Isolation membrane, isolation membrane preparation method and electrochemical device
By setting two coating layers on the isolation film and using nano-kaolin and nano-boehmite powder, the problems of shrinkage deformation and poor conductivity of the isolation film in high-temperature environments are solved, achieving higher high temperature resistance and conductivity. , improving the safety and electrochemical performance of the battery.
Patent Information
- Application Number
- CN202210391737.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-04-14
AI Technical Summary
Existing isolation membranes are prone to shrinkage and deformation in high-temperature environments, leading to safety accidents, and have poor penetrability of conductive ions, affecting the electrochemical performance of the battery.
Two coating layers are provided on the base film. The first coating layer contains a binder and nano-kaolin, and the second coating layer contains nano-boehmite powder with nano-kaolin wrapped on the surface. These materials improve the high temperature resistance of the isolation film. ability and conductive properties.
It effectively improves the high temperature resistance of the isolation membrane, reduces the risk of coating peeling, improves the electrochemical performance and safety of the battery, and enhances conductive ion penetration.
Smart Images

Figure CN114725622B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of isolation membranes, and specifically relates to an isolation membrane, an isolation membrane preparation method and an electrochemical device. Background Art
[0002] In recent years, electrical devices powered by secondary batteries have been widely used and promoted in various electronic products and new energy vehicles, etc. People have put forward higher requirements on the cycle performance of batteries.
[0003] The separator is one of the key internal components of a secondary battery. The separator is placed between the positive electrode and the negative electrode, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through. Improving the performance of the separator is crucial to improving the electrochemical performance of the battery. Summary of the invention
[0004] The embodiments of the present application provide an isolation membrane, an isolation membrane preparation method and an electrochemical device, which can improve the wettability of the isolation membrane to the electrolyte.
[0005] According to a first aspect of an embodiment of the present application, there is provided an isolation film, comprising:
[0006] Basement membrane;
[0007] A first coating layer is disposed on at least one side of the base film in a thickness direction, wherein the first coating layer comprises a binder and nano-kaolin;
[0008] A second coating layer is disposed on a side of the first coating layer away from the base film, wherein the second coating layer comprises a binder and a second substrate;
[0009] Wherein, the second substrate in the second coating layer is nano-boehmite powder with nano-kaolin coated on the surface.
[0010] By adopting the above structure, by setting two coating layers on the base film, not only can the high temperature resistance of the isolation membrane be effectively improved, and the safety accidents caused by the shrinkage and deformation of the isolation membrane in the battery under high temperature environment be reduced, but it also has excellent wetting ability, which can facilitate the penetration of conductive ions and improve the electrochemical performance of the battery. Secondly, through the nano kaolin in the first coating layer and the second coating layer, the stability of the connection between the first coating layer and the second coating layer can also be enhanced, reducing the problem of coating shedding.
[0011] In some optional embodiments of the present application, the ratio of the binder to the nano-kaolin in the first coating layer, by mass, is (1.0 to 3.0):(7.0 to 9.0).
[0012] In some optional embodiments of the present application, the ratio of the binder in the second coating layer to the second substrate, by mass, is (0.3 to 1.0):(9.0 to 9.7), and the ratio of the nano-kaolin to the nano-boehmite in the second substrate, by mass, is (2.0 to 3.0):(7.0 to 8.0).
[0013] In some optional embodiments of the present application, the thickness of the first coating layer is 0.5 μm to 5.0 μm, and the thickness of the second coating layer is 0.1 μm to 5.0 μm.
[0014] In some optional embodiments of the present application, the particle size of the nano-kaolin in the first coating layer is 300 nm to 800 nm.
[0015] With the above structure, by selecting the particle size of the first coating layer to be 300nm to 800nm, it helps to strengthen the bonding force between the first coating layer and the base film, and can reserve filling gaps for the particles in the second coating layer to form a whole.
[0016] In some optional embodiments of the present application, the particle size of the second substrate in the second coating layer is 100 nm to 500 nm.
[0017] In some optional embodiments of the present application, the particle size of the nano-boehmite in the second substrate is 80nm to 400nm, and the particle size of the nano-kaolin is 20nm to 100nm.
[0018] By adopting the above structure, by setting the second substrate to 100nm to 500nm, the particles in the second coating layer can be made smaller than the particles in the first coating layer, which is convenient for forming a stable mosaic structure after melting. Secondly, since the surface of the second substrate is coated with nano-kaolin, which is the same material as the first coating layer, it can achieve a homogeneous effect, which is beneficial to the combination of the first coating layer and the second coating layer.
