A lithium ion battery positive electrode and a lithium replenishing method for a lithium ion battery
By adopting a two-layer active material layer structure in the positive electrode of lithium-ion batteries, lithium-replenishing materials with different decomposition voltages are decomposed under different voltage conditions to achieve secondary lithium replenishment, which solves the problem of battery life caused by insufficient or excessive amounts of lithium-replenishing materials. Shortens problems, extends lithium-ion battery life and improves safety.
Patent Information
- Application Number
- CN202210262302.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-26
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-01-26
AI Technical Summary
In the existing lithium-replenishing method for the positive electrode of lithium-ion batteries, too much lithium-replenishing material can easily lead to lithium precipitation in the negative electrode. If the amount of lithium-replenishing material is too small, the expected effect cannot be achieved, resulting in shortened battery life.
A two-layer active material layer structure is adopted, in which the first active material layer contains a first lithium-replenishing material, whose decomposition voltage is lower than the second lithium-replenishing material in the second active material layer. Different voltage conditions enable the two layers of materials to react at different times. Decompose to achieve secondary lithium replenishment, increase the amount of lithium replenishment materials and extend the battery life.
The design of two active material layers not only increases the amount of lithium-replenishing material, but also avoids the lithium precipitation problem caused by excessive lithium-replenishing material, prolongs the service life of lithium-ion batteries, and uses highly safe iron phosphate The lithium layer avoids the low safety problem of ternary cathode materials.
Smart Images

Figure CN114759184B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a lithium-ion battery positive electrode and a lithium replenishment method for a lithium-ion battery. Background Art
[0002] Since there is inevitable and irreversible lithium loss during the actual use of lithium batteries, it is necessary to replenish lithium at the positive or negative electrode. Commonly used lithium replenishment methods include lithium foil replenishment, lithium powder replenishment, electrochemical replenishment, and positive and negative electrode replenishment. Among them, positive electrode replenishment can directly add lithium replenishment materials during the homogenization process of the positive electrode slurry, without the need for additional process improvements and with low cost, so it is more suitable for the current lithium-ion battery manufacturing process and is hailed as the most promising lithium replenishment technology.
[0003] However, the current positive electrode lithium replenishment is usually achieved by adding lithium replenishing materials to the positive electrode and then using voltage to decompose the lithium replenishing materials to replenish the lithium-ion battery. However, this method has great defects. If the amount of lithium replenished at one time is too much, it is easy to cause lithium deposition at the negative electrode. If the amount of lithium replenished is too little, the expected effect cannot be achieved. Therefore, it is very important to know how to replenish lithium in a targeted manner. Summary of the invention
[0004] In order to solve one or more of the above-mentioned technical problems existing in the prior art, the embodiments of the present application provide a lithium-ion battery positive electrode and a lithium replenishment method for a lithium-ion battery, so as to solve the problems existing in the lithium replenishment method of the prior art that an excessive amount of lithium replenishment material may easily cause lithium deposition on the negative electrode, and an insufficient amount of lithium replenishment material may fail to achieve the expected effect.
[0005] In order to achieve the above-mentioned purpose, the technical solution adopted by this application to solve its technical problems is:
[0006] In a first aspect, the present application provides a lithium-ion battery positive electrode, comprising a stacked current collector, a first active material layer and a second active material layer, wherein the first active material layer contains a first lithium replenishing material, and the second active material layer contains a second lithium replenishing material, and the decomposition voltage of the first lithium replenishing material in the first active material layer is lower than the decomposition voltage of the second lithium replenishing material in the second active material layer.
[0007] As an embodiment, the first lithium supplement material and the second lithium supplement material are different.
[0008] As another embodiment, the first lithium supplement material and the second lithium supplement material are the same.
[0009] It is understandable that even if the lithium supplement material is of the same type, the same lithium supplement material may have different decomposition voltages by adding other materials.
[0010] Furthermore, the first lithium supplement material and / or the second lithium supplement material include metal lithium oxides, such as lithium oxide, lithium peroxide, etc.
[0011] Preferably, the metal lithium oxide includes lithium peroxide Li2O2.
[0012] Furthermore, the first active material layer contains a first positive electrode active material, the second active material layer contains a second positive electrode active material, and the first positive electrode active material is different from the second positive electrode active material.
[0013] Furthermore, the first positive electrode active material and the second positive electrode active material include oxide active materials.
[0014] Furthermore, the first positive electrode active material includes a ternary positive electrode material.
[0015] Optionally, the ternary positive electrode material includes any one of NCM532, NCM811, and NCM333, or a combination of at least two of them.
[0016] Further, the second positive electrode active material includes lithium iron phosphate, and the mass content of the lithium iron phosphate in the second positive electrode active material is greater than 95wt%. Further, the thickness of the first active material layer is greater than the thickness of the second active material layer; preferably, the thickness of the second active material layer is 10-20% of the thickness of the first active material layer.
[0017] Furthermore, the mass content of the lithium supplement material in the first active material layer is 3-5wt%.
[0018] Furthermore, the mass content of the lithium supplement material in the second active material layer is 7-11 wt %.
[0019] Furthermore, the shape of the collector includes a foil shape.
[0020] Furthermore, the current collector includes any one of aluminum, copper, nickel or zinc.
[0021] Optionally, the current collector is a single substance of aluminum, such as aluminum foil.
