate comprising polyetheretherketone (PEEK); a base layer on the substrate; and a recording layer on the base layer.

[0012] From another aspect, the present invention provides a tape box comprising: a shell; and a recording tape at least partially stored in the shell, the recording tape comprising: a substrate comprising polyetheretherketone (PEEK), a bottom layer on the substrate, and a recording layer on the bottom layer.

[0013] Viewed from another aspect, the invention provides a method of manufacturing a recording tape, the method comprising: attaching a base layer to a substrate, the substrate comprising polyetheretherketone (PEEK).

[0014] Viewed from another aspect, the invention provides a method of manufacturing a recording tape, the method comprising: attaching an underlayer to a substrate by radiation induced grafting, the substrate comprising polyetheretherketone (PEEK); and attaching a recording layer to the underlayer.

[0015] According to one method, a recording magnetic tape includes a substrate comprising polyetheretherketone (PEEK). A bottom layer is located on the substrate. A recording layer is located on the bottom layer.

[0016] Recording tapes with PEEK substrates have excellent elasticity for typical tape operations, and exhibit stable creep and recovery for typical storage and operating temperatures of about 0 to about 60° C. It is expected that the shrinkage of the PEEK substrate will be less than 1% over a temperature range of 100° C., including the above operating range. These benefits are found in preferred processes where the chain length of the PEEK is greater than about 20, more preferably about 50 to about 100.

[0017] Recording tapes with PEEK substrates also have low sensitivity to temperature and humidity over the entire operating range described. PEEK is generally hydrophobic, making it water stable. At 50% relative humidity, water absorption is expected to be much less than 1%, which is much less than aramid, which tends to have an absorption of about 10% at 50% relative humidity.

[0018] Recording tapes with PEEK substrates have stable mechanical properties. For example, both the tensile storage (E') modulus and the tensile loss (E") modulus are lower than conventional media substrates, as measured by dynamic mechanical analysis methods such as dynamic mechanical thermal analysis (DMTA) for typical operating and storage environments of tape media. In one aspect, the tensile storage (E') modulus of the substrate measured by dynamic thermal mechanical analysis is in the range of about 4 GPa to about 20 GPa.

[0019] Another advantage of PEEK is that the PEEK raw material can be melted without degradation, which enables PEEK to be processed into films at temperatures around its melting point without losing its desired properties.

[0020] In one aspect, the bottom layer is grafted to the substrate. Grafting results in a stronger interlayer bond than conventional joining techniques, which is advantageous in terms of robustness and stress resistance.

[0021] Each of the above aspects is important to maintaining dimensional stability both in use and during long-term storage.

[0022] A tape cassette according to one aspect includes a housing and a recording tape at least partially stored in the housing. The recording tape has the configuration listed above.

[0023] Other aspects and methods of the present invention will become apparent from the following detailed description which, when taken in conjunction with the accompanying drawings, illustrates, by way of example, the principles of the invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The present invention will now be described, by way of example only, with reference to a preferred embodiment, as shown in the following drawings:

[0025] Figure 1A is a schematic diagram of a simplified tape drive system.

[0026] Figure 1B is a schematic diagram of a tape cassette according to one aspect of the present invention.

[0027] Figure 2A A side view of a flush-mounted bi-directional dual-module tape head is shown in accordance with one aspect of the present invention.

[0028] Figure 2B is from Figure 2A A view of the tape bearing surface taken along line 2B.

[0029] Figure 2C is from Figure 2B Detailed view of circle 2C taken.

[0030] Figure 3 A tape layout according to one approach is shown.

[0031] Figure 4A A scrambled servo pattern written into a dedicated area of ​​a tape medium according to one approach is shown.

[0032] Figure 4B A partial detailed view of a TBS pattern according to one approach is shown.

[0033] Figures 5A-5C is a local top-down representative view of the effects of tape expansion and contraction.

[0034] Figure 6 is a partial cross-sectional view of a basic structure of a magnetic recording medium according to various methods.

[0035] Figure 7 is a graph of dynamic mechanical thermal analysis (DMTA) results comparing the tensile storage modulus (E') in gigapascals (GPa) over the temperature range of a prior art tape substrate example and an 8 micron thick PEEK film.

[0036] Figure 8 Is a description Figure 7 Data is plotted over the temperature range of 0°C to -60°C.

[0037] Fig. 9 Exemplary PEEK according to various methods is shown.

[0038] Fig.10 Exemplary PEEK according to various methods is shown.

[0039] Fig.11 Exemplary PEEK according to various methods is shown.

[0040] Fig.12 Exemplary PEEK according to various methods is shown. DETAILED DESCRIPTION

[0041] The following description is intended to illustrate the general principles of the present invention, but is not intended to limit the inventive concepts claimed herein. In addition, the specific features described herein can be used in combination with other described features in all possible combinations and permutations.

[0042] Unless expressly defined otherwise herein, all terms are to be given their broadest possible interpretation, including the meaning implied in the specification and the meaning understood by those skilled in the art and / or defined in dictionaries, treatises, etc.

[0043] It must also be noted that, as used in the specification and the appended claims, the singular forms "a," "an," and "the" include plural referents unless otherwise indicated.

[0044] The following description discloses various configurations of substrates that are particularly useful in recording tape media, and methods for forming the substrates and recording tape media.

[0045] In one general method, a recording tape includes a substrate comprising polyetheretherketone (PEEK). A bottom layer is located on the substrate. A recording layer is located on the bottom layer.