[0019] In some optional embodiments of the present application, the binder in the first coating layer and the second coating layer is at least one of polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), styrene-butadiene latex, polyvinyl alcohol and polyurethane.
[0020] In some optional embodiments of the present application, the binder in the first coating layer and the second coating layer is polyvinylidene fluoride.
[0021] By adopting the above structure and selecting polyvinylidene fluoride as the binder, better temperature resistance can be obtained, and the viscosity is greater, so as to facilitate better bonding and compatibility with nano-kaolin.
[0022] In some optional embodiments of the present application, the base film is at least one of a polyolefin film, a polypropylene film, a polyethylene film and a propylene-ethylene copolymer film.
[0023] In some optional embodiments of the present application, the base film has a thickness of 7 μm to 20 μm and a porosity of 45% to 65%.
[0024] A second aspect of the embodiments of the present application provides a method for preparing an isolation film, comprising the following steps:
[0025] providing a basement membrane;
[0026] Coating a first coating layer on at least one side of the base film, and pressing after drying;
[0027] A second coating layer is coated on the first coating layer at a side away from the base film, and then pressed after drying.
[0028] According to a third aspect of the embodiments of the present application, an electrochemical device is provided, comprising the above-mentioned isolation membrane.
[0029] Compared with the prior art, in the isolation membrane, isolation membrane preparation method and electrochemical device of the embodiments of the present application, by arranging two coating layers on the base membrane, not only can the high temperature resistance of the isolation membrane be effectively improved, and the safety accidents caused by the shrinkage and deformation of the isolation membrane in the battery under high temperature environment be reduced, but also the isolation membrane has excellent wetting ability, which can facilitate the penetration of conductive ions and improve the electrochemical performance of the battery. Secondly, the nano-kaolin in the first coating layer and the second coating layer can also enhance the stability of the connection between the first coating layer and the second coating layer, and reduce the problem of coating shedding. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without paying creative work.
[0031] Figure 1 It is a cross-sectional view of the isolation film in the present application along the thickness direction.
[0032] Reference numerals:
[0033] 1. Base film; 2. First coating layer; 3. Second coating layer. DETAILED DESCRIPTION
[0034] In order to make the invention purpose, technical scheme and beneficial technical effect of the present application clearer, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the embodiments described in this specification are only for explaining the present application, not for limiting the present application.
[0035] For simplicity, only some numerical ranges are explicitly disclosed herein. However, any lower limit can be combined with any upper limit to form an unambiguous range; and any lower limit can be combined with other lower limits to form an unambiguous range, and any upper limit can be combined with any other upper limit to form an unambiguous range. In addition, although not explicitly stated, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unambiguous range.
[0036] In the description herein, when a composition is described as containing, comprising or including specific components, or when a process is described as containing, comprising or including specific process steps, it is expected that the composition of the present application also consists essentially of or consists of the components, and the process of the present application also consists essentially of or consists of the process steps.
[0037] The use of the terms "including," "comprising," "containing," and "having" should generally be interpreted as open ended and non-limiting unless expressly stated otherwise.
[0038] In the description of this article, it should be noted that, unless otherwise specified, “above” and “below” are inclusive of the number itself, and the “multiple” in “one or more” means more than two.
[0039] The above-mentioned summary of the invention of the present application is not intended to describe each disclosed embodiment or each implementation in the present application. The following description more specifically illustrates exemplary embodiments. In many places throughout the application, guidance is provided by a series of examples, which can be used in various combinations. In each example, enumeration is only used as a representative group and should not be interpreted as exhaustive.
[0040] As one of the most critical internal components in the secondary battery structure, the performance of the separator directly affects the battery's capacity, rate, life, safety and other performance. The interface compatibility between the separator material and the electrode, and the separator's retention of the electrolyte have an important impact on the secondary battery's charge and discharge performance, cycle performance and life.
[0041] In the related art, in order to solve the heat resistance and safety performance of the isolation membrane, the method of coating ceramics on the base membrane is generally adopted to form a composite coating on the surface of the base membrane to improve the heat resistance of the base membrane. For example, when the temperature in the working environment of the isolation membrane is too high, the shrinkage deformation of the isolation membrane is reduced, thereby reducing the short circuit of the battery in a high temperature environment. However, the aforementioned method of coating ceramics mostly uses alumina ceramic materials, and the resulting isolation membrane has poor wettability, which increases the penetration resistance of conductive ions and reduces the electrochemical performance of the battery. On the other hand, the alumina ceramic material in the related art needs to rely on adhesives to connect with the base membrane. In a high temperature environment, the adhesive is prone to decomposition and failure, resulting in the problem of coating shedding.
