Solid polymer electrolyte comprising polyolefin carbonate
By using polycarbonate esters and other polymers in the polymer matrix to form a self-supporting solid electrolyte in solid-state batteries, the problem of insufficient conductivity of solid-state batteries at low temperatures is solved, and the goals of high conductivity and industrial production are achieved, simplifying streamline the production process and reduce costs.
Patent Information
- Application Number
- CN202080052277.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-07-17
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-07-17
AI Technical Summary
The solid electrolyte of existing solid-state batteries has insufficient conductivity under low temperature conditions, and the production method is complex and costly, making it difficult to achieve industrial application.
Using a polymer matrix, including polyolefin carbonate and different polymers, mixed by melt or solvent methods to form a self-supporting solid polymer electrolyte, supporting polyolefin carbonate to improve Li+ ion conductivity, and through specific processing methods such as Heating and drying produce a thin film electrolyte with high conductivity.
Effectively conducts ions at room temperature and above, improves the safety and energy density of solid-state batteries, simplifies the production process, reduces costs, and realizes an industrially applicable solid Li+ ion-conducting electrolyte.
Smart Images

Figure BDA0003477562480000121 
Figure HDA0003477562490000011 
Figure HDA0003477562490000021
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrolytes, in particular to electrolytes for batteries.
[0002] In particular, the present invention relates to the field of electrolytes for solid-state batteries. Background Art
[0003] The marketing of lithium-ion batteries, starting in the 1990s, is a real revolution in the field of energy storage. We see this technology growing exponentially thanks to constant improvements in performance. In particular, battery capacity allows a greater extension of the autonomy of portable electronic systems; today they have reached a threshold that allows their integration into hybrid or pure electric vehicles. The car of the future will be electric. This leads to an increasingly fast-paced race to improve battery performance and its energy density, thus achieving maximum autonomy in electric vehicles.
[0004] Furthermore, the safety of on-board energy storage systems becomes even more important as energy density increases. In the event of an accident, it is crucial to prevent the thermal release of the battery's electrochemical energy. This is the problem posed by conventional lithium-ion batteries. These batteries have flammable organic electrolytes that, if subjected to significant heating, can lead to thermal runaway of the battery and possibly even to explosion. Therefore, lithium-ion battery packs are currently equipped with sophisticated thermal management systems that generally prevent such critical situations from occurring and reduce the risk to near zero levels.
[0005] In this context, efforts have been made to develop "all-solid-state" batteries. The basic idea is to replace the liquid electrolyte with a solid conductive ionic electrolyte. Such a material would prevent the vaporization and ignition of the electrolyte in the event of overheating, thus practically preventing thermal runaway. This would allow to simplify and therefore reduce the thermal management on a large scale (in terms of mass and volume). Moreover, the use of solid materials as electrolytes would allow a different or greater range of electrochemical stabilities compared to traditional solvents (essentially cyclic or linear carbonates). In particular, it is possible to envision a solid electrolyte that is stable to metallic lithium, as is the case with polyethylene oxide (PEO), thus limiting / slowing down dendrite growth compared to the case of a liquid environment. Therefore, the use of metallic lithium, the most reducing element, as the negative electrode would allow to increase the operating voltage of the electrochemical cell and thus its energy density.
[0006] Various technical methods for producing solid electrolytes have been continuously studied.
[0007] One example is solid polymer electrolytes. Among them, PEO is currently the most reliable solution, but requires elevated temperatures (>60°C) to operate effectively. The ether groups of PEO allow the lithium salt (usually LiTFSi) to dissociate, while the chain mobility obtained at high temperatures (70-80°C) favors Li+ The cations diffuse in the polymer matrix. The maximum conductivity of PEO at 80°C is 10 -3 S / cm. Various polymers have been tested, in particular, to obtain better room temperature (RT) conductivity than the latter.
[0008] In light of this, various efforts in the past and present have been related to the development of gel electrolytes. These are polymer systems in which a liquid electrolyte is trapped, thus facilitating ion mobility. However, even though these materials have better conductivity (especially at RT), they still have significant disadvantages, such as a significant loss of mechanical strength. In addition, there is a real risk of electrolyte loss in the event that the system is heated. In other words, the increase in ionic conductivity translates into a loss in terms of battery safety.
