ABS-based resin composition, method for preparing the same, and molded article containing the same

Combined with polyether modified by using a specific proportion of vinyl cyano compound-conjugated diene compound-aromatic vinyl compound graft copolymer and aromatic vinyl compound-vinyl cyano compound copolymer in ABS resin Polysiloxane solves the problem of the coloring performance and gloss reduction when ABS resins improve impact strength, and achieves excellent impact strength, coloring performance and gloss.

CN114568025BActive Publication Date: 2024-11-01LG CHEM LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202180005600.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-09-24
Filing Date
2021-06-09
Publication Date
2024-11-01
Estimated Expiration
2041-06-09

AI Technical Summary

Technical Problem

When existing ABS resins increase impact strength, they often lead to a decrease in coloring performance and glossiness, and cannot take into account the excellent relationship between the three.

Method used

The graft copolymer containing 20-40% of the vinyl cyano compound-conjugated diene compound-aromatic vinyl compound, 60-80% of the aromatic vinyl compound-vinyl cyano compound copolymer and 0.1-5% were used. ABS resin composition with excellent impact strength, coloring properties and glossiness was prepared by a specific melt kneading and extrusion process.

Benefits of technology

It is achieved to improve the impact strength, coloring performance and gloss of ABS resin without damaging the inherent physical properties, and avoid the increase and decrease relationship between impact strength and coloring performance/glossiness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003570927650000081
    Figure BDA0003570927650000081
  • Figure BDA0003570927650000151
    Figure BDA0003570927650000151
  • Figure FDA0004947100100000011
    Figure FDA0004947100100000011
Patent Text Reader

Abstract

The present invention relates to an ABS resin composition, a preparation method thereof and a molded product containing the same. More specifically, the present invention relates to an ABS resin composition, a preparation method thereof and a molded product containing the same, the ABS resin composition comprising: 100 parts by weight of a matrix resin comprising 20% ​​to 40% by weight of a vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer and 60% to 80% by weight of an aromatic vinyl compound-vinyl cyanide compound copolymer; and 0.1 to 5 parts by weight of a polyether-modified polysiloxane. According to the present invention, an ABS resin composition, a preparation method thereof and a molded product manufactured using the same are advantageously provided, the ABS resin composition having excellent impact strength, coloring performance and glossiness, and the conventional trade-off relationship that when the impact strength is improved, the coloring performance and glossiness are poor, and when the coloring performance and glossiness are improved, the impact strength is poor does not occur.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] [CROSS-REFERENCE TO RELATED APPLICATIONS]

[0002] This application claims the priority of Korean Patent Application No. 10-2020-0123587 filed in the Korean Intellectual Property Office on September 24, 2020, the disclosure of which is incorporated into this specification by reference.

[0003] The present invention relates to an ABS-based resin composition, a method for preparing the same, and a molded product comprising the same. More specifically, the present invention relates to an ABS-based resin composition having excellent impact strength, coloring performance, and glossiness by resolving the conventional trade-off relationship that when impact strength is improved, coloring performance and glossiness are poor, and when coloring performance and glossiness are improved, impact strength is poor; a method for preparing the ABS-based resin composition; and a molded product manufactured using the ABS-based resin composition. Background Art

[0004] Vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer (hereinafter referred to as "ABS-type resin") represented by acrylonitrile-butadiene-styrene resin can overcome the shortcomings of conventional high-impact polystyrene (HIPS) such as low heat resistance and rigidity. Vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer has excellent physical properties such as impact resistance, chemical resistance, thermal stability, coloring performance, fatigue resistance, rigidity and processing performance, especially excellent processing performance. Due to these advantages, ABS-type resin is used in various fields such as interior / exterior materials for automobiles, office equipment, parts of various electrical / electronic products, and materials for toys.

[0005] When an ABS-based resin having higher impact strength than conventional ABS-based resins is required, an additive such as silicon is added when preparing the ABS-based resin.

[0006] However, when an additive such as silicon is added to improve the impact strength of an ABS-based resin, the impact strength is improved, but the coloring property and the glossiness are reduced due to a trade-off relationship between physical properties.

[0007] Therefore, it is necessary to develop an ABS-based resin composition having excellent impact strength, coloring properties, and glossiness without deteriorating the inherent physical properties of the ABS-based resin.

[0008] [Related technical literature]

[0009] [Patent Document]

[0010] Korean Patent No.2001-0056186 Summary of the invention

[0011] Technical issues

[0012] Therefore, the present invention has been made in view of the above problems, and an object of the present invention is to provide an ABS-based resin composition having excellent impact strength, coloring property and glossiness by solving the conventional trade-off relationship that when impact strength is improved, coloring property and glossiness are poor, and when coloring property and glossiness are improved, impact strength is poor; a method for preparing the ABS-based resin composition; and a molded article manufactured using the ABS-based resin composition.

[0013] The above objects and other objects can be achieved by the present invention described below.

