Electrode structure, bipolar all-solid-state secondary battery including the same, and method for manufacturing the same
By installing a folding structure and compression pad in the current collector of an all-solid-state secondary battery, the volume changes of the anode layer are absorbed, and the problems of battery performance deterioration and short circuit risk are solved, and the durability and safety of the battery are improved.
Patent Information
- Application Number
- CN202111197977.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-10-30
- Filing Date
- 2021-10-14
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-10-14
Smart Images

Figure CN114447263B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2020-0143878 filed on October 30, 2020, in the Korean Intellectual Property Office, the disclosure of which is incorporated herein by reference in its entirety. Technical Field
[0003] One or more embodiments relate to an electrode structure, a bipolar all-solid-state secondary battery including the same, and a method of manufacturing the electrode structure. Background Art
[0004] Recently, in response to industrial needs, batteries with high energy density and safety have been actively developed. For example, lithium-ion batteries are used not only in the fields of information-related equipment (e.g., electrical appliances) and communication equipment (e.g., electrical appliances), but also in the automotive field. In the automotive field, safety is particularly important because it has an impact on driver and traffic safety.
[0005] Since commercially available lithium-ion batteries use an electrolyte containing a flammable organic solvent, they may overheat and catch fire when a short circuit occurs. In this regard, all-solid batteries using a solid electrolyte instead of an electrolyte have been proposed.
[0006] Since the all-solid-state battery does not use flammable organic solvents, the possibility of fire or explosion can be greatly reduced even if a short circuit occurs. Therefore, the safety of such an all-solid-state secondary battery can be greatly increased (eg, improved) compared to a lithium-ion battery using an electrolyte.
[0007] Furthermore, one of the characteristics of all-solid-state secondary batteries is that, unlike prior art lithium-ion batteries, they can be easily constructed into a bipolar structure, so the number of components can be reduced, and it is easier to flow a large current, thereby allowing the development of high-power and high-energy density batteries with high voltage. However, for a bipolar structure in which electrodes are arranged in series, it is difficult to design a structure that can absorb the volume change caused by the lithium deposition reaction utilized in the anode of the all-solid-state secondary battery. Summary of the invention
[0008] Aspects according to one or more embodiments relate to an electrode structure capable of absorbing a volume change of an anode in an all-solid-state secondary battery.
[0009] Aspects according to one or more embodiments relate to a bipolar all-solid-state secondary battery including the electrode structure.
[0010] Aspects according to one or more embodiments are directed to methods of manufacturing an electrode structure.
[0011] Additional aspects will be set forth in part in the description which follows and, in part, will be obvious from the description, or may be learned by practice of the presented embodiments of the disclosure.
[0012] According to one or more embodiments, the electrode structure comprises:
[0013] a current collector having a folded structure including an outer surface and an inner surface, the inner surface defining an interior space, wherein the outer surface includes a first portion, a second portion facing away from the first portion in an opposite direction, and an intermediate portion between the first portion and the second portion;
[0014] a cathode active material layer on a first portion of the outer surface;
[0015] an anode active material layer on a second portion of the outer surface; and
[0016] A compression pad is disposed inside the inner space of the folded structure of the current collector.
[0017] According to one or more embodiments, a bipolar all-solid-state secondary battery includes a stack structure including a plurality of unit cells, wherein each of the plurality of unit cells includes an electrode structure; and a solid electrolyte layer on a cathode active material layer.
[0018] According to one or more embodiments, a method of manufacturing an electrode structure includes:
[0019] preparing a current collector having a first surface and a second surface opposite to the first surface, the first surface including a first portion, a second portion, and an intermediate portion between the first portion and the second portion;
[0020] coating the first portion with a cathode active material;
[0021] coating the second portion with an anode active material;
[0022] folding the middle portion to create an interior space of the current collector, wherein the second surface is an interior surface of the current collector and the first portion and the second portion are exterior surfaces facing in opposite directions; and
[0023] A compression pad is disposed in the interior space of the current collector. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The above and other aspects, features and enhancements of certain embodiments of the present disclosure will become more apparent from the following description in conjunction with the accompanying drawings, in which:
[0025] Figure 1 is a schematic cross-sectional view of an electrode structure according to an embodiment;
[0026] Figure 2 A schematic diagram for explaining a process of manufacturing an electrode structure according to an embodiment; and
[0027] Figure 3 is a schematic cross-sectional view of a bipolar all-solid-state secondary battery according to an embodiment. DETAILED DESCRIPTION
[0028] The embodiments in the accompanying drawings will now be explained in more detail with reference to their examples, wherein the same reference numerals refer to the same elements throughout. In this regard, the present embodiments may have different forms and should not be construed as being limited to the description set forth herein. Accordingly, the embodiments are described below only by reference to the figures to explain the various aspects of this description. As used herein, the term "and / or" includes any and all combinations of one or more related enumerated items. Expressions such as "at least one of..." when preceding a list of elements, modify the entire list of elements and do not modify the individual elements of the list.
[0029] The subject matter of the present disclosure will now be more fully described with reference to the accompanying drawings in which example embodiments are illustrated. However, the subject matter of the present disclosure may be embodied in many different forms and should not be construed as limited to the embodiments set forth herein, and should be construed to include all modifications, equivalents, and alternatives within the scope of the present disclosure.
[0030] The terms used herein are for the purpose of describing specific embodiments only and are not intended to limit the present disclosure. Singular expressions include plural expressions unless the context clearly indicates otherwise. It will be further understood that the terms "comprises" and / or "comprising" when used in this specification specify the presence of narrated features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or groups thereof. As used herein, the slash " / " or the term "and / or" includes any and all combinations of one or more related enumerated items.
[0031] In the accompanying drawings, the thickness may be enlarged or reduced to clearly illustrate the various layers and regions. Throughout the specification, the same reference numerals are used to refer to the same parts. Throughout the specification, when an element such as a layer, film, region or assembly is referred to as "on" another layer or element, it may be "directly on" another layer or element, or there may be an intervening layer, region or assembly. Although the terms "first", "second", "third", etc., may be used herein to describe various elements, components, regions and / or layers, these elements, components, regions and / or layers should not be limited by these terms. These terms are only used to distinguish one component from another component and are not used for limiting purposes.