[0009] In addition to polymer methods, many inorganic conductive Li + Phases (ceramics or glasses) are also being studied. Examples include: Li 7 La 3 Zr 2 O 12 (LLZO) or alternative components [garnet structure], Li 1+x Al x Ti 2-x (PO4) 3 (LATP) [NASICON structure], and Li 0.05-3x La 0.5+x TiO 3 (LLTO) [perovskite structure], these are commercially available products. Considering Ti 4+ In its structure, LLZO has the great advantage of being stable in the presence of metallic lithium, unlike LATP and LLTO. These products have very good "intracrystalline conductivity" (10 -4 ~10 -3 S / cm). The real problem comes from the grain boundaries; in this case, the resistance contribution of the intergranular interfaces must be limited. This is why these materials are traditionally formed by sintering. The resulting ceramic plates have a significant brittleness, which makes it difficult to minimize their thickness and thus incorporate them into batteries of several Ah. Summary of the invention
[0010] Purpose of the Invention
[0011] The purpose of the present invention is to solve the technical problem of providing an ion-conductive electrolyte capable of improving energy storage safety.
[0012] In particular, the object of the present invention is to solve the technical problem of providing a solid ion-conducting electrolyte, in particular for solid-state batteries.
[0013] The object of the present invention is to solve the technical problem of providing a solid ionic electrolyte having electrical conductivity at a temperature less than or equal to 60°C.
[0014] The purpose of the present invention is to provide a solid Li + Technical issues of ion-conducting electrolytes.
[0015] Another object of the present invention is to solve the technical problem of providing an industrial or industrially applicable process for preparing an ion-conducting electrolyte, in particular a process that is easy to carry out and industrially applicable.
[0016] Another object of the present invention is to solve the above technical problems at a limited cost.
[0017] Detailed description of the invention
[0018] It is surprisingly found that at least one of the above technical problems, preferably all, can be solved by providing a solid polymer electrolyte, which includes a polymer matrix, which includes at least one ionic salt, wherein the polymer matrix includes at least one polyalkene carbonate, at least one second polymer different from the polyalkene carbonate, and at least one alkene carbonate produced by decomposition of the polyalkene carbonate.
[0019] Solutions proposed in the prior art involving the use of polyolefin carbonates include the use of a matrix supporting a solid electrolyte. An example of this is Adv.Ener.Mater.2015,5,1501082, J.Zhang et al., using a nonwoven cellulose membrane as a polyolefin carbonate support (PPC). PPC and LiTFSI salt were dissolved in acetonitrile. The uniform solution flowed through the nonwoven cellulose matrix and then evaporated under vacuum (100°C-24 hours). Therefore, compared with PPC alone, the PPC / cellulose system has better mechanical strength and a thermal conductivity of 3.0x 10 at RT (20°C). -4 S / cm) and above have good conductivity. However, this solution has the technical disadvantage that the polyolefin carbonate must be deposited on the substrate to obtain the desired results. Similarly, Electro.Comm.66 (2016) 46-48, K. Kimura reported the production of a polyvinyl carbonate (PEC) system with 80% LiTFSI with a high salt content. Since the system itself does not have good mechanical strength, a polyimide matrix is used as a porous matrix to support the solid electrolyte. PEC and LiTFSI salts are dissolved in acetonitrile. The solution flows on the polyimide matrix and then evaporates under vacuum (60°C-24 hours). At 30°C, the ionic conductivity of the material is 10 -5 Here, too, the polyalkylene carbonate has to be deposited on a substrate to achieve the desired result, which does not constitute a sufficiently simple process for industrial application.
[0020] Therefore, these prior art solutions are unsatisfactory.
[0021] The present invention also relates to a method for preparing a solid polymer electrolyte according to the present invention, wherein the method comprises: mixing a polyolefin carbonate and a second polymer by melting or by a solvent, wherein the polyolefin and the second polymer are both soluble; and partially decomposing the polyolefin carbonate into olefin carbonate to obtain a solid polymer electrolyte according to the present invention.
[0022] Advantageously, the matrix according to the invention constitutes a self-supporting polymer system capable of efficiently conducting ions, typically Li + ions. The present invention thus makes it possible to overcome the technical problems of the prior art, namely supporting polyalkylene carbonate on a substrate.
[0023] Advantageously, the matrix according to the invention comprises at least one amorphous second polymer.
[0024] Advantageously, the matrix according to the invention comprises a liquid portion of the matrix resulting from the decomposition of the polymer.