[0014] Technical Solution

[0015] According to one aspect of the present invention, there is provided an ABS-based resin composition comprising: 100 parts by weight of a base resin comprising 20 to 40% by weight of a vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer and 60 to 80% by weight of an aromatic vinyl compound-vinyl cyanide compound copolymer; and 0.1 to 5 parts by weight of a polyether-modified polysiloxane.

[0016] The polyether-modified polysiloxane may be a polydialkylsiloxane modified with an alkylene oxide.

[0017] The polyether-modified polysiloxane may include one or more selected from the group consisting of branched polyether-modified polysiloxane, terminal polyether-modified polysiloxane, and branched terminal polyether-modified polysiloxane.

[0018] The polyether-modified polysiloxane may have a weight average molecular weight of about 10,000 g / mol to about 50,000 g / mol.

[0019] The vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer may include 40 to 80 wt % of conjugated diene rubber, 10 to 40 wt % of aromatic vinyl compound, and 1 to 20 wt % of vinyl cyanide compound.

[0020] The aromatic vinyl compound-vinyl cyanide compound copolymer may include 60 to 80 wt % of the aromatic vinyl compound and 20 to 40 wt % of the vinyl cyanide compound.

[0021] The aromatic vinyl compound-vinyl cyanide compound copolymer may have a weight average molecular weight of 50,000 g / mol to 200,000 g / mol.

[0022] The ABS-based resin composition may include 0.1 parts by weight to 5 parts by weight of an inorganic pigment.

[0023] The inorganic pigment may be carbon black.

[0024] The color L value of the ABS-based resin composition measured by a colorimeter (Color-Eye 7000A, SCI mode) may be 28.5 or less.

[0025] The ABS-based resin composition may have a glossiness of 86 or more measured at 45° using a gloss meter VG7000.

[0026] The ABS resin composition may have an impact strength of 30 kgf·cm / cm or more measured using a test specimen having a thickness of 1 / 8" according to ASTM D256.

[0027] According to another aspect of the present invention, there is provided a method for preparing an ABS-based resin composition, the method comprising: melt-kneading 100 parts by weight of a base resin comprising 20 to 40% by weight of a vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer and 60 to 80% by weight of an aromatic vinyl compound-vinyl cyanide compound copolymer; and 0.1 to 5 parts by weight of a polyether-modified polysiloxane under the conditions of 200 to 250° C. and 100 to 400 rpm, and then extruding.

[0028] According to still another aspect of the present invention, provided is a molded article including the ABS-based resin composition.

[0029] Beneficial Effects

[0030] The present invention can provide an ABS-based resin composition having excellent impact strength, coloring properties and glossiness by resolving the conventional trade-off relationship that when impact strength is improved, coloring properties and glossiness are poor, and when coloring properties and glossiness are improved, impact strength is poor; a method for preparing the ABS-based resin composition; and a molded product manufactured using the ABS-based resin composition. DETAILED DESCRIPTION

[0031] Hereinafter, an ABS-based resin composition according to the present invention, a method of preparing the ABS-based resin composition, and a molded article manufactured using the ABS-based resin composition will be described in detail.

[0032] The present inventors have confirmed that when ABS-based resin and SAN-based resin are mixed in a predetermined ratio and a predetermined amount of a predetermined polyether-modified polysiloxane is added to the mixture, impact strength, coloring properties and glossiness are all improved, and the trade-off relationship between impact strength, coloring properties and glossiness applicable to conventional ABS-based resins does not occur. Based on these results, the present inventors conducted further studies to complete the present invention.

[0033] The ABS resin composition of the present invention comprises: 100 parts by weight of a base resin comprising 20 to 40% by weight of a vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer and 60 to 80% by weight of an aromatic vinyl compound-vinyl cyanide compound copolymer; and 0.1 to 5 parts by weight of a polyether-modified polysiloxane. In this case, the conventional trade-off relationship that when the impact strength is improved, the coloring property and glossiness are poor, and when the coloring property and glossiness are improved, the impact strength is poor, does not occur, and all of the impact strength, coloring property and glossiness can be improved.

[0034] Each component constituting the ABS-based resin composition of the present invention will be described in detail below.

[0035] Vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer

[0036] For example, the content of the vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer of the present invention in the base resin may be 20 wt % to 40 wt %, preferably 20 wt % to 35 wt %, more preferably 20 wt % to 30 wt %, and even more preferably 23 wt % to 27 wt %. Within this range, mechanical strength, fluidity and physical property balance may be excellent.

[0037] The vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer is preferably a graft copolymer prepared by graft polymerization of 40 wt % to 80 wt % of a conjugated diene rubber, 10 wt % to 40 wt % of an aromatic vinyl compound and 1 wt % to 20 wt % of a vinyl cyanide compound. In this case, the impact resistance can be excellent.

