Crystallizable shrinkable and thermoformable films and sheets made from reactor-grade resins with recycled content
Crystallizable polyester films and sheets with specific diol monomer combinations address the challenges of controlled shrinkage and recyclability, ensuring compatibility with PET recycling processes and reducing environmental impact.
Patent Information
- Application Number
- CN202080089591.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-25
- Filing Date
- 2020-10-08
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-10-08
AI Technical Summary
Existing shrink films and thermoformable sheets face challenges in achieving low initial shrink temperature, controlled shrinkage, high ultimate shrinkage, low shrink force, low shrinkage in perpendicular direction, film toughness, recyclability, and compatibility with PET recycling processes without interfering with PET flakes.
Development of crystallizable polyester compositions with specific diol monomer combinations that are amorphous but crystallizable, allowing for strain-induced crystallization at high temperatures, ensuring compatibility with PET recycling processes and maintaining film properties.
The crystallizable polyester films and sheets provide controlled shrinkage, high strain-induced crystallization melting point, and recyclability, enabling seamless integration into PET recycling without forming clumps, thus enhancing recycling efficiency and reducing environmental impact.
Smart Images

Figure 10780 
Figure 120916 
Figure 177304
Abstract
Description
Field of the Invention
[0001] The present disclosure relates to crystallizable shrinkable films and thermoformable film(s) and / or sheets comprising a polyester composition having certain advantages and improved properties, the polyester composition comprising residues of terephthalic acid, neopentyl glycol (NPG), 1,4-cyclohexanedimethanol (CHDM), ethylene glycol (EG), and diethylene glycol (DEG) within certain composition ranges. The present disclosure further relates to crystallizable shrinkable films and thermoformable film(s) and / or sheets comprising a polyester composition having certain advantages and improved properties, the polyester composition comprising residues of recycled terephthalic acid, recycled neopentyl glycol (NPG), recycled 1,4-cyclohexanedimethanol (CHDM), recycled ethylene glycol (EG), and recycled diethylene glycol (DEG) within certain composition ranges. Background of the Invention
[0003] There is a commercial need for shrink films having at least one of the following desirable shrink film properties: (1) a low initial shrink temperature, (2) a shrinkage percentage that increases gradually and in a controlled manner with increasing temperature over the temperature range in which shrinkage occurs, (3) a shrink force that is sufficiently low to prevent crushing of the underlying container, (4) a high ultimate shrinkage (shrinkage at maximum temperature), such as 60% or more in the principal shrink direction at 95°C, (5) a low shrinkage in a direction perpendicular to the high shrinkage direction, (6) improved film toughness to prevent unwanted film cracking, rupture, tearing, splitting, blistering or wrinkling during the manufacturing process and before and after shrinking, (7) recyclability, and (8) recycled content.
[0004] There is a commercial need for thermoformable films or sheets having good film or sheet properties and recyclability and / or recycled content. SUMMARY OF THE INVENTION
[0006] It has been found that certain combinations of diol monomers in shrink film resin compositions can be made into films that have good shrink film properties and can also be crystallized so that they do not affect the recovery of PET flakes in the recycling process. These crystallizable shrink film resins can be processed with PET bottles and eventually become components in recyclable PET flakes that leave the recycling process. It has also been found that the selection and amount of specific combinations of diol monomers are important for producing films with good shrink film properties and producing crystallizable films. The optimized polyester resin compositions of the present disclosure are amorphous but crystallizable. Therefore, they exhibit good properties in film applications including as shrink films, but they have a high strain-induced crystallization melting point, so they provide compatibility in the recycling process. The shrink film labels of the present disclosure do not have to be removed during the recycling process, and they do not affect the process.
[0007] Heat shrinkable films must meet various suitability for use criteria to be used in this application. The film must be strong, must shrink in a controlled manner, and must provide sufficient shrink force to hold itself to the bottle without crushing the contents. In addition, when these labels are applied to polyester containers, polyester shrink film labels must not interfere with the recycling process of the bottles. The shrink films of the present disclosure are advantageous because the labels can be recycled with the bottles or containers. Thus, the entire bottle, including the label, can be recycled and converted into new products without incurring additional disposal requirements or creating new environmental issues. Heat shrinkable films are made from a variety of raw materials to meet a range of material requirements. The present disclosure describes unique and unexpected effects measured with certain monomer combinations for shrink film resin compositions.
[0008] Polyester shrink film compositions have been used commercially as shrink film labels for food, beverages, personal care, household products, etc. Typically, these shrink films are used in combination with clear polyethylene terephthalate (PET) bottles or containers. The entire package (bottle plus label) is then put into the recycling process. In a typical recycling center, the PET and shrink film materials usually end up together at the end of the process due to the similarity in composition and density. The PET flakes need to be dried to remove residual water that is left in the PET through the recycling process. Typically, PET is dried at temperatures above 200°C. At these temperatures, typical polyester shrink film resins soften and become sticky, often forming clumps with the PET flakes. These clumps must be removed before further processing. These clumps reduce the yield of PET flakes from the process and result in additional handling steps.
