Three-electrode system soft-pack battery, preparation method thereof and impedance testing method
By fixing the reference tab and polished lithium sheet in the three-electrode system soft-pack battery, the problem of lithium reference electrode displacement is solved, the stability and accuracy of the test results are improved, and the electrode position is ensured. More accurate impedance testing is achieved.
Patent Information
- Application Number
- CN202210294325.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-24
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-03-24
AI Technical Summary
During the preparation process of the three-electrode system soft-pack battery, the lithium reference electrode is easily displaced, affecting the stability and validity of the test results.
By exposing and fixing the reference tab at the end of the aluminum-plastic film, and fixing the lithium piece on the reference tab in a polished state, the position of the lithium reference electrode is ensured to be stable, using ether and nitrile substances. Polishing fluid is used to polish lithium flakes to prevent water absorption and oxidation.
It effectively avoids the displacement of the lithium reference electrode, improves the stability and accuracy of the test results, ensures the fixation of the electrode position, and improves the validity of the test results.
Smart Images

Figure CN114744279B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of secondary batteries, and in particular to a method for preparing a reference electrode, a reference electrode and a method for testing impedance of a soft-pack battery. Background Art
[0002] Lithium-ion battery is a secondary battery with advantages such as high energy density and good charge and discharge cycle performance. It has been widely sought after since its introduction and has now become a leader in the field of secondary batteries, widely used in electric vehicles, electronic devices and even energy storage power stations. Knowing the impedance parameters of lithium-ion batteries is crucial for analyzing the actual performance of lithium-ion batteries.
[0003] Lithium cobalt oxide / graphite battery is a type of lithium-ion battery, and its technology is relatively mature and widely used. It is generally believed that increasing its cut-off voltage can effectively increase its discharge specific capacity, but correspondingly, the impedance of the battery will also increase significantly. In order to study the effect of different electrodes on impedance under high voltage, it is necessary to analyze lithium-ion batteries. When analyzing the inside of lithium-ion batteries, an electrochemical workstation is usually used for two-electrode testing. The impedance results obtained in this way can only reflect the impedance between the positive and negative electrodes of the battery, but cannot analyze the influence of a certain electrode.
[0004] The three-electrode battery system is based on the two-electrode battery system with an additional reference electrode. The positive and negative electrodes are equivalent to the working electrode and the counter electrode respectively. Lithium has a standard potential and high exchange current density, and is a more suitable reference electrode material. Therefore, there are also some technologies that directly place lithium metal between the positive and negative electrode diaphragms as a reference electrode. The main problem with this method is that lithium metal is relatively easy to shift, affecting the test results. Summary of the invention
[0005] Based on this, it is necessary to provide a method for preparing a three-electrode system soft-pack battery that can avoid the displacement of the lithium reference electrode, and further provide a three-electrode system soft-pack battery and an impedance testing method thereof.
[0006] According to one embodiment of the present invention, a method for preparing a three-electrode system soft-pack battery comprises the following steps:
[0007] The positive electrode sheet, the positive electrode diaphragm, the negative electrode diaphragm and the negative electrode sheet are stacked in sequence, and a reference electrode tab is sandwiched between the positive electrode diaphragm and the negative electrode diaphragm;
[0008] Covering the positive electrode sheet and the negative electrode sheet with two aluminum-plastic films respectively, controlling the reference electrode tab to be exposed from one end of the two aluminum-plastic films, and sealing the ends of the two aluminum-plastic films;
[0009] Inserting a lithium sheet between the positive electrode separator and the negative electrode separator, and fixing the lithium sheet on the reference electrode tab;
[0010] The two pieces of aluminum-plastic films are completely sealed.
[0011] In one embodiment, before the lithium sheet is inserted between the positive electrode separator and the negative electrode separator, the step of immersing the lithium sheet in a polishing liquid in a vacuum environment for polishing is also included, and the polishing liquid includes ether substances and nitrile substances.
[0012] In one embodiment, the ether substance is selected from tetrahydrofuran, and the nitrile substance is selected from succinonitrile.
[0013] In one embodiment, the lithium sheet is folded and wrapped around the reference electrode tab so that the lithium sheet is fixed on the reference electrode tab.
[0014] In one embodiment, after the lithium sheet is fixed on the reference tab, the step of applying pressure to the aluminum-plastic film to compact the positive electrode sheet, the positive electrode separator, the negative electrode separator and the negative electrode sheet located inside is also included.