[0038] More preferably, the vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer is a graft copolymer prepared by graft polymerization of 45 wt % to 70 wt % of conjugated diene rubber, 20 wt % to 40 wt % of aromatic vinyl compound and 5 wt % to 20 wt % of vinyl cyanide compound. In this case, the impact resistance can be excellent.

[0039] Still more preferably, the vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer is a graft copolymer prepared by graft polymerization of 50 wt % to 65 wt % of a conjugated diene rubber, 20 wt % to 35 wt % of an aromatic vinyl compound and 5 wt % to 15 wt % of a vinyl cyanide compound. In this case, the impact resistance can be excellent.

[0040] The average particle size of the conjugated diene rubber is preferably 50 nm to 500 nm, more preferably 100 nm to 500 nm, still more preferably 150 nm to 400 nm, still more preferably 200 nm to 350 nm, and most preferably 250 nm to 320 nm. Within this range, the mechanical properties and physical properties such as coloring properties of the ABS resin composition can be excellent.

[0041] In the present disclosure, the average particle size of the conjugated diene rubber can be measured as an intensity value in Gaussian mode using Nicomp 370HPL (Nicomp Co., USA) according to a dynamic laser scattering method. As a specific measurement example, a sample is prepared by diluting 0.1 g of latex (TSC: 35 wt % to 50 wt %) by 1,000 to 5,000 times with distilled water, that is, the sample is appropriately diluted so that it does not significantly deviate from the intensity setting point of 300 kHz, and is placed in a glass tube. Then, the average particle size of the sample is measured using an automatic dilution flow cell in a measurement mode of dynamic light scattering / intensity 300 kHz / intensity-weight Gaussian analysis. At this time, the setting values ​​are as follows: temperature: 23°C; measurement wavelength: 632.8 nm; channel width: 10 microseconds.

[0042] For example, the conjugated diene compound may include one or more selected from the group consisting of 1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-ethyl-1,3-butadiene, 1,3-pentadiene, isoprene, chloroprene, and piperylene.

[0043] For example, the aromatic vinyl compound may include one or more selected from the group consisting of styrene, α-methylstyrene, p-methylstyrene, o-methylstyrene, p-ethylstyrene, and vinyltoluene.

[0044] For example, the vinyl cyanide compound may include one or more selected from acrylonitrile, methacrylonitrile, ethacrylonitrile, and derivatives thereof.

[0045] As a preferred example, the conjugated diene rubber may include one or more of butadiene polymer, butadiene-styrene copolymer, butadiene-acrylonitrile copolymer, ethylene-propylene copolymer, and polymers derived therefrom, without being limited thereto.

[0046] In the present specification, a derived polymer refers to a polymer prepared by copolymerizing another monomer or polymer not included in the initial copolymer, or a polymer prepared by copolymerizing a derivative of the monomer.

[0047] In the present specification, a derivative is a compound produced by replacing a hydrogen atom or a hydrogen atomic group of an initial compound with another atom or an atomic group, for example, refers to a compound produced by substitution with a halogen or an alkyl group.

[0048] For example, the vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer may be prepared by a known method such as emulsion polymerization, suspension polymerization or bulk polymerization, preferably by emulsion polymerization.

[0049] The method for preparing a vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer by emulsion polymerization preferably comprises the following steps: continuously or batchwise adding a monomer mixture containing 1 wt % to 20 wt % of a vinyl cyanide compound and 10 wt % to 40 wt % of an aromatic vinyl compound to a mixed solution containing 40 wt % to 80 wt % of a conjugated diene rubber; and adding 0.1 wt % to 5 wt % of an emulsifier, 0.1 wt % to 3 wt % of a molecular weight regulator and 0.05 wt % to 1 wt % of a polymerization initiator based on a total of 100 wt % of the conjugated diene rubber, the aromatic vinyl compound and the vinyl cyanide compound contained in the graft copolymer.

[0050] For example, the emulsifier may include one or more selected from the group consisting of allyl aryl sulfonate, alkali metal methyl alkyl sulfonate, sulfonated alkyl ester, fatty acid soap, and rosin acid alkali metal salt. In this case, polymerization stability may be excellent.

[0051] For example, the molecular weight regulator may include one or more selected from the group consisting of tert-dodecyl mercaptan, n-dodecyl mercaptan, n-octyl mercaptan and carbon tetrachloride, preferably tert-dodecyl mercaptan.

[0052] For example, the polymerization initiator may include one or more selected from potassium persulfate, sodium persulfate, and ammonium persulfate. In this case, the polymerization efficiency and physical properties of the polymer to be prepared may be excellent.

[0053] For example, latex prepared by emulsion polymerization may be coagulated using a coagulant such as sulfuric acid, MgSO4, CaCl2 or Al2(SO4)3, and the coagulated latex may then be aged, dehydrated and dried to obtain a powdered latex.

[0054] According to the definition of the present invention, when using the conditions, methods and apparatus commonly used in the field to which the present invention belongs, there is no particular limitation on the method for preparing the vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer.