[0009] It has also been found that certain combinations of diol monomers in film or sheet resin compositions can be made into films or sheets with good performance properties and can also be crystallized so that they do not affect the recovery of PET flakes. These crystallizable film or sheet resins can be processed with recycled PET and eventually become components in recyclable PET flakes that leave the recycling process. It has also been found that the selection and amount of a specific combination of diol monomers are important for producing films or sheets with good performance properties and producing crystallizable films or sheets. The optimized polyester resin compositions disclosed herein are amorphous but crystallizable. Therefore, they show good properties in film or sheet applications, including as molded, thermoformed or formed parts and / or articles, but they have a high strain-induced crystallization melting point, so they can be recycled with PET. The films or sheets disclosed herein do not have to be removed during the recycling process, and they do not affect the recycling process.
[0010] One embodiment of the present disclosure is a crystallizable film comprising an amorphous polyester composition comprising: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole % of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: about 75 mole % or more of ethylene glycol residues and about 25 mole % or less of other diols, the other diols comprising one or more of: (i) from about 0 to less than about 24 mole % neopentyl glycol residues; (ii) from about 0 to less than about 24 mole % 1,4-cyclohexanedimethanol residues; (iii) from about 1 to less than about 10 mole % of the total diethylene glycol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid component is 100 mole % and wherein the total mole % of the diol component is 100 mole %; or (b) A diol component comprising: about 75 mole % or more ethylene glycol residues and about 25 mole % or less other diols, wherein the other diols comprise one or more of: (i) about 0.1 to less than about 24 mole % neopentyl glycol residues; (ii) about 0.1 to less than about 24 mole % 1,4-cyclohexanedimethanol residues; (iii) about 1 to less than about 10 mole % of the total diethylene glycol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid component is 100 mole %, and wherein the total mole % of the diol component is 100 mole %.
[0011] One embodiment of the present disclosure is a crystallizable film comprising an amorphous polyester composition comprising: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole % of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: about 75 mole % or more of ethylene glycol residues and about 25 mole % or less of other diols, the other diols comprising one or more of the following: (i) about 15 mole % or less of neopentyl glycol residues; (ii) about 5 mole % or less of 1,4-cyclohexanedimethanol residues; (iii) about 5 mole % or less of total diethylene glycol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid component is 100 mole %, and wherein the total mole % of the diol component is 100 mole %.
[0012] One embodiment of the present disclosure is a crystallizable film comprising an amorphous polyester composition comprising: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole % of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: about 80 mole % or more of ethylene glycol residues and about 20 mole % or less of other diols, the other diols comprising one or more of: (i) from about 5 to less than about 17 mole % neopentyl glycol residues; (ii) from about 2 to less than about 10 mole % 1,4-cyclohexanedimethanol residues; (iii) from about 1 to less than about 5 mole % of total diethylene glycol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid component is 100 mole %, and wherein the total mole % of the diol component is 100 mole %.
[0013] One embodiment of the present disclosure is a crystallizable film comprising an amorphous polyester composition comprising: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole % of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: about 76 mole % or more of ethylene glycol residues and about 24 mole % or less of an amorphous content comprising one or more of: (i) neopentyl glycol residues; (ii) cyclohexanedimethanol residues; and (iii) diethylene glycol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid component is 100 mole %, and wherein the total mole % of the diol component is 100 mole %.
[0014] One embodiment of the present disclosure is a crystallizable film comprising an amorphous polyester composition comprising: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole % of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: about 75 mole % or more of ethylene glycol residues and about 25 mole % or less of other diols, the other diols comprising one or more of: (i) from about 10 to less than about 15 mole % neopentyl glycol residues; (ii) from about 1 to less than about 5 mole % 1,4-cyclohexanedimethanol residues; (iii) from about 1 to less than about 5 mole % of total diethylene glycol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid component is 100 mole %, and wherein the total mole % of the diol component is 100 mole %.
[0015] One embodiment of the present disclosure is a crystallizable film comprising a polyester composition comprising: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole % of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: (i) from about 0 to about 30 mole % of neopentyl glycol residues; (ii) from about 0 to about less than 30 mole % of 1,4-cyclohexanedimethanol residues; (iii) diethylene glycol residues, whether or not formed in situ; and wherein the balance of the diol component comprises: (iv) residues of ethylene glycol, and (v) optionally 0 to 10 mole %, or 0 to 5 mole % of residues of at least one modifying diol; wherein the total mole % of the dicarboxylic acid component is 100 mole %, and wherein the total mole % of the diol component is 100 mole %.
[0016] One embodiment of the present disclosure is the crystallizable film of any preceding embodiment, wherein the film is stretched in at least one direction and the stretched film has a strain-induced crystalline melting point of 190° C. or more or 200° C. or more.
[0017] One embodiment of the present disclosure is an extruded or calendered film comprising the crystallizable film of any of the preceding embodiments.