[0046] In another general approach, a magnetic tape cassette includes a housing and a recording tape at least partially stored in the housing. The recording tape has a configuration as listed above.

[0047] Illustrative operating environment

[0048] Figure 1A A simplified tape drive 100 of a tape-based data storage system that may be used in the context of the present invention is shown. Figure 1A One specific implementation of a tape drive is shown in FIG. 1 , but it should be noted that the method described herein can be implemented in the context of any type of tape drive system.

[0049] As shown, a tape supply cassette 120 and a take-up reel 121 are provided to support a tape 122. One or more reels may form part of a removable cassette and need not be part of the tape drive 100. A tape drive such as Figure 1A The tape drive shown may also include a drive motor to drive the tape supply cassette 120 and take-up reel 121 to move the tape 122 over any type of tape head 126. Such a head may include an array of readers, writers, or both.

[0050] The guide 125 guides the tape 122 past the tape head 126. The tape head 126 is in turn connected to the controller 128 via the cable 130. The controller 128 can be or include a processor and / or any logic for controlling any subsystem of the drive 100. For example, the controller 128 generally controls the head functions, such as servo following, data writing, data reading, etc. The controller 128 can include at least one servo channel and at least one data channel, each of which includes data stream processing logic configured to process and / or store information to be written to and / or read from the tape 122. The controller 128 can operate under logic known in the art and any logic disclosed herein, and thus can be considered in various methods as a processor for any description of the tape drive included herein. The controller 128 can be connected to any known type of memory 136, which can store instructions that can be executed by the controller 128. In addition, the controller 128 can be configured and / or programmable to perform or control some or all of the methods presented herein. Thus, the controller 128 may be considered to be configured to perform various operations via logic programmed into one or more chips, modules and / or blocks, software, firmware, and / or other instructions available to one or more processors, etc., as well as combinations thereof.

[0051] Cable 130 may include read / write circuitry to send data to tape head 126 for recording on magnetic tape 122 and to receive data read by tape head 126 from magnetic tape 122. Actuator 132 controls the position of tape head 126 relative to magnetic tape 122.

[0052] An interface 134 may also be provided for communicating between the tape drive 100 and a host (internal or external) to send and receive data, and for controlling the operation of the tape drive 100 and communicating the status of the tape drive 100 to the host, all of which are understood by those skilled in the art.

[0053] Figure 1B An exemplary tape cartridge 150 is shown, which may include any configuration of the magnetic recording medium described herein in tape form in various methods. Such a tape cartridge 150 may be used with a computer such as Figure 1A As shown, the tape cartridge 150 includes a housing 152, a tape 122 in the housing 152, and an optional non-volatile memory 156 connected to the housing 152. In some approaches, the non-volatile memory 156 may be embedded in the housing 152, such as Figure 1BAs shown. In more methods, the non-volatile memory 156 can be attached to the inside or outside of the housing 152 without modifying the housing 152. For example, the non-volatile memory can be embedded in the self-adhesive label 154. In a preferred method, the non-volatile memory 156 can be a solid-state memory (e.g., flash memory), a read-only memory (ROM) device, etc. embedded or connected to the inside or outside of the tape cartridge 150. The non-volatile memory can be accessed by the tape drive and tape operating software (driver software) and / or another device.

[0054] As an example, Figure 2A A side view of a flat-mounted, bidirectional, dual-module tape head 200 that can be implemented in the context of the present invention is shown. As shown, the head includes a pair of substrates 202, each of which is equipped with a module 204 and is fixed at a small angle α relative to each other. The substrates can be "U-shaped beams" that are adhesively connected together. Each module 204 includes a substrate 204A and a closed body 204B having a thin film portion, which is generally referred to as a "gap", in which a reader and / or writer 206 is formed. In use, a magnetic tape 208 is moved on the module 204 along a medium (tape) bearing surface 209 in the manner shown so that data can be read and written on the magnetic tape 208 using the reader and writer. The wrap angle θ of the magnetic tape 208 at the edge entering and leaving the flat medium support surface 209 is typically between about 0.1 degrees and about 3 degrees.

[0055] The substrate 204A is typically constructed of a wear-resistant material such as ceramic. The closure 204B may be made of the same or similar ceramic as the substrate 204A.

[0056] The readers and writers can be arranged in a piggyback or merged configuration. An illustrative piggyback configuration includes a (magnetically inductive) writer transducer on top of (or below) a (magnetically shielded) reader transducer (e.g., a magnetoresistive reader, etc.), where the writer's poles and the reader's shield are typically separate. An exemplary merged configuration includes a reader shield in the same physical layer as a writer's pole (hence "merged"). The readers and writers can also be arranged in a staggered configuration. Alternatively, each channel array can be just a reader or a writer. Any of these arrays can include one or more servo track readers for reading servo data on the media.

[0057] Figure 2B Shows from Figure 2A 2B intercepts the tape bearing surface 209 of one of the modules 204. A representative tape 208 is shown in phantom. The modules 204 are preferably long enough to support the tape as the head steps between data tapes.

[0058] In this example, magnetic tape 208 includes 4 to 32 data strips, such as Figure 2B The illustrated tape 208 has 16 data bands and 17 servo tracks 210 on a half-inch wide tape. The data bands are defined between the servo tracks 210. Each data band may include many data tracks, for example, 1024 data tracks (not shown). During a read / write operation, the reader and / or writer 206 is positioned to a specific track location within one of the data bands. An external reader, sometimes referred to as a servo reader, reads the servo tracks 210. The servo signals are then used to keep the reader and / or writer 206 aligned with a specific set of tracks during a read / write operation.

