Solar cell and photovoltaic module

By arranging a silicon oxide layer containing nitrogen and phosphorus on the back surface of the N-type semiconductor substrate of the solar cell, the problem of insufficient thickness of the silicon dioxide layer is solved, the passivation effect and tunneling ability of the cell are improved, and the conversion efficiency and The filling factor solves the problem of battery internal resistance and metal ions.

CN114551606BActive Publication Date: 2024-10-15JINKOSOLAR MIDDLE EAST FZCO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210172054.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-16
Publication Date
2024-10-15
Estimated Expiration
2041-09-16

AI Technical Summary

Technical Problem

The thickness of the silicon dioxide layer of the existing Topcon battery is too thin, resulting in defects and pores in the film layer, resulting in short-circuit phenomena and a reduction in the degree of carrier recombination. In addition, an excessively thick silicon dioxide film layer will hinder electron migration and reduce the tunneling effect. and fill factor, which affects the conversion efficiency of the battery.

Method used

A silicon oxide layer containing nitrogen and phosphorus is provided between the back surface of the N-type semiconductor substrate and the phosphorus-doped polysilicon layer. The dielectric constant and passivation effect are increased through the doping of the N element. The doping of the P element in the second The donor impurity energy level is generated in the silicon oxide band gap, which increases the tunneling current and filling factor, forming a multi-layer silicon oxide layer structure to improve the conversion efficiency of the battery.

Benefits of technology

It improves the back surface passivation effect and tunneling ability of the battery, increases the open circuit voltage and filling factor, enhances the conversion efficiency of the solar cell, and at the same time reduces the internal resistance of the battery and the impact on metal ions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114551606B_ABST
    Figure CN114551606B_ABST
Patent Text Reader

Abstract

The present application relates to a solar cell and a photovoltaic module, wherein the solar cell comprises an N-type semiconductor substrate, wherein the N-type semiconductor substrate has a front surface and a rear surface opposite to each other; a boron diffusion layer is provided on the front surface of the N-type semiconductor substrate, a first passivation layer is provided on the surface of the boron diffusion layer, and a first electrode is provided on the surface of the first passivation layer; a phosphorus-doped polysilicon layer is provided on the rear surface of the N-type semiconductor substrate, a silicon oxide layer containing nitrogen and phosphorus elements is provided between the rear surface of the N-type semiconductor substrate and the phosphorus-doped polysilicon layer, a second passivation layer is provided on the surface of the phosphorus-doped polysilicon layer, and a second electrode is provided on the surface of the second passivation layer. The present application provides a silicon oxide layer containing nitrogen and phosphorus elements on the N-type semiconductor substrate and the phosphorus-doped polysilicon layer on the rear surface of the battery, thereby improving the tunneling ability of the rear surface of the battery and improving the passivation effect of the rear surface of the battery, thereby improving the conversion efficiency of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of photovoltaic cells, and in particular to a solar cell and a photovoltaic module. Background Art

[0002] Topcon cells rely on the "tunneling effect" to achieve rear surface passivation. The existing Topcon cell rear surface structure is, from the inside to the outside, a semiconductor substrate, a tunneling oxide layer, a phosphorus-doped polysilicon layer, and a rear surface passivation layer. Since the tunneling oxide layer is made of silicon dioxide, silicon dioxide effectively passivates dangling bonds and defects on the silicon surface, significantly helping and improving the open circuit voltage of the battery, thereby improving the battery conversion efficiency. However, since the thickness of the silicon dioxide layer is too thin, the quality of the film cannot be effectively guaranteed, and there will be many defects and pores in the film layer, which will cause the final battery to short-circuit, and will also greatly reduce the degree of recombination of carriers on the rear surface of the solar cell. If measures are taken to increase the thickness of the silicon dioxide film layer to solve the problem of leakage current, the excessively thick silicon dioxide film layer will seriously hinder the migration of electrons, and the tunneling effect will be reduced, thereby increasing the series resistance of the battery, and the fill factor and current of the battery will be affected and reduced; at the same time, due to the structural characteristics of silicon dioxide itself, during the use of the battery assembly, some ions with smaller ionic radius entering it will destroy the passivation effect, especially the presence of Na ions, which will have a certain impact on the service life of the battery.

[0003] Therefore, it is necessary to study a solar cell that improves the back passivation effect of the cell while also having a strong tunneling effect. Summary of the invention

[0004] In view of this, the present application proposes a solar cell and a photovoltaic module, wherein the solar cell has an excellent back passivation effect and a strong tunneling effect.

[0005] In a first aspect, an embodiment of the present application provides a solar cell, the solar cell comprising:

[0006] An N-type semiconductor substrate having a front surface and a rear surface opposite to each other;

[0007] A boron diffusion layer is provided on the front surface of the N-type semiconductor substrate, a first passivation layer is provided on the surface of the boron diffusion layer, and a first electrode is formed through the first passivation layer to form an electrical connection with the N-type semiconductor substrate;

[0008] A phosphorus-doped polysilicon layer is provided on the rear surface of the N-type semiconductor substrate, a silicon oxide layer containing nitrogen and phosphorus elements is provided between the rear surface of the N-type semiconductor substrate and the phosphorus-doped polysilicon layer, a second passivation layer is provided on the surface of the phosphorus-doped polysilicon layer, and a second electrode electrically connected to the phosphorus-doped polysilicon layer is formed through the second passivation layer.

[0009] In combination with the first aspect, the silicon oxide layer containing nitrogen and phosphorus elements is a single-layer oxide layer structure.

[0010] In combination with the first aspect, the silicon oxide layer is a multi-layer oxide layer structure, and the multi-layer oxide layer structure includes a first oxide sublayer, a second oxide sublayer and a third oxide sublayer, wherein the first oxide sublayer is a nitrogen-doped silicon oxide layer, the second oxide sublayer is made of a silicon dioxide layer, and the third oxide sublayer is a phosphorus-doped silicon oxide layer.