[0018] One embodiment of the present disclosure is a thermoformable film or sheet comprising a polyester composition comprising: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole % of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: about 75 mole % or more of ethylene glycol residues and about 25 mole % or less of other diols, the other diols comprising one or more of: (i) from about 0 to less than about 24 mole % neopentyl glycol residues; (ii) from about 0 to less than about 24 mole % 1,4-cyclohexanedimethanol residues; (iii) from about 1 to less than about 10 mole % of the total diethylene glycol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid component is 100 mole % and wherein the total mole % of the diol component is 100 mole %; or (b) A diol component comprising: about 75 mole % or more ethylene glycol residues and about 25 mole % or less other diols, wherein the other diols comprise one or more of: (i) about 0.1 to less than about 24 mole % neopentyl glycol residues; (ii) about 0.1 to less than about 24 mole % 1,4-cyclohexanedimethanol residues; (iii) about 1 to less than about 10 mole % of the total diethylene glycol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid component is 100 mole %, and wherein the total mole % of the diol component is 100 mole %.
[0019] One embodiment of the present disclosure is a thermoformable film or sheet comprising a polyester composition comprising: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole % of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: about 75 mole % or more of ethylene glycol residues and about 25 mole % or less of other diols, the other diols comprising one or more of the following: (i) about 15 mole % or less of neopentyl glycol residues; (ii) about 5 mole % or less of 1,4-cyclohexanedimethanol residues; (iii) about 5 mole % or less of total diethylene glycol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid component is 100 mole %, and wherein the total mole % of the diol component is 100 mole %.
[0020] One embodiment of the present disclosure is a thermoformable film or sheet comprising a polyester composition comprising: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole % of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: about 80 mole % or more of ethylene glycol residues and about 20 mole % or less of other diols, the other diols comprising one or more of the following: (i) from about 5 to less than about 17 mole % neopentyl glycol residues; (ii) from about 2 to less than about 10 mole % 1,4-cyclohexanedimethanol residues; (iii) from about 1 to less than about 5 mole % of total diethylene glycol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid component is 100 mole %, and wherein the total mole % of the diol component is 100 mole %.
[0021] One embodiment of the present disclosure is a thermoformable film or sheet comprising a polyester composition comprising: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole % of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: about 76 mole % or more of ethylene glycol residues and about 24 mole % or less of an amorphous content comprising one or more of: (i) neopentyl glycol residues; (ii) cyclohexanedimethanol residues; and (iii) diethylene glycol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid component is 100 mole %, and wherein the total mole % of the diol component is 100 mole %.
[0022] One embodiment of the present disclosure is a thermoformable film or sheet comprising a polyester composition comprising: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole % of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: about 75 mole % or more of ethylene glycol residues and about 25 mole % or less of other diols, the other diols comprising one or more of the following: (i) from about 10 to less than about 15 mole % neopentyl glycol residues; (ii) from about 1 to less than about 5 mole % 1,4-cyclohexanedimethanol residues; (iii) from about 1 to less than about 5 mole % of total diethylene glycol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid component is 100 mole %, and wherein the total mole % of the diol component is 100 mole %.
[0023] One embodiment of the present disclosure is a thermoformable film or sheet comprising a polyester composition comprising: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole % of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: (i) from about 0 to about 30 mole % of neopentyl glycol residues; (ii) from about 0 to about less than 30 mole % of 1,4-cyclohexanedimethanol residues; (iii) residues of diethylene glycol, whether or not formed in situ; and wherein the balance of the diol component comprises: (iv) residues of ethylene glycol, and (v) optionally 0 to 10 mole %, or 0 to 5 mole % of residues of at least one modifying diol; wherein the total mole % of the dicarboxylic acid component is 100 mole %, and wherein the total mole % of the diol component is 100 mole %.
[0024] One embodiment of the present disclosure is a molded, thermoformed or shaped article comprising the film or sheet of any of the preceding embodiments.
[0025] One embodiment of the present disclosure is a medical device, medical packaging, healthcare product, commercial food service product, tray, container, food tray, tumbler, storage box, bottle, food processor, blender and mixer bowl, utensil, water bottle, freshness tray, washing machine component, refrigerator component, vacuum cleaner component, ophthalmic lens and frame or toy comprising the thermoformed film or sheet of any of the preceding embodiments.
[0026] One embodiment of the present disclosure is a manufactured article comprising the thermoformed film or sheet of any of the preceding embodiments.
[0027] One embodiment of the present disclosure is a method of making a thermoformed film or sheet of any of the foregoing embodiments, comprising: A. heating a polyester film or sheet; B. applying air pressure, vacuum and / or physical pressure to the heat-softened film or sheet; C. causing the sheet to conform to a mold shape by vacuum or pressure; and D. removing the thermoformed part or article from the mold.
[0028] One aspect of the present disclosure is a method for preparing the polyester of the present disclosure from recycled polyester. One aspect of the present disclosure is a method for preparing copolyester from recycled polyester and / or recycled copolyester.
[0029] In one aspect, the present disclosure provides a method for preparing a linear high molecular weight copolyester from any of the following materials: (A) a recycled polyester and / or a recycled copolyester whose acid component consists of at least 70 mol % terephthalic acid and whose diol component consists of at least 70 mol % ethylene glycol, or (B) a recycled copolyester whose acid component consists of at least 70 mol % terephthalic acid and whose diol component consists of at least 70 mol % of a mixture of ethylene glycol, 1,4-cyclohexanedimethanol and diethylene glycol in a molar ratio of 96:3:1 to 20:68:12, or (C) A recycled copolyester whose acid component consists of at least 70 mol% of terephthalic acid and whose diol component consists of at least 70 mol% of a mixture of two or more diols including ethylene glycol (EG), diethylene glycol (DEG), 1,4-cyclohexanedimethanol (CHDM), neopentyl glycol (NPG) or 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD), butanediol and isosorbide, or (D) a recycled copolyester whose acid component consists of at least 70 mol% of terephthalic acid and whose diol component consists of at least 70 mol% of a mixture of ethylene glycol, 1,4-cyclohexanedimethanol in a molar ratio of 3.5:96.5 to 100:0.