[0015] In one embodiment, the ratio of the area of the lithium sheet facing the positive electrode sheet to the area of the positive electrode sheet facing the lithium sheet is 1:(5-15); and / or
[0016] The ratio of the area of the lithium sheet facing the negative electrode sheet to the area of the negative electrode sheet facing the lithium sheet is 1:(5-15).
[0017] In one embodiment, the positive electrode material on the positive electrode sheet includes a positive electrode active material, a binder and a conductive agent, and the positive electrode active material is selected from lithium cobalt oxide.
[0018] In one embodiment, the negative electrode material on the negative electrode sheet includes a negative electrode active material, a binder and a conductive agent, and the negative electrode active material is selected from graphite.
[0019] Furthermore, a three-electrode system soft-pack battery is prepared according to the preparation method of the three-electrode system soft-pack battery described in the above embodiment.
[0020] And, an impedance testing method for a three-electrode system soft-pack battery, wherein the three-electrode system soft-pack battery is the three-electrode system soft-pack battery according to the above embodiment, and the impedance testing method comprises the following steps:
[0021] One of the positive electrode sheet and the negative electrode sheet is electrically connected to the working electrode of the electrochemical workstation, the other is electrically connected to the counter electrode of the electrochemical workstation, and the reference electrode tab is electrically connected to the reference electrode of the electrochemical workstation, the electrochemical workstation is started, and the impedance between the working electrode and the reference electrode is tested.
[0022] In the traditional technology of preparing three-electrode system soft-pack batteries, the positive electrode sheet, positive electrode separator, lithium reference electrode with reference tab, negative electrode separator and negative electrode sheet are usually stacked in sequence, and then aluminum-plastic film is coated on the outside of the positive electrode sheet and negative electrode sheet and sealed. The inventors found that during the heat sealing process of the aluminum-plastic film, the reference tab will be slightly deformed, which will cause the end of the reference electrode located inside the aluminum-plastic film to drive the lithium metal to shift, thereby affecting the test results of the lithium metal electrode.
[0023] In the preparation method of the above-mentioned three-electrode system soft-pack battery, the reference pole ear is first exposed from one end of the aluminum-plastic film, and then the end of the reference pole ear covered by the aluminum-plastic film is sealed to first fix the reference pole ear. After the reference pole ear is fixed, its end inside the aluminum-plastic film is also fixed. Then the polished lithium sheet is fixed on the reference pole ear so that the position of the lithium reference electrode is fixed. It was found through experiments that the preparation method of the three-electrode system soft-pack battery can more effectively solve the problem of displacement of the lithium reference electrode, ensure the fixed position of the lithium reference electrode, and ensure the stability and effectiveness of the test results. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The charge and discharge curve of the soft-pack battery prepared in Example 2;
[0025] Figure 2 Schematic diagram of the full battery impedance, positive electrode impedance and negative electrode impedance of the soft-pack battery prepared in Example 2. DETAILED DESCRIPTION
[0026] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. Preferred embodiments of the present invention are provided herein. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the technical field of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items. "More than" used herein includes two and more than two items. "Above a certain number" used herein should be understood as a certain number and a range greater than a certain number.
[0028] In the traditional technology of preparing three-electrode system soft-pack batteries, the positive electrode sheet, positive electrode separator, lithium reference electrode with reference tab, negative electrode separator and negative electrode sheet are usually stacked in sequence, and then aluminum-plastic film is coated on the outside of the positive electrode sheet and negative electrode sheet and sealed. The inventors found that during the heat sealing process of the aluminum-plastic film, the reference tab will be slightly deformed, which will cause the end of the reference electrode located inside the aluminum-plastic film to drive the lithium metal to shift, thereby affecting the test results of the lithium metal electrode.
[0029] Based on this, the inventor redesigned the preparation method of the three-electrode system soft-pack battery and proposed the preparation method of the three-electrode system soft-pack battery of the present invention. Specifically, according to one embodiment of the present invention, a preparation method of a three-electrode system soft-pack battery comprises the following steps:
[0030] The positive electrode sheet, the positive electrode diaphragm, the negative electrode diaphragm and the negative electrode sheet are stacked in sequence, and a reference electrode ear is sandwiched between the positive electrode diaphragm and the negative electrode diaphragm;
[0031] Covering the positive electrode sheet and the negative electrode sheet with two aluminum-plastic films respectively, controlling the reference electrode tab to be exposed from one end of the two aluminum-plastic films, and sealing the ends of the two aluminum-plastic films;
[0032] Insert the lithium sheet between the positive electrode separator and the negative electrode separator, and fix the lithium sheet on the reference electrode ear;
[0033] Completely seal the two pieces of aluminum plastic film.
