Silicon wafer cleaning method and battery

Through a three-step cleaning method, including first water washing, chemical cleaning and second water washing, combined with ultrasonic and pulling cleaning, the problem of removing dust and particles on the surface of coated silicon wafers is solved, the conductive properties are maintained, and the battery performance and preparation efficiency are improved.

CN114783857BActive Publication Date: 2024-10-11TONGWEI SOLAR (JINTANG) CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210358935.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-07
Publication Date
2024-10-11
Estimated Expiration
2042-04-07

AI Technical Summary

Technical Problem

In traditional heterojunction battery preparation technology, it is difficult to efficiently remove dust and particles from the surface of coated silicon wafers, resulting in reduced battery performance and low preparation efficiency. Existing cleaning methods cannot be accurately controlled and can easily damage silicon wafers or cause secondary pollution.

Method used

Adopt a three-step cleaning method: first water washing, chemical cleaning and second water washing, use acid or alkali solution to corrode to remove closely adhered dust and particles, combine with ultrasonic and pull-up cleaning, control concentration, temperature and time to ensure conductive performance of maintenance.

Benefits of technology

Efficiently remove dust and particles on the surface of coated silicon wafers to avoid damage to battery performance, extend the service life of screen printing, and reduce preparation costs and losses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114783857B_ABST
    Figure CN114783857B_ABST
Patent Text Reader

Abstract

The present invention relates to a silicon wafer cleaning method and a battery. In the silicon wafer cleaning method, the silicon wafer is sequentially subjected to a first water wash, a chemical wash, a second water wash and a pulling wash to obtain a cleaned silicon wafer; the reagent used in the chemical wash is an alkali solution or an acid solution, the mass concentration of the acid solution is 0.4% to 5%, the components of the acid solution include HF, and the mass concentration of the alkali solution is 0.3% to 0.9%; the temperature of the chemical wash step is 20°C to 30°C, and the time is 100s to 300s; the silicon wafer includes a silicon substrate and a transparent conductive film coated on the surface of the silicon substrate. The silicon wafer cleaning method can efficiently remove dust or particles attached to the surface of the coated silicon wafer without damaging the coated silicon wafer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a silicon wafer cleaning method and a battery. Background Art

[0002] HJT cell is short for heterojunction cell. Compared with the currently used PERC cell, HJT cell has higher improvement potential, lower temperature coefficient and low photoinduced degradation, high stability, and the HJT process preparation flow is relatively simplified. It uses N-type single crystal silicon wafer as substrate, and goes through four steps including texturing, amorphous silicon thin film deposition, metal oxide conductive layer TCO preparation, and screen printing to produce positive and negative electrodes for current extraction. The process is simple.

[0003] In the traditional preparation technology of heterojunction batteries, the PVD process is generally used to prepare the metal oxide conductive layer TCO. PVD refers to the technology of using physical methods to vaporize solid or liquid raw material sources into gaseous atoms or molecules, or partially ionize them into ions under vacuum conditions, and deposit a thin film with certain special functions on the surface of the substrate through a low-pressure gas or plasma process. Raw material dust and particles will inevitably be generated during the PVD process.

[0004] Therefore, the existing technology still needs to be improved. Summary of the invention

[0005] Based on this, the present invention provides a silicon wafer cleaning method and a battery, wherein the silicon wafer cleaning method can efficiently remove dust or particles attached to the surface of the coated silicon wafer without damaging the coated silicon wafer.

[0006] One aspect of the present invention provides a silicon wafer cleaning method, comprising the following steps:

[0007] The silicon wafer is sequentially subjected to a first water wash, a chemical wash, and a second water wash to obtain a cleaned silicon wafer;

[0008] The chemical cleaning agent is alkaline solution or acid solution, the mass concentration of the acid solution is 0.4% to 5%, and the components of the acid solution include HF; the mass concentration of the alkaline solution is 0.3% to 0.9%;

[0009] The temperature of the chemical cleaning step is 20°C to 30°C, and the time is 100s to 300s;

[0010] The silicon wafer comprises a silicon substrate and a transparent conductive film coated on the surface of the silicon substrate.

[0011] In some embodiments, the first water washing step is performed under ultrasonic conditions, and the frequency of the ultrasound is 1 KHz to 2.4 KHz.