[0059] Figure 2C Described in Figure 2B A plurality of readers and / or writers 206 are formed in gaps 218 on the modules 204 in circle 2C. As shown, the array of readers and writers 206 includes, for example, 16 writers 214, 16 readers 216, and two servo readers 212, although the number of elements may vary. Exemplary approaches include 8, 16, 32, 40, and 64 active readers and / or writers 206 per array, and optionally staggered designs having an odd number of readers or writers, such as 17, 25, 33, etc. Illustrative approaches include 32 readers per array and / or 32 writers per array, where the actual number of transducer elements may be greater, such as 33, 34, etc. This allows the tape to travel slower while reducing speed-induced tracking (track) and mechanical difficulties and / or performing fewer "wraps" to fill or read the tape. Although as Figure 2C As shown, the readers and writers can be arranged in a piggyback configuration, but the readers 216 and writers 214 can also be arranged in a staggered configuration. Alternatively, each array of readers and / or writers 206 can be only a reader or writer, and the array can include one or more servo readers 212. As considered together Figure 2A and 2B -2C notes that each module 204 may include a set of complementary readers and / or writers 206 for purposes such as bidirectional reading and writing, simultaneous read and write capabilities, backward compatibility, etc.

[0060] Timing-based servo systems

[0061] The write and read elements allow magnetic regions in the recording layer of the recording tape to be magnetized to form bits of magnetic segments that appear as rectangular portions showing increasing or decreasing magnetic signals detected by a magnetically sensitive detector such as a magnetic force microscope (MFM) detector.

[0062] Placing data in isolated tracks requires real-time position information about the location of existing written information on the tape to prevent accidental erasure of previously written information. In the case of an initial write of data to a formatted tape that contains no written data, the location of the initial data band needs to be carefully controlled and recorded to allow subsequent data bands to be correctly positioned so as not to overwrite or encroach on previously written data.

[0063] Modern high density tape formats use very precise servo patterns known as timing based servo, which are well known to those skilled in the art. A description of an illustrative timing based servo scheme is provided below.

[0064] Track following servo involves transitions that are recorded at more than one azimuth orientation across the width of the servo track. In a controlled, precise factory format operation, the timing of the signal derived from a read at any point across the width of the written pattern created in the tape media is used to calculate the position of the recording head in real time. The pattern is read by a servo reader that is small in width compared to the servo track width. The combination of a wide servo pattern and a narrow servo reader provides excellent position sensing linearity and dynamic range.

[0065] Position sensing with a timing-based servo system is accomplished by deriving the ratio of the two servo pattern spacings and is therefore insensitive to tape velocity during readback of the recorded signal. Detecting the center of the servo pattern during tape motion provides a precise reference point for each data band. The difference between the centers of the two servo readers used in each read or write movement of the tape across the recording head is a measure of the spacing between two servo bands on the tape previously recorded during factory formatting. The servo readers are fixed in the head structure but move on a very small nanometer scale due to stress and environmental factors. Therefore, the actual spacing positions between the servo bands written on the tape do move relative to each other and result in changes in the actual spacing between data bands previously existing or written on existing data tracks.

[0066] Temporary reference Figure 3 , depicts an illustrative tape layout according to one method. As shown, tape 300 has a tape layout that implements five servo bands 0-servo bands 4 and four data bands 0-data bands 3, such as the LTO format and 300. The height H of each servo band is measured in a cross-track direction 304 approximately orthogonal to the length L of the tape 300. According to one example, according to the LTO format, the height H of each servo band can be approximately 186 microns. In addition, also according to the LTO format, the spacing β between the servo bands shown can be approximately 2859 microns.

[0067] An exemplary tape head 302 is also shown as having two modules and positioned on a portion of the tape 300 according to one approach. The read and / or write transducers can be positioned on either module of the tape head 302 according to any of the approaches described herein and can be used to read data from and / or write data to the data tape. In addition, the head 302 can include a servo reader that can be used to read the servo patterns in the servo tape according to any of the approaches described herein. It should also be noted that Figure 3 The dimensions of the various components included in the drawings are presented by way of example only and are by no means limiting.

[0068] Some tape drives may be configured to operate at low tape speeds and / or with nano head position settings. These tape drives may use servo formats targeting barium ferrite (BaFe) tape media, 4 or 8 data bands, 32 or 64 data lanes operation, allow very low speed operation, support large bandwidth actuator operation, and improve parameter estimation to minimize the standard deviation of the position error signal (PES), thereby enabling track density scaling for tape cartridge capacities up to 100TB and higher.

[0069] However, according to some methods, the tape may be further enhanced with additional features that provide additional functionality. Thus, an HD servo pattern may be implemented in place of a standard TBS servo pattern, e.g. Figure 3 As shown, the HD servo pattern can be used to improve the track following performance.

[0070] In yet other methods, a standard TBS servo pattern (e.g., Figure 3 ) may be combined with one or more HD servo patterns (e.g., see below Figure 4A ) combination implementation. One implementation includes a hybrid servo pattern pattern in which the standard TBS pattern is retained and an additional HD pattern is provided in a dedicated, preferably currently unused area of ​​the tape media. In some approaches, this type of pattern can be achieved by increasing the number of data channels from 16 to 32 and reducing the width of the TBS pattern from 186 microns to 93 microns.