[0034] In the preparation method of the above-mentioned three-electrode system soft-pack battery, the reference pole ear is first exposed from one end of the aluminum-plastic film, and then the end of the reference pole ear covered by the aluminum-plastic film is sealed to first fix the reference pole ear. After the reference pole ear is fixed, its end inside the aluminum-plastic film is also fixed. Then the polished lithium sheet is fixed on the reference pole ear so that the position of the lithium reference electrode is fixed. It was found through experiments that the preparation method of the three-electrode system soft-pack battery can more effectively solve the problem of displacement of the lithium reference electrode, ensure the fixed position of the lithium reference electrode, and ensure the stability and effectiveness of the test results.
[0035] However, lithium sheets are very easy to absorb water and oxygen, and are easy to react with trace amounts of water and oxygen even in a glove box filled with argon, which results in the presence of impurities generated by oxidation on the surface of the lithium sheet. Impurities generated by oxidation will also affect the accuracy of the experimental results. Therefore, in one specific example, before the lithium sheet is inserted between the positive electrode diaphragm and the negative electrode diaphragm, the step of immersing the lithium sheet in a polishing liquid in a vacuum environment for polishing is also included, and the polishing liquid includes ether substances and nitrile substances.
[0036] In one specific example, the ether substance is selected from tetrahydrofuran, and the nitrile substance is selected from succinonitrile. Further, the mass ratio of the ether substance to the nitrile substance is (2-8):1, and optionally, the mass ratio of the ether substance to the nitrile substance is 5:1.
[0037] There are many ways to fix the lithium sheet to the reference tab. In one specific example, the lithium sheet is fixed to the reference tab by folding and winding the lithium sheet on the reference tab. Specifically, the lithium sheet can be folded in half and sandwiched on the reference tab, so that the lithium sheet can be fixed on the reference tab. For example, the lithium sheet can be in the shape of 1cm×1cm. After heat-sealing one end of the aluminum-plastic film, the shape of the reference tab is fixed, and the lithium sheet can be extended between the positive electrode separator and the negative electrode separator from the end of the aluminum-plastic film that has not been heat-sealed, and the lithium sheet can be folded and wound on the reference tab.
[0038] In one specific example, after the lithium sheet is folded, wound and fixed on the reference electrode tab, the process also includes applying pressure to the aluminum-plastic film to compact the positive electrode sheet, positive electrode separator, negative electrode separator and negative electrode sheet inside.
[0039] In one specific example, the ratio of the area of the lithium sheet facing the positive electrode sheet to the area of the positive electrode sheet facing the lithium sheet is 1:(5-15). In one specific example, the ratio of the area of the lithium sheet facing the negative electrode sheet to the area of the negative electrode sheet facing the lithium sheet is 1:(5-15).
[0040] In one specific example, the positive electrode material on the positive electrode sheet includes a positive electrode active material, a binder and a conductive agent, and the positive electrode active material is selected from lithium cobalt oxide. It can be understood that the binder in the positive electrode material can be selected from, for example, polyvinylidene fluoride, and the conductive agent can be selected from carbon materials, such as acetylene black. The mass ratio of the positive electrode active material, the binder and the conductive agent is 8:1:1.
[0041] Furthermore, the positive electrode sheet can be prepared as follows. Dissolve polyvinylidene fluoride in nitrogen methyl pyrrolidone and stir until completely dissolved to obtain a mixed solution. Weigh the lithium cobalt oxide powder and acetylene black according to the preset mass ratio and grind them thoroughly to obtain a mixture. Degas and slurry the prepared mixed solution and the mixture to obtain a slurry. Apply the slurry on the current collector. The current collector coated with the slurry can then be placed in a blast drying oven to dry, and after drying, it can be moved into a 120°C vacuum drying oven to dry. The dried electrode sheet is placed in a roller press to roll and prepare the positive electrode sheet. When preparing a soft-pack battery, the positive electrode sheet can be cut into a specific size, such as 3cm×3cm, and the positive electrode tab can be connected to the positive electrode sheet. The tab is generally in the shape of a long strip, for example, with a size of 1.5cm×0.5cm.