[0022] Furthermore, the current collector includes any one of aluminum, copper, nickel or zinc alloy.
[0023] Furthermore, the first active material layer and the second active material layer also include a binding material.
[0024] Optionally, the bonding material comprises a fluorine-containing bonding material.
[0025] Optionally, the fluorine-containing bonding material includes polyvinylidene fluoride.
[0026] Furthermore, the positive electrode active material layer also includes a conductive material.
[0027] Optionally, the conductive material includes any one of acetylene black, Ketjen black, super-P or carbon fiber, or a combination of at least two of them; the combination exemplarily includes a combination of acetylene black and Ketjen black or a combination of super-P and carbon fiber, etc.
[0028] Optionally, the conductive material is super-P.
[0029] In a second aspect, the present application further provides a method for preparing the positive electrode of the lithium ion battery according to the first aspect, the preparation method comprising:
[0030] Dissolving a first positive electrode active material, a first lithium supplement material, a binding material and a conductive material in a first preset ratio in a preset solvent to obtain a first positive electrode slurry, coating the first positive electrode slurry on a current collector and drying it to obtain a first active material layer;
[0031] Dissolving a second positive electrode active material, a second lithium supplement material, a binding material and a conductive material in a preset solvent in a second preset ratio to obtain a second positive electrode slurry, coating the second positive electrode slurry on the first active material layer and drying it to obtain a second active material layer;
[0032] Wherein, the decomposition voltage of the first lithium supplement material in the first active material layer is lower than the decomposition voltage of the second lithium supplement material in the second active material layer.
[0033] The present application has no special requirements on the mass ratio of the first positive electrode active material, the binding material and the conductive material in the first positive electrode active material layer, and it is sufficient to be within the existing material system framework and meet the mass content of the first lithium supplement material; as an illustrative example rather than a limitation on the scope of protection, the content of the first positive electrode active material is greater than 90wt%, preferably greater than 92wt%; the proportion of the binding material is less than 5wt%, preferably less than 3wt%; the proportion of the conductive material is between 3wt% and 5wt%.
[0034] The present application has no special requirements on the mass ratio of the second positive electrode active material, the binding material and the conductive material in the second positive electrode active material layer, and it is sufficient to be within the framework of the existing material system and meet the mass content of the second lithium supplement material; as an illustrative example rather than a limitation on the scope of protection, the content of the second positive electrode active material is greater than 85wt%, preferably greater than 90wt%; the proportion of the binding material is less than 5wt%, preferably less than 3wt%; the proportion of the conductive material is between 3wt% and 5wt%.
[0035] In a third aspect, the present application further provides a lithium replenishment method for a lithium ion battery comprising the lithium ion battery positive electrode according to the first aspect, wherein the lithium ion battery further comprises at least a negative electrode and a diaphragm laminate, the lithium ion battery positive electrode sequentially comprises a current collector, a first active material layer and a second active material layer arranged in a stacked manner, the first active material layer comprises a first lithium replenishment material, the second active material layer comprises a second lithium replenishment material, and the decomposition voltage of the first lithium replenishment material in the first active material layer is less than the decomposition voltage of the second lithium replenishment material in the second active material layer;
[0036] The lithium supplementation method comprises:
[0037] Charging the lithium-ion battery with a first voltage so that the first lithium-supplementing material decomposes and the lithium-ion battery is replenished with lithium for the first time;
[0038] When the capacity of the lithium-ion battery drops to a preset threshold, the lithium-ion battery is charged with a second voltage, so that the second lithium replenishing material is decomposed, and the lithium-ion battery is replenished with lithium for the second time; wherein the first voltage is less than the second voltage.
[0039] In a fourth aspect, the present application also provides a lithium-ion battery, comprising a negative electrode, a diaphragm stack and the above-mentioned lithium-ion battery positive electrode.
[0040] The beneficial effects of the technical solution provided by the embodiment of the present application are:
[0041] The lithium-ion battery positive electrode and the lithium replenishment method of the lithium-ion battery provided in the embodiments of the present application, the lithium-ion battery positive electrode includes a current collector, a first active material layer arranged on the surface of the current collector, and a second active material layer arranged on the surface of the first active material layer, the first active material layer contains a first lithium replenishment material, the second active material layer contains a second lithium replenishment material, the decomposition voltage of the first lithium replenishment material in the first active material layer is lower than the decomposition voltage of the second lithium replenishment material in the second active material layer, so that the lithium replenishment materials in the two active material layers are decomposed at different times to achieve the purpose of secondary lithium replenishment, which not only increases the amount of lithium replenishment material added, but also overcomes the problem in the prior art that too much lithium replenishment material is easily caused by negative electrode lithium precipitation, while too little lithium replenishment material cannot achieve the expected effect, thereby greatly extending the service life of the lithium-ion battery.