[0032] Hereinafter, a bipolar laminated unit cell structure and an all-solid-state secondary battery including the same according to an embodiment will be described in more detail.
[0033] In the related art, it is difficult to design a structure capable of absorbing volume changes caused by the lithium deposition reaction utilized (e.g., occurring) in the anode of an all-solid-state secondary battery having a bipolar structure, and in the absence of a buffer structure of the anode layer, thickness changes on the inside of the battery may become severe due to non-uniform lithium electrodeposition, and localized charge-discharge may occur, which may degrade battery performance and cause (e.g., increase) the risk of short circuit.
[0034] In all-solid-state secondary batteries in the related art, a structure has been proposed in which stacked batteries are placed in a bipolar structure to increase the capacity of the battery, but a structure for absorbing volume changes may be required (eg, may not have been proposed yet).
[0035] Accordingly, in order to solve the above-mentioned problems in bipolar batteries utilizing the same current collector, the content disclosed by the entity of the present invention is intended to provide an electrode structure capable of having a buffer structure on the same current collector (for example, a space formed by the same current collector), a bipolar all-solid-state secondary battery including the same, and a method for manufacturing the electrode structure.
[0036] Electrode structure
[0037] An electrode structure according to an embodiment includes:
[0038] A current collector having a first surface and a second surface opposite to the first surface (e.g., facing in opposite directions), wherein the first surface includes a first portion, a second portion, and an intermediate portion between the first portion and the second portion, the first portion and the second portion are arranged toward the outside in opposite directions around the intermediate portion, and the second surface has an inwardly folded structure. That is, the current collector forms a folded structure, the second surface forms an inner surface of the folded structure, and the first portion and the second portion form outer surfaces of the folded structure facing in opposite directions;
[0039] a cathode active material layer on a first portion of the first surface;
[0040] an anode active material layer on the second portion of the first surface; and
[0041] A compression mat is disposed inside the inwardly folded structure of the current collector (eg, inside an interior space of the folded structure defined (eg, surrounded) by the second surface).
[0042] In the electrode structure according to the embodiment, a compression pad is provided inside the folded current collector to absorb the volume change of the anode layer during charging and discharging. Through this buffer structure of the current collector, the anode layer can be protected from the volume change during charging and discharging, thereby improving the durability of the bipolar all-solid-state secondary battery.
[0043] For example, the electrode structure can be manufactured by the following method.
[0044] A method of manufacturing an electrode structure according to an embodiment includes:
[0045] preparing a current collector having a first surface and a second surface opposite to the first surface, the first surface including a first portion, a second portion, and an intermediate portion between the first portion and the second portion;
[0046] coating the first portion with a cathode active material;
[0047] coating the second portion with an anode active material;
[0048] folding the middle portion to create an interior space, wherein the second surface is an interior surface and the first portion and the second portion are exterior surfaces facing in opposite directions; and
[0049] A compression pad is provided for the inner side of the inward fold of the current collector.
[0050] Figure 1 Schematic cross-sectional view of an electrode structure according to an embodiment. Figure 1 As shown in FIG. 1 , the electrode structure 1 has a current collector 10 having a folded structure, a cathode active material layer 20 , an anode active material layer 30 , and a compression pad 40 disposed within the folded structure of the current collector 10 (eg, the inner space of the folded structure).
[0051] Figure 2 Schematic diagram for explaining a process of manufacturing an electrode structure according to an embodiment. Figure 2 , the current collector 10 has both a first surface 11 and a second surface 12, and the first surface 11 includes a first portion 11a, a second portion 11b, and an intermediate portion 11c separating (eg, dividing / connecting) the first portion 11a from the second portion 11b.
[0052] The cathode active material layer 20 is applied to the first portion 11a of the first surface 11, and the anode active material layer 30 is applied to the second portion 11b. The middle portion 11c is an uncoated portion on which the active material layer is not applied. Meanwhile, the entire second surface 12 may be an uncoated portion.
[0053] When the collector 10 is folded and bent around the middle portion 11c, the first portion 11a coated with the cathode active material layer 20 and the second portion 11b coated with the anode active material layer 30 are arranged toward the outside in opposite directions to each other (e.g., forming the outer surface of the collector 10), and the second surface 12 is folded inward (e.g., forming the inner surface of the collector 10).
[0054] As such, the compression pad 40 is disposed inside the folded structure of the current collector 10, thereby forming the electrode structure 1 having a buffer structure. The compression pad 40 is disposed inside the folded current collector 10, thereby being able to absorb the volume change of the anode active material layer 30 during charge and discharge.
[0055] The solid electrolyte layer 50 ( Figure 3 ) is disposed on the cathode active material layer 20 of the electrode structure 1, thereby forming a unit cell 2 constituting the all-solid-state secondary battery according to the embodiment.
[0056] Hereinafter, each component will be described in more detail.
[0057] Current Collector
[0058] As a current collector 10 of a bipolar battery that can serve as both a cathode and an anode, a current collector having a wide withstand voltage range (e.g., a wide voltage range) can be used. For example, the voltage range (e.g., withstand voltage range) of the current collector 10 can be about -1 V to about 5.5 V or about -0.5 V to about 5.5 V. Within the above range, it can be suitably used as a current collector 10 of a bipolar battery.
[0059] For example, the current collector 10 may be made of a material that does not react with lithium, that is, does not form an alloy and / or compound with lithium. Examples of materials suitable for constituting the current collector 10 may include, but are not limited to, stainless steel, aluminum (Al), copper (Cu), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), alloys thereof, and claddings thereof. Any suitable material for constituting a current collector of a bipolar battery in the related art may be utilized. The current collector 10 may be made of one of the above-mentioned metals or an alloy of two or more metals, and / or may be made of a coating material.
[0060] According to an embodiment, the current collector 10 may be made of stainless steel. Since stainless steel has a wide withstand voltage range of about -0.5 V to about 5.5 V, it can be appropriately used as the current collector 10 of the bipolar battery. According to an embodiment, an Al-Cu clad alloy (an alloy that can withstand a wide range of dislocations) may also be appropriately used for the current collector 10.
[0061] The current collector 10 may be manufactured in the form of a plate or a foil.