[0012] In some of the embodiments, in the pulling and cleaning step, the pulling speed is controlled to be 3 mm / s to 5 mm / s.

[0013] In some embodiments, the temperature of the pulling and cleaning is 55°C to 80°C.

[0014] In some embodiments, the temperature of the first water washing step is 20° C. to 30° C., and the time is 100 s to 300 s.

[0015] In some embodiments, the temperature of the second water washing step is 20° C. to 30° C., and the time is 100 s to 300 s.

[0016] In some embodiments, the acid solution further comprises HCl.

[0017] In some embodiments, the alkali in the alkali solution is selected from alkali metal hydroxides.

[0018] In some embodiments, the transparent conductive film is prepared by physical vapor deposition.

[0019] Another aspect of the present invention provides a battery, wherein the battery comprises a silicon wafer produced by the silicon wafer cleaning method as described above.

[0020] In the above silicon wafer cleaning method, the silicon wafer is sequentially subjected to a first water wash, a chemical wash, a second water wash and a lifting wash. The first water wash removes most of the loosely adhered dust and particles on the surface of the silicon wafer. Acid or alkali solution is further used for chemical washing. The acid or alkali solution reacts with the dust and particles, thereby corroding the tightly adhered dust or particles on the surface of the silicon wafer. At the same time, by controlling the components and concentrations of the acid or alkali solution, and controlling the temperature and time of the chemical washing step, the acid or alkali solution corrodes the tightly adhered dust or particles on the surface of the silicon wafer without damaging the silicon substrate and the transparent conductive film on its surface. Then, a second water wash and a lifting wash are performed to wash away the residual acid or alkali solution and the residual dust particles. In this way, while efficiently removing the dust or particles attached to the surface of the silicon wafer, the coated silicon wafer is not damaged, so that the original conductive properties are maintained.

[0021] Among them, when acid solution is used for chemical cleaning, HF can remove SiO2 on the surface of the silicon wafer. SiO2 has polar bonds and is hydrophilic. After HF can remove SiO2 on the surface of the coated silicon wafer, the surface of the silicon wafer becomes hydrophobic, making the surface of the coated silicon wafer dehydrated in the subsequent second water washing step, thereby reducing the watermark on the coated silicon wafer after cleaning.

[0022] Furthermore, the first water washing step is carried out under ultrasonic conditions, and the frequency of the ultrasound is controlled to be 1KHz to 2.4KHz. Under the action of ultrasound of a specific frequency, the dust and particles on the surface of the coated silicon wafer are promoted to separate from the coated silicon wafer. While further promoting the removal of dust and particles, the silicon substrate and the transparent conductive film on its surface are not damaged, so that the original conductive properties are maintained.

[0023] Furthermore, in the step of pulling and cleaning, the pulling speed is controlled to be 3mm / s to 5mm / s, and the silicon wafer is slowly pulled and cleaned to gradually detach the washing liquid attached to the surface of the silicon wafer, thereby reducing the washing liquid attached to the surface of the coated silicon wafer after washing. While reducing the watermark on the coated silicon wafer after cleaning, it further avoids the dust or particles carried in the washing liquid from re-attaching to the coated silicon wafer, further improving the cleaning effect.

[0024] The battery comprises a silicon wafer obtained by the above-mentioned silicon wafer cleaning method, and the above-mentioned silicon wafer cleaning method can effectively remove dust or particles attached to the surface of the coated silicon wafer without damaging the coated silicon wafer. In this way, the adverse effects of dust and particles on battery performance are avoided, the battery performance is improved, and the service life of the screen during screen printing can be increased, thereby improving the preparation efficiency of the battery and reducing the loss cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a photo of the uncleaned coated silicon wafer of Example 1;

[0026] Figure 2 This is a photo of the coated silicon wafer after cleaning in Example 1;

[0027] Figure 3 This is a trend diagram of the photoelectric conversion efficiency of the experimental group of Example 1;

[0028] Figure 4 This is a trend diagram of the photoelectric conversion efficiency of the control group in Example 1. DETAILED DESCRIPTION

[0029] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively below, and preferred embodiments of the present invention are provided. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0031] The words "preferably", "more preferably", etc. in the present invention refer to embodiments of the present invention that may provide certain beneficial effects in certain circumstances. However, other embodiments may also be preferred under the same circumstances or other circumstances. In addition, the description of one or more preferred embodiments does not imply that other embodiments are not applicable, nor is it intended to exclude other embodiments from the scope of the present invention.