[0011] In combination with the first aspect, at least one of the first oxide sublayer, the second oxide sublayer and the third oxide sublayer contains Al element and / or Ta element.

[0012] In combination with the first aspect, the total thickness of the silicon oxide layer is less than or equal to

[0013] In combination with the first aspect, the doping concentration of the phosphorus-doped polysilicon layer is 1×10 19 cm -3 ~1×10 21 cm -3 .

[0014] In combination with the first aspect, the first passivation layer includes at least one of silicon nitride, silicon oxynitride and aluminum oxide.

[0015] In combination with the first aspect, the second passivation layer includes at least one of silicon nitride, silicon oxynitride and aluminum oxide.

[0016] In combination with the first aspect, the first electrode is a silver electrode or a silver / aluminum electrode, and / or the second electrode is a silver electrode.

[0017] In a second aspect, the present application provides a photovoltaic assembly, wherein the photovoltaic assembly comprises a plurality of solar cell strings, wherein the solar cell strings comprise the solar cells described in the first aspect.

[0018] The technical solution of the present application has at least the following beneficial effects:

[0019] (1) The present application changes the composition of the battery contact interface by setting a silicon oxide layer containing nitrogen and phosphorus elements between the rear surface of the N-type semiconductor substrate and the phosphorus-doped polysilicon layer, thereby improving the tunneling ability of the battery rear surface and the passivation effect of the battery rear surface, thereby improving the conversion efficiency of the battery.

[0020] (2) The silicon oxide layer containing nitrogen and phosphorus in the present application includes a nitrogen-doped silicon oxide layer, a silicon dioxide layer and a phosphorus-doped silicon oxide layer. The doping of N element in the nitrogen-doped silicon oxide layer can increase the dielectric constant of the silicon oxide layer interface, improve the passivation effect and increase the open circuit voltage. However, the doping of N element will increase the internal resistance of the battery and reduce the filling factor. At this time, by doping P element in the phosphorus-doped silicon oxide layer, a donor impurity energy level is generated near the conduction band position in the silicon dioxide band gap, which can increase the tunneling current of the electron, reduce the internal resistance of the battery and improve the battery filling factor. The silicon oxide layer containing nitrogen and phosphorus obtained by doping the above two elements in the present application can simultaneously achieve the improvement of open circuit voltage and filling factor, thereby improving the conversion efficiency of solar cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present application or the technical solutions of the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0022] Figure 1 Schematic diagram of the structure of the solar cell for this application Figure 1 ;

[0023] Figure 2 Schematic diagram of the structure of the solar cell for this application Figure 2 ;

[0024] Figure 3 Preparation process of solar cells for this application Figure 1 ;

[0025] Figure 4 Preparation process of solar cells for this application Figure 2 .

[0026] In the figure:

[0027] 10-N type semiconductor substrate;

[0028] 20-boron diffusion layer;

[0029] 30- first passivation layer;

[0030] 40- a first electrode;

[0031] 50-a silicon oxide layer containing nitrogen and phosphorus elements;

[0032] 501- first oxide sublayer;

[0033] 502- second oxide sublayer;

[0034] 503- third oxide sublayer;

[0035] 60-phosphorus-doped polysilicon layer;

[0036] 70- second passivation layer;

[0037] 80 - second electrode. DETAILED DESCRIPTION

[0038] In order to better understand the technical solution of the present application, the embodiments of the present application are described in detail below with reference to the accompanying drawings.

[0039] It should be clear that the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.

[0040] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0041] It should be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0042] Topcon batteries rely on the "tunneling effect" to passivate the rear surface of the battery. The existing rear surface structure of Topcon batteries is, from the inside to the outside, an N-type semiconductor substrate, a tunneling oxide layer, a phosphorus-doped polysilicon layer, and a rear surface passivation layer. The presence of the tunneling oxide layer and the doped polysilicon thin layer together form a passivation contact structure, which can effectively reduce surface recombination and metal contact recombination, and form an ohmic contact with the metal electrode, leaving much room for improvement in conversion efficiency. However, since the thickness of the silicon dioxide layer is generally thin, there will be many defects and pores in the film layer, resulting in a short circuit in the final prepared battery. If measures are taken to increase the thickness of the silicon dioxide film layer to solve the short circuit problem, an excessively thick silicon dioxide film layer will seriously hinder the migration of electrons, and the tunneling effect will be reduced, increasing the series resistance of the battery, and the fill factor and current of the battery will be affected and reduced.

[0043] Therefore, in order to overcome the imperfections of the prior art, the present invention provides a solar cell, in which a silicon oxide layer containing nitrogen and phosphorus elements is arranged between the N-type semiconductor substrate and the phosphorus-doped polysilicon layer on the rear surface of the cell, so as to improve the tunneling ability of the rear surface of the cell and the passivation effect of the rear surface of the cell, thereby improving the conversion efficiency of the cell.

[0044] First, Figure 1 A schematic diagram of the structure of a solar cell provided in an embodiment of the present application is shown in FIG. Figure 1 As shown, the solar cell includes an N-type semiconductor substrate 10, and the N-type semiconductor substrate 10 has a front surface and a rear surface opposite to each other;

[0045] A boron diffusion layer 20 is provided on the front surface of the N-type semiconductor substrate 10, a first passivation layer 30 is provided on the surface of the boron diffusion layer 20, and a first electrode 40 is formed through the first passivation layer 30 and electrically connected to the N-type semiconductor substrate 10;

[0046] A phosphorus-doped polysilicon layer 60 is provided on the rear surface of the N-type semiconductor substrate 10, a silicon oxide layer 50 containing nitrogen and phosphorus elements is provided between the rear surface of the N-type semiconductor substrate 10 and the phosphorus-doped polysilicon layer 60, a second passivation layer 70 is provided on the surface of the phosphorus-doped polysilicon layer 60, and a second electrode 80 is formed by passing through the second passivation layer 70 and electrically connected to the phosphorus-doped polysilicon layer 60.