[0055] Aromatic vinyl compound-vinyl cyanide compound copolymer

[0056] For example, the content of the aromatic vinyl compound-vinyl cyanide compound copolymer of the present invention in the base resin may be 60 to 80 wt %, preferably 65 to 80 wt %, more preferably 70 to 80 wt %, and even more preferably 73 to 77 wt %. Within this range, mechanical strength, fluidity, and physical property balance may be excellent.

[0057] In the present specification, the aromatic vinyl compound-vinyl cyanide compound copolymer may be an aromatic vinyl compound-vinyl cyanide compound copolymer (SAN-based resin) commonly used in the field to which the present invention belongs without particular limitation, and preferably contains 60 to 80 wt % of an aromatic vinyl compound and 20 to 40 wt % of a vinyl cyanide compound. In this case, the fluidity of the ABS-based resin composition may be improved, thereby improving processability and productivity.

[0058] As another example, the aromatic vinyl compound-vinyl cyanide compound copolymer may contain 70 wt % to 80 wt % of the aromatic vinyl compound and 20 wt % to 30 wt % of the vinyl cyanide compound. In this case, the ABS-based resin composition may have excellent processability and productivity, and may have excellent mechanical properties such as impact strength, heat resistance, and coloring properties.

[0059] As another example, the aromatic vinyl compound-vinyl cyanide compound copolymer may contain 70 wt % to 75 wt % of the aromatic vinyl compound and 25 wt % to 30 wt % of the vinyl cyanide compound. In this case, the ABS-based resin composition may have excellent processability and productivity, and may have excellent mechanical properties such as impact strength, heat resistance, and coloring properties.

[0060] For example, the aromatic vinyl compound-vinyl cyanide compound copolymer can be prepared by bulk polymerization or emulsion polymerization. In terms of production cost, bulk polymerization is preferably used.

[0061] The weight average molecular weight of the aromatic vinyl compound-vinyl cyanide compound copolymer is preferably 50,000 g / mol to 200,000 g / mol, more preferably 80,000 g / mol to 180,000 g / mol, still more preferably 100,000 g / mol to 150,000 g / mol, still more preferably 120,000 g / mol to 150,000 g / mol. Within this range, desired fluidity can be obtained, and processability, productivity and coloring properties can be excellent.

[0062] The weight average molecular weight can be measured by gel permeation chromatography (GPC). As a specific example, the weight average molecular weight can be obtained as a relative value of a polystyrene standard measured by GPC.

[0063] In the present disclosure, the weight average molecular weight can be measured by gel permeation chromatography (GPC, Waters Breeze) using tetrahydrofuran (THF) as an eluent. In this case, the weight average molecular weight is obtained as a relative value of a polystyrene standard (PS) sample. The specific measurement conditions are as follows: solvent: THF, column temperature: 40°C, flow rate: 0.3 ml / min, sample concentration: 20 mg / ml, injection volume: 5 μl, column model: 1×PLgel 10 μm MiniMix-B (250×4.6 mm) + 1×PLgel 10 μmMiniMix-B (250×4.6 mm) + 1×PLgel 10 μm MiniMix-B Guard (50×4.6 mm), equipment name: Agilent 1200 series system, differential refractometer: Agilent G1362 RID, RI temperature: 35°C, data processing: Agilent ChemStation S / W, test method (Mn, Mw and PDI): OECD TG 118.

[0064] According to the definition of the present invention, there is no particular limitation on the method for preparing the aromatic vinyl compound-vinyl cyanide compound copolymer when the conditions, methods and apparatuses commonly used in the field to which the present invention belongs are used.

[0065] Polyether modified polysiloxane

[0066] For example, based on 100 parts by weight of the base resin, the content of the polyether-modified polysiloxane of the present invention may be 0.1 to 5 parts by weight, preferably 0.2 to 3 parts by weight, more preferably 0.3 to 3 parts by weight, still more preferably 0.4 to 2.5 parts by weight, still more preferably 0.5 to 2.5 parts by weight, still more preferably 1 to 2.5 parts by weight, still more preferably 1.5 to 2.5 parts by weight. Within this range, impact strength, coloring properties and glossiness may all be excellent, and in particular, chemical resistance may be excellent.

[0067] The polyether-modified polysiloxane is preferably a polysiloxane modified with an alkylene oxide, such as ethylene oxide, propylene oxide, butylene oxide or tetrahydrofuran, and more preferably a polydialkylsiloxane modified with ethylene oxide and / or propylene oxide. In this case, impact strength, coloring properties and glossiness can all be excellent.

[0068] The polyether-modified polysiloxane preferably includes one or more selected from polydimethylsiloxane, polydiethylsiloxane, polydipropylsiloxane, polydibutylsiloxane and polydipentylsiloxane. In this case, impact strength, coloring property and glossiness can all be excellent.