[0032] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0033] Raw material dust and particles are inevitably generated during the coating process. On the one hand, the raw material dust or particles will fall onto the surface of the silicon wafer, resulting in poor appearance of the manufactured battery cell. On the other hand, the raw material dust or particles are brought into the subsequent screen printing step of preparing electrodes, which will scratch the screen or block the holes of the screen plate, thereby affecting the screen printing performance and ultimately affecting the efficiency of the battery cell.

[0034] The inventor of this application found in the process of engaging in technical work in this field that in this field, compressed air or blowing N2 or suction is generally used to remove raw material dust or particles on the surface of coated silicon wafers. After a large number of actual process technology operations, the inventor of this application further found that the process of using compressed air or blowing N2 cannot be accurately controlled. For example, if the air volume is small, the particles cannot be blown away. If the air volume is large, the silicon wafer will be damaged, and even the dust will be blown onto the silicon wafer without dust, which will cause secondary pollution and have a greater negative impact. When the suction method is used, some of the smaller particles produced by PVD are tightly adhered to the surface of the film and cannot be completely sucked away. If the suction force is too large, it will damage the silicon wafer, which will increase the production and manufacturing cost of the battery. Based on this, the technical personnel of this application took a different approach. After a large number of creative experimental explorations, they obtained a cleaning method in this application that can efficiently remove dust or particles attached to the surface of coated silicon wafers without damaging the coated silicon wafers.

[0035] An embodiment of the present invention provides a silicon wafer cleaning method, comprising the following step S10.

[0036] Step S10, sequentially performing a first water wash, a chemical wash, a second water wash and a pulling wash on the silicon wafer to obtain a cleaned silicon wafer.

[0037] The reagent used for chemical cleaning is alkali solution or acid solution, the mass concentration of the acid solution is 0.4% to 5%, and the components of the acid solution include HF; the mass concentration of the alkali solution is 0.3% to 0.9%;

[0038] The coated silicon wafer comprises a silicon substrate and a transparent conductive film coated on the surface of the silicon substrate.

[0039] In the above-mentioned silicon wafer cleaning method, the silicon wafer is sequentially subjected to a first water wash, a chemical wash, a second water wash and a pull-up wash. The first water wash removes most of the loosely adhered dust and particles on the surface of the coated silicon wafer. Acid or alkali solution is further used for chemical washing. The acid or alkali solution reacts with the dust and particles, thereby corroding away the tightly adhered dust or particles on the surface of the coated silicon wafer. At the same time, by controlling the components and concentrations of the acid or alkali solution, and controlling the temperature and time of the chemical washing step, the acid or alkali solution corrodes away the tightly adhered dust or particles on the surface of the coated silicon wafer without damaging the silicon substrate and the transparent conductive film on its surface. Then, a second water wash and a pull-up wash are performed to wash away the residual acid or alkali solution and the residual dust particles. In this way, while efficiently removing the dust or particles attached to the surface of the coated silicon wafer, the coated silicon wafer is not damaged, so that the original conductive properties are maintained.

[0040] Among them, when acid solution is used for chemical cleaning, HF can remove SiO2 on the surface of the coated silicon wafer. SiO2 has polar bonds and is hydrophilic. After HF can remove SiO2 on the surface of the coated silicon wafer, the surface of the coated silicon wafer becomes hydrophobic, so that the surface of the coated silicon wafer exhibits dehydration in the subsequent second water washing step, reducing the watermark on the coated silicon wafer after cleaning.

[0041] It is understandable that due to the process characteristics of the existing coating process, dust or particles will inevitably exist on the surface of the coated silicon wafer. A small part of these dust or particles comes from the dust carried in the air, and the vast majority are raw material particles or dust generated by the coating raw material source during the coating process. For example, if the film layer on the coating surface is a transparent conductive film, then the vast majority of the dust is particles generated by the raw materials for forming the transparent conductive film during the coating process.

[0042] In some of the embodiments, the transparent conductive film is prepared by physical vapor deposition.