[0047] In the above scheme, a silicon oxide layer 50 containing nitrogen and phosphorus elements is provided between the rear surface of the N-type semiconductor substrate 10 and the phosphorus-doped polysilicon layer 60. By doping with the N element, the dielectric constant of the silicon oxide layer interface can be increased, the passivation effect can be improved, and the open circuit voltage can be increased. However, the doping with the N element will cause the internal resistance of the battery to increase and the fill factor to decrease. At this time, by doping with the P element, a donor impurity energy level is generated in the silicon dioxide band gap near the conduction band position, which can increase the tunneling current of the electrons, that is, reduce the internal resistance of the battery and increase the fill factor. The present application can simultaneously achieve the improvement of the open circuit voltage and the fill factor by doping with the above two elements, thereby improving the conversion efficiency of the solar cell.

[0048] In one embodiment, the silicon oxide layer 50 containing nitrogen and phosphorus elements is a single silicon oxide layer structure containing both nitrogen and phosphorus elements.

[0049] In some embodiments, the silicon oxide layer 50 containing nitrogen and phosphorus elements is a multi-layer structure, such as Figure 2As shown, the silicon oxide layer includes a first oxide sublayer 501, a second oxide sublayer 502 and a third oxide sublayer 503 in the direction from the N-type semiconductor substrate to the phosphorus-doped polysilicon layer 60. The first oxide sublayer 501 is a nitrogen-doped silicon oxide layer, the second oxide sublayer 502 is a silicon dioxide layer, and the third oxide sublayer 503 is a phosphorus-doped silicon oxide layer. It can be understood that the silicon oxide layer 50 containing nitrogen and phosphorus elements can be designed as a multilayer structure in the present application, which can simultaneously increase the passivation effect and the tunneling ability of the rear surface of the battery, thereby improving the conversion efficiency of the solar cell.

[0050] In some embodiments, in the actually prepared product, since the silicon oxide layer 50 containing nitrogen and phosphorus elements is very thin, the first oxide sublayer 501, the second oxide sublayer 502 and the third oxide sublayer 503 are mixed into an integrated structure. It can be understood that the silicon oxide layer 50 containing nitrogen and phosphorus elements is characterized, and the silicon oxide layer includes nitrogen and phosphorus elements.

[0051] In some embodiments, the material of the nitrogen-doped silicon oxide layer includes SiO x N y , where y / (x+y) < 15%. It can be understood that as the N content continues to increase, the interface changes from Si-SiO x Bonding to Si-SiN x Transformation, SiN x The mismatch between the lattice constant and the thermal expansion coefficient and Si is large, which will lead to the formation of a large number of defects, becoming traps and recombination centers for carriers, affecting the mobility of carriers, and SiN x The internal stress of the film is very large, and the film layer may break, resulting in complete failure of the passivation layer. Therefore, the content of the N element cannot be too much. In this application, the N-doped ratio in the nitrogen-doped silicon oxide layer should be controlled within 15%; the nitrogen doping concentration in the nitrogen-doped silicon oxide layer gradually decreases from the N-type semiconductor substrate 10 to the phosphorus-doped polysilicon layer 60. It can be understood that the above-mentioned doping concentration gradient is determined by the doping process.

[0052] In some embodiments, the thickness of the first oxide sublayer 501 is Specifically, the thickness of the first oxide sublayer 501 may be and The first oxide sub-layer 501 of the present application is very thin, which can increase the dielectric constant of the silicon oxide layer interface and improve the passivation effect without affecting the migration of carriers.

[0053] In some embodiments, the material of the second oxide sub-layer 502 is silicon dioxide, which serves as an insulating layer. The silicon dioxide layer is conducive to the tunneling of majority electrons into the polysilicon layer while blocking the recombination of minority holes. Then, electrons are laterally transmitted in the polysilicon layer and collected by metal, thereby greatly reducing the metal contact recombination current and improving the open circuit voltage and short circuit current of the battery.

[0054] In some embodiments, the thickness of the second oxide sublayer 502 is The specific thickness can be and The thickness of the second oxide sublayer 502 is controlled within the above range, which is beneficial to the transmission of the majority carriers and significantly reduces the recombination of the interface. When the thickness of the second oxide layer is greater than When , the carriers cannot pass through effectively.

[0055] In some embodiments, the pinhole density of the second oxide sub-layer 502 is 10 -6 ~10 -3 , the specific pinhole density can be 10 -6 , 10 -5 , 10 -4 and 10 -3 It can be understood that carriers can be transported through pinholes. Pinholes serve as a shunt path for carrier transport. When carriers are transported through pinholes, the series resistance can be reduced, the fill factor can be increased, and the conversion efficiency of solar cells can be improved. If the number of pinholes is greater than 10 -3 , it will reduce the barrier height of the junction, lower the open circuit voltage, thereby reducing the passivation performance and increasing the surface recombination, thereby reducing the battery performance.

[0056] In some embodiments, the third oxide sublayer 503 is a phosphorus-doped silicon oxide layer. In the present application, the silicon oxide is doped with P elements to form a donor energy level near the conduction band of the silicon oxide. The presence of this impurity energy level and the heavily doped polysilicon layer on the surface can improve the tunneling ability of electrons, reduce the obstacles to electron migration, and improve the fill factor. At the same time, the phosphorus-silicate glass (BSG) formed by P doping on the surface is resistant to some metal ions, especially Na + It has a strong barrier effect, reducing the impact of metal ions on battery components during use.