[0042] In one specific example, the negative electrode material on the negative electrode sheet includes a negative electrode active material, a binder and a conductive agent, and the negative electrode active material is selected from graphite. It can be understood that the binder in the negative electrode material can also be selected from polyvinylidene fluoride, and the conductive agent can also be selected from carbon materials, such as acetylene black. The mass ratio of the negative electrode active material, the binder and the conductive agent is 8:1:1.
[0043] Furthermore, the negative electrode sheet can be prepared as follows. Dissolve polyvinylidene fluoride in nitrogen methyl pyrrolidone and stir until completely dissolved to obtain a mixed solution. Weigh the graphite powder and acetylene black according to the preset mass ratio and grind them thoroughly to obtain a mixture. Degas and slurry the prepared mixed solution and the mixture to obtain a slurry. Apply the slurry on the current collector. The current collector coated with the slurry can then be placed in a blast drying oven to dry, and after drying, it can be moved into a 120°C vacuum drying oven to dry. The dried electrode sheet is placed in a roller press to roll and prepare the negative electrode sheet. When preparing a soft-pack battery, the negative electrode sheet can be cut into the same size as the positive electrode sheet, for example 3cm×3cm, and the negative electrode tab can be connected to the negative electrode sheet.
[0044] Furthermore, the present invention also provides a three-electrode system soft-pack battery prepared by the above preparation method. The position of the reference electrode in the three-electrode system soft-pack battery is fixed and not easily displaced, so that the accuracy of the result of the three-electrode system soft-pack battery when used to test the positive electrode impedance or the negative electrode impedance can be significantly improved.
[0045] Furthermore, the present invention also provides an impedance testing method for a three-electrode system soft-pack battery, wherein the three-electrode system soft-pack battery is a three-electrode system soft-pack battery according to any of the above embodiments, and its impedance testing method comprises the following steps: electrically connecting one of the positive electrode sheet and the negative electrode sheet to the working electrode of the electrochemical workstation, and the other to the counter electrode of the electrochemical workstation, and electrically connecting the reference electrode tab to the reference electrode of the electrochemical workstation, starting the electrochemical workstation, and testing the impedance between the working electrode and the reference electrode.
[0046] It can be understood that the connection method between the electrodes of the soft-pack battery and the electrodes of the electrochemical workstation may also be different depending on the actual test results required. For example, when testing the impedance of the full battery, the positive electrode of the soft-pack battery is connected to the working electrode of the electrochemical workstation, and the negative electrode is connected to the reference electrode and the counter electrode of the electrochemical workstation at the same time. When testing the positive electrode impedance, the positive electrode of the soft-pack battery is connected to the working electrode of the electrochemical workstation, the reference electrode of the reference pole ear of the soft-pack battery is connected to the reference electrode of the electrochemical workstation, and the negative electrode of the soft-pack battery is connected to the counter electrode of the electrochemical workstation. When testing the negative electrode impedance, the positive electrode of the soft-pack battery is connected to the counter electrode of the electrochemical workstation, the reference electrode of the reference pole ear of the soft-pack battery is connected to the reference electrode of the electrochemical workstation, and the negative electrode of the soft-pack battery is connected to the working electrode of the electrochemical workstation.
[0047] The impedance testing method of the three-electrode system soft-pack battery provided by the present invention can be used to monitor the impedance of the whole battery, the impedance of the positive electrode and the impedance of the negative electrode in real time during the high voltage cycle, so as to analyze the relationship between the impedance evolution and the battery degradation phenomenon.
[0048] In order to make it easier to understand and implement the present invention, the following more specific and detailed embodiments and comparative examples are provided as references. Through the description and performance results of the following specific embodiments and comparative examples, the embodiments of the present invention and their advantages will also be apparent.
[0049] Unless otherwise specified, the raw materials used in the following examples can be purchased from the market.
[0050] In addition, in the actual preparation process, the actual thickness of each layer may be slightly different from the tested thickness, but it does not affect the implementation of the comparative examples and embodiments.
[0051] The preparation methods of the pole pieces used in the embodiments and comparative examples are as follows.