[0043] In other words, the silicon wafers are coated by physical vapor deposition. Taking ITO film as an example, ITO (In2O3 doped with tin) target material is usually used to deposit on the surface of silicon wafers by PVD to form a transparent conductive film. During the deposition process, while depositing on the surface of the silicon wafer, it will also deposit on the cavity part of the equipment. The continuous accumulation and deposition, coupled with the changes in temperature and humidity, will form dust. In the mass production process, the dust will fall on the surface of the silicon wafer and then be brought into the screen production section, affecting the screen printing, thereby affecting the overall efficiency of the battery.

[0044] In some embodiments, the transparent conductive film includes at least one of a metal film and a semiconductor film.

[0045] Furthermore, the transparent conductive film is a transparent conductive oxide film. Specifically, it includes but is not limited to: ITO film, IWO film

[0046] In some embodiments, the first water washing step is performed under ultrasonic conditions, and the ultrasonic frequency is 1KHZ to 2.4KHZ.

[0047] Under the action of ultrasound of a specific frequency, the dust and particles on the surface of the coated silicon wafer are separated from the coated silicon wafer. While further promoting the removal of dust and particles, the silicon substrate and the transparent conductive film on its surface are not damaged, allowing it to maintain its original conductive properties.

[0048] In some embodiments, the temperature of the chemical cleaning step is 20° C. to 30° C., and the time is 100 s to 300 s.

[0049] In some embodiments, the temperature of the above-mentioned pulling and cleaning is 55°C to 80°C.

[0050] Control the temperature of the pull-cleaning process within a higher range to prepare for subsequent drying.

[0051] In some of the embodiments, the first water washing and / or chemical cleaning and / or the second water washing can be performed using a tank type device or a chain type device.

[0052] Specifically, the first water washing and / or chemical washing and / or the second water washing may be performed by circulating washing or overflow washing.

[0053] In some embodiments, the temperature of the first water washing step is 20° C. to 30° C., and the time is 100 s to 300 s.

[0054] In some embodiments, the temperature of the second water washing step is 20° C. to 30° C., and the time is 100 s to 300 s.

[0055] In some embodiments, the pulling speed in the above-mentioned pulling and cleaning step is controlled to be 3 mm / s to 5 mm / s.

[0056] It is understandable that during the coating process of the silicon wafer, part of the silicon on its surface will inevitably be oxidized into hydrophilic silicon dioxide. By controlling the pulling speed of the coated silicon wafer and slowly pulling the cleaned coated silicon wafer, the washing liquid attached to the surface of the coated silicon wafer will gradually detach, thereby reducing the washing liquid attached to the surface of the coated silicon wafer after washing. While reducing the watermark on the cleaned coated silicon wafer, it further avoids the dust or particles carried in the washing liquid from re-attaching to the coated silicon wafer, thereby further improving the cleaning effect.

[0057] Specifically, the cleaning liquid for the above-mentioned pulling cleaning is water, and the cleaning is carried out specifically by overflow cleaning.

[0058] In some embodiments, the acid solution further comprises HCl.

[0059] It should be noted that, when the components of the above-mentioned acid solution also include HCl, the mass concentration of the acid solution refers to the total mass concentration of HCl and HF.

[0060] In some embodiments, the alkali in the alkali solution is selected from alkali metal hydroxides.

[0061] Specifically, the alkali in the alkali solution is selected from at least one of potassium hydroxide and sodium hydroxide.

[0062] In some embodiments, the acid solution or alkali solution is an aqueous solution of an acid or an aqueous solution of an alkali.

[0063] In some of the embodiments, after the second water washing step, a step of drying the washed coated silicon wafer is also included.

[0064] The present invention further provides a battery in an embodiment, wherein the battery comprises a silicon wafer produced by the silicon wafer cleaning method as described above.

[0065] The above silicon wafer cleaning method can effectively remove dust or particles attached to the surface of the coated silicon wafer without damaging the coated silicon wafer. In this way, the adverse effects of dust and particles on battery performance are avoided, the battery performance is improved, and the service life of the screen during screen printing can be increased, thereby improving the production efficiency of the battery and reducing the loss cost.