[0057] In some embodiments, the phosphorus doping concentration in the phosphorus-doped silicon oxide layer is 1×10 10 cm -3 ~1×10 18 cm -3 , the specific doping concentration can be 1×10 10cm -3 , 1×10 11 cm -3 , 1×10 12 cm -3 , 1×10 13 cm -3 , 1×10 14 cm -3 , 1×10 15 cm -3 , 1×10 16 cm -3 , 1×10 17 cm -3 and 1×10 18 cm -3 The phosphorus doping concentration in the phosphorus-doped silicon oxide layer is higher than 1×10 18 cm -3 Too much P element will cause impurity defects, becoming a trap and recombination center for carriers. At the same time, during the use of battery components, too much P element will cause the transmittance of the passivation layer to decrease, affecting the battery efficiency. The phosphorus doping concentration in the phosphorus-doped silicon oxide layer is less than 1×10 10 cm -3 , the improvement of electron tunneling ability is insufficient and cannot meet the requirements.

[0058] In some embodiments, the doping concentration of phosphorus in the phosphorus-doped silicon oxide layer gradually increases from the N-type semiconductor substrate 10 to the phosphorus-doped polysilicon layer.

[0059] In some embodiments, the thickness of the third oxide sublayer 503 is Specifically, the thickness of the third oxide sublayer 503 may be and wait.

[0060] The sum of the thicknesses of the first oxide sublayer 501, the second oxide sublayer 502 and the third oxide sublayer 503 is less than or equal to The specific thickness can be and It is understandable that if the thickness is too thick, it will seriously hinder the migration of electrons. Therefore, the present application controls the total thickness of the first oxide sublayer 501, the second oxide sublayer 502 and the third oxide sublayer 503 to be within Within.

[0061] It is understandable that the first oxide sublayer, the second oxide sublayer and the third oxide sublayer may also be doped with at least one of Al (aluminum) and Ta (tantalum) that provide holes, thereby improving the passivation effect.

[0062] The present application also provides a method for preparing a solar cell. Figure 3 The process of a solar cell manufacturing method provided in this embodiment is shown as follows Figure 1 , including the following steps:

[0063] Step S10, performing boron diffusion on the front surface of the textured N-type semiconductor substrate 10 to form a boron diffusion layer 20;

[0064] Step S20, oxidizing the rear surface of the N-type semiconductor substrate 10 to form a silicon oxide layer 50 containing nitrogen and phosphorus elements;

[0065] Step S30, depositing a polysilicon layer on the surface of the silicon oxide layer 50 containing nitrogen and phosphorus elements, and performing secondary phosphorus diffusion on the polysilicon layer to form a phosphorus-doped polysilicon layer 60;

[0066] Step S40, forming a second passivation layer 70 on the surface of the phosphorus-doped polysilicon layer 60;

[0067] Step S50 , forming a first passivation layer 30 on the surface of the boron diffusion layer 20 , forming a first electrode 40 on the first passivation layer 30 , and forming a second electrode on the second passivation layer 70 .

[0068] In the above technical solution, a silicon oxide layer 50 containing nitrogen and phosphorus elements is provided between the rear surface of the N-type semiconductor substrate 10 and the phosphorus-doped polysilicon layer 60. By doping with the N element, the dielectric constant of the silicon oxide layer interface can be increased, the passivation effect can be improved, and the open circuit voltage can be increased. However, the doping with the N element will cause the internal resistance of the battery to increase and the filling factor to decrease. At this time, by doping with the P element, a donor impurity energy level is generated in the silicon dioxide band gap near the conduction band position, thereby increasing the tunneling current of the electrons, that is, reducing the internal resistance of the battery and increasing the filling factor. The present application can simultaneously achieve the improvement of the open circuit voltage and the filling factor by doping with the above two elements, thereby improving the conversion efficiency of the solar cell.

[0069] Specifically, the method for manufacturing a solar cell provided in the embodiment of the present application can be used to manufacture an N-type solar cell, and can further be used to manufacture an N-type Topcon cell. Below, the method for manufacturing the N-type Topcon cell of the present application will be clearly and completely described in conjunction with the drawings in the embodiments of the present application. The described embodiments are only part of the embodiments of the present application, not all of the embodiments.

[0070] Figure 4 A process of preparing a solar cell provided in this embodiment Figure 2 ,like Figure 4 As shown, Example 1 of the present application provides a method for preparing a solar cell, comprising the following steps:

[0071] Step S10 , performing boron diffusion on the front surface of the textured N-type semiconductor substrate 10 to form a boron diffusion layer 20 .

[0072] Specifically, before the boron diffusion, the front and rear surfaces of the N-type semiconductor substrate 10 can be subjected to a texturing treatment to form a velvet surface or surface texture structure (e.g., a pyramid structure). The texturing treatment can be carried out by chemical etching, laser etching, mechanical method, plasma etching, etc., which are not limited here. Exemplarily, the front and rear surfaces of the N-type semiconductor substrate can be subjected to a texturing treatment using a NaOH solution. Since the corrosion of the NaOH solution is anisotropic, a pyramid velvet surface structure can be prepared.

[0073] It can be understood that the surface of the N-type semiconductor substrate 10 has a velvet structure through the texturing process, which produces a light trapping effect, increases the amount of light absorbed by the solar cell, and thus improves the conversion efficiency of the solar cell.

[0074] In some embodiments, the front surface of the N-type semiconductor substrate 10 is the surface facing the sun, and the rear surface is the surface facing away from the sun. It should also be noted that the semiconductor substrate can be a crystalline silicon substrate (silicon substrate), such as a polycrystalline silicon substrate, a single crystal silicon substrate, or a quasi-single crystal silicon substrate. The embodiment of the present invention does not limit the specific type of the semiconductor substrate.

[0075] In step S10 , a boron diffusion layer 20 may be formed on the front surface of the N-type semiconductor substrate 10 by using any one or more methods of high temperature diffusion, slurry doping or ion implantation.