[0071] Figure 4AA hybrid servo pattern 410 is shown that includes a standard TBS pattern 402 written in a servo band and an HD pattern 404 written in an HD band (e.g., a dedicated area) of a magnetic tape medium 408. In addition, each HD pattern 404 includes many HD tracks, each HD track having its own periodic waveform. In some approaches, the salient features of the original TBS pattern 402 are retained, such as a servo frame structure consisting of four servo bursts containing many servo stripes, where the servo stripes of adjacent servo bursts are written at alternating azimuth angles. Other parameters of the conventional servo pattern, such as the servo pattern height and other geometric dimensions, and the number of servo stripes per burst, may be modified as desired.

[0072] The HD pattern 404 may include periodic waveforms of various frequencies written alternately in the length direction L along the longitudinal axis of the tape. The standard TBS pattern 402 may be used to provide initial identification of the servo band (e.g., by providing a servo band ID); initial positioning of the head 406 at the appropriate servo position; acquisition of initial servo channel parameters such as tape speed, lateral head position, head-tape skew, longitudinal position (LPOS), etc., etc. In addition, the HD pattern 404 may enable more accurate and more frequent estimation of the servo channel parameters, thereby enabling improved head positioning over a much wider range of tape speeds and supporting greater bandwidth head actuation. In this way, track density scaling for very large cartridge capacities may be achieved, as well as improved data rate scaling to host computer requirements by supporting a wider range of speeds.

[0073] Reference again Figure 4A , which shows a tape layout 400 with a hybrid servo pattern 410 in which an HD pattern 404 is written in space adjacent to a standard TBS pattern 402, according to one approach. According to the present approach, since the TBS pattern 402 is used, no orthogonal sequence is included, which is contrary to products that implement servo functionality in hard disk drives.

[0074] See temporarily Figure 4B, a partial detailed view of a TBS pattern 402 (e.g., a TBS frame) according to an exemplary method is shown. As shown, a plurality of servo stripes 412 together form a servo burst 414, and corresponding servo bursts 414 pairs form a servo subframe. Thus, the described TBS frame has four servo bursts 414 and two servo subframes. In the present method, the servo bursts 414 included in the left servo subframe each have five servo stripes 412, while the servo bursts 414 included in the right servo subframe each have four servo stripes 412. The servo stripes 412 included in a given servo burst 414 are oriented so that they have the same azimuth slope represented by an angle α. In addition, corresponding servo bursts 414 pairs have opposite azimuth slopes, thereby forming a V-shaped pattern. The height H and thickness t of the servo stripes 412 may vary depending on the servo writer used to write the TBS pattern 402. According to an exemplary method which is by no means intended to limit the present invention, the height H may be about 186 μm, the angle α may be about 6°, and the thickness t may be about 2.1 μm. In addition, the spacing S between the servo stripes 412 and / or the distance d between the servo bursts 414 having the same azimuth slope may vary according to the desired method. According to an exemplary method which is by no means intended to limit the present invention, the spacing S may be about 5 μm, and the distance d may be about 100 μm. As described above, such as Figure 4B The patterned transitions shown allow an estimate of the lateral position of the head to be determined by evaluating the relative pulse timing generated by a servo reader that reads the servo stripes 412 of the servo burst 414 as they pass by the servo reader.

[0075] Tape Dimensional Stability Issues

[0076] Figures 5A-5C The effects of lateral expansion and contraction of the tape on the position of the transducer array relative thereto are described and are in no way intended to limit the invention. Figure 5A The transducer array 500 is depicted relative to a magnetic tape 502, wherein the magnetic tape has a nominal width. As shown, the transducers 504 are advantageously aligned with the data tracks 506 on the magnetic tape 502. However, Figure 5B The effect of lateral contraction of the tape is shown. As shown, the contraction of the tape also causes the data tracks to contract, resulting in the outermost transducer 505 being positioned along the outer edge of the outer data track. In addition, Figure 5C The effect of lateral expansion of the tape is depicted. Here, the expansion of the tape causes the data tracks to move farther apart, with the result that the outermost transducers 505 are positioned along the inner edges of the outer data tracks. If the tape contracts laterally by more than Figure 5B shown, or the tape expands laterally greater than Figure 5CAs shown, the outermost transducer 505 will cross over onto an adjacent track, causing the adjacent track to be overwritten during a write operation and / or causing the wrong track to be read back during a readback operation. In addition, operational effects, such as tape skew and lateral offset, may exacerbate this problem, particularly for tapes with shingled data tracks.

[0077] Thus, lateral expansion and contraction of tape is an ongoing problem in tape development and is currently the limiting factor in further reducing increasing data densities on tape.

[0078] Manufacturing of magnetic recording media and layers thereof

[0079] Figure 6 A partial cross-sectional view of the basic structure of a magnetic recording medium 600 not drawn to scale according to various methods described herein is shown. As an option, the magnetic recording medium 600 of the present invention can be implemented in combination with features from any other method listed herein, such as those described with reference to other figures. However, such a magnetic recording medium 600 and other media proposed herein can be used for various applications and / or replacements, which may or may not be specifically described in the illustrative methods listed herein. In addition, the magnetic recording medium 600 proposed herein can be used in any desired environment. The magnetic recording medium 600 in the various replacements disclosed herein has been developed to improve the stability and performance of the tape storage medium under the desired use and storage environment.