[0042] The inventor of this application has found through research that by setting two layers of high temperature resistant coating on the base film, the tolerance of the isolation membrane in a high temperature environment can be effectively improved, and the coating layer materials are selected from nano kaolin and nano boehmite, which can not only obtain high temperature resistance, but also good thermal stability, and can also ensure the wettability of the isolation membrane to the electrolyte, with high ionic conductivity, so that the electrochemical performance of the battery can be guaranteed, with excellent rate performance and long-term cycle performance, and high safety. In view of this, the embodiment of the present application provides a separation membrane, a method for preparing a separation membrane, and an electrochemical device.
[0043] like Figure 1 As shown, Figure 1 : is a cross-sectional view of the isolation film in the present application along the thickness direction. The present application provides an isolation film, including a base film, a first coating layer and a second coating layer. The first coating layer is arranged in the thickness direction of the base film ( Figure 1 The first coating layer includes a binder and nano-kaolin. The second coating layer is arranged on a side of the first coating layer away from the base film, and the second coating layer includes a binder and a second substrate. The second substrate in the second coating layer is a nano-boehmite powder with a surface coated with nano-kaolin.
[0044] By setting two coating layers on the base film, not only can the high temperature resistance of the isolation membrane be effectively improved and the safety accidents caused by the shrinkage and deformation of the isolation membrane in a high temperature environment of the battery be reduced, but it also has excellent wetting ability, which can facilitate the penetration of conductive ions and improve the electrochemical performance of the battery. Secondly, the nano kaolin in the first coating layer and the second coating layer can also enhance the stability of the connection between the first coating layer and the second coating layer and reduce the problem of coating shedding.
[0045] In some optional embodiments of the present application, the ratio of the binder to the nano-kaolin in the first coating layer, by mass, is (1.0 to 3.0):(7.0 to 9.0).
[0046] In some optional embodiments of the present application, the ratio of the binder to the second substrate in the second coating layer, by mass, is (0.3 to 1.0):(9.0 to 9.7), and the ratio of the nano-kaolin to the nano-boehmite in the second substrate, by mass, is (2.0 to 3.0):(7.0 to 8.0).
[0047] In some optional embodiments of the present application, the thickness of the first coating layer is 0.5 μm to 5.0 μm, and the thickness of the second coating layer is 0.1 μm to 5.0 μm.
[0048] In some optional embodiments of the present application, the particle size of the nano-kaolin in the first coating layer is 300 nm to 800 nm.
[0049] In some optional embodiments of the present application, the particle size of the second substrate in the second coating layer is 100 nm to 500 nm.
[0050] In some optional embodiments of the present application, the binder in the first coating layer and the second coating layer is at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, styrene-butadiene latex, polyvinyl alcohol, polyurethane and polyionic liquid.
[0051] In some optional embodiments of the present application, the binder in the first coating layer and the second coating layer is polyvinylidene fluoride.
[0052] In some optional embodiments of the present application, the base film is at least one of a polyolefin film, a polypropylene film, a polyethylene film and a propylene-ethylene copolymer film.
[0053] In some optional embodiments of the present application, the base film has a thickness of 7 μm to 20 μm and a porosity of 45% to 65%.
[0054] In some optional embodiments of the present application, a method for preparing an isolation film is also provided, comprising the following steps:
[0055] S01, providing a basement membrane;
[0056] S02, coating a first coating layer on at least one side of the base film, and pressing after drying;
[0057] S03, coating a second coating layer on a side of the first coating layer away from the base film, and pressing after drying.
[0058] Specifically, step S02 also includes: preparing the first coating layer, providing a binder and nano-kaolin, fully dissolving the two and mixing them evenly to obtain a first coating layer coating.
[0059] Specifically, step S03 also includes: preparing the second coating layer, providing a binder and a second substrate, fully dissolving the two and mixing them evenly to obtain a second coating layer coating.
[0060] In some optional embodiments of the present application, an electrochemical device is also provided, comprising the above-mentioned isolation membrane.