[0030] The process provides a rapid polymerization rate, and the polymers produced therefrom can be used to make plastics, fibers, films, shrinkable films, sheets, moldings, and other shaped articles having good physical properties. In one aspect, the disclosed process describes a method for converting post-industrial and post-consumer waste products into high-quality copolyester resins that can be used to make new plastics with high levels of recycled content. In another aspect, the disclosed process describes a method for converting post-industrial and post-consumer waste products into resins that can be used to make high-quality shrinkable films.
[0031] One aspect of the present disclosure is a method for producing a copolyester from a recycled copolyester, comprising:
[0032] (a) introducing recycled PET, recycled PETG, recycled PCT, recycled PCTG, recycled PCTA, recycled PCTM and / or recycled PETM; terephthalic acid (TPA); and ethylene glycol (EG) into a paste tank to form a slurry, which is stirred and heated at a temperature of up to 150° C.;
[0033] (b) transferring the paste tank slurry to the first reaction zone;
[0034] (c) introducing into the first reaction zone at least one additional diol comprising 1,4-cyclohexanedimethanol (CHDM), neopentyl glycol (NPG), or 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD), and optionally adding additional recycled PET, recycled PETG, recycled PCTM, and / or recycled PETM; terephthalic acid (TPA); and ethylene glycol (EG) at a molar ratio of EG:TPA of 1:1 to 4:1, and optionally a catalyst;
[0035] (d) reacting TPA with EG and the at least one additional diol (e.g., CHDM) in a first reaction zone at a melt temperature of at least 200° C. and a pressure of up to 40 psi to form a first esterification product comprising oligomers and unreacted TPA, EG, and the additional diol (e.g., CHDM);
[0036] (e) conveying the first esterification product to a second reaction zone;
[0037] (f) esterifying unreacted TPA, EG, and additional diol (e.g., CHDM) in the first esterified product in a second reaction zone at a melt temperature of at least 200° C. and a pressure of up to 20 psi to form a second esterified product comprising a copolyester oligomer;
[0038] (g) conveying the second esterification product to a third reaction zone;
[0039] (h) polycondensing the second esterification product in a third reaction zone, optionally in the presence of a polycondensation catalyst, to form a prepolymerization product comprising a copolyester; and
[0040] (i) The prepolymer product is passed to one or more finishing zones.
[0041] One aspect of the present disclosure is a method for producing a copolyester from a recycled copolyester, comprising:
[0042] (a) introducing recycled PET, recycled PETG, recycled PCT, recycled PCTG or recycled PCTA; terephthalic acid (TPA); and ethylene glycol (EG) into a paste tank to form a slurry, which is stirred and heated at a temperature of up to 150° C.;
[0043] (b) transferring the paste tank slurry to the first reaction zone;
[0044] (c) introducing into the first reaction zone at least one additional diol comprising 1,4-cyclohexanedimethanol (CHDM), DEG or neopentyl glycol (NPG), optionally in the presence of an esterification catalyst, and optionally adding additional recycled PET, recycled PETG, recycled PCT, recycled PCTG or recycled PCTA; terephthalic acid (TPA); and ethylene glycol (EG) at a molar ratio of EG:TPA of 1:1 to 4:1;
[0045] (d) reacting TPA with EG and the at least one additional diol (e.g., CHDM) in a first reaction zone at a melt temperature of at least 200° C. and a pressure of up to 40 psi to form a first esterification product comprising oligomers and unreacted TPA, EG, and the additional diol (e.g., CHDM and / or NPG and / or DEG);
[0046] (e) conveying the first esterification product to a second reaction zone;
[0047] (f) esterifying unreacted TPA, EG, and additional diol (e.g., CHDM) in the first esterified product in a second reaction zone at a melt temperature of at least 200° C. and a pressure of up to 20 psi to form a second esterified product comprising a copolyester oligomer;
[0048] (g) conveying the second esterification product to a third reaction zone;
[0049] (h) polycondensing the second esterification product in a third reaction zone, optionally in the presence of a polycondensation catalyst, to form a prepolymerization product comprising a copolyester; and
[0050] (i) The prepolymer product is passed to one or more finishing zones.
[0051] One aspect of the present disclosure is the method of any of the preceding aspects, wherein the method further comprises adding a catalyst or additive by adding recycled polyester, wherein the catalyst or additive is a component of the recycled polyester; such as Sb, Ti, Co, Mn, Li, Al, P.