[0080] Unless otherwise described herein, the various layers of magnetic recording medium 600 can have conventional construction, design and / or function. In various methods, new and novel layers can be used with conventional layers. In further methods, multiple new and novel layers can be used with other conventional layers.

[0081] Unless otherwise described herein, the various layers of the magnetic recording medium 600 may be formed using conventional methods, particularly where the various layers have conventional structures.

[0082] The magnetic recording medium 600 is preferably a recording magnetic tape, but is otherwise a different type of deformable medium.

[0083] like Figure 6 As shown, there are generally four basic layers in the magnetic recording medium 600. An optional back coating layer 602 is disposed along one side (the lower side in the figure) of a substrate 604. An underlayer 606 is disposed along the other side (the upper side in the figure) of the substrate 604. A recording layer 608 is disposed on the underlayer 606. In various approaches, additional layers of conventional structure may be present in the magnetic recording medium 600.

[0084] Back coating

[0085] The back coating 602 may or may not be present in the magnetic recording medium 600. The back coating 602 may be a known material and is selected to be a material that can be grafted to the substrate 604 by radiation-induced grafting. Preferably, the back coating 602 is composed of a material that provides one or more of the following benefits: facilitating separation from another portion of the tape wound on the reel, friction improvement, static dissipation, etc. The preferred thickness of the back coating 602 is less than about 0.3 microns, preferably less than about 0.2 microns.

[0086] Substrate

[0087] As disclosed herein, substrate 604 has a new and novel construction. Substrate 604 is formed of polyetheretherketone (PEEK). As used herein, PEEK refers more broadly to a class of materials collectively referred to as PEEK materials in the art, such as various types of polyaryletherketone (PAEK), polyetheretherketone, etc.

[0088] The recording tape having the PEEK substrate 604 has stable mechanical properties. For example, the tensile storage (E') modulus and the tensile loss (E"") modulus as measured by dynamic mechanical analysis methods such as dynamic mechanical thermal analysis (DMTA) for typical tape media operating and storage environments are lower than conventional media substrates. Typically, the typical tape media operating and storage environment is in the range of about 0°C to about 60°C, and at a relative humidity of about 5% to about 80%.

[0089] Recording tapes with PEEK substrate 604 also have low sensitivity to temperature and humidity over this entire operating range. PEEK is generally hydrophobic, making it water stable. At 50% relative humidity, water absorption is expected to be much less than 1%, which is much less than aramid, which tends to have an absorption of about 10% at 50% relative humidity.

[0090] The recording tape having the PEEK substrate 604 also has excellent elasticity for typical tape operations and exhibits stable creep and recovery at typical storage and operating temperatures of about 0°C to about 60°C, with shrinkage of the PEEK substrate expected to be less than 1% over the entire 100°C temperature range including the above operating range.

[0091] Another advantage of PEEK is that the PEEK raw material can be melted without degradation, which enables PEEK to be processed into films at temperatures around its melting point without losing its desired properties.

[0092] Each of the above is important to maintaining dimensional stability both in use and during long-term storage.

[0093] PEEK has not been considered a suitable material for recording tapes so far due to the focus on its use in capacitors and other applications. PEEK is also not one of the materials used by tape media substrate manufacturers for other applications. In addition, the conventional wisdom of trying to improve the dimensional stability of tape media to address the changes in tape width and the stability of data track positioning has always been to pursue an increase in the stiffness or modulus of the substrate in the transverse direction (TD). However, in this method, the composition of the conventional substrate must be adjusted to achieve an increase in the TD modulus of the substrate. Therefore, the inventive discovery disclosed herein about using PEEK as a substrate material is contrary to conventional wisdom.

[0094] Figure 7 700 is a graph comparing DMTA results (DMTA@10 Hz) of tensile storage modulus (E') in GPa over the entire temperature range for an example of a prior art tape substrate and an 8 micron thick PEEK film from Shin Etsu, Ltd. The prior art tape substrate used in the experiment is: TORAY Spaltan TM - Blends of chopped modified aromatic polyamide (Mictron) in polyethylene terephthalate (PET); TORAY Mictron TM - modified aromatic polyamide; and TD stretched PEN from TEIJEN Ltd.

[0095] Compare this Figure 8 The graph 800 of FIG. 8 is further zoomed in on the temperature range (0°C - 60°C) over which the tape is typically used and stored. Only two of the substrates show a stable mechanical response within this temperature range, namely Toray Spaltan TM and PEEK film samples. It has been found that Toray Spaltan TM The PEEK substrate exhibits good transverse dimensional stability (TDS), an increasingly important property for magnetic tapes to achieve higher track densities. However, it suffers from sensitivity to humidity and poor creep recovery. The PEEK substrate according to the various methods disclosed herein addresses and overcomes these problems.

[0096] Preferably, the tensile storage modulus E' of the PEEK substrate according to various aspects is from about 4 GPa to about 20 GPa, more preferably from about 5 GPa to about 15 GPa, and ideally from about 5.5 GPa to about 12 GPa, with values ​​near the upper end of this range being preferred. The tensile storage modulus E' can be controlled to some extent by controlling the molecular weight of the PEEK, and potentially improved by increasing the crystalline chain orientation of higher molecular weight PEEK materials, which are currently unavailable but will become available in view of the teachings provided herein, and the need for them may be established once for future tape media.