[0042] Furthermore, in the lithium-ion battery positive electrode and the lithium replenishment method of the lithium-ion battery provided in the embodiments of the present application, the first active material layer contains a first positive electrode active material, the second active material layer contains a second positive electrode active material, the first positive electrode active material is different from the second positive electrode active material, the first positive electrode active material includes a ternary positive electrode material, the second positive electrode active material includes lithium iron phosphate, and the lithium replenishment material includes lithium peroxide. By arranging a ternary material with high capacity but low safety in the first active material layer close to the current collector side, it is known that the NCM ternary material has a catalytic effect on the decomposition of Li2O2, and the decomposition of Li2O2 can be achieved at a lower voltage to complete the lithium replenishment process; lithium iron phosphate with higher safety is arranged in the second active material layer close to the negative electrode, and lithium replenishment material is arranged in each active material layer Li2O2, utilizing the high decomposition voltage of Li2O2, the Li2O2 in the second active material layer containing lithium iron phosphate will not decompose during the formation and general circulation process, but because the ternary positive electrode material NCM has a catalytic effect on Li2O2, the decomposition voltage of Li2O2 in the first active material layer containing the ternary positive electrode material is reduced. Therefore, in the formation stage, the Li2O2 in the first active material layer is completely decomposed, and the first lithium replenishment of the battery is achieved. As the battery is recycled, the battery capacity decreases. When it is reduced to a certain threshold (such as when it drops to 90% for the first time, etc.), high voltage charging is used to decompose the Li2O2 in the second positive electrode active material layer to complete the second lithium replenishment, thereby extending the battery life. In addition, the second active material layer adopts a highly safe lithium iron phosphate layer, which avoids the problem of low safety of the ternary positive electrode material.
[0043] Not all products in this application need to have all the above effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0045] Figure 1 is a schematic structural diagram of a positive electrode of a lithium-ion battery provided in an embodiment of the present application;
[0046] Figure 2 It is a flow chart of a method for preparing a positive electrode of a lithium-ion battery provided in an embodiment of the present application;
[0047] Figure 3 It is a flow chart of a lithium replenishment method for a lithium-ion battery provided in an embodiment of the present application. DETAILED DESCRIPTION
[0048] In order to make the purpose, technical solutions and advantages of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below in conjunction with the drawings in the embodiments of this application. Obviously, the described embodiments are only part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0049] As described in the background art, the prior art method of replenishing lithium at the positive electrode is usually to replenish lithium once, which has the problems of easily causing lithium deposition at the negative electrode if the amount of lithium replenished is too much, and failing to achieve the expected effect if the amount of lithium replenished is too little.
[0050] In order to solve one or more of the above problems, the present application creatively proposes a new lithium-ion battery positive electrode, by arranging two layers of active material layers on the surface of the current collector, a lithium-replenishing material is arranged in each active material layer, and the decomposition voltage of the lithium-replenishing material in the first active material layer is different from the decomposition voltage in the second active material layer, so that the lithium-replenishing material in the two active material layers is decomposed at different times to achieve the purpose of secondary lithium replenishment, which not only increases the amount of lithium-replenishing material added, but also overcomes the problem in the prior art that too much lithium-replenishing material is easily caused by lithium precipitation at the negative electrode, while too little lithium-replenishing material cannot achieve the expected effect, thereby greatly extending the service life of the lithium-ion battery.
[0051] The solution provided by the embodiments of the present application is described in detail below with reference to the accompanying drawings.
[0052] Figure 1 is a schematic diagram of the structure of the positive electrode of a lithium-ion battery provided in an embodiment of the present application, referring to Figure 1 As shown, the lithium-ion battery positive electrode provided in the embodiment of the present application at least includes a current collector 1 and an active material layer arranged on the surface of the current collector 1. The current collector includes but is not limited to aluminum foil and the like. Among them, in the embodiment of the present application, the active material layer includes at least a two-layer structure of a first active material layer 2 and a second active material layer 3. The first active material layer 2 is directly arranged on the surface of the current collector and contacts the surface of the current collector 1, and the second active material layer 3 is arranged on the surface of the first active material layer 2, that is, the first active material layer 2 is arranged between the current collector 1 and the second active material layer 3. The first active material layer 2 contains a first lithium supplement material, the second active material layer 3 contains a second lithium supplement material, and the decomposition voltage of the first lithium supplement material in the first active material layer is set to be less than the decomposition voltage of the second lithium supplement material in the second active material layer.
[0053] Specifically, the lithium-ion battery positive electrode described in the present application adopts the above-mentioned structure and composition, so that the first lithium replenishing material in the first active material layer decomposes under relatively low voltage conditions (such as during formation and general circulation), thereby realizing the first lithium replenishment of the battery. As the battery is recycled, the battery capacity decreases. At this time, a higher voltage (such as high-voltage charging) is used to make the voltage reach the decomposition voltage of the second lithium replenishing material in the second active material layer, thereby causing the second lithium replenishing material in the second active material layer to decompose and complete the second lithium replenishment. This not only increases the amount of lithium replenishment and extends the battery life, but also avoids the problem of lithium precipitation caused by excessive lithium replenishing material.
[0054] The following are optional technical solutions for this application, but are not intended to limit the technical solutions provided in this application. Through the following optional technical solutions, the technical objectives and beneficial effects of this application can be better achieved and realized.
[0055] As a preferred implementation, in the embodiment of the present application, the first lithium supplement material and / or the second lithium supplement material includes metal lithium oxide, such as lithium oxide, lithium peroxide, etc. Preferably, the metal lithium oxide includes lithium peroxide.
[0056] Specifically, the lithium replenishing material usually adopts metallic lithium oxide. Since the decomposition voltage of lithium peroxide can be as high as 4.8V under normal circumstances, in the embodiment of the present application, as a preferred implementation method, the first lithium replenishing material and the second lithium replenishing material both adopt lithium peroxide, utilizing its higher decomposition voltage and arranging different positive electrode active materials in different active material layers, so that the decomposition voltages of lithium peroxide in the two active material layers are different.