[0062] For example, the electrode structure 1 may further include a film (not shown) containing an element capable of forming an alloy with lithium on the second portion 11b of the first surface 11 of the current collector 10. The film may be disposed between the current collector 10 and the anode active material layer 30. For example, the film contains an element capable of forming an alloy with lithium. Examples of elements capable of forming an alloy with lithium may include, but are not limited to, gold, silver, zinc, tin, indium, silicon, aluminum, and bismuth. Any element capable of forming an alloy with lithium in the relevant field may be utilized. The film may be formed of one of these metals or may be formed of an alloy of several kinds (e.g., types) of metals. For example, since the film is disposed between the current collector 10 and the anode active material layer 30, the second anode active material layer in the form of a deposition deposited between the film and the anode active material layer 30 may be further flattened, and the cycle characteristics of the all-solid-state secondary battery 3 may be further improved.
[0063] For example, the thickness of the film may be from about 1nm to about 800nm, from about 10nm to about 700nm, from about 50nm to about 600nm or from about 100nm to about 500nm. When the thickness of the film is less than about 1nm, it may be difficult to function as a film. When the film is too thick, the film itself absorbs lithium, so that the amount of lithium deposited in the anode is reduced, so that the energy density of the all-solid-state secondary battery 3 is reduced, and the cycle characteristics of the all-solid-state secondary battery 3 may be deteriorated. For example, the film may be arranged on the collector 10 and the second anode collector 10' by vacuum deposition, sputtering, electroplating and / or similar methods, but the present disclosure is not necessarily limited to these methods. Any suitable method capable of forming a film in the relevant art may be utilized.
[0064] Compression pads
[0065] The compression pad 40 inside the folded structure of the current collector 10 may be made in the form of a thin sheet including an elastic material.
[0066] The elastic material may include at least one selected from the following: polyurethane, natural rubber, spandex, butyl rubber (isobutylene isoprene rubber, IIR), fluoroelastomer, ethylene-propylene rubber (EPR), styrene-butadiene rubber (SBR), chloroprene, elastin, epichlorohydrin rubber, nylon, terpene, isoprene rubber, polybutadiene, nitrile rubber, thermoplastic elastomer, silicone rubber, ethylene-propylene-diene rubber (EPDM), ethylene vinyl acetate (EVA), halogenated butyl rubber and copolymers thereof. However, the present disclosure is not limited thereto, and any elastic material may be utilized without limitation as long as it has elasticity. According to an embodiment, the compression pad 40 may be made of a urethane-based material, for example, polyurethane.
[0067] According to an embodiment, the compression pad 40 may be formed of a urethane-based polymer sheet having a deformation rate of about 30% to about 60%.
[0068] The compressed mat 40 may be pressed (e.g., may be capable of being pressed) to have a thickness of about 40% to about 90% of the initial thickness of the compressed mat 40 before being pressed. For example, the compressed mat 40 may be pressed to have a thickness of about 50% to about 85%, about 60% to about 80%, or about 65% to about 75% of the initial thickness of the compressed mat 40 before being pressed. Because the volume change of the anode is effectively absorbed within the above range, it is possible to smoothly charge and discharge the all-solid-state secondary battery.
[0069] The thickness of the compression pad 40 may be in the range of about 200% to about 500% of the thickness of the lithium deposition layer of the anode formed when the all-solid-state secondary battery is charged. In the all-solid-state secondary battery, the thickness of the lithium deposition layer of the anode is determined in proportion to the current density of the cathode. That is, the thickness of the lithium deposition layer of the anode is determined according to the amount of lithium moved from the cathode to the anode, and thereby the volume change of the anode occurs (for example, thereby increasing the volume of the anode). Accordingly, the thickness of the compression pad 40 may be determined to absorb the volume change of the anode. Therefore, the thickness of the compression pad 40 may be set to be in the range of about 200% to about 500% of the thickness of the lithium deposition layer of the anode formed when the all-solid-state secondary battery is charged, thereby effectively absorbing the volume change of the anode. For example, the thickness of the compression pad 40 may be in the range of about 250% to about 450% or about 300% to about 400% of the thickness of the lithium deposition layer of the anode formed when the all-solid-state secondary battery is charged.
[0070] The thickness of the compression pad 40 may be set within a range of about 50 μm to about 300 μm, and in some cases, may be selectively set within a range of about 100 μm to about 150 μm, about 200 μm to about 300 μm, or about 50 μm to about 100 μm.
[0071] As such, since compression pad 40 is disposed in the folded structure of current collector 10 , volume changes caused by a deposition reaction of lithium (Li) used in the anode can be absorbed and thus the anode layer can be protected, thereby improving the durability of the bipolar all-solid secondary battery.
[0072] Cathode layer
[0073] like Figure 1 As shown in FIG. 1 , in the electrode structure 1 , the cathode active material layer 20 is disposed on the first portion 11 a of the first surface 11 of the current collector 10 .
[0074] Cathode active material layer: Cathode active material
[0075] For example, the cathode active material layer 20 includes a cathode active material and a solid electrolyte. The solid electrolyte included in the cathode active material layer 20 may be similar to or different from the solid electrolyte included in the solid electrolyte layer 50. For further details of the solid electrolyte, refer to those of the solid electrolyte layer 50.
[0076] The cathode active material is a cathode active material that can reversibly absorb and desorb lithium ions. For example, the cathode active material may be a lithium transition metal oxide (e.g., lithium cobalt oxide (LCO), lithium nickel oxide, lithium nickel cobalt oxide, lithium nickel cobalt aluminum oxide (NCA) and / or lithium nickel cobalt manganese oxide (NCM)), lithium manganate, lithium phosphate and iron phosphate, nickel sulfide, copper sulfide, lithium sulfide, iron oxide and / or vanadium oxide, etc., but is not limited thereto, and any one of the cathode active materials in the relevant field may be used. The cathode active materials may be used individually or as a mixture of two or more thereof.