[0097] In various methods, PEEK material having an aromatic polyaryletherketone chemical structure and a chain length n of at least n=20 is preferably used for the substrate material. Preferably, the chain length is n=40 or higher, such as n=50 to 100, etc. The chain length should not be so long that PEEK cannot be processed or becomes brittle.

[0098] Various aromatic polyaryletherketones can be used in various methods within the scope of the present invention. Several exemplary PEEK materials are described below. This is done by way of example only, not limitation, to illustrate several different types of PEEK that can be used in many aspects of the present invention.

[0099] Reference again Figure 6 , substrate 604 can be the thickest layer in the recording tape. The use of PEEK enables thinner substrates than conventional substrates currently used, thereby enabling more tape to be wound into a conventional tape cassette. In some approaches, the substrate has a thickness as low as about 2.5 microns measured in a direction perpendicular to the plane of the tape, such as in the range of about 3 microns to about 8 microns, preferably in the range of about 3 microns to about 4.5 microns, but can be thicker or slightly thinner than the outer values ​​of these ranges.

[0100] Exemplary PEEK Materials

[0101] Fig. 9 An exemplary PEEK 900 is shown according to various methods described herein. As an option, the PEEK 900 of the present invention can be implemented in combination with features from any other method listed herein, such as those described with reference to other figures. However, such PEEK 900 and other features given herein can certainly be used in various applications and / or permutations, which may or may not be specifically described in the illustrative methods listed herein. In addition, the PEEK 900 proposed herein can be used in any desired environment. The PEEK 900 in the various permutations disclosed herein improves the stability and performance of the tape storage media under the desired use and storage environment.

[0102] Fig.10Another exemplary PEEK 1000 according to various methods described herein is shown. As an option, this PEEK 1000 can be implemented in combination with features from any other method listed herein, such as those described with reference to other figures. However, this PEEK 1000 and other features given herein can be used in various applications and / or permutations, which may or may not be specifically described in the illustrative methods listed herein. In addition, the PEEK 1000 proposed herein can be used in any desired environment. The various permuted PEEK 1000 disclosed herein improve the stability and performance of the tape storage media under the desired use and storage environment.

[0103] Known manufacturing techniques can be used to make PEEK feedstock that can be used to form the substrate. In some methods, a step-growth polycondensation reaction is used.

[0104] Fig.11 Another exemplary PEEK 1100 according to various methods described herein is shown. As an option, this PEEK 1100 can be implemented in combination with features from any other method listed herein, such as those described with reference to other figures, however, this PEEK 1100 and other features given herein can certainly be used in various applications and / or permutations, which may or may not be specifically described in the illustrative methods listed herein. In addition, the PEEK 1100 proposed herein can be used in any desired environment. The various permuted PEEK 1100 disclosed herein improve the stability and performance of the tape storage medium in the desired use and storage environment.

[0105] Fig.12 Another exemplary PEEK 1200 and an exemplary formation path thereof according to various methods described herein are shown. As an option, this PEEK 1200 can be implemented in combination with features from any other method listed herein, such as those described with reference to other figures. However, this PEEK 1200 and other PEEKs given herein can be used in various applications and / or replacements, which may or may not be specifically described in the illustrative methods listed herein. In addition, the PEEK 1200 proposed herein can be used in any desired environment. The various replacement PEEK 1200 disclosed herein improve the stability and performance of magnetic tape storage media in the desired use and storage environment.

[0106] As mentioned above, PEEK 1200 can be produced using a step-growth polycondensation reaction. Fig.12The exemplary step-growth polycondensation process shown involves reacting a diphenyl ether such as diphenyl ether with terephthaloyl chloride (TPC) in the presence of a metal chloride such as AlCl or FeCl, with the release of HCl as a byproduct. The reaction is typically carried out at high temperatures in the melt or in an aromatic solvent so that HCl leaves as a gas and drives the reaction to very efficient chain growth.

[0107] The end groups of PEEK 1200 can be similar to Fig.12 The end groups shown in or others.

[0108] In some methods, PEEK raw materials can be purchased as ready-made materials from manufacturers or suppliers of such materials. In a preferred method, the manufacturer can manufacture suitable PEEK materials with desired properties such as chain length, etc., according to the requirements of the recording tape manufacturer, following the guidance provided herein. Typically, PEEK is sold in the form of pellets, which can be processed as described below to form a substrate for recording tape. In other methods, PEEK substrate sheets can be produced and / or purchased for use in the tape manufacturing process.

[0109] PEEK materials are available from Solvay (Solvay Specialty Polymers USA, LLC, 4500 McGinnis Ferry Road, Alpharetta. GA 30005-3914 USA).

[0110] PEEK materials are also available from Victrex (Victrex USA, Inc, 300 Conshohocken State Road Suite 120, West Conshohocken, PA, 19428 USA).

[0111] Currently produced PEEK films are not well suited for use as tape substrates. However, using the teachings provided herein, one skilled in the art can produce PEEK films having appropriate thickness, molecular weight, extrudability, and molecular orientation suitable for use as tape substrates.

[0112] PEEK is particularly advantageous for magnetic tape applications because it has a very low hygroscopic expansion coefficient and is insoluble in organic solvents. Therefore, PEEK substrates are not susceptible to water-induced dimensional changes. However, PEEK can be melted and formed into films. PEEK does not degrade at the higher temperatures used during manufacturing, such as melt extrusion. In contrast, aramids used in conventional magnetic tape products are modified to be soluble because they degrade during melting and cannot be melt extruded into films. In order to make aramids soluble in even very hot polar organic solvents, the aramid chains need to be modified to increase solubility. This results in increased water absorption and reduces the overall dimensional stability of the magnetic tape media at normal use and storage temperatures.