[0057] As a preferred implementation, in the embodiment of the present application, the first active material layer contains a first positive electrode active material, the second active material layer contains a second positive electrode active material, and the first positive electrode active material is different from the second positive electrode active material.
[0058] Specifically, in the present application, different positive electrode active materials are arranged in two different active material layers, and the characteristics of the positive electrode active materials themselves are utilized to make the decomposition voltage of the lithium replenishing material in the first active material layer lower than the decomposition voltage in the second active material layer, thereby achieving the decomposition of the lithium replenishing materials in the two active material layers under different voltage conditions, and realizing secondary lithium replenishment. It should be noted here that the present application does not limit the specific implementation method of the different decomposition voltages of the lithium replenishing materials in the two active material layers. In addition to the above-mentioned method, without violating the inventive concept of the present application, it can also be set according to actual needs to achieve different decomposition voltages of the lithium replenishing materials in the two active material layers.
[0059] As a preferred implementation manner, in the embodiment of the present application, the positive electrode active material includes an oxide active material.
[0060] As a preferred implementation manner, in the embodiment of the present application, the first positive electrode active material includes a ternary positive electrode material.
[0061] Specifically, ternary materials refer to materials composed of three chemical components (elements), components (single substances and compounds) or parts (parts), including alloys, inorganic non-metallic materials, organic materials, polymer composite materials, etc., which are widely used in mineral extraction, metal smelting, materials processing, new energy and other industries.
[0062] Optionally, the ternary cathode material includes lithium nickel cobalt manganese oxide, which is a key ternary cathode material for lithium-ion batteries and has a higher specific capacity and lower cost than unit cathode materials. Lithium nickel cobalt manganese oxide has the characteristics of high energy density, good cycle performance, high voltage platform, good thermal stability, etc., and it replaces more than two-thirds of the cobalt in lithium cobalt oxide with relatively cheap nickel and manganese, and has a very obvious cost advantage. Compared with other lithium-ion battery cathode materials such as lithium manganese oxide and lithium iron phosphate, lithium nickel cobalt manganese oxide material and lithium cobalt oxide are very close in electrochemical properties and processing properties, making lithium nickel cobalt manganese oxide material a new battery material and gradually replacing lithium cobalt oxide.
[0063] Optionally, the ternary positive electrode material includes any one of NCM532, NCM811, and NCM333, or a combination of at least two of them.
[0064] As a preferred implementation, in the embodiment of the present application, the second positive electrode active material includes lithium iron phosphate.
[0065] Specifically, although the ternary positive electrode material has advantages such as high capacity, it also has the defect of low safety, and lithium iron phosphate has the characteristic of high safety. Therefore, the ternary positive electrode material is arranged as the first positive electrode active material in the first active material layer close to the current collector side, and the lithium iron phosphate is arranged as the second positive electrode active material in the second active material layer close to the negative electrode side. Since the decomposition voltage of lithium peroxide is high, the lithium peroxide in the second active material layer provided with lithium iron phosphate will not decompose during the formation and general circulation process. However, since the ternary positive electrode material has a catalytic effect on lithium peroxide, the second active material layer provided with the ternary positive electrode material The decomposition voltage of lithium peroxide is reduced, therefore, in the formation stage, the lithium peroxide in the second active material layer will be completely decomposed, realizing the first lithium replenishment of the battery. As the battery is recycled, the battery capacity decreases. When it decreases to a certain threshold (such as when the battery capacity drops to 90% for the first time), high-voltage charging is used to decompose the lithium peroxide in the second active material layer to realize the second lithium replenishment. This not only increases the amount of lithium replenishment material added and extends the battery life, but also overcomes the lithium precipitation problem caused by excessive lithium replenishment material in the prior art. In addition, the second active material layer uses highly safe lithium iron phosphate, which avoids the problem of low safety of the ternary positive electrode material.
[0066] As a preferred implementation, in the embodiment of the present application, the thickness of the first active material layer is greater than the thickness of the second active material layer; preferably, the thickness of the second active material layer is 10-20% of the thickness of the first active material layer.
[0067] Specifically, considering the influence of the electrochemical properties and mechanical properties of the battery, optionally, the thickness of the first active material layer can be 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20% of the thickness of the second active material layer.
[0068] As a preferred implementation, in the embodiment of the present application, the mass content of the lithium supplement material in the first active material layer is 3-5wt%.
[0069] Specifically, the mass content of the lithium-replenishing material in the first active material layer can be adjusted according to the actual formula system. Optionally, the mass content of the lithium-replenishing material in the first active material layer can be 3wt%, 3.2wt%, 3.4wt%, 3.6wt%, 3.8wt%, 4wt%, 4.2wt%, 4.4wt%, 4.6wt%, 4.8wt% or 5wt%, etc.
[0070] As a preferred implementation, in the embodiment of the present application, the mass content of the lithium supplement material in the second active material layer is 7-11 wt %.
[0071] Specifically, the mass content of the lithium-replenishing material in the second active material layer can also be adjusted according to the actual formula system. Optionally, the mass content of the lithium-replenishing material in the second active material layer can be 7wt%, 7.5wt%, 8wt%, 8.5wt%, 9wt%, 9.5wt%, 10wt%, 10.5wt% or 11wt%, etc.