[0052] One aspect of the present disclosure is a method of introducing or establishing recycled content in a polyester made by the method of the preceding aspect, comprising:
[0053] a. obtaining a recycled monomer allocation or credit for at least one recycled monomer including TPA, EG, DMT, CHDM, NPG or DEG;
[0054] b. converting the recovered monomer in a synthesis process to produce polyester;
[0055] c. marking at least a portion of the polyester as corresponding to at least a portion of the recycled monomer quota or credit; and
[0056] d. Optionally, offering for sale or selling polyester containing or obtained by recycled monomer content corresponding to such designation. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 : Differential scanning calorimeter thermogram showing the first heating strain-induced crystallization melting point of Embrace LV
[0059] Figure 2 : Shrinkage properties of films made with Embrace LV (10 sec residence time)
[0060] Figure 3 : Shrinkage performance
[0061] Figure 4 : DSC thermogram of film N stretched at the first heating at 80 °C
[0062] Figure 5 : DSC thermogram of film N stretched at the second heating at 80 °C
[0063] Figure 6 are flow charts of various methods according to the present disclosure.
[0064] Figure 7 . Sb catalyst levels in the final material as a function of rPET raw material loading levels.
[0065] Details
[0066] The present disclosure can be more easily understood by referring to the following detailed description of certain embodiments and examples of the present disclosure. According to (one or more) purposes of the present disclosure, certain embodiments of the present disclosure are described in the Summary of the Invention and are further described below. Other embodiments of the present disclosure are also described herein.
[0067] Heat shrinkable plastic films are used as covers to hold items together and as outer packaging for bottles, cans and other types of containers. For example, such films are used to cover the cap, neck, shoulder or ridge of a bottle or the entire bottle for the purpose of marking, protecting, packaging or adding value to the product; and for other reasons. In addition, such films can be used as covers to pack together groups of items such as boxes, bottles, boards, sticks or notebooks, and such films can also be tightly attached as packaging materials. The above uses take advantage of the shrinkability and internal shrinkage stress of the film.
[0068] In the past, poly(vinyl chloride) (PVC) films dominated the shrink film market. However, polyester films have become an important alternative because polyester films do not have the environmental issues associated with PVC films. Polyester shrink films would ideally have properties very similar to those of PVC films so that polyester films could serve as a "drop-in" replacement film and could be processed in existing shrink tunnel equipment. Properties of PVC films that are desired to be replicated include the following: (1) a relatively low shrink initiation temperature, (2) a total shrinkage that increases gradually and in a controlled manner with increasing temperature, (3) a low shrink force to prevent crushing of the underlying container, (4) a high total shrinkage (e.g., 50% or greater), (5) an inherent film toughness to prevent unwanted tearing and splitting of the film before and after shrinking, and (6) a high strain-induced crystalline melting temperature.
[0069] Heat shrinkable films must meet various suitability for use criteria to be used in this application. The film must be strong, must shrink in a controlled manner, and must provide sufficient shrinkage force to hold itself on the bottle without crushing the contents. In addition, when these labels are applied to polyester containers, they must not interfere with the recycling process of the PET bottles. In fact, it would be advantageous if the label were also recyclable so that the entire bottle could be recycled and converted into new products without incurring additional disposal requirements or creating new environmental problems. Heat shrinkable films are made from a variety of raw materials to meet a range of material requirements. The present disclosure describes unique and unexpected effects measured with certain monomer combinations that improve the recyclability of polyester shrink film labels.
[0070] Shrink film compositions are used commercially as shrink film labels for food, beverages, personal care, household products, etc. Typically, these shrink films are used in combination with clear polyethylene terephthalate (PET) bottles or containers. The entire package (bottle plus label) is then put into the recycling process. In a typical recycling center, the PET and shrink film materials usually end up together at the end of the process due to the similarity in composition and density. The PET flakes need to be dried to remove residual water that is left in the PET through the recycling process. Typically, PET is dried at temperatures above 200°C. At these temperatures, typical polyester shrink film resins will soften and become sticky, often forming clumps with the PET flakes. These clumps must be removed before further processing. These clumps reduce the yield of PET flakes from the process and result in additional handling steps.
[0071] It has been found that certain combinations of diol monomers in shrink film resin compositions can produce films that have good shrink film properties and can also be crystallized so that they do not interfere with the recovery of PET flakes in the recycling process. These crystallizable shrink film resins can be processed with PET bottles and ultimately become a component in the recyclable PET flakes that leave the recycling process. It has also been found that the selection and amount of a specific combination of diol monomers is important for producing films with good shrink film properties and producing crystallizable films.