[0061] Specifically, the electrochemical device may be a battery cell, including at least a housing and a pole piece assembly disposed in the housing, wherein the pole piece assembly includes a positive pole piece, a negative pole piece, and a separator disposed between the positive pole piece and the negative pole piece. The battery cell may be a secondary battery cell or a primary battery cell, or a lithium-ion battery cell, a sodium-ion battery cell, or a magnesium-ion battery cell, etc., which is not limited in the embodiments of the present application. The battery cell may be cylindrical, flat, rectangular, or in other shapes.
[0062] Example
[0063] The following examples describe the disclosure of the present application in more detail, and these examples are intended for illustrative purposes only, as it will be apparent to those skilled in the art that various modifications and variations may be made within the scope of the disclosure of the present application. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.
[0064] Example 1
[0065] Preparation of isolation film:
[0066] (1) Preparation of the first coating layer: Weigh 0.4 g of polyvinylidene fluoride and dissolve it in 8.6 g of anhydrous N-methylpyrrolidone (NMP), stir at room temperature for 4 hours, and obtain a polyvinylidene fluoride solution with a mass fraction of 4%. Mix nano-kaolin (HNT) with a particle size of 300 nm and the obtained polyvinylidene fluoride solution in a mass ratio of 9:1, stir at room temperature for 10 hours and ultrasonicate for 1.0 hour to obtain the first coating layer.
[0067] (2) Preparation of the second coating layer: Weigh 0.4g of polyvinylidene fluoride and dissolve it in 9.6g of anhydrous N-methylpyrrolidone, stir at room temperature for 4 hours to obtain a polyvinylidene fluoride solution with a mass fraction of 4%. Mix 2.0g of nano-kaolin and 8.0g of boehmite, grind them at room temperature for 5 hours using a high-energy ball mill to obtain a second substrate of nano-kaolin coated boehmite with a particle size of 100nm. Mix the second substrate with the obtained polyvinylidene fluoride solution in a mass ratio of 9.7:0.3, stir at room temperature for 10 hours and ultrasonicate for 1.0 hour to obtain a second coating layer.
[0068] (3) Coating: Take the first coating layer and evenly apply it on both sides of the 9μm polyethylene base film with a scraper to a thickness of 3μm. After a large amount of solvent evaporates, place it in a vacuum oven at 50°C for 12 hours, and press it with a hot press at a pressure of 4MPa for 30 seconds after drying. Take the second coating layer and evenly apply it on the side of the first coating layer away from the base film with a scraper to a thickness of 1μm. After a large amount of solvent evaporates, place it in a vacuum oven at 50°C for 12 hours, and press it with a hot press at a pressure of 4MPa for 50 seconds after drying to obtain a separator.
[0069] Example 2
[0070] Preparation of isolation film:
[0071] (1) Preparation of the first coating layer: Weigh 0.4 g of polyvinylidene fluoride and dissolve it in 9.6 g of anhydrous N-methylpyrrolidone, stir at room temperature for 4 hours, and obtain a polyvinylidene fluoride solution with a mass fraction of 4%. Nano-kaolin with a particle size of 400 nm and the obtained polyvinylidene fluoride solution are mixed in a mass ratio of 8:1, stirred at room temperature for 10 hours and ultrasonicated for 1.0 hour to obtain the first coating layer.
[0072] (2) Preparation of the second coating layer: Weigh 0.4g of polyvinylidene fluoride and dissolve it in 9.6g of anhydrous N-methylpyrrolidone, stir at room temperature for 4 hours to obtain a polyvinylidene fluoride solution with a mass fraction of 4%. Mix 2.0g of nano-kaolin and 8.0g of boehmite, grind them at room temperature for 5 hours using a high-energy ball mill to obtain a second substrate of nano-kaolin coated boehmite with a particle size of 200nm. Mix the second substrate with the obtained polyvinylidene fluoride solution in a mass ratio of 9.5:0.5, stir at room temperature for 10 hours and ultrasonicate for 1.0 hour to obtain a second coating layer.
[0073] (3) Coating: Take the first coating layer and evenly apply it on both sides of the 9μm polyethylene base film with a scraper to a thickness of 3μm. After a large amount of solvent evaporates, place it in a vacuum oven at 50°C for 12 hours, and press it with a hot press at a pressure of 4MPa for 30 seconds after drying. Take the second coating layer and evenly apply it on the side of the first coating layer away from the base film with a scraper to a thickness of 1μm. After a large amount of solvent evaporates, place it in a vacuum oven at 50°C for 12 hours, and press it with a hot press at a pressure of 4MPa for 50 seconds after drying to obtain a separator.