[0052] Positive electrode sheet: Dissolve 1 part by mass of polyvinylidene fluoride in nitrogen methyl pyrrolidone and stir until completely dissolved. Weigh 8 parts by mass of lithium cobalt oxide powder and 1 part by mass of acetylene black, mix and grind thoroughly. Add the ground lithium cobalt oxide powder and acetylene black powder to the polyvinylidene fluoride solution for degassing and slurrying to obtain a slurry. Apply the slurry on the current collector. Then place the current collector coated with the slurry in a blast drying oven to dry, and after drying, move it to a 120°C vacuum drying oven to dry. The dried electrode sheet is placed in a roller press to roll and prepare the positive electrode sheet. Cut the positive electrode sheet into a size of 3cm×3cm, and connect the positive electrode tab to the positive electrode sheet. The material of the positive electrode tab is aluminum. The tab size is 1.5cm×0.5cm.
[0053] Negative electrode sheet: Dissolve 1 part by mass of polyvinylidene fluoride in nitrogen methyl pyrrolidone and stir until completely dissolved. Weigh 8 parts by mass of graphite powder and 1 part by mass of acetylene black, mix and grind thoroughly. Add the ground graphite powder and acetylene black powder to the polyvinylidene fluoride solution for degassing and slurrying to obtain a slurry. Apply the slurry on the current collector. Then place the current collector coated with the slurry in a blast drying oven to dry, and after drying, move it to a 120°C vacuum drying oven to dry. The dried electrode sheet is placed in a roller press to roll and prepare the negative electrode sheet. Cut the positive electrode sheet into a size of 3cm×3cm, and connect the negative electrode tab to the negative electrode sheet. The material of the negative electrode tab is nickel. The size of the negative electrode tab is 1.5cm×0.5cm.
[0054] Example 1
[0055] The positive electrode sheet, the positive electrode separator, the negative electrode separator and the negative electrode sheet are stacked in sequence, and a reference electrode tab is sandwiched between the positive electrode separator and the negative electrode separator. The reference electrode tab is exposed from between the positive electrode separator and the negative electrode separator to connect to the external electrode.
[0056] Two aluminum-plastic films are respectively covered on the surface of the positive electrode sheet away from the positive electrode separator and the surface of the negative electrode sheet away from the negative electrode separator, and the reference electrode tab is controlled to be exposed from the top of the aluminum-plastic film, and a part of the reference electrode tab is retained in the aluminum-plastic film;
[0057] Heat-seal the tops of the two aluminum-plastic films to fix the aluminum-plastic films and the reference tabs;
[0058] A 1.0 cm × 1.0 cm lithium sheet is inserted between the positive electrode separator and the negative electrode separator, and the lithium sheet is folded around the reference electrode tab to fix the lithium sheet on the reference electrode tab;
[0059] Completely seal the two pieces of aluminum plastic film.
[0060] Example 2
[0061] The positive electrode sheet, the positive electrode separator, the negative electrode separator and the negative electrode sheet are stacked in sequence, and a reference electrode tab is sandwiched between the positive electrode separator and the negative electrode separator. The reference electrode tab is exposed from between the positive electrode separator and the negative electrode separator to connect to the external electrode.
[0062] Two aluminum-plastic films are respectively covered on the surface of the positive electrode sheet away from the positive electrode separator and the surface of the negative electrode sheet away from the negative electrode separator, and the reference electrode tab is controlled to be exposed from the top of the aluminum-plastic film, and a part of the reference electrode tab is retained in the aluminum-plastic film;
[0063] Heat-seal the tops of the two aluminum-plastic films to fix the aluminum-plastic films and the reference tabs;
[0064] A 1.0 cm × 1.0 cm lithium sheet was immersed in a polishing liquid and polished for 8 hours. The polishing liquid was a mixture of tetrahydrofuran and succinonitrile in a mass ratio of 5:1. The main function of polishing was to remove the oxide layer on the surface of the original lithium, thereby achieving uniform current distribution on the lithium surface during the cycle, preventing polarization of the reference electrode due to uneven local current density, and a stable surface can reduce the uneven deposition of the original lithium, inhibit the formation of lithium dendrites and improve the cycle performance.
[0065] Inserting the polished lithium sheet between the positive electrode separator and the negative electrode separator, and folding the lithium sheet around the reference electrode tab to fix the lithium sheet on the reference electrode tab;
[0066] Completely seal the two pieces of aluminum plastic film.
[0067] Comparative Example 1
[0068] The positive electrode sheet, the positive electrode separator, the negative electrode separator and the negative electrode sheet are stacked in sequence, and a reference electrode tab is sandwiched between the positive electrode separator and the negative electrode separator. The reference electrode tab is exposed from between the positive electrode separator and the negative electrode separator to connect to the external electrode.