[0066] Specifically, the preparation of the above battery includes the following steps:

[0067] The silicon wafer substrate is textured, then coated by physical vapor deposition, then cleaned by the silicon wafer cleaning method as described above, and finally electrodes are made to obtain a battery.

[0068] In some embodiments, before the step of coating by physical vapor deposition, the silicon wafer after texturing is deposited with amorphous silicon thin film by PECVD. At this time, the battery obtained is a heterojunction battery. Specifically, silver grid lines are printed on the silicon wafer by screen printing technology to make positive and negative electrode leads.

[0069] The present invention will be described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments. It should be understood that the attached claims summarize the scope of the present invention. Under the guidance of the concept of the present invention, those skilled in the art should realize that certain changes made to the various embodiments of the present invention will be covered by the spirit and scope of the claims of the present invention.

[0070] The following are specific embodiments.

[0071] Example 1

[0072] (1) Preparation of HF solution: Mix 49 wt% hydrofluoric acid and water in a volume ratio of 1:60 to obtain an HF solution. The concentration of the HF solution is 0.8% by mass.

[0073] Prepare coated silicon wafers: Use PVD to deposit ITO film on silicon wafers to form coated silicon wafers. The photo of coated silicon wafers is shown below. Figure 1 As described above, there are fine dust and particles on the surface of the coated silicon wafer.

[0074] (2) Place the coated silicon wafer after PVD treatment in a water tank and wash it at 23 + / - 3 ° C for 300 seconds under the action of 2.4 kHz ultrasonic waves;

[0075] The washed coated silicon wafer is placed in an HF solution for circulation cleaning at 23+ / -3°C for 150s; then, it is overflow cleaned in a water tank at 23+ / -3°C for 150s, and then, in overflow cleaning mode at 60°C, the coated silicon wafer is pulled and cleaned at a pulling speed of 3mm / s to 5mm / s, and the coated silicon wafer is pulled out of the water tank for 60s, and then dried at 90°C for 900s to obtain the cleaned coated silicon wafer.

[0076] The photo of the coated silicon wafer after cleaning is shown in Figure 2 As shown, there is no dust or particles on the surface of the coated silicon wafer after cleaning, and the film surface is intact and undamaged.

[0077] (3) Repeat steps (1) to (2) 100 times to clean 100 coated silicon wafers. If there is no dust or particles on the surface of the coated silicon wafer after cleaning, it is considered as a qualified silicon wafer. If there is no dust or particles on the surface of the coated silicon wafer after cleaning, and the film surface is intact and undamaged, it is a qualified product, and the cleaning pass rate and yield rate are further calculated according to the following formula:

[0078] Cleaning pass rate = number of cleaned silicon wafers / total number of silicon wafers × 100%

[0079] Yield rate = qualified products ÷ total number of silicon wafers × 100%

[0080] Please see Table 1 for specific results.

[0081] (4) The uncleaned and cleaned coated silicon wafers were set as the experimental group and the control group, and solar cells were made and the electrical performance tests were carried out respectively. The test process was based on the conventional solar cell standard: 3A standard, 25℃, AM1.5, 1000W / m 2 The photoelectric conversion efficiency diagrams of the experimental group and the control group are shown in Figure 3 and Figure 4 As shown, Figure 3 and Figure 4 The horizontal and vertical axes represent the number of silicon wafers, and the vertical axes represent the photoelectric conversion efficiency.

[0082] Furthermore, the average values ​​of the parameters in the electrical performance test were calculated. The specific results are shown in Table 2.

[0083] Table 2

[0084] quantity Eta Uoc Isc FF Experimental Group 8432 24.041 0.7446 10.481 84.45 Photo shooting team 6343 23.985 0.7436 10.506 84.17

[0085] Among them, quantity refers to the number of coated silicon wafers used in the experiment; Eta is the photoelectric conversion efficiency, in %; Uoc is the open circuit voltage, in V; Isc is the short circuit current, in A; FF is the fill factor, in %.

[0086] Comparing the efficiency trend charts of the two, it can be seen that after removing the powder layer on the surface of the silicon wafer, the efficiency stability of the cleaned coated silicon wafer is significantly higher, while the efficiency of the uncleaned part continues to decline due to the influence of the powder layer on the screen; when it is finally reflected in the average efficiency, it can be seen from the data Eta in Table 2 that the average efficiency of the experimental group is 0.05% higher.