[0076] In a specific embodiment, boron atoms are diffused through a boron source to form a boron diffusion layer 20. The boron source can be, for example, boron tribromide for diffusion treatment, so that the microcrystalline silicon phase of the crystalline silicon is transformed into a polycrystalline silicon phase. Since the surface of the N-type semiconductor substrate 10 has a high concentration of boron, a borosilicate glass layer (BSG) is usually formed. This borosilicate glass layer has a metal gettering effect, which will affect the normal operation of the solar cell and needs to be removed later.

[0077] Optionally, before the texturing process, a step of cleaning the N-type semiconductor substrate 10 may be included to remove metal and organic pollutants on the surface.

[0078] Step S20 , oxidizing the rear surface of the N-type semiconductor substrate 10 to form a silicon oxide layer 50 containing nitrogen and phosphorus elements.

[0079] In some embodiments, the silicon oxide layer containing nitrogen and phosphorus The specific thickness can be and It is understandable that if the thickness of the silicon oxide layer 50 containing nitrogen and phosphorus is too thick, it will seriously hinder the migration of electrons. Therefore, the thickness of the silicon oxide layer is controlled within Within.

[0080] It should be noted that the embodiment of the present invention does not limit the specific operation method of forming oxidation. Specifically, the N-type semiconductor substrate 10 can be oxidized after the rear surface is etched by ozone oxidation, high temperature thermal oxidation, or nitric acid oxidation. For example, the rear surface of the N-type semiconductor substrate 10 can be oxidized by thermal oxidation.

[0081] It can be understood that compared with the existing thin oxide layer or tunneling oxide layer, the present application maintains the ability of silicon oxide to increase electron tunneling without increasing the thickness, while also improving the degree of recombination of carriers on the rear surface of the battery.

[0082] Step S21 : oxidizing the back surface of the N-type semiconductor substrate 10 . During the oxidation process, the oxidized product is subjected to a phosphorus diffusion process to form a third oxide sublayer 503 .

[0083] The specific steps are: use a phosphorus source as a doping source, pass O2 at a flow rate of 10L / min to 12L / min, the ventilation time is 3min to 5min, and after stopping the ventilation, the oxidation product is subjected to a phosphorus diffusion, the temperature of the phosphorus diffusion is 780℃ to 820℃, and the time of the phosphorus diffusion is 50s to 60s.

[0084] In the above steps, the in-situ doping method is used to simultaneously perform oxidation and phosphorus diffusion operations, and the oxidation adopts any one of the ozone oxidation method, high-temperature thermal oxidation method, and nitric acid oxidation method; the phosphorus diffusion treatment refers to the formation of a doping layer by diffusing pentavalent phosphorus atoms under high temperature conditions (generally >600°C).

[0085] In some embodiments, during the phosphorus diffusion process, the phosphorus source is POCl3 or PH3, preferably POCl3, POCl3 is liquid and very volatile, and in the doping process, the phosphorus source can be introduced by introducing oxygen, and oxidation and doping are performed simultaneously, and the introduction of oxygen causes the pentavalent phosphorus source to generate phosphorus pentoxide, which reacts with silicon to generate phosphorus atoms, and the addition of oxygen avoids the corrosion of the phosphide on the surface of the semiconductor substrate. The POCl3 liquid source diffusion method has the advantages of high production efficiency and good diffusion layer surface.

[0086] In some embodiments, the O2 input flow rate is 10L / min to 12L / min, and the specific flow rate can be 10L / min, 11L / min and 12L / min, etc. It can be understood that when the O2 input flow rate is higher than 12L / min, the grown oxide layer is too thick, resulting in obstruction of electron migration; when the O2 input flow rate is lower than 10L / min, the grown oxide layer is too thin, and the quality of the film cannot be effectively guaranteed.

[0087] In some embodiments, the ventilation time is 3 min to 5 min, and the specific ventilation time can be 3 min, 4 min, 5 min, etc.

[0088] The temperature of the primary phosphorus diffusion is 780°C to 820°C, and the specific temperature of the primary phosphorus diffusion can be 780°C, 790°C, 800°C, 810°C and 820°C, etc. The time of the primary phosphorus diffusion is 50s to 60s, and the specific time of the primary phosphorus diffusion can be 50s, 51s, 52s, 53s, 54s, 55s, 56s, 57s, 58s, 59s and 60s, etc. If the primary phosphorus diffusion temperature is lower than 780°C, the time is increased and the yield is reduced, and the diffusion uniformity and repeatability become worse; if the primary phosphorus diffusion temperature is higher than 820°C, the time is shortened, and the diffusion uniformity and repeatability cannot be guaranteed.

[0089] In some embodiments, the thickness of the third oxide sublayer 503 is Specifically, the thickness of the third oxide sublayer 503 may be and wait.

[0090] Step S22 , after obtaining the third oxide sublayer 503 in step S21 , further oxidation is performed to form a second oxide sublayer 502 , wherein the second oxide sublayer 502 is located between the third oxide sublayer 503 and the N-type semiconductor substrate 10 .

[0091] The specific steps are: introduce O2 at a flow rate of 8L / min~10L / min, ventilate for 3min~5min, then stop ventilation and carry out oxidation, the oxidation temperature is 500℃~530℃, and the oxidation time is 350s~450s.

[0092] In some embodiments, the O2 input flow rate is 8 L / min to 10 L / min, and the specific flow rate can be 8 L / min, 9 L / min and 10 L / min, etc. It can be understood that when the O2 input flow rate is higher than 10 L / min, the grown oxide layer is too thick, resulting in obstruction of electron migration; when the O2 input flow rate is lower than 10 L / min, the grown oxide layer is too thin, and the quality of the film cannot be effectively guaranteed.

[0093] In some embodiments, the ventilation time is 3 minutes to 5 minutes, and the specific ventilation time can be 3 minutes, 4 minutes, 5 minutes, etc.