[0077] For example, the cathode active material may be a compound represented by one of the following: Li a A 1-b B b D2 (where 0.90≤a≤1 and 0≤b≤0.5); Li a E 1-b B b O 2-c D c (where 0.90≤a≤1, 0≤b≤0.5 and 0≤c≤0.05); LiE 2- b B b O 4-c D c (where 0≤b≤0.5 and 0≤c≤0.05); Li a Ni 1-b-c Co b B c D α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05 and 0<α≤2); Li a Ni 1-b-c Co b B c O 2-α H α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2); Li a Ni 1-b-c Co b B c O 2-α H2 (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2); Lia Ni 1-b-c Mn b B c D α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05 and 0<α≤2); Li a Ni 1-b-c Mn b B c O 2-α H α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2); Li a Ni 1-b-c Mn b B c O 2-α H2 (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2); Li a Ni b E c G d O2 (where 0.90≤a≤1, 0≤b≤0.9, 0≤c≤0.5 and 0.001≤d≤0); Li a Ni b Co c Mn d G e O2 (where 0.90≤a≤1, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5 and 0.001≤e≤0.1); Li a NeG b O2 (where 0.90≤a≤1 and 0.001≤b≤0.1); Li a CoG b O2 (where 0.90≤a≤1 and 0.001≤b≤0.1); Li a MnG b O2 (where 0.90≤a≤1 and 0.001≤b≤0.1); Li a Mn b O4 (where 0.90≤a≤1 and 0.001≤b≤0.1); Li a Ni b Co c Mn d G e O2 (where 0.90≤a≤1, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5 and 0.001≤e≤0.1); Li a NeG b O2 (where 0.90≤a≤1 and 0.001≤b≤0.1); Lia CoG b O2 (where 0.90≤a≤1 and 0.001≤b≤0.1); Li a MnG b O2 (where 0.90≤a≤1 and 0.001≤b≤0.1); Li a Mn b O4 (where 0.90≤a≤1 and 0.001≤b≤0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiLO2; LiNiVO4; Li (3-f) J2(PO4)3(0≤f≤2);Li (3-f) Fe2(PO4)3(0≤f≤2); and LiFePO4. In these compounds, A is Ni, Co, Mn or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element or a combination thereof; D is O, F, S, P or a combination thereof; E is Co, Mn or a combination thereof; H is F, S, P or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V or a combination thereof; Q is Ti, Mo, Mn or a combination thereof; L is Cr, V, Fe, Sc, Y or a combination thereof; and J is V, Cr, Mn, Co, Ni, Cu or a combination thereof. Compounds having a coating added to their surfaces may also be utilized, and mixtures having the above compounds and a coating added thereto may also be utilized. For example, the coating added to the surface of the compound includes a coating element compound of an oxide, hydroxide, oxyhydroxide, oxycarbonate and / or basic carbonate of the coating element. The compound forming the coating is amorphous or crystalline. The coating element included in the coating may be Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr or a mixture thereof. The method for forming the coating may be any suitable method that does not adversely affect the performance of the cathode active material. For example, the coating method may be spraying, coating and / or dipping. Because the specific coating method can be well understood by those skilled in the art, its detailed description will be omitted.
[0078] For example, the cathode active material may include a lithium salt of a transition metal oxide having a layered rock salt type (e.g., type) structure among the above-mentioned lithium transition metal oxides. For example, the "layered rock salt type (e.g., type) structure" is a structure in which oxygen atom layers and metal atom layers are alternately and regularly arranged in the <111> direction of the cubic rock salt type (e.g., type) structure, whereby each atom layer forms a two-dimensional plane. The "cubic rock salt type (e.g., type) structure" refers to the sodium chloride type (e.g., type) (NaCl type (e.g., type)) structure, which is a type (e.g., type) of crystal structure, and specifically, has a structure in which each of the cations and anions is arranged in a face-centered cubic lattice (FCC) and is displaced by 1 / 2 of the ridge of the unit lattice from each other. The lithium transition metal oxide having a layered rock salt type (e.g., type) structure may be a ternary lithium transition metal oxide, for example, LiNi x Co y Al z O2 (NCA) and / or LiNi x Co y Mn z O2 (NCM) (0 < x < 1, 0 < y < 1, 0 < z < 1, x + y + z = 1). When the cathode active material includes a ternary lithium transition metal oxide having a layered rock salt type (e.g., type) structure, the energy density and thermal stability of the all-solid-state secondary battery 3 are further improved.
[0079] As described above, the cathode active material may be covered with a coating. The coating may be any one suitable as a coating for the cathode active material of the all-solid-state secondary battery. For example, the coating may be Li2O-ZrO2 and / or the like.
[0080] When the cathode active material includes a ternary lithium transition metal oxide containing nickel (Ni) (such as NCA and / or NCM), the capacity density of the all-solid-state secondary battery 3 can be increased, whereby the metal dissolution of the cathode active material in the charged state can be reduced. As a result, the cycle characteristics of the all-solid-state secondary battery 3 in the charged state are improved.
[0081] For example, the shape of the cathode active material may be spherical or ellipsoidal. The particle size of the cathode active material is not particularly limited and may be within the range applicable to all-solid-state secondary batteries in the relevant field. The content of the cathode active material in the cathode active material layer 20 is also not particularly limited and may be within the range applicable to all-solid-state secondary batteries in the relevant field.
[0082] Cathode active material layer: Solid electrolyte
[0083] For example, the cathode active material layer 20 may include a solid electrolyte. The solid electrolyte included in the cathode active material layer 20 may be the same as or different from the solid electrolyte included in the solid electrolyte layer 50. For details of the solid electrolyte, refer to those of the solid electrolyte layer 50.
[0084] The solid electrolyte included in the cathode active material layer 20 may have an average particle size D50 of particles of the solid electrolyte that is smaller than the average particle size D50 of particles of the solid electrolyte included in the solid electrolyte layer 50. For example, the average particle size D50 of particles of the solid electrolyte included in the cathode active material layer 20 may be about 90% or less, about 80% or less, about 70% or less, about 60% or less, about 50% or less, about 40% or less, about 30% or less, or about 20% or less of the average particle size D50 of particles of the solid electrolyte included in the solid electrolyte layer 50.
[0085] For example, the average particle diameter D50 is the median particle diameter D50. For example, the median particle diameter D50 is a particle size corresponding to 50% cumulative volume calculated from particles having a small particle diameter in a particle size distribution measured by a laser diffraction method.