[0072] The term "polyester" as used herein is intended to include "copolyester" and should be understood to refer to a synthetic polymer prepared by the reaction of one or more difunctional carboxylic acids and / or polyfunctional carboxylic acids with one or more difunctional hydroxyl compounds and / or polyfunctional hydroxyl compounds, such as branching agents. Typically, the difunctional carboxylic acid can be a dicarboxylic acid, and the difunctional hydroxyl compound can be a dihydric alcohol, such as a glycol and diol. The term "glycol" as used herein includes, but is not limited to, a glycol (diol, glycol) and / or a polyfunctional hydroxyl compound, such as a branching agent. Alternatively, the difunctional carboxylic acid can be a hydroxycarboxylic acid, such as p-hydroxybenzoic acid, and the difunctional hydroxyl compound can have an aromatic core with 2 hydroxyl substituents, such as hydroquinone. The term "residue" as used herein refers to any organic structure incorporated into a polymer from the corresponding monomer by polycondensation and / or esterification reactions. The term "repeat unit" as used herein refers to an organic structure having a dicarboxylic acid residue and a diol residue bonded by an ester group. Thus, for example, the dicarboxylic acid residue may be derived from a dicarboxylic acid monomer or its associated acyl halide, ester, salt, anhydride and / or mixtures thereof. In addition, the term "diacid" as used herein includes polyfunctional acids, such as branching agents. Thus, the term "dicarboxylic acid" as used herein is intended to include dicarboxylic acids and any derivatives of dicarboxylic acids that can be used in the reaction process of reacting with a diol to make a polyester, including its associated acyl halide, ester, half ester, salt, half salt, anhydride, mixed anhydride and / or mixtures thereof. The term "terephthalic acid" as used herein is intended to include terephthalic acid itself and its residues that can be used in the reaction process of reacting with a diol to make a polyester, as well as any derivatives of terephthalic acid, including its associated acyl halide, ester, half ester, salt, half salt, anhydride, mixed anhydride and / or mixtures thereof or residues thereof.
[0073] The polyester used in the present disclosure can generally be prepared from dicarboxylic acids and diols that react in substantially equal proportions and are incorporated into the polyester polymer as their corresponding residues. The polyester of the present disclosure may therefore contain substantially equal molar proportions of acid residues (100 mole %) and diol (and / or multifunctional hydroxy compound) residues (100 mole %) to make the total mole number of repeating units equal to 100 mole %. Therefore, the mole percentage provided in the present disclosure may be based on the total mole number of acid residues, the total mole number of diol residues, or the total mole number of repeating units. For example, a polyester containing 10 mole % of isophthalic acid based on total acid residues means that the polyester contains 10 mole % of isophthalic acid residues in a total of 100 mole % of acid residues. Therefore, there are 10 moles of isophthalic acid residues in every 100 moles of acid residues. In another example, a polyester containing 25 mole % of 1,4-cyclohexanedimethanol based on total diol residues means that the polyester contains 25 mole % of 1,4-cyclohexanedimethanol residues in a total of 100 mole % of diol residues. Thus, there are 25 moles of 1,4-cyclohexanedimethanol residues for every 100 moles of diol residues.
[0074] In certain embodiments, terephthalic acid or its esters, such as dimethyl terephthalate or a mixture of terephthalic acid residues and their esters may constitute part or all of the dicarboxylic acid component used to form a polyester that can be used in the present disclosure. In certain embodiments, terephthalic acid residues may constitute part or all of the dicarboxylic acid component used to form a polyester that can be used in the present disclosure. For the purposes of the present disclosure, the terms "terephthalic acid" and "dimethyl terephthalate" are used interchangeably herein. In one embodiment, dimethyl terephthalate is part or all of the dicarboxylic acid component used to make a polyester that can be used in the present disclosure. In embodiments, 70 to 100 mol%; or 80 to 100 mol%; or 90 to 100 mol%; or 99 to 100 mol%; or 100 mol% terephthalic acid and / or dimethyl terephthalate and / or mixtures thereof may be used.
[0075] In addition to terephthalic acid, the dicarboxylic acid component of the polyester that can be used in the present disclosure can include up to 30 mol%, up to 20 mol%, up to 10 mol%, up to 5 mol% or up to 1 mol% of one or more modified aromatic dicarboxylic acids. Another embodiment contains 0 mol% modified aromatic dicarboxylic acid. Therefore, if present, it is contemplated that the amount of one or more modified aromatic dicarboxylic acids can start from any of these aforementioned endpoint values, including, for example, 0.01 to 10 mol%, 0.01 to 5 mol% and 0.01 to 1 mol%. In one embodiment, the modified aromatic dicarboxylic acids that can be used in the present disclosure include, but are not limited to, those having up to 20 carbon atoms, and they can be linear, para-oriented or symmetrical. Examples of modified aromatic dicarboxylic acids that can be used in the present disclosure include, but are not limited to, isophthalic acid, 4,4'-biphenyl dicarboxylic acid, 1,4-, 1,5-, 2,6-, 2,7-naphthalene dicarboxylic acid and trans-4,4'-stilbene dicarboxylic acid, and their esters. In one embodiment, the modifying aromatic dicarboxylic acid is isophthalic acid.
[0076] The carboxylic acid component of the polyester that can be used for the present disclosure can be further modified with up to 10 mol %, such as up to 5 mol % or up to 1 mol % of one or more aliphatic dicarboxylic acids containing 2-16 carbon atoms, such as cyclohexanedicarboxylic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid and / or dodecanedicarboxylic acid. Certain embodiments may also include 0.01 to 10 mol %, such as 0.1 to 10 mol %, 1 or 10 mol %, 5 to 10 mol % of one or more modified aliphatic dicarboxylic acids. Another embodiment contains 0 mol % modified aliphatic dicarboxylic acids. The total mole % of the dicarboxylic acid component is 100 mol %. In one embodiment, adipic acid and / or glutaric acid are provided in the modified aliphatic dicarboxylic acid component of the polyester and the adipic acid and / or glutaric acid can be used for the present disclosure.