[0025] Advantageously, the matrix according to the invention has a specific morphology with very good ionic conductivity.
[0026] According to the invention, the matrix may comprise one or more polymers different from polyalkylene carbonate.Thus, according to the invention, the matrix may comprise one or more polymers of a second type.
[0027] In one embodiment, the matrix includes one or more polymers selected from the following group as the second polymer: polyolefins, polycarbonates, halogenated polymers, acrylic polymers, acrylate polymers, methacrylate polymers, vinyl acetate polymers, polyethers, polyesters, polyamides, aromatic polymers and elastomeric polymers, such as HNBR, polyisoprene, rubbery polymers and any mixtures thereof.
[0028] Preferably, the second polymer is an elastomer.
[0029] Typically, the matrix comprises at least two polymer phases, one of which comprises at least one polyalkylene carbonate capable of being degraded or reduced to an alkylene carbonate, and the other of which is at least one second polymer.
[0030] Typically, the matrix comprises at least 10 ppm of acene carbonate relative to the total mass of the matrix. In a variant, the matrix comprises at least 100 ppm, or at least 1000 ppm, of olefin carbonate relative to the total mass of the matrix.
[0031] Typically, the decomposition of the polyethylene carbonate is no more than 99% by mass, preferably no more than 70% by mass, even more preferably no more than 50% relative to the initial mass of polyethylene carbonate.In a variant, the matrix comprises at least 50% of phenyl carbonate relative to the total mass of the matrix.
[0032] In one variation, the olefin carbonate is in monomeric form.
[0033] Advantageously, according to the present invention, the matrix has no macroscopic separation between the phase comprising the polyalkylene carbonate and the phase comprising the second polymer.
[0034] Therefore, the second polymer is selected to avoid phase macroseparation. "No phase macroseparation" means that essentially no separation of pure non-dispersed polymer phases with a size greater than a few hundred μm is detected. It is possible to search for phase macroseparation by nano-infrared Fourier transform spectroscopy. It is also possible to search for phase macroseparation by scanning electron microscopy (SEM).
[0035] More generally, all polymer groups can be associated with the polyalkylene carbonates as long as the morphology does not exhibit any macroscopic phase separation as defined above.
[0036] Generally speaking, the polyalkylene carbonate is present in an amount not exceeding 80% (mass / mass) relative to the total amount of the polymer, and sufficient mechanical properties can be obtained through electrochemical cycling or contact with metallic lithium, thereby preparing a satisfactory solid electrolyte.
[0037] In one embodiment, the polyalkylene carbonate is present in an amount of 5 to 80% by mass, preferably 10 to 70% by mass, relative to the total mass of the polymer of the matrix.
[0038] In one embodiment, the amount of polyolefin carbonate is preferably 10 to 70% (mass / mass). Generally, the amount of polyolefin carbonate is more preferably 15 to 60% (mass / mass). More preferably, the amount of polyolefin carbonate is 20 to 50% (mass / mass).
[0039] Polyalkylene carbonate has no specific molar mass. It can be used alone or in a mixture of different molar masses.
[0040] Advantageously, the polymer matrix comprises polyalkylene carbonates having a high molar mass and polyalkylene carbonates having a low molar mass relative to each other.
[0041] Therefore, with low molar mass ( <15000 g / mol) can be plasticized to have a high molar mass (> 15000 g / mol) of polymer to achieve solid fluidization of the mixture. The advantage of this embodiment is that the final viscosity of the mixture can be adjusted relative to the selected method (with or without solvent), or the final formulation (with or without filler), or the final product (with greater or less thickness). Therefore, the proportion of polyalkylene carbonate with low molar mass relative to the total amount of polyalkylene carbonate is generally 0.1 to 99.9%, preferably 5 to 90%, more preferably 10 to 80%.
[0042] An example of a polyalkylene carbonate with a low molar mass is a PPC polyol such as Converge 212-10, and an example of a polyalkylene carbonate with a high molar mass is 40.
[0043] In one embodiment, the ionic salt is selected from metal ionic salts, wherein the metal belongs to Group 1 of the Periodic Table of Elements.
[0044] Thus, the one or more ionic salts are at least partially dissociated in at least one polymer phase.