[0094] The oxidation temperature is 500°C to 530°C, and the specific oxidation temperature can be 500°C, 510°C, 520°C and 530°C, etc. The oxidation time is 350s to 450s, and the specific oxidation time can be 350s, 350s, 370s, 380s, 390s, 400s, 410s, 420s, 430s, 440s and 450s, etc. By controlling the oxidation time and oxidation temperature within the above range, a thickness of The silicon oxide layer is beneficial to improving the tunneling ability of carriers.

[0095] Step S23 , after obtaining the second oxide sublayer 502 of step S22 , further oxidation is performed, and during the oxidation process, nitrogen is diffused from the oxide to form a first oxide sublayer 501 , and the first oxide sublayer 501 is located between the second oxide sublayer 502 and the N-type semiconductor substrate 10 .

[0096] The specific steps are: using a mixed gas of O2 and N2O with a volume ratio of (2 to 4):1 as a doping source, the flow rate of the mixed gas is 8L / min to 10L / min, the ventilation time is 3min to 5min, and after stopping the ventilation, the oxidation result is nitrogen diffused, the nitrogen diffusion temperature is 500°C to 530°C, and the nitrogen diffusion time is 40s to 60s.

[0097] In some embodiments, the volume ratio of O2 and N2O is (2-4):1, and the specific volume ratio can be 2:1, 3:1 and 4:1, etc. By using the mixed gas of O2 and N2O as a doping source, oxidation and nitrogen doping are performed simultaneously, and the flow rate of the above-mentioned mixed gas is 8L / min-10L / min, and the specific flow rate can be 8L / min, 9L / min and 10L / min, etc. The mixed gas flow rate is controlled within the above range, the proportion of the doped nitrogen element is controlled, and the passivation effect is improved.

[0098] In some embodiments, the ventilation time is 3 minutes to 5 minutes, and the specific ventilation time can be 3 minutes, 4 minutes, 5 minutes, etc.

[0099] The oxidation temperature is 500°C to 530°C, and the specific oxidation temperature can be 500°C, 510°C, 520°C and 530°C, etc. The oxidation time is 350s to 450s, and the specific oxidation time can be 350s, 350s, 370s, 380s, 390s, 400s, 410s, 420s, 430s, 440s and 450s, etc. Controlling the oxidation time and oxidation temperature within the above range is beneficial to the diffusion of doping elements, thereby increasing the dielectric constant of the silicon oxide layer interface and improving the passivation effect.

[0100] In step S20, the nitrogen- and phosphorus-containing silicon oxide layer structure of the first oxide sublayer 501 / second oxide sublayer 502 / third oxide sublayer 503 prepared in the present application is very thin, and only the surface of the single crystal silicon needs to be oxidized, without the need for additional deposited silicon, and the entire reaction process is from top to bottom, that is, first reacting to generate the P-doped third oxide sublayer, then reacting to generate the undoped second oxide sublayer, and finally reacting to generate the N-doped first oxide sublayer.

[0101] Step S30 , depositing a polysilicon layer on the surface of the silicon oxide layer 50 containing nitrogen and phosphorus elements, and performing secondary phosphorus diffusion on the polysilicon layer to form a phosphorus-doped polysilicon layer 60 .

[0102] In the above steps, a phosphorus-doped polysilicon layer 60 is deposited on the surface of the silicon oxide layer 50 containing nitrogen and phosphorus elements to protect the silicon oxide layer 50. Next, the polysilicon is doped to form a high-low junction (n / n + -Si), which can effectively reduce the recombination rate of carriers on the back of the battery and further improve the conversion efficiency of solar cells.

[0103] In some embodiments, a polysilicon layer may be deposited on the surface of the third oxide sublayer 503 by using any one of low pressure chemical vapor deposition, plasma enhanced chemical vapor deposition, and atmospheric pressure chemical vapor deposition.

[0104] In some embodiments, a two-step heat treatment method may be used for the secondary phosphorus diffusion, that is, the phosphorus source is first decomposed at about 1000°C and deposited on the surface of the N-type semiconductor substrate 10, and then heat treated in the range of 800°C to 900°C, so that the phosphorus atoms on the surface diffuse into the polysilicon layer to form a phosphorus-doped polysilicon layer 60. Of course, a one-step deposition method may also be used, that is, a polysilicon layer is deposited on the surface of the third oxide sublayer 503 and an in-situ doping treatment is performed at the same time to form the phosphorus-doped polysilicon layer 60. The phosphorus diffusion process may also use any one or more methods of high-temperature diffusion, slurry doping or ion implantation, which are not limited here.

[0105] In some embodiments, the doping concentration of the phosphorus-doped polysilicon layer is 1×10 19 cm -3~1×10 21 cm -3 The doping concentration can be specifically 1×10 19 cm -3 , 1×10 20 cm -3 , 1×10 21 cm -3 Etc., controlling the doping concentration within the above range is beneficial to improving the passivation performance.

[0106] In some embodiments, the phosphosilicate glass layer formed on the back side of the cell during the phosphorus diffusion process and the borosilicate glass layer formed on the front side of the cell during the boron diffusion process are removed.

[0107] Step S40: forming a second passivation layer 70 on the surface of the phosphorus-doped polysilicon layer.

[0108] In some embodiments, a second passivation layer 70 is formed on the surface of the phosphorus-doped polysilicon layer. The second passivation layer 70 may include but is not limited to a single layer of silicon nitride, silicon oxynitride, aluminum oxide, etc., or an oxide layer structure containing nitrogen and phosphorus.

[0109] For example, the second passivation layer 70 is composed of silicon nitride. The silicon nitride thin film layer can play the role of an anti-reflection film, and the silicon nitride thin film has good insulation, density, stability and masking ability for impurity ions. The silicon nitride thin film layer can have a passivation effect on the semiconductor substrate, significantly improving the photoelectric conversion efficiency of the solar cell.

[0110] Step S50 , forming a first passivation layer 30 on the surface of the boron diffusion layer 20 , forming a first electrode 40 on the first passivation layer 30 , and forming a second electrode 80 on the second passivation layer 70 .