[0072] As a preferred implementation manner, in the embodiments of the present application, the shape of the collector includes a foil shape.
[0073] As a preferred implementation, in the embodiment of the present application, the collector includes any one of aluminum, copper, nickel or zinc.
[0074] Optionally, the current collector is a single substance of aluminum, such as aluminum foil.
[0075] As a preferred implementation manner, in the embodiments of the present application, the collector includes any one of aluminum, copper, nickel or zinc alloy.
[0076] As a preferred implementation manner, in the embodiment of the present application, the first active material layer and the second active material layer also include a bonding material.
[0077] Optionally, the bonding material comprises a fluorine-containing bonding material.
[0078] Optionally, the fluorine-containing bonding material includes polyvinylidene fluoride.
[0079] As a preferred implementation, in the embodiment of the present application, the positive electrode active material layer also includes a conductive material.
[0080] Optionally, the conductive material includes any one of acetylene black, Ketjen black, super-P or carbon fiber, or a combination of at least two of them; the combination exemplarily includes a combination of acetylene black and Ketjen black or a combination of super-P and carbon fiber, etc.
[0081] In the present application, conductive materials are added to the first active material layer and the second active material layer, which can significantly improve the conductivity of the first active material layer and the second active material layer, thereby improving the performance of the battery.
[0082] As an embodiment, the binding material and the conductive material in the first active material layer are the same as those in the second active material layer;
[0083] As another embodiment, the binding material and the conductive material in the first active material layer are different from those in the second active material layer.
[0084] Figure 2is a flow chart of the method for preparing the positive electrode of a lithium-ion battery provided in the embodiment of the present application, with reference to Figure 2 As shown, the present application embodiment also provides a method for preparing the above-mentioned lithium ion battery positive electrode, the preparation method comprising:
[0085] S101: dissolving a first positive electrode active material, a first lithium supplement material, a binding material and a conductive material in a first preset ratio in a preset solvent to obtain a first positive electrode slurry, coating the first positive electrode slurry on a current collector and drying it to obtain a first active material layer;
[0086] S102: dissolving a second positive electrode active material, a second lithium supplement material, a binding material and a conductive material in a preset solvent in a second preset ratio to obtain a second positive electrode slurry, coating the second positive electrode slurry on the first active material layer and drying it to obtain a second active material layer;
[0087] Wherein, the decomposition voltage of the first lithium supplement material in the first active material layer is lower than the decomposition voltage of the second lithium supplement material in the second active material layer.
[0088] The present application has no special requirements on the mass ratio of the first positive electrode active material, the binding material and the conductive material in the first positive electrode active material layer, and it is sufficient to be within the existing material system framework and meet the mass content of the first lithium supplement material; as an illustrative example rather than a limitation on the scope of protection, the content of the first positive electrode active material is greater than 90wt%, preferably greater than 92wt%; the proportion of the binding material is less than 5wt%, preferably less than 3wt%; the proportion of the conductive material is between 3wt% and 5wt%.
[0089] The present application has no special requirements for the mass ratio of the second positive electrode active material, the binding material and the conductive material in the second positive electrode active material layer, and it is sufficient to be within the existing material system framework and meet the mass content of the second lithium supplement material; as an illustrative example rather than a limitation on the scope of protection, the content of the first positive electrode active material is greater than 85wt%, preferably greater than 90wt%; the proportion of the binding material is less than 5wt%, preferably less than 3wt%; the proportion of the conductive material is between 3wt% and 5wt%.
[0090] Specifically, in the embodiment of the present application, the first preset ratio and the second preset ratio are not specifically limited, and can be set according to actual needs without violating the inventive concept of the present application. The preset solvent includes but is not limited to N-methylpyrrolidone (NMP) and the like.
[0091] Figure 3 is a flow chart of a lithium replenishment method for a lithium-ion battery provided in an embodiment of the present application, referring to Figure 3As shown, the embodiment of the present application also provides a lithium replenishment method for a lithium ion battery, wherein the lithium ion battery comprises at least a lithium ion battery positive electrode, a negative electrode and a diaphragm laminate, wherein the lithium ion battery positive electrode comprises a current collector, a first active material layer and a second active material layer which are stacked in sequence, wherein the first active material layer comprises a first lithium replenishment material, and the second active material layer comprises a second lithium replenishment material, wherein the decomposition voltage of the first lithium replenishment material in the first active material layer is less than the decomposition voltage of the second lithium replenishment material in the second active material layer, and the lithium replenishment method comprises:
[0092] S201: charging the lithium-ion battery using a first voltage so that the first lithium replenishing material is decomposed, thereby replenishing lithium for the lithium-ion battery for the first time;
[0093] S202: When the capacity of the lithium-ion battery drops to a preset threshold, the lithium-ion battery is charged with a second voltage, so that the second lithium replenishing material is decomposed, and the lithium-ion battery is replenished with lithium for the second time;
[0094] Wherein, the first voltage is smaller than the second voltage.
[0095] It should be noted here that the lithium replenishment method for the lithium ion battery provided in the present application is based on the positive electrode of the above-mentioned lithium ion battery. The contents of the lithium replenishment method for the lithium ion battery that are the same or similar to the positive electrode of the above-mentioned lithium ion battery can be referred to the above introduction and will not be repeated later.