[0077] Can use terephthalic acid ester and other modified dicarboxylic acid or their corresponding ester and / or salt to replace dicarboxylic acid.Suitable example of dicarboxylic acid ester includes but not limited to dimethyl ester, diethyl ester, dipropyl ester, diisopropyl ester, dibutyl ester and diphenyl ester.In one embodiment, this ester is selected from at least one of following: methyl ester, ethyl ester, propyl ester, isopropyl ester and phenyl ester.
[0078] In one embodiment, the diol component that can be used for the polyester composition and the polyester blend composition of the present disclosure may include 1,4-cyclohexanedimethanol. In another embodiment, the diol component that can be used for the polyester composition and the polyester blend composition of the present disclosure includes 1,4-cyclohexanedimethanol and 1,3-cyclohexanedimethanol. The molar ratio of cis / trans 1,4-cyclohexanedimethanol may be 50 / 50 to 0 / 100, for example 40 / 60 to 20 / 80.
[0079] The diol component that can be used for the polyester composition and polyester blend composition of the present disclosure can include, but is not limited to, wherein the sum of the residues of 1,4-cyclohexanedimethanol and the residues of neopentyl glycol in the final polyester composition is 0 to 30 mol%, or 1 to 30 mol%, or 1 to 25 mol%, 1 to 20 mol%, or 1 to 15 mol%, or 1 to 10 mol%, or 2 to 30 mol%, or 2 to 25 mol%, or 2 to 20 mol%, or 2 to 15 mol%, or 2 to 10 mol%, or 3 to 30 mol%, or 3 to 25 mol%, or 3 to 20 mol%, or 3 to 15 mol%, or 3 to 10 mol%, 4 to 30 mol%, or 4 to 25 mol%, or 4 to 20 mol%, or 4 to 15 mol%, or 4 to 10 mol%, or 5 to 30 mol%, or 5 to 25 mol%, or 5 to 20 mol%, or 5 to 15 mol%, or 5 ... % or 4 to 15 mol%, or 4 to 10 mol%, or 5 to 30 mol%, or 5 to 25 mol%, 5 to 20 mol%, or 5 to 15 mol%, or 5 to 10 mol%, 6 to 30 mol%, or 6 to 25 mol%, 6 to 20 mol%, or 6 to 15 mol%, or 6 to 10 mol%, 7 to 30 mol%, or 7 to 25 mol%, 7 to 20 mol%, or 7 to 15 mol%, or 7 to 10 mol%, 8 to 30 mol%, or 8 to 25 mol%, 8 to 20 mol%, or 8 to 15 mol%, or 8 to 10 mol%, 9 to 30 mol%, or 9 to 25 mol%, 9 to 20 mol%, or 9 to 15 mol%, or 9 to 10 mol%, 10 to 30 mol%, or 10 to 25 mol%, 10 to 20 mol%, or 10 to 15 mol%, or 11 to 30 mol%, 11 to 30 mol%, or 11 to 25 mol%, 11 to 20 mol%, or 11 to 15 mol%, or 12 to 30 mol%, 12 to 25 mol%, or 12 to 20 mol%, 12 to 15 mol%, or 13 to 30 mol%, or 13 to 25 mol%, 13 to 20 mol%, or 13 to 15 mol%, 14 to 30 mol%, or 14 to 25 mol%, or 14 to 20 mol%, 14 to 15 mol%, or 15 to 30 mol%, 15 to 25 mol%, or %, or 15 to 20 mol%, or 16 to 20 mol%, or 18 to 20 mol%, or 10 to 18 mol%, or 16 to 18 mol%, or 12 to 16 mol%, or 16 to 20 mol%, or 14 to 18 mol%, or 11 to 30 mol%, or 13 to 30 mol%, or 14 to 30 mol%, or 10 to 29 mol%, or 11 to 29 mol%, or 12 to 29 mol%, or 13 to 29 mol%, or 14 to 29 mol%, or 15 to 29 mol%, or 10 to 28 mol%, or 11 to 28 mol%, or 12 to 28 mol%, or 13 to 28 mol%, or 14 to 28 mol%, or 15 to 28 mol%.In one embodiment, the sum of the residues of 1,4-cyclohexanedimethanol and the residues of neopentyl glycol in the final polyester composition may be 4 to 15 mol%, or 2 to 21 mol%, or 2 to less than 20 mol%, or 4 to 20 mol%, or 5 to 18 mol%, or 10 to 21 mol%, or 12 to 21 mol%, wherein the total mol% of the diol component is 100 mol%.
[0080] In one embodiment, the diol component of the polyester composition and the polyester blend composition that can be used in the present disclosure may contain 0 to 30 mol% of neopentyl glycol based on the total mole % of the diol component as 100 mol%. In one embodiment, the diol component of the polyester composition and the polyester blend composition that can be used in the present disclosure may contain 0 to 25 mol% of neopentyl glycol based on the total mole % of the diol component as 100 mol%. In one embodiment, the diol component of the polyester composition and the polyester blend composition that can be used in the present disclosure may contain 0 to 17 mol% of neopentyl glycol based on the total mole % of the diol component as 100 mol%. In one embodiment, the diol component of the polyester composition and the polyester blend composition that can be used in the present disclosure may contain 5 to 20 mol% of neopentyl glycol based on the total mole % of the diol component as 100 mol%. In one embodiment, the diol component of the polyester composition and the polyester blend composition that can be used in the present disclosure may contain 10 to 20 mol% of neopentyl glycol based on the total mole % of the diol component as 100 mol%. In one embodiment, the diol component that can be used in the polyester composition and the polyester blend composition of the present disclosure may contain 10 to 15 mol% of neopentyl glycol based on the total mol% of the diol component being 100 mol%. In one embodiment, the diol component that can be used in the polyester composition and the polyester blend composition of the present disclosure may contain 15 to 25 mol% of neopentyl glycol based on the total mol% of the diol component being 100 mol%.