[0111] In some embodiments, the first passivation layer 30 may include but is not limited to a single layer of silicon nitride, silicon oxynitride, aluminum oxide, or an oxide layer structure containing nitrogen and phosphorus. Of course, the first passivation layer 30 may also be other types of passivation layers, and the present invention does not limit the specific material of the first passivation layer 30. For example, in other embodiments, the first passivation layer 30 may also be a silicon oxide layer containing nitrogen and phosphorus of silicon dioxide and silicon nitride. The above-mentioned first passivation layer 30 can produce a good passivation effect on the semiconductor substrate, which helps to improve the conversion efficiency of the battery. In some embodiments, aluminum-doped silver paste is used to print the front main grid and the front sub-grid on the front surface of the semiconductor substrate, and dried to form the first electrode 40. In some embodiments, silver paste can be used to print the rear surface main grid and the rear surface sub-grid on the rear surface of the semiconductor substrate, and dried to form the second electrode 80. Finally, the dried battery cell is sintered to obtain a solar cell.

[0112] It should be noted that the first electrode 40 passes through the first passivation layer 30 to form an ohmic contact with the boron diffusion layer 20; the second electrode 80 passes through the second passivation layer 70 to form an ohmic contact with the phosphorus-doped polysilicon layer 60, and the phosphorus-doped polysilicon layer 60 and the silicon oxide layer containing N and P (the first oxide sublayer 501, the second oxide sublayer 502 and the third oxide sublayer 503) form a TopCon battery structure.

[0113] The embodiment of the present invention does not limit the specific materials of the first electrode 40 and the second electrode 80. For example, the first electrode 40 is a silver electrode or a silver / aluminum electrode, and the second electrode 80 is a silver electrode.

[0114] The specific types of the first passivation layer 30 and the second passivation layer 70 are not limited in the embodiment of the present invention, and may be, for example, a silicon nitride layer, a silicon oxynitride layer, an aluminum oxide / silicon nitride silicon oxide layer structure containing nitrogen and phosphorus, and the like.

[0115] In a second aspect, the present application provides a photovoltaic module, comprising a first substrate, a first packaging layer, a battery string structure, a second packaging layer and a second substrate stacked in sequence to form a stacked structure, and the stacked structure is laminated. During the lamination process, a photovoltaic module is obtained by electrically connecting wires and battery cells.

[0116] In some embodiments, the photovoltaic module includes a plurality of solar cell strings, each solar cell string includes a plurality of solar cells connected by conductive ribbons, and the solar cell may be the solar cell described above or a solar cell manufactured by the preparation method described above.

[0117] In some embodiments, a plurality of solar cells are located on the same plane and are electrically connected with a certain gap (small gap) or without a gap.

[0118] The following is a further description of the embodiments of the present application in multiple embodiments. The embodiments of the present application are not limited to the following specific embodiments. Within the scope of the unchanged main rights, appropriate changes can be made to the implementation.

[0119] Example 1

[0120] Step S10 , performing boron diffusion on the front surface of the textured N-type semiconductor substrate 10 to form a boron diffusion layer 20 .

[0121] Step S20, depositing a silicon oxide layer on the surface of the single crystal silicon by plasma enhanced chemical vapor deposition:

[0122] Step S21, turn on the POCl3 source. The substance is in liquid state and needs to be brought out by O2. The O2 flow rate is 12L / min. After ventilation for 5 minutes, stop ventilation and maintain the temperature at 800°C for 60 seconds to react to form a phosphorus-doped silicon oxide layer.

[0123] Step S22, close the POCl3 source, maintain the flow rate of O2 at 10 L / min, ventilate for 5 minutes, stop ventilating, maintain the temperature at 500°C and react for 450 seconds to form a silicon oxide layer;

[0124] Step S23, using a doping source as a mixed gas of O2 and N2O, the mixed volume ratio is O2:N2O=3:1, the gas flow rate is 10L / min, after ventilation for 5 minutes, stop ventilation, maintain the temperature between 500°C and react for 60 seconds to form a nitrogen-doped silicon oxide layer.

[0125] Step S30: depositing a polysilicon layer on the surface of the phosphorus-doped silicon oxide layer by plasma enhanced chemical vapor deposition, and performing secondary phosphorus diffusion on the polysilicon layer to form a phosphorus-doped polysilicon layer.

[0126] Step S40: forming a second passivation layer on the surface of the phosphorus-doped polysilicon layer, and forming a second electrode on the second passivation layer.

[0127] Example 2

[0128] Step S10 , performing boron diffusion on the front surface of the textured N-type semiconductor substrate 10 to form a boron diffusion layer 20 .

[0129] Step S20, depositing a silicon oxide layer on the surface of the single crystal silicon by plasma enhanced chemical vapor deposition:

[0130] Step S21, turn on the POCl3 source. The substance is in liquid state and needs to be brought out by O2. The O2 flow rate is 10L / min. After ventilation for 4 minutes, stop ventilation and maintain the temperature between 780°C for 55 seconds to react to form a phosphorus-doped silicon oxide layer.

[0131] Step S22, close the POCl3 source, maintain the flow rate of O2 at 9 L / min, ventilate for 5 min, stop ventilating, maintain the temperature between 510°C and react for 450 s to form a silicon oxide layer;

[0132] Step S23, using a doping source as a mixed gas of O2 and N2O, the mixed volume ratio is O2:N2O=4:1, the gas flow rate is 10L / min, after ventilation for 5 minutes, stop ventilation, maintain the temperature between 530°C and react for 60 seconds to form a nitrogen-doped silicon oxide layer.

[0133] Step S30: depositing a polysilicon layer on the surface of the phosphorus-doped silicon oxide layer by plasma enhanced chemical vapor deposition, and performing secondary phosphorus diffusion on the polysilicon layer to form a phosphorus-doped polysilicon layer.