[0069] Two aluminum-plastic films are respectively covered on the surface of the positive electrode sheet away from the positive electrode separator and the surface of the negative electrode sheet away from the negative electrode separator, and the reference electrode tab is controlled to be exposed from the top of the aluminum-plastic film, and a part of the reference electrode tab is retained in the aluminum-plastic film;
[0070] A 1.0 cm × 1.0 cm lithium sheet is inserted between the positive electrode separator and the negative electrode separator, and the lithium sheet is folded around the reference electrode tab to fix the lithium sheet on the reference electrode tab;
[0071] Completely seal the two pieces of aluminum plastic film.
[0072] Comparative Example 2
[0073] The positive electrode sheet, the positive electrode separator, the negative electrode separator and the negative electrode sheet are stacked in sequence, and a reference electrode tab is sandwiched between the positive electrode separator and the negative electrode separator. The reference electrode tab is exposed from between the positive electrode separator and the negative electrode separator to connect to the external electrode.
[0074] Two aluminum-plastic films are respectively covered on the surface of the positive electrode sheet away from the positive electrode separator and the surface of the negative electrode sheet away from the negative electrode separator, and the reference electrode tab is controlled to be exposed from the top of the aluminum-plastic film, and a part of the reference electrode tab is retained in the aluminum-plastic film;
[0075] A 1.0 cm × 1.0 cm lithium sheet was immersed in a polishing solution and polished for 8 hours. The polishing solution was a mixture of tetrahydrofuran and succinonitrile in a mass ratio of 5:1.
[0076] Insert the polished lithium sheet between the positive electrode separator and the negative electrode separator, and fold the lithium sheet around the reference electrode tab to fix the lithium sheet on the reference electrode tab;
[0077] Completely seal the two pieces of aluminum plastic film.
[0078] Test Example: The soft-pack batteries prepared in Examples 1 to 2 and Comparative Example 1 were charged and discharged. The charge and discharge cycle process was as follows: first, the battery was charged to 4.6V at a rate of 0.7C, then charged at a constant voltage for 1h, and then discharged to 3V at a rate of 0.7C. The charge and discharge curve of the battery in Example 2 during the cycle can be seen in Figure 1 . Figure 1 The charge and discharge curves from right to left in the figure are the charge and discharge curves for 4, 50, 100, 150 and 200 cycles respectively.
[0079] When the cycles are 50, 150 and 200, the soft-pack battery is connected to the electrochemical workstation to test the full battery impedance, positive electrode impedance and negative electrode impedance of the soft-pack battery. The connection method of the soft-pack battery and the electrochemical workstation when testing different impedances is as follows.
[0080] When testing the full-cell impedance, the positive electrode of the soft-pack battery is connected to the working electrode of the electrochemical workstation, and the negative electrode is connected to the reference electrode and counter electrode of the electrochemical workstation at the same time.
[0081] When testing the positive electrode impedance, the positive electrode of the soft-pack battery is connected to the working electrode of the electrochemical workstation, the reference tab of the soft-pack battery is connected to the reference electrode of the electrochemical workstation, and the negative electrode of the soft-pack battery is connected to the counter electrode of the electrochemical workstation.
[0082] When testing the negative electrode impedance, the positive electrode of the soft-pack battery is connected to the counter electrode of the electrochemical workstation, the reference tab of the soft-pack battery is connected to the reference electrode of the electrochemical workstation, and the negative electrode of the soft-pack battery is connected to the working electrode of the electrochemical workstation.
[0083] Among them, the lithium reference electrode prepared in Example 1, Comparative Example 1 and Comparative Example 2 will shift to a certain extent, resulting in greater fluctuations in the test results. Compared with Example 2, Example 1 and Comparative Example 1 will show a more obvious accelerated decay behavior of the discharge specific capacity after a certain number of cycles, which may correspond to the degradation of the surface properties of the lithium sheet, making it difficult to adapt to the impedance evaluation during long-term cycles.
[0084] The test results of Example 2 can be found in Figure 2 , Figure 2 The words "full battery", "positive electrode" and "negative electrode" represent the test results of full battery impedance, positive electrode impedance and negative electrode impedance respectively; the numbers 50, 150 and 200 represent the test results of battery components after 50, 150 and 200 cycles respectively.