[0086] Cathode active material layer: Binder
[0087] The cathode active material layer 20 may include a binder. Examples of the binder may include, but are not limited to, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, and polyethylene. Any appropriate binder used in the related art may be used.
[0088] Cathode active material layer: conductive material
[0089] The cathode active material layer 20 may include a conductive material. Examples of the conductive material may include, but are not limited to, graphite, carbon black, acetylene black, Ketjen black, carbon fiber, and metal powder. Any suitable conductive material used in the related art may be used.
[0090] Cathode active material layer: other additives
[0091] The cathode active material layer 20 may further include additives such as a filler, a coating agent, a dispersant, and / or an ion conductive aid, in addition to the above-mentioned cathode active material, solid electrolyte, binder, and conductive material.
[0092] Any appropriate material generally used for electrodes of all-solid-state secondary batteries in the related art may be used as the filler, coating agent, dispersant and / or ion conduction aid included in the cathode active material layer 20 .
[0093] Electrolyte layer
[0094] like Figure 3, the solid electrolyte layer 50 is disposed on the cathode active material layer 20, thereby forming a unit cell 2 including the electrode structure 1 and the solid electrolyte layer 50. The solid electrolyte layer 50 may be a solid electrolyte layer.
[0095] Solid electrolyte layer: solid electrolyte
[0096] For example, the solid electrolyte may be a sulfide solid electrolyte. For example, the sulfide solid electrolyte may be at least one selected from the following: Li2S-P2S5, Li2S-P2S5-LiX (wherein X is a halogen element), Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n (wherein m and n are each a positive number, and Z is one selected from Ge, Zn and Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q (wherein p and q are each positive numbers, and M is one selected from P, Si, Ge, B, Al, Ga, and In), Li 7-x PS 6-x Cl x (0≤x≤2), Li 7-x PS 6-x Br x (0≤x≤2) and Li 7-x PS 6-x I x (0≤x≤2). In some embodiments, the sulfide solid electrolyte can be prepared by treating a starting material, such as Li2S and / or P2S5, by a melt quenching method or a mechanical grinding method. After the treatment, a heat treatment may be performed. The solid electrolyte may be amorphous, crystalline, or a mixed state thereof. The solid electrolyte may include sulfur (S), phosphorus (P), and / or lithium (Li) as constituent elements among the above-mentioned sulfide solid electrolyte materials. For example, the solid electrolyte may be a material including Li2S-P2S5. When a solid electrolyte including Li2S-P2S5 is used as a material for a sulfide solid electrolyte forming a solid electrolyte, the mixing molar ratio of Li2S and P2S5 may be, for example, in the range of Li2S:P2S5=about 50:50 to about 90:10.
[0097] For example, the sulfide-based solid electrolyte may include an argyrodite-type (eg, type) solid electrolyte represented by the following Formula 1:
[0098] Formula 1
[0099] Li + 12-n-x A n+ X 2- 6-x Y - x ,
[0100] In Formula 1, A is P, As, Ge, Ga, Sb, Si, Sn, Al, In, Ti, V, Nb or Ta; X is S, Se or Te; Y is Cl, Br, I, F, CN, OCN, SCN or N3; and 1≤n≤5 and 0≤x≤2 are satisfied. The sulfide-based solid electrolyte may be a argyrodite-type (e.g., type) compound, which includes a compound selected from Li 7-x PS 6-x Cl x (0≤x≤2), Li 7-x PS 6-x Br x (0≤x≤2) and Li 7-x PS 6-x I x (0≤x≤2). For example, the sulfide-based solid electrolyte may be an argyrodite-type (eg, type) compound including at least one selected from Li6PS5Cl, Li6PS5Br, and Li6PS5I.
[0101] The density of the argyrodite type (e.g., type) solid electrolyte may be about 1.5 g / cc to about 2.0 g / cc. Since the argyrodite type (e.g., type) solid electrolyte has a density of 1.5 g / cc or more, the internal resistance of the all-solid-state secondary battery can be reduced, and the penetration of the solid electrolyte by Li can be effectively suppressed.
[0102] Solid electrolyte layer: Binder
[0103] For example, the solid electrolyte layer 50 may include a binder. Examples of the binder included in the solid electrolyte layer 50 may include, but are not limited to, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, and polyethylene. Any suitable binder used in the relevant art may be used. The binder included in the solid electrolyte 50 layer may be the same as or different from the binder included in the cathode active material layer 20 and the anode active material layer 30. In some embodiments, the binder may be omitted.
[0104] Relative to the total weight of the solid electrolyte layer 50, the content of the binder included in the solid electrolyte layer 50 may be about 0wt% to about 10wt%, about 0wt% to about 5wt%, about 0wt% to about 3wt%, about 0wt% to about 1wt%, about 0wt% to about 0.5wt% or about 0wt% to about 0.1wt%.
[0105] Anode layer
[0106] like Figure 1 As shown in FIG. 1 , in the electrode structure 1 , the anode active material layer 30 is disposed on the second portion 11 b of the first surface 11 of the current collector 10 .
[0107] Anode active material layer: Anode active material
[0108] For example, the anode active material layer 30 may include an anode active material and a binder.
[0109] For example, the anode active material included in the anode active material layer 30 may have a particle shape. For example, the average particle size of the anode active material having a particle shape may be about 4 μm or less, about 3 μm or less, about 2 μm or less, about 1 μm or less, or about 900 nm or less. For example, the average particle size of the anode active material having a particle shape may be about 10 nm to about 4 μm, about 10 nm to about 3 μm, about 10 nm to about 2 μm, about 10 nm to about 1 μm, or about 10 nm to about 900 nm. When the anode active material has an average particle size within these ranges, the reversible absorption and / or desorption of lithium during charging and discharging may be easier. For example, the average particle size of the anode active material is the median particle size (D50) measured using a laser particle size distribution analyzer.
[0110] For example, the anode active material included in the anode active material layer 30 may include at least one selected from a carbon-based anode active material and a metal or metalloid anode active material.