[0087] In the large-scale production of SHJ batteries, the improvement of efficiency means the reduction of costs. For example, according to the calculation of 0.05% efficiency improvement, at 1.2 yuan per watt, and the original efficiency of SHJ batteries is roughly calculated at 24%, the annual increase in revenue per GW production capacity is: 1.2×1000000000×0.05%÷24%=5 million yuan.

[0088] Example 2

[0089] (1) Preparation of HF solution: Mix 49 wt% hydrofluoric acid and water in a volume ratio of 1:10 to obtain an HF solution. The concentration of the HF solution is 4.9% by mass.

[0090] Prepare coated silicon wafers: Use PVD to deposit ITO film on silicon wafers to form coated silicon wafers. The photo of coated silicon wafers is shown below. Figure 1 As described above, there are fine dust and particles on the surface of the coated silicon wafer.

[0091] Steps (2) to (3): Same as steps (2) to (3) in Example 1. See Table 1 for specific results.

[0092] Example 3

[0093] (1) Preparation of HF solution: 49 wt% hydrofluoric acid and water are mixed in a volume ratio of 1:120 to obtain an HF solution. The concentration of the HF solution is 0.4% by mass.

[0094] Prepare coated silicon wafers: Use PVD to deposit ITO film on silicon wafers to form coated silicon wafers. The photo of coated silicon wafers is shown below. Figure 1 As described above, there are fine dust and particles on the surface of the coated silicon wafer.

[0095] Steps (2) to (3): Same as steps (2) to (3) in Example 1. See Table 1 for specific results.

[0096] Example 4

[0097] (1) Same as step (1) of Example 1.

[0098] (2) Place the coated silicon wafer after PVD treatment in a water tank and wash it at 23 + / - 3 ° C for 300 seconds under the action of 1 kHz ultrasonic wave;

[0099] The remaining steps are the same as step (2) in the embodiment.

[0100] After cleaning, there is no dust or particles on the surface of the coated silicon wafer, and the film surface is intact and undamaged.

[0101] Step (3): Same as step (3) of Example 1. See Table 1 for specific results.

[0102] Example 5

[0103] (1) Preparation of KOH solution: A KOH aqueous solution with a concentration of 46 wt% and water are mixed in a volume ratio of 1:100 to obtain a KOH solution. The concentration of the KOH solution is 0.45% by mass.

[0104] Prepare coated silicon wafers: Use PVD to deposit ITO film on silicon wafers to form coated silicon wafers. There are fine dust and particles on the surface of the coated silicon wafers.

[0105] (2) Place the coated silicon wafer after PVD treatment in a water tank and wash it at 23 + / - 3 ° C for 300 seconds under the action of 2.4 kHz ultrasonic wave;

[0106] The washed coated silicon wafer is placed in a KOH solution for circulation cleaning at 23+ / -3℃ for 150s; then, it is overflow cleaned in a water tank at 23+ / -3℃ for 150s, and then, in overflow cleaning mode at 60℃, the coated silicon wafer is pulled at a pulling speed of 3mm / s to 5mm / s, and the coated silicon wafer is pulled out of the water tank in 60s, and then dried at 90℃ for 900s to obtain the cleaned coated silicon wafer. There is no dust or particles on the surface of the cleaned coated silicon wafer, and the film surface is intact and undamaged.

[0107] (3) Repeat steps (1) to (2) 100 times to clean 100 coated silicon wafers. After cleaning, the coated silicon wafers are free of dust and particles on the surface and the film surface is intact and undamaged, which is considered a good product. The yield rate is calculated as follows:

[0108] Yield rate = number of qualified silicon wafers ÷ total number of silicon wafers × 100%

[0109] Please see Table 1 for specific results.

[0110] Example 6

[0111] Example 6 is basically the same as Example 1, except that: in step (2), the pull-up cleaning is performed at a pull-up speed of 100 mm / s, the coated silicon wafer is pulled out of the water tank in 60 seconds, and then dried at 90° C. for 900 seconds to obtain a cleaned coated silicon wafer. The other steps and conditions are the same as those in Example 1. See Table 1 for specific results.