[0074] Example 3
[0075] Preparation of isolation film:
[0076] (1) Preparation of the first coating layer: Weigh 0.4 g of polyvinylidene fluoride and dissolve it in 9.6 g of anhydrous N-methylpyrrolidone, stir at room temperature for 4 hours, and obtain a polyvinylidene fluoride solution with a mass fraction of 4%. Nano-kaolin with a particle size of 500 nm and the obtained polyvinylidene fluoride solution are mixed in a mass ratio of 7:1, stirred at room temperature for 10 hours and ultrasonicated for 1.0 hour to obtain the first coating layer.
[0077] (2) Preparation of the second coating layer: Weigh 0.4g of polyvinylidene fluoride and dissolve it in 9.6g of anhydrous N-methylpyrrolidone, stir at room temperature for 4 hours to obtain a polyvinylidene fluoride solution with a mass fraction of 4%. Mix 2.0g of nano-kaolin and 8.0g of boehmite, grind them at room temperature for 5 hours using a high-energy ball mill to obtain a second substrate of nano-kaolin coated boehmite with a particle size of 300nm. Mix the second substrate with the obtained polyvinylidene fluoride solution in a mass ratio of 9.5:0.5, stir at room temperature for 10 hours and ultrasonicate for 1.0 hour to obtain a second coating layer.
[0078] (3) Coating: Take the first coating layer and evenly apply it on both sides of the 9μm polyethylene base film with a scraper to a thickness of 3μm. After a large amount of solvent evaporates, place it in a vacuum oven at 50°C for 12 hours, and press it with a hot press at a pressure of 4MPa for 30 seconds after drying. Take the second coating layer and evenly apply it on the side of the first coating layer away from the base film with a scraper to a thickness of 1μm. After a large amount of solvent evaporates, place it in a vacuum oven at 50°C for 12 hours, and press it with a hot press at a pressure of 4MPa for 50 seconds after drying to obtain a separator.
[0079] Example 4
[0080] Preparation of isolation film:
[0081] (1) Preparation of the first coating layer: Weigh 0.4 g of polyvinylidene fluoride and dissolve it in 9.6 g of anhydrous N-methylpyrrolidone, stir at room temperature for 4 hours, and obtain a polyvinylidene fluoride solution with a mass fraction of 4%. Nano-kaolin with a particle size of 700 nm and the obtained polyvinylidene fluoride solution are mixed in a mass ratio of 8:2, stirred at room temperature for 10 hours and ultrasonicated for 1.0 hour to obtain the first coating layer.
[0082] (2) Preparation of the second coating layer: Weigh 0.4g of polyvinylidene fluoride and dissolve it in 9.6g of anhydrous N-methylpyrrolidone, stir at room temperature for 4 hours to obtain a polyvinylidene fluoride solution with a mass fraction of 4%. Mix 2.5g of nano-kaolin and 7.5g of boehmite, grind them at room temperature for 5 hours using a high-energy ball mill to obtain a second substrate of nano-kaolin coated boehmite with a particle size of 400nm. Mix the second substrate with the obtained polyvinylidene fluoride solution in a mass ratio of 9:1, stir at room temperature for 10 hours and ultrasonicate for 1.0 hour to obtain a second coating layer.
[0083] (3) Coating: Take the first coating layer and evenly apply it on both sides of the 9μm polyethylene base film with a scraper to a thickness of 3μm. After a large amount of solvent evaporates, place it in a vacuum oven at 50°C for 12 hours, and press it with a hot press at a pressure of 4MPa for 30 seconds after drying. Take the second coating layer and evenly apply it on the side of the first coating layer away from the base film with a scraper to a thickness of 1μm. After a large amount of solvent evaporates, place it in a vacuum oven at 50°C for 12 hours, and press it with a hot press at a pressure of 4MPa for 50 seconds after drying to obtain a separator.
[0084] Example 5
[0085] Preparation of isolation film:
[0086] (1) Preparation of the first coating layer: Weigh 0.4 g of polyvinylidene fluoride and dissolve it in 9.6 g of anhydrous N-methylpyrrolidone, stir at room temperature for 4 hours, and obtain a polyvinylidene fluoride solution with a mass fraction of 4%. Nano-kaolin with a particle size of 800 nm and the obtained polyvinylidene fluoride solution are mixed in a mass ratio of 7:3, stirred at room temperature for 10 hours and ultrasonicated for 1.0 hour to obtain the first coating layer.