[0111] In some embodiments, the carbon-based anode active material may be amorphous carbon. Examples of amorphous carbon may include, but are not limited to, carbon black (CB), acetylene black (AB), furnace black (FB), Ketjen black (KB), and graphene. Any material may be used as long as it is classified as amorphous carbon in the relevant field. Amorphous carbon is carbon that has no crystallinity or has very low crystallinity, and is distinguished from crystalline carbon or graphite-based carbon.
[0112] The metal or metalloid anode active material may include at least one selected from gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn) and zinc (Zn), but the present disclosure is not limited thereto. Any suitable material may be used as a metal anode active material or a metalloid anode active material that forms an alloy or compound with lithium in the relevant field. For example, nickel (Ni) is not a metal anode active material because it does not form an alloy with lithium.
[0113] The anode active material layer 30 may include the type of anode active material among these anode active materials, or a mixture of multiple different anode active materials. For example, the anode active material layer 30 may include only amorphous carbon, or may include at least one selected from the following: gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn) and zinc (Zn). In some embodiments, the anode active material layer 30 may include a mixture of amorphous carbon and at least one selected from gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn) and zinc (Zn). For example, in terms of weight ratio, the mixing ratio of a mixture of amorphous carbon and gold, etc. may be about 10: 1 to about 1: 2, about 5: 1 to about 1: 1 or about 4: 1 to about 2: 1, but the present disclosure is not limited thereto, and the mixing ratio may be selected according to the characteristics of the solid secondary battery 3. When the anode active material has such a composition, the cycle characteristics of the all-solid-state secondary battery are further improved.
[0114] For example, the anode active material included in the anode active material layer 30 may include a mixture of first particles made of amorphous carbon and second particles made of metal or metalloid. Examples of metals or metalloids may include gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn) and zinc (Zn). In some embodiments, the metalloid may be a semiconductor. Based on the total weight of the mixture, the content of the second particle may be about 8wt% to about 60wt%, about 10wt% to about 50wt%, about 15wt% to about 40wt% or about 20wt% to about 30wt%. For example, when the second particle has a content within these ranges, the cycle characteristics of the all-solid-state secondary battery 3 are further improved.
[0115] Anode active material layer: Binder
[0116] Examples of the binder included in the anode active material layer 30 may include, but are not limited to, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, and polymethyl methacrylate. Any suitable binder used in the relevant field may be used. The binder may be a single binder or a plurality of different binders.
[0117] When the anode active material layer 30 includes a binder, the anode active material layer 30 is stable on the current collector 10. Further, despite the volume change and / or relative position change of the anode active material layer 30 during the charge-discharge process, the rupture of the anode active material layer 30 is suppressed. For example, when the anode active material layer 30 does not include a binder, the anode active material layer 30 may be easily separated from the current collector 10. When the anode active material layer 30 is separated from the current collector 10, the current collector 10 contacts the solid electrolyte layer 50 at the exposed portion of the current collector 10, thereby increasing the possibility of a short circuit. The anode active material layer 30 may be prepared by applying a slurry in which a material constituting the anode active material layer 30 is dispersed on the current collector 10, and drying the slurry. When a binder is included in the anode active material layer 30, the anode active material may be stably dispersed in the slurry. For example, when the slurry is applied to the current collector 10 by a screen printing method, clogging of the screen (for example, clogging by aggregates of the anode active material) may be suppressed.
[0118] Anode active material layer: other additives
[0119] The anode active material layer 30 may further include additives used in all-solid-state secondary batteries in the related art, for example, a filler, a coating agent, a dispersant, and / or an ion-conducting aid.
[0120] Anode layer: anode active material layer
[0121] For example, the thickness of the anode active material layer 30 may be about 50% or less, about 40% or less, about 30% or less, about 20% or less, about 10% or less, or about 5% or less of the thickness of the cathode active material layer 20. For example, the thickness of the anode active material layer 30 may be about 1 μm to about 20 μm, about 2 μm to about 10 μm, or about 3 μm to about 7 μm. When the anode active material layer 30 is too thin, the lithium dendrites formed between the anode active material layer 30 and the current collector 10 may collapse the anode active material layer 30, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery 3. When the thickness of the anode active material layer 30 is excessively increased (for example, becomes too thick), the energy density of the all-solid-state secondary battery 3 is reduced, and the internal resistance of the all-solid-state secondary battery 3 is increased due to the anode active material layer 30, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery 3.
[0122] For example, when the thickness of the anode active material layer 30 is reduced, the charge capacity of the anode active material layer 30 is also reduced. For example, the charge capacity of the anode active material layer 30 may be about 50% or less, about 40% or less, about 30% or less, about 20% or less, about 10% or less, about 5% or less, or about 2% or less of the charge capacity of the cathode active material layer 20. For example, the charge capacity of the anode active material layer 30 may be about 0.1% to about 50%, about 0.1% to about 40%, about 0.1% to about 30%, about 0.1% to about 20%, about 0.1% to about 10%, about 0.1% to about 5%, or about 0.1% to about 2% of the charge capacity of the cathode active material layer 20. When the charge capacity of the anode active material layer 30 is too small, the anode active material layer 30 becomes very thin. Therefore, lithium dendrites formed between the anode active material layer 30 and the current collector 10 during repeated charging and discharging processes may collapse the anode active material layer 30, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery 3. When the charging capacity of the anode active material layer 30 is excessively increased, the energy density of the all-solid-state secondary battery 3 is reduced, and the internal resistance of the all-solid-state secondary battery 3 is increased due to the anode active material layer 30, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery 3.
[0123] The charge capacity of the cathode active material layer 20 is obtained by multiplying the charge capacity density (mAh / g) of the cathode active material by the mass of the cathode active material in the cathode active material layer 20. When several kinds (e.g., types) of cathode active materials are used, the value of the charge capacity density x mass is calculated for each cathode active material, and the sum of these values is the charge capacity of the cathode active material layer 20. The charge capacity of the anode active material layer 30 is calculated in the same manner. That is, the charge capacity of the anode active material layer 30 is obtained by multiplying the charge capacity density (mAh / g) of the anode active material by the mass of the anode active material in the anode active material layer 30. When several types of anode active materials are used, the value of the charge capacity density x mass is calculated for each anode active material, and the sum of these values is the charge capacity of the anode active material layer 30. Here, the charge capacity density of the cathode active material and the anode active material is estimated using an all-solid-state half-cell using lithium metal as a counter electrode. The charge capacity of the cathode active material layer 20 and the anode active material layer 30 is directly measured by measuring the charge capacity of the all-solid-state half-cell. When the measured charge capacity is divided by the mass of each active material, the charge capacity density is obtained. In some embodiments, the charge capacity of the cathode active material layer 20 and the anode active material layer 30 may be an initial charge capacity measured during the first charge cycle.