[0045] In one embodiment, the ionic salt is selected from LiBETI, LiC 2 F 5 SO 3 ,LiC 4 F 9 SO 3 、LiCF 3 SO 3 , NaI, NaSCN, NaBr, KI, KBr, LiClO 4 , LiBF 4 、LiAsF 6 、LiPF 6 、LiNO 3 、Li(CF 3 SO 2 ) 2 N、Li(CF 3 SO 2 ) 3 C,LiN(SO 2 C 2 F 5 ) 2 , alkyl lithium fluorophosphate, lithium difluoro(oxalate)borate, lithium bis(oxalate)borate, MTFSiLi, STFSiLi, and any mixture thereof.
[0046] In one embodiment, the matrix comprises a solid mineral or organic filler.
[0047] Thus, in one embodiment, the matrix includes solid mineral or organic fillers to impart various properties, such as mechanical reinforcement, improved ionic conductivity, or insertion or removal of metal ions.
[0048] By way of example only, solid fillers that may improve conductivity include:
[0049] - Inert fillers, such as Al 2 O 3 、SiO 2 , cellulose and starch, which do not conduct cations but can help the transport of ions through surface interactions of fillers.
[0050] - and a filler (such as ceramic or glass) having volume conductivity for cations.
[0051] In one embodiment, the matrix includes a solid filler that allows for the insertion and removal of an "active" metal salt. An example is C-LiFePO 4 , but all active materials known to those skilled in the art, such as the positive electrode (such as LiCoO 2 、LiMnO 4 and LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O 2 ...) or the negative electrode (such as Li 4 Ti 5 O 12 and graphite) should be considered.
[0052] In one embodiment, the matrix includes a conductive filler. An example is conductive carbon black, as well as graphite, graphene, carbon nanofibers and carbon nanotubes, and mixtures thereof.
[0053] In one embodiment, the solid polymer electrolyte is in the form of a thin film having a thickness of less than 1 mm.
[0054] The film according to the invention typically has a thickness of 10 to 500 μm, such as 80 to 300 μm, typically 90 to 200 μm.
[0055] Generally, the preparation method according to the present invention comprises mixing polymers, including polyalkylene carbonate and a second polymer, by a dry process (also called a melt process) or a solvent process (also called a wet process) of "melting polymers".
[0056] In one embodiment, the method includes applying heat during mixing of the polyalkylene carbonate and the second polymer.
[0057] Advantageously, in one embodiment, all or part of the mixing is melt mixed or subsequently heated at a temperature sufficient to partially decompose the polyalkylene carbonate to alkylene carbonate.
[0058] In one variation, melt mixing is performed entirely at a temperature sufficient to partially decompose the polyalkylene carbonate to form alkylene carbonate.
[0059] In one variation, melt mixing is carried out partially, preferably at the end of mixing, at a temperature sufficient to partially decompose the polyalkylene carbonate to alkylene carbonate.
[0060] In one embodiment, the solvent process mixing is carried out at RT (typically 20°C) and the mixture is then dried at a temperature sufficient to eliminate the solvent and partially decompose the polyalkylene carbonate to alkylene carbonate.
[0061] Preferably, in a liquid process, a solvent is used which has a boiling point below the decomposition temperature of the polyalkylene carbonate.
[0062] In one embodiment, the method includes melt mixing a polyalkylene carbonate and a second polymer, wherein the mixing is performed at least partially in contact with an inorganic filler that promotes partial decomposition of the polyalkylene carbonate to form alkylene carbonate.
[0063] In one embodiment, the method comprises adding a reducing metal, such as lithium, after drying, under conditions that partially decompose the polyalkylene carbonate to alkylene carbonate. Advantageously, in the presence of such a metal, heating is not required to partially decompose the polyalkylene carbonate to alkylene carbonate.
[0064] Preferably, the mixture is then formed into a film and then dried.
[0065] Advantageously, and unlike the above-mentioned prior art, the mixing of polymers makes it possible to obtain films which do not require a matrix.
[0066] Preferably, the mixture is dried in the drying step.
[0067] Typically, the mixture is dried for a sufficient time to obtain the desired dryness, for example for at least one hour under vacuum at 60° C. The vacuum is generated under conditions known to those skilled in the art, for example by means of a vacuum pump.
[0068] Preferably, in a variation, after drying in a liquid process, or at the end of mixing in a melt process, the process is heated to a temperature that results in the in-situ release of the alkylene carbonate moiety within the polymer matrix. Thus, in a variation, the process comprises heating to a temperature ("conditioning temperature") sufficient to partially decompose the polyalkylene carbonate into alkylene carbonate.