[0069] The polyether-modified polysiloxane preferably includes one or more selected from branched polyether-modified polysiloxane, terminal polyether-modified polysiloxane and branched terminal polyether-modified polysiloxane, more preferably includes one or more selected from branched polyether-modified polydialkylsiloxane, terminal polyether-modified polydialkylsiloxane and branched terminal polyether-modified polydialkylsiloxane. In this case, impact strength, coloring properties and glossiness can all be excellent.

[0070] Branched polyether modification means that a polyether residue is bonded to a side chain relative to the polysiloxane main chain, terminal polyether modification means that a polyether residue is bonded to a chain terminal, and branched terminal polyether modification means that a polyether residue is bonded to both a side chain and a chain terminal.

[0071] More preferably, the branched polyether-modified polydialkylsiloxane is a polymer represented by the following Chemical Formula 1. In this case, impact strength, coloring properties, and glossiness may all be excellent.

[0072] [Chemical formula 1]

[0073]

[0074] In Chemical Formula 1, PE represents a polyether residue; R1 represents an alkyl group; R2 represents an alkylene group; x, y, and z are arbitrary numbers, specifically, integers of 50 to 1,000.

[0075] In the present specification, the alkyl group may be an alkyl group having 1 to 20 carbon atoms, preferably an alkyl group having 1 to 16 carbon atoms, more preferably an alkyl group having 1 to 12 carbon atoms, still more preferably an alkyl group having 1 to 8 carbon atoms, still more preferably an alkyl group having 1 to 4 carbon atoms.

[0076] For example, the alkyl group may be a linear, branched or cyclic alkyl group.

[0077] As a specific example, the alkyl group may include one or more selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, isopentyl, neopentyl, n-hexyl, n-heptyl, n-octyl, cyclobutyl, cyclopentyl, cyclohexyl and cycloheptyl.

[0078] Additionally, the alkyl group may be optionally substituted with one or more substituents.

[0079] In the present specification, for example, the alkylene group may be an alkylene group having 1 to 20 carbon atoms, preferably an alkylene group having 1 to 16 carbon atoms, more preferably an alkylene group having 1 to 12 carbon atoms, still more preferably an alkylene group having 1 to 8 carbon atoms, still more preferably an alkylene group having 1 to 4 carbon atoms.

[0080] For example, the alkylene group may be a linear, branched or cyclic alkylene group.

[0081] Additionally, the alkylene group is optionally substituted with one or more substituents.

[0082] For example, the substituent of the substituted alkyl or alkylene group may be an alkyl group, an alkoxy group, an alkenyl group, an epoxy group, a cyano group, a thiol group, a carboxyl group, an acryloyl group, a methacryloyl group, an acryloyloxy group, a methacryloyloxy group, or an aryl group, without being limited thereto.

[0083] The surface tension of the polyether-modified polysiloxane is preferably 15 mN / m to 30 mN / m. Within this range, impact strength, coloring properties and glossiness can all be excellent.

[0084] In this specification, the present invention can use the surface tension measurement method commonly used in the field to which the present invention belongs without particular limitation. As a specific example, the surface tension can be measured using a drop method.

[0085] The weight average molecular weight of the polyether-modified polysiloxane is preferably 10,000 g / mol to 50,000 g / mol, more preferably 20,000 g / mol to 35,000 g / mol. Within this range, impact strength, coloring properties, and glossiness may all be excellent.

[0086] The weight average molecular weight can be measured using gel permeation chromatography (GPC). In this case, the weight average molecular weight is obtained as a relative value to a polystyrene standard.

[0087] According to the definition of the present invention, there is no particular limitation on the method for preparing the polyether-modified polysiloxane when using conditions, methods and apparatus commonly used in the field to which the present invention belongs.

[0088] Inorganic Pigments

[0089] The inorganic pigment of the present invention is preferably carbon black, titanium dioxide (TiO2) or a mixture thereof. In this case, mechanical properties can be maintained, coloring properties can be excellent, and the degree of discoloration can be reduced.

[0090] The carbon black preferably includes one or more selected from Ketjen black, acetylene black, furnace black and channel black. In this case, mechanical properties can be maintained, coloring properties can be excellent, and the degree of discoloration can be reduced.

[0091] The carbon black is preferably a masterbatch mixed with an aromatic vinyl compound-vinyl cyanide compound copolymer. In this case, mechanical properties can be maintained, coloring properties can be excellent, and the degree of discoloration can be reduced.

[0092] The carbon black masterbatch preferably contains 30 to 70% by weight of the aromatic vinyl compound-vinyl cyanide compound copolymer and 30 to 70% by weight of carbon black, and more preferably contains 50 to 70% by weight of the aromatic vinyl compound-vinyl cyanide compound copolymer and 30 to 50% by weight of carbon black. Within this range, mechanical properties can be maintained, coloring properties can be excellent, and the degree of discoloration can be reduced.