[0124] Anode layer: Second anode active material layer (deposition layer)
[0125] In some embodiments, the all-solid-state secondary battery 3 may further include a second anode active material layer (not shown) disposed between the current collector 10 and the anode active material layer 30 by charging. The second anode active material layer is a metal layer including lithium and / or a lithium alloy. The metal layer includes lithium and / or a lithium alloy. Accordingly, because the second anode active material layer is a metal layer including lithium, it acts, for example, as a lithium storage device. Examples of lithium alloys may include, but are not limited to, Li-Al alloys, Li-Sn alloys, Li-In alloys, Li-Ag alloys, Li-Au alloys, Li-Zn alloys, Li-Ge alloys, and Li-Si alloys. Any suitable lithium alloy used in the relevant field can be used. The second anode active material layer may be made of one of these lithium alloys, and / or may be made of several types of alloys.
[0126] The thickness of the second anode active material layer is not particularly limited, but may be, for example, about 1 μm to about 1000 μm, about 1 μm to about 500 μm, about 1 μm to about 200 μm, about 1 μm to about 150 μm, about 1 μm to about 100 μm, or about 1 μm to about 50 μm. When the second anode active material layer is too thin, the second anode active material layer is difficult to use as a lithium storage device. When the second anode active material layer is too thick, the mass and volume of the all-solid-state secondary battery 3 may increase, and its cycle characteristics may be considerably deteriorated. For example, the second anode active material layer may be a metal foil having a thickness within these ranges.
[0127] In the all-solid-state secondary battery 3, the second anode active material layer may be disposed between the current collector 10 and the anode active material layer 30 before the assembly of the all-solid-state secondary battery 3, or the second anode active material layer may be deposited between the current collector 10 and the anode active material layer 30 by charging after the assembly of the all-solid-state secondary battery 3. When the second anode active material layer is disposed between the current collector 10 and the anode active material layer 30 before the assembly of the all-solid-state secondary battery 3, because the second anode active material layer is a metal layer including lithium, it acts as a lithium storage. For example, lithium foil may be disposed between the current collector 10 and the anode active material layer 30 before the assembly of the all-solid-state secondary battery 3. Therefore, the cycle characteristics of the all-solid-state secondary battery 3 including the second anode active material layer are further improved. When the second anode active material layer is deposited by charging after the assembly of the all-solid-state secondary battery 3, the second anode active material layer is not included during the assembly of the all-solid-state secondary battery 3, so that the energy density of the all-solid-state secondary battery 3 is increased. For example, when the all-solid-state secondary battery 3 is charged, the all-solid-state secondary battery 3 is charged beyond the charge capacity of the anode active material layer 30. That is, the anode active material layer 30 is overcharged. In the initial stage of charging, lithium is absorbed in the anode active material layer 30. The anode active material included in the anode active material layer 30 forms an alloy or compound with lithium ions that have migrated from the cathode active material layer 20. For example, when the all-solid-state secondary battery 3 is charged beyond the charge capacity of the anode active material layer 30, lithium is deposited on the rear surface of the anode active material layer 30, that is, between the collector 10 and the anode active material layer 30, and a metal layer corresponding to the second anode active material layer is formed by the deposited lithium. The second anode active material layer is a metal layer mainly including lithium (that is, metallic lithium). For example, when the anode active material included in the anode active material layer 30 is composed of a material that forms an alloy or compound with lithium, this result is obtained. During discharge, the lithium in the anode active material layer 30 and the second anode active material layer, that is, the metal layer is ionized and moves toward the cathode active material layer 20. Accordingly, it is possible to utilize lithium as the anode active material in the all-solid-state secondary battery 3. Further, because the anode active material layer 30 covers the second anode active material layer, it serves as a protective layer for the second anode active material layer, that is, a metal layer, and is used to suppress the deposition growth of lithium dendrites. Therefore, the short circuit and capacity reduction of the all-solid-state secondary battery 3 are suppressed, and as a result, the cycle characteristics of the all-solid-state secondary battery 3 are improved. Further, when the second anode active material layer is set by charging after the assembly of the all-solid-state secondary battery 3, in the initial state of the all-solid-state secondary battery 3 or in the state after discharge, the current collector 10 and the anode active material layer 30 and the area between the current collector 10 and the anode active material layer 30 are, for example, a Li-free area that does not include lithium (Li).
[0128] All-solid-state secondary battery
[0129] An all-solid-state secondary battery, which is a bipolar battery utilizing the same current collector, has a buffer structure inside the same current collector (e.g., inside an inner space formed by folding one current collector), making it possible to protect the anode layer from volume changes during charging and discharging, thereby improving the durability of the battery.
[0130] Figure 3 is a schematic cross-sectional view of an all-solid-state secondary battery according to an embodiment.
[0131] like Figure 3 , the all-solid-state secondary battery 3 is a bipolar all-solid-state secondary battery, which includes: a unit cell 2, the unit cell 2 including an electrode structure 1 and a solid electrolyte layer 50 disposed on a cathode active material layer 20, wherein a plurality of unit cells 2 are stacked. The all-solid-state secondary battery 3 has a structure in which a plurality of electrode structures 1 are stacked to have a bipolar connection structure, and a desired voltage design can be performed (e.g., obtained) through the bipolar connection structure.
[0132] According to an embodiment, 2 to 12 unit cells 2 may be laminated to constitute the all-solid secondary battery 3. The all-solid secondary battery 3 having a suitable voltage range may be manufactured by stacking 2 to 12 unit cells 2.