[0096] The present application also provides a lithium-ion battery, including a negative electrode, a diaphragm laminate and the positive electrode of the lithium-ion battery. The same or similar contents of the positive electrode of the lithium-ion battery can be referred to the above introduction, and will not be repeated in the following.
[0097] As a preferred implementation, in the embodiment of the present application, the negative electrode includes a negative electrode collector and a negative electrode active material layer disposed on the negative electrode collector.
[0098] As a preferred implementation manner, in the embodiments of the present application, the shape of the negative electrode collector includes a foil shape.
[0099] Optionally, the negative electrode current collector includes any one of aluminum, copper, nickel or zinc.
[0100] Optionally, the negative electrode current collector is a single substance of copper, such as copper foil.
[0101] Optionally, the negative electrode current collector includes any one of aluminum, copper, nickel or zinc alloy.
[0102] As a preferred implementation manner, in the embodiment of the present application, the negative electrode active material layer includes a negative electrode active material.
[0103] Optionally, the negative electrode active material includes any one of a metal active material, a carbon active material or an oxide active material, or a combination of at least two of the above. The combination exemplarily includes a combination of a metal active material and a carbon active material, a combination of an oxide active material and a metal active material, or a combination of a carbon active material and an oxide active material.
[0104] Optionally, the metal active material includes any one of Si, Sn, In, Si-Al alloy or Si-In alloy, or a combination of at least two thereof.
[0105] Optionally, the carbon active material includes any one of graphite, hard carbon or soft carbon, or a combination of at least two of them; the combination exemplarily includes a combination of graphite and hard carbon, a combination of graphite and soft carbon, or a combination of hard carbon and soft carbon, etc.
[0106] Optionally, the oxide active material includes Li4Ti5O 12 .
[0107] As a preferred implementation manner, in the embodiment of the present application, the negative electrode active material layer also includes a negative electrode binding material.
[0108] Optionally, the negative electrode binding material includes CMC+SBR.
[0109] As a preferred implementation, in the embodiment of the present application, the negative electrode active material layer also includes a conductive material.
[0110] Optionally, the conductive material includes any one of acetylene black, Ketjen black, super-P or carbon fiber, or a combination of at least two of them; the combination exemplarily includes a combination of acetylene black and Ketjen black or a combination of super-P and carbon fiber, etc.
[0111] In the present application, a conductive material is added to the negative electrode active material layer, which can significantly improve the conductivity of the negative electrode active material layer, thereby improving the performance of the battery.
[0112] Example 1
[0113] A lithium-ion battery is provided in an embodiment of the present application, which includes a negative electrode, a diaphragm stack and a positive electrode of the lithium-ion battery, wherein the positive electrode of the lithium-ion battery includes a current collector and an active material layer arranged on the surface of the current collector, the active material layer at least includes a first active material layer in contact with the surface of the current collector and a second active material layer arranged on the surface of the first active material layer, the first active material layer contains a first lithium-replenishing material, the second active material layer contains a second lithium-replenishing material, and the decomposition voltage of the first lithium-replenishing material in the first active material layer is lower than the decomposition voltage of the second lithium-replenishing material in the second active material layer.
[0114] Specifically, the preparation process of lithium-ion batteries is as follows:
[0115] NCM532, Li2O2, PVDF and SUPER-P are mixed in a mass ratio of 90:5:2:3, dissolved in NMP to obtain a first positive electrode slurry, and the first positive electrode slurry is coated on an aluminum foil and dried to obtain a first active material layer;
[0116] LiFePO4, Li2O2, PVDF and SUPER-P are mixed in a mass ratio of 88:8:2:2, dissolved in NMP to obtain a second positive electrode slurry, and the second positive electrode slurry is coated on the first active material layer and dried to obtain a lithium ion battery positive electrode sheet;
[0117] Graphite, (CMC+SBR) and super-P are dissolved in NMP in a ratio of 95:2:3 to obtain a negative electrode slurry, and the negative electrode slurry is coated on a copper foil and dried to obtain a negative electrode sheet;
[0118] The positive electrode sheet, the negative electrode sheet, and the diaphragm are stacked, and then injected and formed to obtain a lithium-ion battery. The formation process is as follows:
[0119] The lithium-ion battery was charged using a battery charging and discharging cabinet. The battery was charged to 3.6V at a constant current of 0.05C and to 4.0V at a constant current of 0.02C.
[0120] Battery cycle performance test:
[0121] At room temperature (temperature: 25℃±2℃)
[0122] S101: Charge to the final voltage with a charging current of 1C, a cut-off current of 0.05C, and let stand for 30 minutes;
[0123] S102: Discharge at 1C to the final discharge voltage, record the discharge capacity, and let stand for 30 minutes;
[0124] S101-S102 is cyclically executed until the discharge capacity decreases to 90% of the initial discharge capacity, and the charge cut-off voltage of the next cycle is increased to 4.1V. After one charge and discharge cycle, S101-S102 is repeated again until the discharge capacity decreases to 90% of the initial discharge capacity again. The experiment is terminated and the final number of cycles is recorded.