[0093] The content of the inorganic pigment is preferably 0.1 to 5 parts by weight, more preferably 0.5 to 3 parts by weight, still more preferably 0.5 to 2 parts by weight, still more preferably 0.5 to 1.5 parts by weight, based on 100 parts by weight of the base resin. Within this range, mechanical properties can be maintained, coloring properties can be excellent, and the degree of discoloration can be reduced.

[0094] ABS resin composition

[0095] The ABS resin composition of the present invention preferably has a melt index (MFR) measured under the conditions of 220° C. and 10 kg of 15 to 25 g / 10 min, more preferably 18 to 25 g / 10 min, and even more preferably 18 to 23 g / 10 min. Within this range, the balance between processability and physical properties can be excellent.

[0096] The color L value of the ABS-based resin composition measured using a colorimeter (Color-Eye 7000A, SCI model) is preferably 28.5 or less, more preferably 28 or less, and still more preferably 27.5 or less. Within this range, coloring performance and physical property balance can be excellent.

[0097] The ABS-based resin composition preferably has a glossiness measured at 45° using a gloss meter VG7000 of 86 or more, more preferably 87 or more, and still more preferably 88 or more. Within this range, glossiness and physical properties may be excellent in balance.

[0098] When a sample having a size of 200 mm×12.7 mm×3.2 mm is fixed to a bending jig having a strain of 1.1%, 1 cc of a thinner is applied thereto, and then the time when cracks appear in the sample is measured, the chemical resistance of the ABS-based resin composition is preferably 400 seconds or more, more preferably 450 seconds or more, still more preferably 480 seconds or more, still more preferably 500 seconds or more, still more preferably 550 seconds or more, and most preferably 600 seconds or more. Within this range, the balance between chemical resistance and physical properties can be excellent.

[0099] The ABS resin composition has an impact strength of preferably 30 kgf·cm / cm or more, more preferably 32 kgf·cm / cm or more, and still more preferably 33 kgf·cm / cm or more using a test specimen having a thickness of 1 / 8" according to ASTM D256. As a preferred example, it is 30 to 35 kgf·cm / cm, as a more preferred example, it is 32 to 35 kgf·cm / cm, and as a still more preferred example, it is 33 to 35 kgf·cm / cm. Within this range, the impact strength and the physical properties can be excellently balanced.

[0100] According to needs, based on 100 parts by weight of the base resin, the ABS resin composition may include 0.5 to 5 parts by weight, preferably 1 to 4 parts by weight, and more preferably 1.5 to 3 parts by weight of one or more selected from lubricants, flame retardants, heat stabilizers, antioxidants, light stabilizers, compatibilizers, pigments (however, excluding inorganic pigments), dyes, and inorganic additives. Within this range, the inherent effects of the additives can be effectively expressed without impairing the desired effects of the present invention.

[0101] For example, the lubricant may include one or more selected from wax, silicone oil, and stearamide.

[0102] For example, the silicone oil may include one or more selected from dimethyl silicone oil, methyl hydrogen silicone oil, hydroxy silicone oil, carbinol-modified silicone oil, vinyl silicone oil, and silicone acrylate.

[0103] For example, the heat stabilizer may include one or more selected from tris(nonylphenyl) phosphite, tris(2,4-di-tert-butylphenyl) phosphite (TBPP), 2,4,6-tri-tert-butylphenyl-2-butyl-2-ethyl-1,3-propanediol phosphite, diisodecyl pentaerythritol diphosphite, distearyl pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite (PEP24), bis(2,4-diisopropylphenyl) pentaerythritol diphosphite and tetrakis(2,4-di-tert-butylphenyl)[1,1-biphenyl]-4,4'-diyl diphosphonate.

[0104] For example, the antioxidant may include a hindered phenolic antioxidant, a phosphide antioxidant, or a mixture thereof.

[0105] Method for preparing ABS resin composition

[0106] The method for preparing the ABS resin composition of the present invention preferably comprises the steps of: melt-kneading 100 parts by weight of a base resin comprising 20 to 40% by weight of a vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer and 60 to 80% by weight of an aromatic vinyl compound-vinyl cyanide compound copolymer; and 0.1 to 5 parts by weight of a polyether-modified polysiloxane at 200 to 250° C. and 100 to 400 rpm, and then extruding. In this case, an ABS resin composition having excellent impact strength, coloring property and glossiness is advantageously provided, without the conventional trade-off relationship that when the impact strength is improved, the coloring property and glossiness are poor, and when the coloring property and glossiness are improved, the impact strength is poor.

[0107] The step of performing melt kneading and extrusion is preferably performed at 210 to 250° C. and 200 to 350 rpm, more preferably 210 to 240° C. and 250 to 350 rpm. Within this range, the desired effects of the present invention can be well expressed.

[0108] For example, when melt-kneading is performed, based on 100 parts by weight of the base resin, 0.1 to 5 parts by weight, preferably 0.3 to 4 parts by weight, more preferably 0.5 to 3 parts by weight of one or more selected from lubricants, flame retardants, heat stabilizers, anti-drip agents, antioxidants, light stabilizers, compatibilizers, pigments (however, excluding inorganic pigments), dyes and inorganic additives may also be included. Within this range, the inherent effects of the additives can be effectively expressed without damaging the desired effects of the present invention.