[0133] The bipolar all-solid-state secondary battery 3 may further include: a first end plate 60 and a second end plate 60', the first end plate 60 and the second end plate 60' being respectively arranged on the solid electrolyte layer 50 and the anode active material layer 30 present at two opposite ends of the stacked unit cells 2; a first half cell 4, the first half cell 4 including a second anode active material layer 30', a second current collector 10' and a compression pad 40' between the solid electrolyte layer 50 and the first end plate 60 present at one end of the battery stack; and a second half cell 5, the second half cell 5 including a second electrolyte layer 50', a second cathode active material layer 20' and a third current collector 10" between the anode active material layer 30 and the second end plate 60' present at the other end of the unit cell stack.
[0134] According to some embodiments, the electrode structure may protect the anode layer by absorbing the volume change of the anode during charge and discharge, thereby improving the durability of the battery.
[0135] It should be understood that the embodiments described herein should be considered in a descriptive sense only and not for limiting purposes. The description of features or aspects within each embodiment should generally be considered as other similar features or aspects that can be used in other embodiments. Although one or more embodiments have been described with reference to the figures, it will be understood by those of ordinary skill in the art that various appropriate changes in form and detail may be made therein without departing from the spirit and scope of the present disclosure as defined by the appended claims and their equivalents.
Claims
1. An electrode structure, comprising: a current collector having a folded structure including an outer surface and an inner surface, the inner surface defining an interior space, wherein the outer surface includes a first portion, a second portion facing away from the first portion in an opposite direction, and an intermediate portion between the first portion and the second portion; a cathode active material layer, the cathode active material layer being on the first portion of the outer surface; an anode active material layer, the anode active material layer being on the second portion of the outer surface; and a compression pad disposed inside the inner space of the folded structure of the current collector, The compression pad is made of elastic material. wherein the elastic material comprises at least one selected from the group consisting of polyurethane, natural rubber, spandex, butyl rubber, isobutylene isoprene rubber, fluoroelastomer, ethylene-propylene rubber, styrene-butadiene rubber, chloroprene, elastin, epichlorohydrin rubber, nylon, terpene, isoprene rubber, polybutadiene, nitrile rubber, thermoplastic elastomer, silicone rubber, ethylene-propylene-diene rubber, ethylene vinyl acetate, halogenated butyl rubber, and copolymers thereof, wherein the compressed mat is capable of being compressed to have a thickness of 40% to 90% of the initial thickness of the compressed mat before being compressed, and The thickness of the compression mat is 200% to 500% of the thickness of a lithium deposition layer of an anode formed when an all-solid-state secondary battery including the electrode structure is charged.
2. An electrode structure, comprising: a current collector having a folded structure including an outer surface and an inner surface, the inner surface defining an interior space, wherein the outer surface includes a first portion, a second portion facing away from the first portion in an opposite direction, and an intermediate portion between the first portion and the second portion; a cathode active material layer, the cathode active material layer being on the first portion of the outer surface; an anode active material layer, the anode active material layer being on the second portion of the outer surface; and a compression pad disposed inside the inner space of the folded structure of the current collector, wherein the compression pad is formed of a urethane polymer sheet having a deformation rate of 30% to 60%, wherein the compressed mat is capable of being compressed to have a thickness of 40% to 90% of the initial thickness of the compressed mat before being compressed, and The thickness of the compression mat is 200% to 500% of the thickness of a lithium deposition layer of an anode formed when an all-solid-state secondary battery including the electrode structure is charged.
3. The electrode structure according to claim 1 or 2, wherein the middle portion of the outer surface and the inner surface are uncoated. 4 . The electrode structure according to claim 1 , wherein the compression pad has a thickness of 50 μm to 300 μm. The electrode structure according to claim 1 , wherein the current collector is made of stainless steel.
6. The electrode structure according to claim 1 or 2, wherein the current collector is made of at least one selected from the group consisting of aluminum, copper, titanium, iron, cobalt, nickel, and alloys thereof.
7. The electrode structure according to claim 1 or 2, further comprising: a second anode active material layer between the current collector and the anode active material layer, wherein the second anode active material layer is a metal layer including lithium and / or a lithium alloy.
8. A bipolar all-solid-state secondary battery, comprising a stacked structure comprising a plurality of unit cells, Each of the plurality of unit cells comprises: The electrode structure according to any one of claims 1 to 7; and a solid electrolyte layer on the cathode active material layer.
9. The bipolar all-solid-state secondary battery according to claim 8, wherein the solid electrolyte layer comprises a sulfide-based solid electrolyte, and the sulfide-based solid electrolyte is at least one selected from the group consisting of: Li2S-P2S5; Li2S-P2S5-LiX, wherein X is a halogen element; Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S-P2S5-Z m S n , wherein m and n are each a positive number and Z is one of Ge, Zn and Ga; Li2S-GeS2; Li2S-SiS2-Li3PO4; Li2S-SiS2-Li p MO q , wherein p and q are each a positive number and M is one selected from P, Si, Ge, B, Al, Ga and In; Li 7-x PS 6-x Cl x , where 0≤x≤2; Li 7-x PS 6-x Br x where 0≤x≤2; and Li 7-x PS 6-x I x , where 0≤x≤2. 10 . The bipolar all-solid-state secondary battery according to claim 8 , wherein the stacked structure comprises 2 to 12 of the unit cells.
11. The bipolar all-solid-state secondary battery according to claim 8, further comprising: a first end plate on the solid electrolyte layer at a first end of the stack; and a second end plate on the anode active material layer at a second end of the stacked structure opposite the first end; a first half-cell between the solid electrolyte layer and the first end plate at the first end of the stack, the first half-cell comprising a second anode active material layer, a second current collector, and a second compression mat; as well as A second half cell between the anode active material layer and the second end plate at the second end of the stacked structure includes a second electrolyte layer, a second cathode active material layer, and a third current collector.
12. A method for manufacturing the electrode structure according to any one of claims 1 to 7, the method comprising: preparing a current collector having a first surface and a second surface opposite to the first surface, the first surface including a first portion, a second portion, and an intermediate portion between the first portion and the second portion; coating the first portion with a cathode active material; coating the second portion with an anode active material; folding the middle portion to create an interior space of the current collector, wherein the second surface is an interior surface of the current collector and the first portion and the second portion are exterior surfaces facing in opposite directions; as well as A compression pad is disposed in the interior space of the current collector.