[0069] Advantageously, the conditioning temperature can be reduced in the presence of a metal that promotes partial decomposition of polyalkylene carbonate to alkylene carbonate, such as to prepare a solid electrolyte in contact with a metal anode (e.g., lithium metal). Advantageously, in an embodiment, the step of heating to the conditioning temperature occurs on a battery comprising a solid polymer electrolyte, such as before sale or use.
[0070] In one embodiment, the method includes heating the solid polymer electrolyte to a conditioning temperature after mixing.
[0071] For example, the condition temperature is greater than 80°C, such as greater than 100°C, or greater than 120°C.
[0072] In one embodiment, the condition temperature is greater than 150°C, such as greater than 170°C.
[0073] Therefore, advantageously, in one embodiment, the mixture obtained according to the process of the present invention is treated at a conditioned temperature for a sufficient time to increase its ionic conductivity (generally 1 to 30 minutes) and then returned to ambient temperature.
[0074] In one variation, the method includes adding specific additives to the polymer mixture to improve and / or optimize the process for producing the solid polymer electrolyte.
[0075] In a variant, the method comprises crosslinking one or more second polymers, preferably during mixing with polyalkylene carbonate. This crosslinking can occur only on one or more second polymers (different from polyalkylene carbonate), or it can occur together with polyalkylene carbonate without hindering the in-situ generation of the corresponding alkylene carbonate.
[0076] In one variation, the method includes adding one or more crosslinker-forming compounds to the one or more second polymers mixed with the polyalkylene carbonate.
[0077] In a variation, the method includes adding one or more agents that promote crosslinking and homogenization thereof. Examples of crosslinking agents include organic peroxides or triallyl cyanurate as auxiliary agents. However, all compounds that allow the second polymer to be crosslinked can also be utilized, such as photoinitiators or sulfur compounds, which are typical compounds for rubber crosslinking, for example. It is also possible to use bifunctional compounds to chemically react on the side chains of the second polymer (if any), such as maleic anhydride, epoxy resin or acid, alcohol, amine, amide or ester moieties, because the reaction on the side group moiety can lead to the formation of bridges between the polymer chains and correspondingly lead to the crosslinking of the system. Advantageously, crosslinking can increase the cohesion of the matrix. Therefore, the use of crosslinking agents and (if applicable) auxiliary agents is useful, but not necessary for the present invention, and directly depends on the intended application and the intended method.
[0078] The invention also relates to an electrode comprising at least one solid polymer electrolyte according to the invention or a solid polymer electrolyte obtainable by a process according to the invention.
[0079] The invention also relates to a battery comprising at least one solid polymer electrolyte according to the invention or a solid polymer electrolyte obtainable by a process according to the invention.
[0080] In one variation, the battery is a solid polymer electrolyte lithium battery.
[0081] In particular, solid polymer electrolytes in thin film form are used as membranes in energy storage batteries. The membrane is usually inserted between the two electrodes of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0082] Figure 1 express Figure 1 Voltage (V) as a function of time (h) for a system with a solid polymer electrolyte according to Example 2b between two lithium metals at 60°C.
[0083] Figure 2 Represents the solid polymer electrolyte system according to Example 4 between two lithium metal electrodes at 60° C.; short circuiting occurred in less than half an hour of use.
[0084] Figure 3 The first discharge of an electrode having the composition described in Example 5 is shown.
[0085] Figure 4 The cycling stability of a half-cell using a C-LFP electrode (Example 5) with metallic lithium is shown. DETAILED DESCRIPTION
[0086] Example
[0087] Unless otherwise stated, percentages are by mass relative to the total mass of the relevant composition.
[0088] Unless otherwise stated, the temperature is RT (20° C.) Unless otherwise stated, the pressure is atmospheric pressure (101325 Pa).
[0089] Electrochemical analysis was performed using electrochemical impedance spectroscopy (MTZ-35, BioLogic Instruments) with a temperature control accessory (ITS Instruments, BioLogic). Morphology was obtained by SEM images.
[0090] Example 1: Solid electrolyte prepared by a melting method (or dry method).
[0091] 1.a. Place 10.1 g of HNBR (zetpol 2010), 5.5 g of PPC (QPac40), 5.3 g of PPC polyol (Converge 212-10) and 8.5 g of LiTFSI in an internal mixer to prepare a mixture. After adding the raw materials, mix at 85±10°C for 5 minutes.