[0109] The extruded product obtained through the melt-kneading and extrusion steps is preferably pellets.

[0110] The vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer, aromatic vinyl compound-vinyl cyanide compound copolymer, polyether-modified polysiloxane and inorganic pigment contained in the ABS resin composition are the same as those described above, so repeated description thereof will be omitted.

[0111] Molding

[0112] The molded article of the present invention comprises the ABS resin composition. In this case, there is an advantage of providing a molded article having excellent impact strength, coloring property and glossiness without the conventional trade-off relationship that when the impact strength is improved, the coloring property and glossiness are poor, and when the coloring property and glossiness are improved, the impact strength is poor.

[0113] The molded product is preferably an injection molded product, and more preferably an automobile interior or exterior material or a household appliance exterior material. In this case, a product satisfying required physical properties can be manufactured.

[0114] The molded article is preferably manufactured by a step including injection molding the ABS resin composition of the present invention or its pellets. In this case, the injection molding is preferably performed at an injection temperature of 210° C. to 250° C., more preferably 215° C. to 240° C., and still more preferably 220° C. to 230° C., at an injection speed of 7 mm / sec to 13 mm / sec, more preferably 75 mm / sec to 85 mm / sec. Within this range, the desired effects of the present invention can be well exhibited.

[0115] According to the definition of the present invention, there is no particular limitation on the method for producing the molded article as long as conditions, methods and equipment commonly used in the field to which the present invention pertains are used.

[0116] Hereinafter, the present invention will be described in more detail with reference to the following preferred embodiments. However, these embodiments are provided for illustrative purposes only and should not be construed as limiting the scope and design of the present invention. In addition, it will be apparent to those skilled in the art that, without departing from the concept and scope of the present invention, various changes and modifications may be made, and such changes and modifications are also within the scope of the appended claims.

[0117] [Example]

[0118] The components used in the following examples and comparative examples are as follows:

[0119] (A) Vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer by emulsion polymerization: DP270 (LG Chemical Co.) containing 60 wt % of a butadiene polymer having an average particle size of 300 nm, 10 wt % of acrylonitrile and 30 wt % of styrene was used.

[0120] (B) Aromatic vinyl compound-vinyl cyanide compound copolymer: 92HR (LG Chemical Co.) having a weight average molecular weight of 130,000 g / mol and containing 27% by weight of acrylonitrile was used.

[0121] (C-1) Polyether-modified polysiloxane: Polyether-modified polydimethylsiloxane (BYK-333) was used.

[0122] (C-2) Polyether-modified polysiloxane: Polyether-modified polydimethylsiloxane (BYK-378) was used.

[0123] (C-3) Unmodified polysiloxane: polydimethylsiloxane (KF-96-100cs, Shin-Etsu Silicone Co.) was used.

[0124] (D) Inorganic pigment: A carbon black masterbatch (product name: BK50, Muil Hwasung Co.) was used.

[0125] Examples 1 to 4 and Comparative Examples 1 to 3

[0126] The components shown in Table 1 were introduced into a twin-screw extruder according to the contents shown in Table 1, and melt-kneaded and extruded at 220° C. and 600 rpm to prepare ABS resin composition pellets. In addition, the ABS resin composition pellets were dried at 80° C. for 3 hours, and then injection molded using an injection molding machine under the conditions of an injection temperature of 220° C., a mold temperature of 60° C., and an injection speed of 30 mm / sec to prepare a specimen for measuring physical properties.

[0127] [Test example]

[0128] The properties of the samples prepared in Examples 1 to 4 and Comparative Examples 1 to 3 were measured according to the following methods, and the results are shown in Table 1 below.

[0129] *Izod impact strength (kgf·cm / cm): The Izod impact strength was measured using a specimen having a thickness of 1 / 4" in accordance with ASTM D256.

[0130] *Flowability (g / 10 min): Melt viscosity was measured under the conditions of 220° C. and 10 kg according to ASTM D256.

[0131] *Gloss: Gloss was measured at 45° using a gloss meter VG7000 (1 / 8 inch injection gloss).

[0132] *Color L: The color L, a, and b values ​​of the sample were measured using a colorimeter (Colar-Eye 7000A, SCI mode). For reference, the color "L" value is a numerical value indicating brightness. As the color "L" value decreases, the degree of black increases. The color "a" value is a numerical value indicating the degree of red and green. As the color "a" value decreases, the degree of green increases. The color "b" is a numerical value indicating the degree of yellow and blue. As the color "b" value decreases, the degree of blue increases.