[0087] (2) Preparation of the second coating layer: Weigh 0.4g of polyvinylidene fluoride and dissolve it in 9.6g of anhydrous N-methylpyrrolidone, stir at room temperature for 4 hours to obtain a polyvinylidene fluoride solution with a mass fraction of 4%. Mix 3.0g of nano-kaolin and 7.0g of boehmite, grind them at room temperature for 5 hours using a high-energy ball mill to obtain a second substrate of nano-kaolin coated boehmite with a particle size of 500nm. Mix the second substrate with the obtained polyvinylidene fluoride solution in a mass ratio of 9:1, stir at room temperature for 10 hours and ultrasonicate for 1.0 hour to obtain a second coating layer.
[0088] (3) Coating: Take the first coating layer and evenly apply it on both sides of the 9μm polyethylene base film with a scraper to a thickness of 3μm. After a large amount of solvent evaporates, place it in a vacuum oven at 50°C for 12 hours, and press it with a hot press at a pressure of 4MPa for 30 seconds after drying. Take the second coating layer and evenly apply it on the side of the first coating layer away from the base film with a scraper to a thickness of 1μm. After a large amount of solvent evaporates, place it in a vacuum oven at 50°C for 12 hours, and press it with a hot press at a pressure of 4MPa for 50 seconds after drying to obtain a separator.
[0089] Example 6
[0090] This embodiment is substantially the same as the embodiment 1, except that the binder in the first coating layer and the second coating layer is polyvinylidene fluoride-hexafluoropropylene, and the base film is a polyolefin film.
[0091] Example 7
[0092] This embodiment is substantially the same as the embodiment 1, except that the binder in the first coating layer and the second coating layer is polyvinylidene fluoride-hexafluoropropylene, and the base film is a polypropylene film.
[0093] Example 8
[0094] This embodiment is substantially the same as the embodiment 1, except that the binder in the first coating layer and the second coating layer is styrene-butadiene latex, and the base film is a propylene-ethylene copolymer film.
[0095] Example 9
[0096] This embodiment is substantially the same as the first embodiment, except that the binder in the first coating layer and the second coating layer is polyvinyl alcohol.
[0097] Example 10
[0098] This embodiment is substantially the same as the first embodiment, except that the adhesive in the first coating layer and the second coating layer is polyurethane.
[0099] Comparative Example 1
[0100] Preparation of isolation film:
[0101] Alumina ceramics with a particle size of 500 nm are dispersed with polyvinylidene fluoride to form a uniform slurry, which is then double-sided coated on the surface of a polyethylene base film with a thickness of 20 μm according to a conventional coating process to obtain an isolation film.
[0102] Test Method
[0103] Wettability determination:
[0104] The wettability is characterized by the amount of liquid absorbed, and the amount of liquid absorbed is measured by the electrolyte. The isolation membrane sample is cut into 2cm×2cm squares, weighed M1, and the electrolyte used is 1mol / L LiPF6. The electrolyte system is ethylene carbonate (EC): dimethyl carbonate (DMC): diethyl carbonate (EMC) = 1:1:1 (V / V). The sample membrane is soaked in the electrolyte for 30 minutes and then taken out. The electrolyte on the surface of the sample membrane is absorbed with filter paper, and M2 is weighed. The wettability is calculated according to the following formula.
[0105] The calculation formula is: P = (M2-M1) / M1×100%
[0106] Where: M1—mass of base film (g); M2—mass after immersion (g).
[0107] Specific capacity determination:
[0108] The positive electrode part of the battery is made of active material LiCoO2, conductive agent (Super-P carbon) and binder polyvinylidene fluoride, which are uniformly mixed in a mass ratio of 8:1:1 to form a slurry, which is evenly coated on an aluminum foil with a scraper, naturally dried and then beaten into discs, and vacuum dried at 105°C to obtain an electrode sheet. The metal lithium sheet is the negative electrode, and the electrolyte is 1 mol / L LiPF6 of ethylene carbonate (EC), diethyl carbonate (DEC) and dimethyl carbonate (DMC) in a volume ratio of 1:1:1. The isolation membrane obtained in the above embodiment is used to assemble a CR2032 button battery in an argon environment, and the electrochemical performance is tested using a CT2001A battery testing system. The constant current charge and discharge method is used, and the test is performed at 25°C with a voltage of 2.0V to 4.2V to measure the specific capacity.