[0092] Table 1
[0093] substance %(m / m) HNBR (Zetpol 2010L) 34.4 PPC(QPac40) 18.8 PPC (Converge212-10) 17.9 LiTFSI 28.9
[0094] % (m / m): mass % relative to the total mass of the mixed substance.
[0095] The final mixture was pressed into several films of approximately 100 μm thickness using a Dr Collin Teachline CR72T. The films were then dried at 60°C for at least 12 hours under vacuum generated by an Edwards RV12 pump.
[0096] 1.b. Films with the same composition were conditioned at 190°C for 1 hour.
[0097] The conductivity of various films was measured. The results are shown in Table 5 below.
[0098] Example 2: Solid electrolyte prepared by melting method
[0099] 2.a. Place 13.4 g of HNBR (zetpol 2010), 2.7 g of PPC (QPac40), 2.8 g of PPC polyol (Converge 212-10) and 8.2 g of LiTFSI in a sealed mixer to prepare a mixture. After adding the raw materials, mix at 85±10°C for 5 minutes.
[0100] Table 2
[0101] substance %(m / m) HNBR (Zetpol 2010L) 49.4 PPC(QPac40) 10.3 PPC (Converge212-10) 10.0 LiTFSI 30.3
[0102] % (m / m): mass % relative to the total mass of the mixed substance.
[0103] The final mixture was pressed into several films of approximately 100 μm thickness using a Dr Collin Teachline CR72T. The films were then dried at 60°C for at least 12 hours under vacuum generated by an Edwards RV12 pump.
[0104] 2.b. Films with the same composition were conditioned at 190°C for 1 hour.
[0105] Finally, the conductivity of various films was measured. The results are shown in Table 5. The polarization behavior of the modulated films was investigated under different current densities ( Figure 1 ) was tested between two lithium metal electrodes.
[0106] Example 3: Solid electrolyte prepared by melting method
[0107] 3.a. 8.4 g of HNBR (zetpol 0020), 5.6 g of PPC (QPac40), 5.3 g of PPC polyol (Converge 212-10) and 8.4 g of LiTFSI were placed in a sealed mixer to prepare a mixture. After adding the raw materials, mix at 85±10°C for 5 minutes.
[0108] Table 3
[0109] substance %(m / m) HNBR (Zetpol 0020) 30.4 PPC(QPac40) 20.1 PPC (Converge212-10) 19.2 LiTFSI 30.3
[0110] % (m / m): mass % relative to the total mass of the mixed substance.
[0111] The final mixture was pressed into several films of approximately 100 μm thickness using a Dr Collin Teachline CR72T. The films were then dried at 60°C for at least 12 hours under vacuum generated by an Edwards RV12 pump.
[0112] 3.b. Films with the same composition were conditioned at 190°C for 1 hour.
[0113] Finally, the conductivity of the various films was measured. The results are shown in Table 5 below.
[0114] Example 4: Comparative Example
[0115] In a 30 ml internal mixer, a mixture was prepared from 12.2 g of PPC (QPac40), 11.6 g of PPC polyol (Converge 212-10), and 10.2 g of LiTFSI. After adding the raw materials, mixing was carried out at 65±5° C. for 5 minutes.
[0116] Table 4
[0117] substance %(m / m) PPC(QPac40) 35.9 PPC (Converge212-10) 34.1 LiTFSI 30.0
[0118] % (m / m): mass % relative to the total mass of the mixed substance.
[0119] The conductivity of the films was measured; the results are shown in Table 5. The polarization behavior of the modulated films was 2 Under the conditions ( Figure 1 ) was tested between two lithium metal electrodes.
[0120] Table 5: Results
[0121]
[0122] **The film is liquid at 60°C.
[0123] Example 5: Electrode comprising a solid polymer electrolyte prepared by a melt process
[0124] In a 30 ml internal mixer, add 4.8 g HNBR (zetpol 2010), 3.0 g PPC (QPac40), 2.9 g PPC polyol (Converge 212-10), 4.6 g LiTFSI, and 33.5 g LiFePO 4 (Lifepower P2), 2.6 g of carbon black (Timcal C65). After adding the raw materials, mix at 85±10°C for 5 minutes.
[0125] The final mixture had the following composition.