[0134] Step S40: forming a second passivation layer on the surface of the phosphorus-doped polysilicon layer, and forming a second electrode on the second passivation layer.

[0135] Example 3

[0136] Step S10 , performing boron diffusion on the front surface of the textured N-type semiconductor substrate 10 to form a boron diffusion layer 20 .

[0137] Step S20: Depositing a silicon oxide layer on the surface of the single crystal silicon by plasma enhanced chemical vapor deposition:

[0138] Step S21, turn on the POCl3 source. The substance is in liquid state and needs to be brought out by O2. The O2 flow rate is 10L / min. After ventilation for 5 minutes, stop ventilation and maintain the temperature between 820°C for 60 seconds to react to form a phosphorus-doped silicon oxide layer.

[0139] Step S22, close the POCl3 source, maintain the flow rate of O2 at 8 L / min, ventilate for 5 min, stop ventilating, maintain the temperature at 530°C and react for 450 s to form a silicon oxide layer;

[0140] Step S23, using a doping source as a mixed gas of O2 and N2O, the mixed volume ratio is O2:N2O=2:1, the gas flow rate is 9L / min, after ventilation for 5 minutes, stop ventilation, maintain the temperature between 510°C and react for 60 seconds to form a nitrogen-doped silicon oxide layer.

[0141] Step S30: depositing a polysilicon layer on the surface of the phosphorus-doped silicon oxide layer by plasma enhanced chemical vapor deposition, and performing secondary phosphorus diffusion on the polysilicon layer to form a phosphorus-doped polysilicon layer.

[0142] Step S40: forming a second passivation layer on the surface of the phosphorus-doped polysilicon layer, and forming a second electrode on the second passivation layer.

[0143] Comparative Example 1

[0144] Different from the embodiment 1, step 2 specifically comprises: using the LPCVD method to generate a thickness of The specific parameters are as follows: the flow rate of O2 is 15L / min, after ventilation for 5 minutes, ventilation is stopped, and the temperature is maintained at 500℃ for 550s to react to form a silicon oxide layer.

[0145] The performance tests of the above-mentioned Examples 1 to 3 and Comparative Example 1 are shown in Table 1 below.

[0146] Table 1. Comparison of performance parameters between Example 1 and Comparative Example 1

[0147]

[0148] It can be seen from Table 1 above that in Examples 1 to 3 of the present application, a nitrogen- and phosphorus-containing silicon oxide layer 50 structure including a nitrogen-doped silicon oxide layer 501, a silicon dioxide layer 502 and a phosphorus-doped silicon oxide layer 503 is disposed between the rear surface 10 of the N-type semiconductor substrate and the phosphorus-doped polysilicon layer 60 at one time, and the open circuit voltage and fill factor of the battery are significantly improved by doping with N elements and P elements, thereby improving the conversion efficiency of the solar cell. The conversion efficiency of the solar cell prepared in the examples of the present application is increased by a maximum of 0.31% compared with that in Comparative Example 1. It can be seen that the solar cell prepared in the present application is of great significance for the utilization of solar energy and the development of solar cells.

[0149] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

[0150] Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the claims. Any technical personnel in this field may make several possible changes and modifications without departing from the concept of the present application. Therefore, the scope of protection of the present application shall be based on the scope defined by the claims of the present application.

Claims

1. A solar cell, characterized in that: The solar cell comprises: An N-type semiconductor substrate having a front surface and a rear surface opposite to each other; A boron diffusion layer is provided on the front surface of the N-type semiconductor substrate, a first passivation layer is provided on the surface of the boron diffusion layer, and a first electrode is formed through the first passivation layer and is electrically connected to the N-type semiconductor substrate; A phosphorus-doped polysilicon layer is provided on the rear surface of the N-type semiconductor substrate, and a silicon oxide layer containing nitrogen and phosphorus elements is provided between the rear surface of the N-type semiconductor substrate and the phosphorus-doped polysilicon layer. The silicon oxide layer is a multi-layer oxide layer structure, and the multi-layer oxide layer structure includes a first oxide sublayer, a second oxide sublayer and a third oxide sublayer, wherein the first oxide sublayer is a nitrogen-doped silicon oxide layer, the second oxide sublayer is made of a silicon dioxide layer, the third oxide sublayer is a phosphorus-doped silicon oxide layer, and a second passivation layer is provided on the surface of the phosphorus-doped polysilicon layer, and a second electrode electrically connected to the phosphorus-doped polysilicon layer is formed through the second passivation layer.

2. The solar cell according to claim 1, characterized in that: The first oxide sublayer, the second oxide sublayer and the third oxide sublayer are sequentially arranged along a direction from the N-type semiconductor substrate to the phosphorus-doped polysilicon layer.

3. The solar cell according to claim 1, characterized in that At least one of the first oxide sublayer, the second oxide sublayer and the third oxide sublayer contains Al element and / or Ta element.

4. The solar cell according to any one of claims 1 to 3, characterized in that: The total thickness of the silicon oxide layer is less than or equal to 5. The solar cell according to any one of claims 1 to 4, characterized in that: The doping concentration of the phosphorus-doped polysilicon layer is 1×10 19 cm -3 ~1×10 21 cm -3 .

6. The solar cell according to any one of claims 1 to 5, characterized in that: The first passivation layer includes at least one of silicon nitride, silicon oxynitride and aluminum oxide.

7. The solar cell according to any one of claims 1 to 6, characterized in that: The second passivation layer includes at least one of silicon nitride, silicon oxynitride and aluminum oxide.

8. The solar cell according to any one of claims 1 to 7, characterized in that: The first electrode is a silver electrode or a silver / aluminum electrode, and / or the second electrode is a silver electrode.

9. A photovoltaic module, characterized in that: The photovoltaic assembly comprises a plurality of solar cell strings, and the solar cell strings comprise the solar cell according to any one of claims 1 to 8.