[0109] Shrinkage determination:
[0110] (1) Cut 5 100 mm × 100 mm isolation films (if the width is less than 100 mm, cut 100 mm in the length direction);
[0111] (2) Measure the width of the specimen according to the national standard and record it as L1;
[0112] (3) Place the isolation film sample in an electric constant temperature air drying oven (DHG-9076A) for drying at 105°C for 2 hours;
[0113] (4) Take out the isolation film after high temperature baking and measure the width of the isolation film, which is recorded as L2;
[0114] (5) Calculate the shrinkage ratio as (L1-L2) / L1*100%.
[0115] The specific test results are shown in Table 1.
[0116] Table 1: Preparation parameters and test results of Examples 1 to 10 and Comparative Example 1
[0117]
[0118] It can be seen from Table 1 that, compared with Comparative Example 1, the isolation films obtained in Examples 1-10 of the present application have better shrinkage rate and specific capacity, and the wetting liquid of the isolation films obtained in Examples 1-10 of the present application is significantly better than that of Comparative Example 1.
[0119] Compared with the prior art, in the isolation membrane, isolation membrane preparation method and electrochemical device of the embodiments of the present application, by arranging two coating layers on the base membrane, not only can the high temperature resistance of the isolation membrane be effectively improved, and the safety accidents caused by the shrinkage and deformation of the isolation membrane in the battery under high temperature environment be reduced, but also the isolation membrane has excellent wetting ability, which can facilitate the penetration of conductive ions and improve the electrochemical performance of the battery. Secondly, the nano-kaolin in the first coating layer and the second coating layer can also enhance the stability of the connection between the first coating layer and the second coating layer, and reduce the problem of coating shedding.
[0120] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed in the present application, and these modifications or replacements should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.
Claims
1. A separation film, characterized in that: include: Basement membrane; A first coating layer is disposed on at least one side of the base film in a thickness direction, wherein the first coating layer comprises a binder and nano-kaolin; A second coating layer is disposed on a side of the first coating layer away from the base film, the second coating layer comprises a binder and a second substrate, and the binder and the second substrate in the second coating layer are in a ratio of (0.3 to 1.0):(9.0 to 9.7) by mass; Wherein, the second substrate in the second coating layer is nano-boehmite powder with nano-kaolin coated on the surface; The particles in the second coating layer are smaller than the particles in the first coating layer; The first coating layer has a thickness of 3 μm to 5.0 μm, and the second coating layer has a thickness of 0.1 μm to 1 μm.
2. The isolation film according to claim 1, characterized in that: The binder and the nano-kaolin in the first coating layer are in a mass ratio of (1.0 to 3.0):(7.0 to 9.0).
3. The isolation film according to claim 2, characterized in that: The ratio of the nano-kaolin to the nano-boehmite in the second substrate is (2.0 to 3.0):(7.0 to 8.0) by mass.
4. The isolation film according to any one of claims 1 to 3, characterized in that: The particle size of the nano-kaolin in the first coating layer is 300nm to 800nm.
5. The isolation film according to any one of claims 1 to 3, characterized in that: The particle size of the second base material in the second coating layer is 100 nm to 500 nm.
6. The isolation film according to claim 1, characterized in that: The binder in the first coating layer and the second coating layer is at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, styrene-butadiene latex, polyvinyl alcohol and polyurethane.
7. The isolation film according to claim 6, characterized in that: The binder in the first coating layer and the second coating layer is polyvinylidene fluoride.
8. The isolation film according to claim 6, characterized in that: The base film is a polyolefin film.
9. The isolation film according to claim 8, characterized in that: The base film is at least one of a polypropylene film, a polyethylene film and a propylene-ethylene copolymer film.
10. A method for preparing an isolation film, used for preparing the isolation film according to any one of claims 1 to 9, characterized in that: The following steps are involved: providing a basement membrane; Coating a first coating layer on at least one side of the base film, and pressing after drying; A second coating layer is coated on the first coating layer at a side away from the base film, and then dried and pressed.
11. An electrochemical device, characterized in that: The isolation film according to claim 1 is included.
Citation Information
Patent Citations
Lithium ion battery diaphragm, lithium ion battery and manufacturing method thereof
CN110783516A
High-heat-resistance diaphragm as well as preparation method and application thereof
CN113745754A