[0113] In order to form a substrate, according to a method, the PEEK raw material is melt-extruded and oriented so that the crystallization regions are aligned so that the crystallization regions of the resulting substrate are substantially aligned with each other. The melt extrusion process includes heating the PEEK raw material to a temperature that enables the PEEK raw material to be extruded by a melt extrusion device to form a film of a desired thickness. The melt extrusion device and method can be a known design of the PEEK material used in other industries, and generally include a die (such as a nozzle, a roller, etc.) through which PEEK is extruded and a mechanism for pulling the extruded PEEK. An exemplary substrate production line can use melt extrusion and a process called tenting, which uses a clamp on a magnetic track and a chain frame, which clamps the ends of the extruded sheet and pulls them in a heating furnace in a transverse and length direction to achieve very controlled MD and TD orientation or stretching.

[0114] The temperature used during melt extrusion should be below the degradation temperature of the PEEK raw material, which is material dependent, and is generally well above the melting temperature determined by conventional thermal analysis techniques such as differential scanning calorimetry (DSC) or thermogravimetric analysis (TGA), as will be understood by those skilled in the art after being informed of this specification. In general, PEEK polymers are very stable until well above their softening point or true melting point. Depending on the molecular structure and chain length of the PEEK polymer, softening occurs well above 150°C. Some polymers can degrade in air when heated above 300°C, which is considered to be well above the practical usable processing temperature for film formation suitable for tape substrates. In general, the processing temperature used in the film production process is optimized around the specific properties of the polymer feed entering the initial extrusion die to achieve good flow and orientation of the initial sheet when it is picked up by the clamp, and then the clamp simultaneously pulls the film in the cross-web direction and down along the web to achieve the desired orientation or stretching in the final cooled film.

[0115] Conventional conditions for aligning the crystalline regions of conventional substrate films can be used in the case of PEEK in the following manner as will be understood by those skilled in the art once informed of the present disclosure. For example, during melt extrusion, as molten PEEK is drawn out, the molecular chains tend to align in the direction of flow and move in the direction of minimum free volume. Orientation of the film to align the crystalline regions allows for the production of films with higher modulus without sensitivity to water and near fully elastic creep recovery, which is expected to provide the TDS control required for existing tension compensation schemes.

[0116] The resulting PEEK sheet can be stored for subsequent additional processing, or additional layers can be added to the PEEK sheet. In one aspect, the PEEK sheet is wound onto a reel. On the other hand, one or more additional layers are added to the PEEK sheet.

[0117] PEEK sheets with or without additional layers can be cut to the width required for subsequent processing and / or the specifications of the final product. For example, a wide PEEK sheet can be cut into strips having a width suitable for use with conventional coating equipment to add additional layers thereto.

[0118] Bottom Layer

[0119] According to various methods, any base layer 606 known in the art may be used with the PEEK substrate 604. The base layer 606 may be a known material, and preferably a material capable of being grafted to the substrate 604 by radiation induced grafting.

[0120] Recording Layer

[0121] Any recording layer 608 known in the art may be used with the PEEK substrate 604 according to various methods.

[0122] Exemplary Tape Manufacturing Techniques

[0123] As discussed in more detail below, one or more additional layers, such as a primer layer and / or a back coating layer, are attached to the PEEK substrate to produce the recording tape.

[0124] Existing recording tape manufacturing techniques rely on solvent interactions to make the layers adhere to each other or require surface treatment such as plasma cleaning prior to coating. An obvious downside to such surface modification is that the substrate is then susceptible to water-induced dimensional changes.

[0125] One or more additional layers may be added to improve adhesion of the coating and / or provide a controlled roughness for improved handling, as currently used in tape substrates, and may also be added to the PEEK film. Modification of the PEEK film to improve adhesion of coatings that may be used to produce future recording tape products may require modification of the PEEK film surface by coextrusion of additional film materials on one surface or oxidation of one surface using plasma treatment, as currently practiced with existing tape substrates. In the case of radiation-cured coatings, especially for very thin coatings anticipated in future tape designs, sufficient activation of sites on the PEEK film may be achieved with UV light to resolve adhesion issues, thereby eliminating the need for additional surface treatments. Modification of the monomers used to construct PEEK specifically optimized for use as a magnetic media substrate may introduce functional groups into the PEEK film that may be activated upon exposure to UV light and react with functional groups in the coating, thereby completely resolving any adhesion issues and further improving the performance of the film for tape media applications.

[0126] In a preferred method, one or more additional layers, such as a bottom layer and / or a back coating layer, are connected to a PEEK substrate via radiation-induced grafting of the layer, such as photoinduced curing (e.g., crosslinking) to the substrate. For example, the bottom layer can be extruded adjacent to the PEEK substrate, laminated thereon, and grafted thereon in real time by exposure to ultraviolet (UV) light and / or other radiation. The aromatic compounds in PEEK tend to be photoactive, thus causing them to themselves undergo the required radiation-induced curing. In addition, the PEEK raw material and / or adjacent layers can be manufactured to have the desired chemical structure that allows radiation-induced grafting, as will be understood by those skilled in the art when reading this specification. In some methods, there is no adhesive between the bottom layer and the substrate.