[0126] Table 6
[0127] substance %(m / m)t HNBR (Zetpol 2010) 9.3 PPC(QPac40) 5.9 PPC (Converge212-10) 5.6 LiTFSI 9 <![CDATA[LiFePO 4 ]]> 65.2 C65 5
[0128] % (m / m): mass % relative to the total mass of the mixed substance.
[0129] The final mixture was pressed into several films of approximately 50 μm thickness using a Dr Collin Teachline CR72T. These films were then plated on current collectors and dried at 60°C for at least 12 hours under vacuum created by an Edwards RV12 pump.
[0130] The electrodes were assembled into button cells using the mixture of Example 1 as a separator with a thickness of about 75 μm and metallic lithium as the anode. The two films were conditioned at 190°C for 1 hour before assembly into button cells. We obtained a capacity of 164 mAh / g LFP at the first discharge rate of C / 20 at 60°C ( Figure 3 ) and remained stable for at least 12 cycles ( Figure 4 ).
Claims
1. A solid polymer electrolyte comprising a polymer matrix containing at least one ionic salt, in, The ionic salt is selected from LiBETI, LiC 2 F 5 SO 3 ,LiC 4 F 9 SO 3 、LiCF 3 SO 3 , NaI, NaSCN, NaBr, KI, KBr, LiClO 4 , LiBF 4 、LiAsF 6 、LiPF 6 、LiNO 3 、Li(CF 3 SO 2 ) 2 N、Li(CF 3 SO 2 ) 3 C、LiN(SO 2 C 2 F 5 ) 2 , alkyl fluorolithium phosphate, lithium difluoro(oxalate)borate, lithium bis(oxalate)borate, MTFSiLi, STFSiLi and any mixture thereof, wherein the polymer matrix comprises at least one polyalkylene carbonate, at least one second polymer different from the polyalkylene carbonate, and at least one alkylene carbonate produced by decomposition of the polyalkylene carbonate, wherein the amount of olefin carbonate is at least 1000 ppm relative to the total mass of the polymer matrix, and the decomposition of polyethylene carbonate is not more than 70% by mass, Wherein, the second polymer is an elastic polymer, and the elastic polymer is selected from HNBR, polyisoprene, rubber-like polymer and any mixture thereof.
2. The solid polymer electrolyte according to claim 1, It is characterized in that The polyalkylene carbonate is present in an amount of 20 to 50% by mass relative to the total mass of the polymer of the matrix.
3. The solid polymer electrolyte according to claim 1 or 2, It is characterized in that The polymer matrix comprises a polyalkylene carbonate of high molar mass and a polyalkylene carbonate of low molar mass relative to each other.
4. The solid polymer electrolyte according to claim 1 or 2, It is characterized in that The matrix has no macroscopic separation between the phase containing the polyalkylene carbonate and the phase containing the second polymer.
5. The solid polymer electrolyte according to claim 1 or 2, It is characterized in that The matrix comprises a solid mineral or organic filler.
6. The solid polymer electrolyte according to claim 1 or 2, It is characterized in that The solid polymer electrolyte is in the form of a thin film having a thickness of less than 1 mm.
7. The solid polymer electrolyte according to claim 1 or 2, It is characterized in that The polymer matrix is obtained by mixing the polyalkylene carbonate and the second polymer by melting or by using a solvent, wherein the polyalkylene carbonate and the second polymer are both soluble.
8. A method for preparing a solid polymer electrolyte according to any one of claims 1 to 7, in, The method comprises: mixing the polyalkylene carbonate and the second polymer by melting or by a solvent, wherein the polyalkylene carbonate and the second polymer are both soluble; and partially decomposing the polyalkylene carbonate into alkylene carbonate to obtain the solid polymer electrolyte.
9. The method according to claim 8, It is characterized in that The method includes heating the solid polymer electrolyte.
10. An electrode comprising at least one solid polymer electrolyte according to any one of claims 1 to 7 or a solid polymer electrolyte obtained by the method according to any one of claims 8 to 9.
11. A battery comprising at least one solid polymer electrolyte according to any one of claims 1 to 7 or a solid polymer electrolyte obtained by the method according to any one of claims 8 to 9.
12. The battery according to claim 11, It is characterized in that The battery is a solid polymer electrolyte lithium battery.
Citation Information
Patent Citations
High-conductivity polymer electrolyte and preparation method thereof
CN107195963A
Ionically conductive polymer electrolyte, production thereof, and polymer battery
JP1999060870A