[0125] Example 2
[0126] The difference from Example 1 is that the preparation process of the lithium ion battery is as follows:
[0127] NCM811, Li2O2, PVDF and SUPER-P are mixed in a mass ratio of 92:3:2:3, dissolved in NMP to obtain a first positive electrode slurry, and the first positive electrode slurry is coated on an aluminum foil and dried to obtain a first active material layer;
[0128] LiFePO4, Li2O2, PVDF and SUPER-P are mixed in a mass ratio of 89:7:2:2, dissolved in NMP to obtain a second positive electrode slurry, and the second positive electrode slurry is coated on the first active material layer and dried to obtain a lithium-ion battery positive electrode sheet;
[0129] Graphite, (CMC+SBR) and super-P are dissolved in NMP in a ratio of 95:2:3 to obtain a negative electrode slurry, and the negative electrode slurry is coated on a copper foil and dried to obtain a negative electrode sheet;
[0130] The positive electrode sheet, the negative electrode sheet, and the diaphragm are stacked and injected with liquid to form a lithium-ion battery. The formation process is as follows:
[0131] The lithium-ion battery was charged using a battery charging and discharging cabinet. The battery was charged to 3.7V at 0.05C constant current and to 4.0V at 0.02C constant current.
[0132] The battery cycle performance test process in this embodiment is different from that in embodiment 1 in that:
[0133] S101-S102 is cyclically executed until the discharge capacity decreases to 90% of the initial discharge capacity, and the charge cut-off voltage of the next cycle is increased to 4.15V. After one charge and discharge cycle, S101-S102 is repeated again until the discharge capacity decreases to 90% of the initial discharge capacity again. The experiment is terminated and the final number of cycles is recorded.
[0134] Example 3
[0135] The difference from Example 1 is that the preparation process of the lithium ion battery is as follows:
[0136] NCM333, Li2O2, PVDF and SUPER-P are mixed in a mass ratio of 92:4:2:2, dissolved in NMP to obtain a first positive electrode slurry, and the first positive electrode slurry is coated on an aluminum foil and dried to obtain a first active material layer;
[0137] LiFePO4, Li2O2, PVDF and SUPER-P are mixed in a mass ratio of 87:9:2:2, dissolved in NMP to obtain a second positive electrode slurry, and the second positive electrode slurry is coated on the first active material layer and dried to obtain a lithium-ion battery positive electrode sheet;
[0138] Graphite, (CMC+SBR) and super-P are dissolved in NMP in a ratio of 95:2:3 to obtain a negative electrode slurry, which is then coated on a copper foil and dried to obtain a negative electrode sheet;
[0139] The positive electrode sheet, the negative electrode sheet, and the diaphragm stack are injected with liquid to form a lithium-ion battery, wherein the formation process is as follows:
[0140] The lithium-ion battery was charged using a battery charging and discharging cabinet. The battery was charged to 3.65V at a constant current of 0.05C and to 4.0V at a constant current of 0.02C.
[0141] The battery cycle performance test process in this embodiment is different from that in embodiment 1 in that
[0142] S101-S102 is cyclically executed until the discharge capacity decreases to 90% of the initial discharge capacity, and the charge cut-off voltage of the next cycle is increased to 4.2V. After one charge and discharge cycle, S101-S102 is repeated again until the discharge capacity decreases to 90% of the initial discharge capacity again. The experiment is terminated and the final number of cycles is recorded.
[0143] Comparative Example 1
[0144] The difference from Example 1 is that the preparation process of the lithium ion battery is as follows:
[0145] NCM532, Li2O2, PVDF and SUPER-P are mixed in a mass ratio of 90:5:2:3, dissolved in NMP to obtain a first positive electrode slurry, and the first positive electrode slurry is coated on an aluminum foil and dried to obtain a positive electrode sheet;
[0146] Graphite, (CMC+SBR) and super-P were dissolved in NMP in a mass ratio of 95:2:3 to obtain a negative electrode slurry, which was coated on a copper foil and dried to obtain a negative electrode sheet;
[0147] The positive electrode sheet, negative electrode sheet and diaphragm are stacked and injected with liquid to obtain a lithium-ion battery.
[0148] The battery cycle performance test process in this embodiment is different from that in embodiment 1 in that
[0149] The cycle of S101 to S102 is performed until the discharge capacity decreases to 90% of the initial discharge capacity, the experiment is terminated, and the final number of cycles is recorded.
[0150] Comparative Example 2
[0151] The difference from Example 1 is that the preparation process of the lithium ion battery is as follows:
[0152] NCM532, Li2O2, PVDF and SUPER-P are mixed in a mass ratio of 89:7:2:2, dissolved in NMP to obtain a first positive electrode slurry, and the first positive electrode slurry is coated on an aluminum foil and dried to obtain a positive electrode sheet;
[0153] Graphite, (CMC+SBR) and super-P are dissolved in NMP in a ratio of 95:2:3 to obtain a negative electrode slurry, which is then coated on a copper foil and dried to obtain a negative electrode sheet;
[0154] The positive electrode sheet, negative electrode sheet and diaphragm are stacked and injected with liquid to obtain a lithium-ion battery.
[0155] The battery cycle performance test process in this embodiment is different from that in embodiment 1 in that:
[0156] The cycle of S101 to S102 is performed until the discharge capacity decreases to 90% of the initial discharge capacity, the experiment is terminated, and the final number of cycles is recorded.