[0112] Comparative Example 1

[0113] Comparative Example 1 is substantially the same as Example 1, except that the concentration of the HF solution at the sampling point is different. The HF solution is prepared by mixing hydrofluoric acid having a concentration of 49 wt % and water in a volume ratio of 1:5 to obtain an HF solution. The concentration of the HF solution is 10% by mass.

[0114] The other steps and conditions are the same as those in Example 1. See Table 1 for specific results.

[0115] Comparative Example 2

[0116] Comparative Example 2 is substantially the same as Example 1, except that in step (2), the coated silicon wafer after PVD treatment is placed in a water tank and washed at 23+ / -3°C for 300s under 5KHZ ultrasonic waves. Other steps and conditions are the same as those in Example 1.

[0117] Please see Table 1 for specific results.

[0118] Comparative Example 3

[0119] Comparative Example 3 is substantially the same as Example 5, except that the concentration of the alkali solution used is different: KOH solution is prepared by mixing a 46 wt % KOH aqueous solution and water in a volume ratio of 1:10 to obtain a KOH solution. The concentration of the KOH solution is 4.6% by mass. The other steps and conditions are the same as those of Example 5.

[0120] Please see Table 1 for specific results.

[0121] Comparative Example 4

[0122] Comparative Example 4 is basically the same as Example 1, except that: in step (2), when the coated silicon wafer after water washing is placed in the HF solution for cleaning, the temperature is controlled to be 60+ / -3°C, and the other steps and conditions are the same as those in Example 1.

[0123] Please see Table 1 for specific results.

[0124] Comparative Example 5

[0125] Comparative Example 5 is basically the same as Example 1, except that: in step (2), when the coated silicon wafer after water washing is placed in the HF solution for cleaning, the cleaning time is controlled to be 600 seconds, and the other steps and conditions are the same as those in Example 1.

[0126] Please see Table 1 for specific results.

[0127] Table 1

[0128] Cleaning pass rate Yield Example 1 99% 98.2% Example 2 98.5% 98.1% Example 3 98.6% 98.1% Example 4 98.9% 98.2% Example 5 98.3% 98% Example 6 98.5% 95% Comparative Example 1 50% 49.2% Comparative Example 2 95% 94.3% Comparative Example 3 10% 9.8% Comparative Example 4 60% 59.2% Comparative Example 5 90.1% 85.5%

[0129] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0130] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A silicon wafer cleaning method, characterized in that: The steps include: The silicon wafer is sequentially subjected to a first water wash, a chemical wash, a second water wash and a pulling wash to obtain a cleaned silicon wafer; The chemical cleaning agent is alkaline solution or acid solution, the mass concentration of the acid solution is 0.4% to 5%, and the components of the acid solution include HF; the mass concentration of the alkaline solution is 0.3% to 0.9%; The temperature of the chemical cleaning step is 20°C to 30°C, and the time is 100s to 300s; The silicon wafer comprises a silicon substrate and a transparent conductive film coated on the surface of the silicon substrate; In the step of pulling and cleaning, the pulling speed is controlled to be 3 mm / s to 5 mm / s.

2. The silicon wafer cleaning method according to claim 1, characterized in that: The first water washing step is performed under ultrasonic conditions, and the frequency of the ultrasound is 1 KHz to 2.4 KHz.

3. The silicon wafer cleaning method according to any one of claims 1 to 2, characterized in that: The temperature of the pulling and cleaning is 55°C to 80°C.

4. The silicon wafer cleaning method according to any one of claims 1 to 2, characterized in that: The temperature of the first water washing step is 20° C. to 30° C., and the time is 100 s to 300 s.

5. The silicon wafer cleaning method according to any one of claims 1 to 2, characterized in that: The temperature of the second water washing step is 20° C. to 30° C., and the time is 100 s to 300 s.

6. The silicon wafer cleaning method according to any one of claims 1 to 2, characterized in that: The acid solution also includes HCl.

7. The silicon wafer cleaning method according to any one of claims 1 to 2, characterized in that: The alkali in the alkali solution is selected from hydroxides of alkali metals.

8. The silicon wafer cleaning method according to any one of claims 1 to 2, characterized in that: The transparent conductive film is prepared by physical vapor deposition.

9. A battery, characterized in that: The battery comprises a silicon wafer produced by the silicon wafer cleaning method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Cleaning method of solar cell