[0085] in accordance with Figure 2 After 200 cycles of the soft-pack battery obtained in Example 2, the measured ohmic impedance of the whole battery was 3.315Ω, the membrane impedance was 26.14Ω, and the charge transfer impedance was 42.82Ω. The measured ohmic impedance of the positive electrode was 1.694Ω, the membrane impedance was 22.17Ω, and the charge transfer impedance was 40Ω. The measured ohmic impedance of the negative electrode was 1.16Ω, the membrane impedance was 3.468Ω, and the charge transfer impedance was 1.952Ω. The inventors also tested multiple groups of batteries under the same conditions, and after comparison, it can be determined that the above impedance test results have a high reproducibility, indicating that the impedance test method of the three-electrode system soft-pack battery provided by the present invention can be used to accurately monitor the impedance of the whole battery, the positive electrode impedance and the negative electrode impedance during high-voltage cycling, thereby analyzing the relationship between impedance evolution and battery degradation.
[0086] The technical features of the above embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0087] The above embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a three-electrode system soft-pack battery, characterized in that: The steps include: The positive electrode sheet, the positive electrode separator, the negative electrode separator and the negative electrode sheet are stacked in sequence, and a reference electrode tab is sandwiched between the positive electrode separator and the negative electrode separator; Covering the positive electrode sheet and the negative electrode sheet with two aluminum-plastic films respectively, controlling the reference electrode tab to be exposed from one end of the two aluminum-plastic films, and sealing the ends of the two aluminum-plastic films; Inserting a lithium sheet between the positive electrode separator and the negative electrode separator, and fixing the lithium sheet on the reference electrode tab; The two pieces of aluminum-plastic films are completely sealed.
2. The method for preparing a three-electrode system soft-pack battery according to claim 1, characterized in that: Before the lithium sheet is inserted between the positive electrode separator and the negative electrode separator, the method further includes immersing the lithium sheet in a polishing liquid in a vacuum environment for polishing, wherein the polishing liquid includes an ether substance and a nitrile substance.
3. The method for preparing a three-electrode system soft pack battery according to claim 2, characterized in that: The ether substance is selected from tetrahydrofuran, and the nitrile substance is selected from succinonitrile.
4. The method for preparing a three-electrode system soft pack battery according to claim 1, characterized in that: The lithium sheet is folded and wound around the reference electrode tab so that the lithium sheet is fixed on the reference electrode tab.
5. The method for preparing a three-electrode system soft pack battery according to claim 1, characterized in that: After the lithium sheet is fixed on the reference electrode tab, the method further includes applying pressure to the aluminum-plastic film to compact the positive electrode sheet, the positive electrode separator, the negative electrode separator and the negative electrode sheet located inside.
6. The method for preparing a three-electrode system soft-pack battery according to any one of claims 1 to 5, characterized in that: The ratio of the area of the lithium sheet facing the positive electrode sheet to the area of the positive electrode sheet facing the lithium sheet is 1:(5-15); and / or The ratio of the area of the lithium sheet facing the negative electrode sheet to the area of the negative electrode sheet facing the lithium sheet is 1:(5-15).
7. The method for preparing a three-electrode system soft-pack battery according to any one of claims 1 to 5, characterized in that: The positive electrode material on the positive electrode sheet includes a positive electrode active material, a binder and a conductive agent, and the positive electrode active material is selected from lithium cobalt oxide.
8. The method for preparing a three-electrode system soft-pack battery according to any one of claims 1 to 5, characterized in that: The negative electrode material on the negative electrode sheet includes a negative electrode active material, a binder and a conductive agent, and the negative electrode active material is selected from graphite. 9 . A three-electrode system soft-pack battery prepared according to the method for preparing a three-electrode system soft-pack battery according to any one of claims 1 to 8 .
10. An impedance testing method for a three-electrode system soft-pack battery, characterized in that: The three-electrode system soft-pack battery is the three-electrode system soft-pack battery according to claim 9, and the impedance testing method comprises the following steps: One of the positive electrode sheet and the negative electrode sheet is electrically connected to the working electrode of the electrochemical workstation, the other is electrically connected to the counter electrode of the electrochemical workstation, and the reference electrode tab is electrically connected to the reference electrode of the electrochemical workstation, the electrochemical workstation is started, and the impedance between the working electrode and the reference electrode is tested.
Citation Information
Patent Citations
Battery cell, battery and charging method
CN113937340A
Three electrode cell fabrication kit
KR1020160133382A