[0133] *Chemical resistance (ESCR, seconds): A specimen measuring 200 mm × 12.7 mm × 3.2 mm was fixed to a bending fixture with a strain of 1.1%, 1 cc of a thinner was applied thereto, and then the time until cracks appeared in the specimen was measured. When no cracks appeared until 600 seconds, the specimen was evaluated as having good chemical resistance. Specimens satisfying the chemical resistance evaluation were denoted as >600.

[0134] [Table 1]

[0135]

[0136] As shown in Table 1, in the case of the ABS-based resin compositions according to the present invention (Examples 1 to 4), the fluidity was maintained within the range capable of easy processing, and the impact strength, glossiness, and coloring properties were excellent, as compared to the ABS-based resin compositions not containing the polyether-modified polysiloxane according to the present invention or containing the polyether-modified polysiloxane according to the present invention in a content outside the range of the present invention (Comparative Examples 1 to 3).

[0137] In summary, as in the conventional method, when polydimethylsiloxane is mixed to improve the impact strength in the ABS-based resin composition of Comparative Example 1 as in Comparative Examples 2 and 3, a trade-off relationship is observed in which the impact strength is improved but the coloring property and glossiness are poor. However, as in Examples 1 to 4, when a predetermined amount of the polyether-modified polysiloxane according to the present invention is mixed, the trade-off relationship disappears, and the impact strength, coloring property and glossiness are improved at the same time.

Claims

1. An ABS resin composition, comprising: 100 parts by weight of a base resin comprising 20 to 40 wt % of a vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer and 60 to 80 wt % of an aromatic vinyl compound-vinyl cyanide compound copolymer; and 1.5 to 2.5 parts by weight of polyether-modified polysiloxane, in, The polyether-modified polysiloxane is a branched polyether-modified polysiloxane in which a polyether residue represented by the following Chemical Formula 1 is bonded to a side chain relative to the main chain of the polysiloxane: [Chemical formula 1] In Chemical Formula 1, PE represents a polyether residue; R1 represents an alkyl group having 1 to 20 carbon atoms; R2 represents an alkylene group having 1 to 20 carbon atoms; and x, y, and z are any integers of 50 to 1,000, respectively.

2. The ABS resin composition according to claim 1, wherein The polyether-modified polysiloxane has a weight average molecular weight of 10,000 g / mol to 50,000 g / mol.

3. The ABS resin composition according to claim 1, wherein The vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer comprises 40 to 80 wt % of a conjugated diene rubber, 10 to 40 wt % of an aromatic vinyl compound and 1 to 20 wt % of a vinyl cyanide compound.

4. The ABS resin composition according to claim 1, wherein The aromatic vinyl compound-vinyl cyanide compound copolymer includes 60 to 80 wt % of an aromatic vinyl compound and 20 to 40 wt % of a vinyl cyanide compound.

5. The ABS resin composition according to claim 1, wherein The aromatic vinyl compound-vinyl cyanide compound copolymer has a weight average molecular weight of 50,000 g / mol to 200,000 g / mol.

6. The ABS resin composition according to claim 1, wherein The ABS-based resin composition includes 0.1 parts by weight to 5 parts by weight of an inorganic pigment.

7. The ABS resin composition according to claim 6, wherein The inorganic pigment is carbon black.

8. The ABS resin composition according to claim 1, wherein The color L value of the ABS-based resin composition measured by using a colorimeter Color-Eye 7000A in an SCI mode is 28.5 or less.

9. The ABS resin composition according to claim 1, wherein The ABS resin composition has a glossiness of 86 or more when measured at 45° using a gloss meter VG7000.

10. The ABS resin composition according to claim 1, wherein The ABS resin composition has an impact strength of 30 kgf·cm / cm or more when measured according to ASTM D256 using a test specimen having a thickness of 1 / 8″.

11. A method for preparing an ABS resin composition, comprising: 100 parts by weight of a base resin comprising 20 to 40% by weight of a vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer and 60 to 80% by weight of an aromatic vinyl compound-vinyl cyanide compound copolymer; and 1.5 to 2.5 parts by weight of a polyether-modified polysiloxane are melt-kneaded at 200 to 250° C. and 100 to 400 rpm, and then extruded, The polyether-modified polysiloxane is a branched polyether-modified polysiloxane in which a polyether residue represented by the following chemical formula 1 is bonded to a side chain relative to the main chain of the polysiloxane: [Chemical formula 1] In Chemical Formula 1, PE represents a polyether residue; R1 represents an alkyl group having 1 to 20 carbon atoms; R2 represents an alkylene group having 1 to 20 carbon atoms; and x, y, and z are any integers of 50 to 1,000, respectively.

12. A molded article comprising the ABS-based resin composition according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Infrared transmission lens powder and infrared transmission lens

    KR1020200123587A

  • Contact component with reduced squeak noise made from thermoplastic resin composition

    CN103108915A

  • Extrusion-grade ABS polymer having improved properties and process for its preparation

    CN1414985A

  • Cooking apparatus

    JP1996070999A

  • Rubber toughened styrenic resin composition

    JP2001323127A