[0157] It should be noted that in the embodiments of the present application, in addition to the above-mentioned battery cycle performance test, the present application also includes a needle puncture test and a lithium precipitation test. The needle puncture test process is as follows:
[0158] Fully charge with standard charging method;
[0159] Use a φ5mm~φ8mm high temperature resistant steel needle (the cone angle of the needle tip is 45°~60°, the surface of the needle is smooth, free of rust, oxide layer and oil), penetrate the battery cell plate in a direction perpendicular to the battery cell plate at a speed of (25±5)mm / s, the penetration position should be close to the geometric center of the pierced surface, and the steel needle stays in the battery cell;
[0160] Observe for 1 hour.
[0161] Record battery safety level
[0162] The lithium analysis test process is as follows:
[0163] The lithium-ion batteries prepared in the above embodiments and comparative examples were charged at a rate of 5C and discharged at a rate of 0.5C for 20 cycles, and then the lithium-ion batteries were dissected to check the lithium deposition.
[0164] The test results are as follows:
[0165] First cycle number Second cycle number Whether it has lithium deposition acupuncture Example 1 901 1100 no pass Example 2 880 932 no pass Example 3 1006 1212 no pass Comparative Example 1 982 / no no Comparative Example 2 935 / have no
[0166] It can be seen from the test results that the lithium-ion battery provided by the present application is provided with two layers of active material layers, each layer of active material layer is provided with lithium supplement material Li2O2, a ternary positive electrode material with high capacity but low safety is provided in the first active material layer close to the current collector, and a lithium iron phosphate with high safety is provided in the second active material layer close to the negative electrode layer, so that the service life of the lithium-ion battery is extended, and the acupuncture test with the most stringent safety requirements is passed. This is because the decomposition voltage of Li2O2 is high, and the Li2O2 in the lithium iron phosphate layer will not decompose during the formation and general circulation process, but because the ternary positive electrode material NCM has a catalytic effect on Li2O2, the decomposition voltage of Li2O2 in the first active material layer is reduced. Therefore, in the formation stage, the Li2O2 in the first active material layer is decomposed to achieve the first lithium supplement of the battery. As the battery is used in a cycle, the battery capacity decreases. When the first reduction is to 90%, high voltage charging is used to decompose the Li2O2 in the second active material layer to complete the second lithium supplement, thereby extending the battery life.
[0167] In the description of the present application, it should be understood that the terms "vertical", "parallel", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. In addition, the terms "first" and "second" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present application, unless otherwise specified, "multiple" means two or more.
[0168] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A positive electrode for a lithium-ion battery, characterized in that: The positive electrode of the lithium-ion battery includes a current collector, a first active material layer and a second active material layer which are stacked in sequence, the first active material layer contains a first lithium supplement material, the second active material layer contains a second lithium supplement material, the first active material layer contains a first positive electrode active material, the second active material layer contains a second positive electrode active material, and the first positive electrode active material is different from the second positive electrode active material; By utilizing the characteristics of the positive electrode active material itself, the decomposition voltage of the first lithium supplement material in the first active material layer is made lower than the decomposition voltage of the second lithium supplement material in the second active material layer.
2. The lithium ion battery positive electrode according to claim 1, characterized in that The first positive electrode active material includes a ternary positive electrode material; The second positive electrode active material includes lithium iron phosphate, and the mass content of the lithium iron phosphate in the second positive electrode active material is greater than 95wt%.
3. The lithium ion battery positive electrode according to claim 1, characterized in that The first lithium supplement material and / or the second lithium supplement material includes metal lithium oxide.
4. The lithium ion battery positive electrode according to claim 3, characterized in that The metal lithium oxide is Li2O2.
5. The lithium ion battery positive electrode according to any one of claims 1 to 4, characterized in that: The mass content of the first lithium supplementing material in the first active material layer is 3-5wt%.
6. The lithium ion battery positive electrode according to any one of claims 1 to 4, characterized in that: The mass content of the second lithium supplementing material in the second active material layer is 7-11 wt %.
7. The lithium ion battery positive electrode according to any one of claims 1 to 4, characterized in that: The thickness of the first active material layer is greater than the thickness of the second active material layer.
8. The lithium ion battery positive electrode according to claim 7, characterized in that The thickness of the second active material layer is 10-20% of the thickness of the first active material layer.
9. The lithium ion battery positive electrode according to claim 1, characterized in that: The first lithium supplement material and the second lithium supplement material are the same or different.
10. A method for replenishing lithium of a lithium ion battery comprising the lithium ion battery positive electrode according to any one of claims 1 to 9, characterized in that: The steps include: Charging the lithium-ion battery with a first voltage so that the first lithium-supplementing material decomposes and the lithium-ion battery is replenished with lithium for the first time; When the capacity of the lithium-ion battery drops to a preset threshold, the lithium-ion battery is charged with a second voltage, so that the second lithium replenishing material is decomposed, and the lithium-ion battery is replenished with lithium for the second time; The characteristics of the positive electrode active material are utilized to ensure that the decomposition voltage of the first lithium supplement material in the first active material layer is lower than the decomposition voltage of the second lithium supplement material in the second active material layer, and the first voltage is lower than the second voltage.
Citation Information
Patent Citations
All-solid-state lithium ion battery
CN111740153A
Pole piece and preparation method thereof
CN112838190A
Electrochemical device and electronic device
CN113078288A
Lithium supplement method for lithium ion battery
CN113540591A
Positive electrode for lithium ion secondary battery, and lithium ion secondary battery
JP2016178070A