[0127] It is worth mentioning that a high degree of cure is not required. Instead, a small number (a few) of chemical bonds per hundred monomer units are sufficient for good adhesion, since chemical bonds are much stronger than the weaker bonding techniques used in conventional tape media. The chemical bonding of the preferred aspects is also advantageous in terms of robustness and stress resistance, since chemical bonds must be severed in order for the layers to detach.

[0128] Typically, UV light will not penetrate plastics thicker than 1 micron. However, the base layer used in the preferred method is less than 1 micron thick, thus enabling UV curing to occur.

[0129] Various benefits of recording tapes having the new PEEK substrate relative to existing recording tape media include, but are not limited to, one or more of the following: higher dimensional stability, greater tear resistance, greater resistance to aging (creep) effects, and the like.

[0130] It will be apparent that the various features of the foregoing systems and / or methods may be combined in any manner, resulting in multiple combinations from the description presented above.

[0131] It will also be appreciated that the method of the present invention may be provided as a customer-delivered service.

[0132] The inventive concepts disclosed herein have been presented by way of example to illustrate their numerous features in a number of illustrative scenarios, embodiments, and / or implementations. It should be understood that the generally disclosed concepts are considered modular and can be implemented in any combination, permutation, or synthesis thereof. In addition, any modifications, alterations, or equivalents of the currently disclosed features, functions, and concepts that will be understood by a person of ordinary skill in the art upon reading this specification should also be considered within the scope of the present disclosure.

[0133] The description of various embodiments of the present invention has been given for the purpose of illustration, but it is not intended to be exhaustive or limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope of the described embodiments. The terms used herein are selected to best explain the principles of the embodiments, practical applications, or technical improvements over existing technologies on the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

Claims

1. Recording tapes, including: A substrate comprising polyetheretherketone (PEEK); A bottom layer on a substrate; as well as A recording layer on the bottom layer, wherein the chain length of polyetheretherketone (PEEK) is greater than about 20, wherein the bottom layer is grafted to the substrate.

2. The recording tape of claim 1, wherein the chain length of the polyetheretherketone (PEEK) is about 50 to about 100.

3. A recording tape according to any one of the preceding claims, wherein the tensile storage modulus of the substrate as measured by dynamic thermomechanical analysis is in the range of about 4 GPa to about 20 GPa.

4. The recording tape of claim 1 or 2, wherein the tensile storage modulus of the substrate as measured by dynamic thermomechanical analysis is in the range of about 5.5 GPa to about 12 GPa.

5. A recording magnetic tape as claimed in claim 1 or 2, wherein the crystalline regions of the substrate are substantially aligned with each other.

6. The recording tape of claim 1 or 2, wherein the thickness of the substrate is in the range of about 2.5 microns to about 8 microns.

7. The recording tape of claim 1 or 2, wherein the thickness of the substrate is in the range of about 3 microns to about 4.5 microns.

8. A recording tape as claimed in claim 1 or 2, wherein no adhesive is present between the base layer and the substrate.

9. With box, including: case; as well as a recording tape at least partially stored in the housing, The tape includes: A substrate comprising polyetheretherketone (PEEK), The bottom layer on the substrate, and A recording layer on the bottom layer, wherein the chain length of polyetheretherketone (PEEK) is greater than about 20, wherein the bottom layer is grafted to the substrate.

10. A cassette as claimed in claim 9, comprising a non-volatile memory connected to the housing.

11. The tape cassette of claim 9 or 10, wherein the polyetheretherketone (PEEK) has a chain length of about 50 to about 100.

12. The cassette of claim 9 or 10, wherein the substrate has a tensile storage modulus in the range of about 4 GPa to about 20 GPa as measured by dynamic thermomechanical analysis.

13. The cassette of claim 9 or 10, wherein the substrate has a tensile storage modulus in the range of about 5.5 GPa to about 12 GPa as measured by dynamic thermomechanical analysis.

14. A cassette as claimed in claim 9 or 10, wherein the crystalline regions of the substrate are generally aligned with each other.

15. The cassette of claim 9 or 10, wherein the substrate has a thickness in the range of about 2.5 microns to about 8 microns.

16. The cassette of claim 9 or 10, wherein the substrate has a thickness in the range of about 3 microns to about 4.5 microns.

17. A cassette as claimed in claim 9 or 10, wherein there is no adhesive between the base layer and the substrate.

18. A method for manufacturing a recording magnetic tape, the method comprising: attaching the bottom layer to a substrate comprising polyetheretherketone (PEEK) by radiation induced grafting; and connecting the recording layer to the bottom layer, wherein the chain length of the polyetheretherketone (PEEK) is greater than about 20.

19. The method of claim 18, wherein the polyetheretherketone (PEEK) has a chain length of about 50 to about 100.

20. The method of claim 18 or 19, wherein the substrate has a tensile storage modulus in the range of about 4 GPa to about 20 GPa as measured by dynamic thermomechanical analysis.

21. The method of claim 18 or 19, wherein the substrate has a tensile storage modulus in the range of about 5.5 GPa to about 12 GPa as measured by dynamic thermomechanical analysis.

22. The method of claim 18 or 19, wherein the crystalline regions of the substrate are substantially aligned with each other.

23. The method of claim 18 or 19, wherein the thickness of the substrate is in the range of about 2.5 microns to about 8 microns.

24. The method of claim 18 or 19, wherein the thickness of the substrate is in the range of about 3 microns to about 4.5 microns.

25. The method of claim 18 or 19, wherein no adhesive is present between the base layer and the substrate.