[0081] In one embodiment, the diol component useful in the polyester composition and polyester blend composition of the present disclosure may contain 0 to 30 mol%, or 0.01 to 30 mol%, or 0 to 20 mol%, or 0.1 to 20 mol%, or 2 to 20 mol%, or 0.01 to 15 mol%, or 0.01 to 14 mol%, or 0.01 to 13 mol%, or 0.01 to 12 mol%, or 0.01 to 11 mol%, or 0.01 to 10 mol%, or 0.01 to 9 mol%, or 0.0 1 to 8 mol%, or 0.01 to 7 mol%, or 0.01 to 6 mol%, or 0.01 to 5 mol%, or 3 to 15 mol%, or 3 to 14 mol%, or 3 to 13 mol%, or 3 to 12 mol%, or 3 to 11 mol%, or 3 to 10 mol%, or 3 to 9 mol%, or 3 to 8 mol%, or 3 to 7 mol%, or 2 to 10 mol%, or 2 to 9 mol%, or 2 to 8 mol%, or 2 to 7 mol%, or 2 to 5 mol%, or 1 to 7 mol%, or 1 to 5 mol%, or 1 to 3 mol% of 1,4-cyclohexanedimethanol residues.
[0082] In one embodiment, the diol component that can be used for the polyester composition of the present disclosure may contain 0.01 to 15 mol% of 1,4-cyclohexanedimethanol based on the total mol% of the diol component as 100 mol%. In one embodiment, the diol component that can be used for the polyester composition of the present disclosure may contain 0 to less than 15 mol% of 1,4-cyclohexanedimethanol based on the total mol% of the diol component as 100 mol%. In one embodiment, the diol component that can be used for the polyester composition of the present disclosure may contain 0.01 to 10 mol% of 1,4-cyclohexanedimethanol based on the total mol% of the diol component as 100 mol%. In one embodiment, the diol component that can be used for the polyester composition of the present disclosure may contain 0 to less than 10 mol% of 1,4-cyclohexanedimethanol based on the total mol% of the diol component as 100 mol%. In one embodiment, the diol component that can be used for the polyester composition of the present disclosure may contain 0.01 to 5 mol% of 1,4-cyclohexanedimethanol based on the total mol% of the diol component as 100 mol%. In one embodiment, the diol component useful in the polyester composition of the present disclosure may contain 0 to less than 5 mole % of 1,4-cyclohexanedimethanol based on the total mole % of the diol component being 100 mole %.
[0083] It should be understood that some other diol residues may be formed in situ during processing. The total amount of diethylene glycol residues may be present in the polyesters useful for the present disclosure, whether formed in situ during processing or intentionally added, or both, in any amount, for example, from 1 to 15 mol%, or 2 to 12 mol%, or 2 to 11 mol%, or 2 to 10 mol%, or 2 to 9 mol%, or 3 to 12 mol%, or 3 to 11 mol%, or 3 to 10 mol%, or 3 to 9 mol%, or 4 to 12 mol%, or 4 to 11 mol%, or 4 to 10 mol%, or 4 to 9 mol%, or 5 to 12 mol%, or 5 to 11 mol%, or 5 to 10 mol%, or 5 to 9 mol% of diethylene glycol residues, based on the total mol% of the diol component being 100 mol%.
[0084] In one embodiment, the total amount of diethylene glycol residues present in the polyesters useful in the present disclosure, whether formed in situ during processing or intentionally added, or both, can be 4 mol% or less, or 3.5 mol% or less, or 3.0 mol% or less, or 2.5 mol% or less, or 2.0 mol% or less, or 1.5 mol% or less, or 1.0 mol% or less, or 1 to 4 mol%, or 1 to 3 mol%, or 1 to 2 mol% of diethylene glycol residues, or 2 to 8 mol%, or 2 to 7 mol%, or 2 to 6 mol%, or 2 to 5 mol%, or 3 to 8 mol%, or 3 to 7 mol%, or 3 to 6 mol%, or 3 to 5 mol%, or in some embodiments, no intentionally added diethylene glycol residues, based on the total mol% of the diol component being 100 mol%. In certain embodiments, the polyester contains no added modifying glycol.
[0085] For all embodiments, the balance of the diol component may comprise any amount of ethylene glycol residues based on the total mole % of the diol component being 100 mole %. In one embodiment, the polyester portion of the polyester composition useful in the present disclosure may contain 50 mole % or more, or 55 mole % or more, or 60 mole % or more, or 65 mole % or more, or 70 mole % or more, or 75 mole % or more, or 80 mole % or more, or 85 mole % or more, or 90 mole % or more, or 95 mole % or more, or 50 to 80 mole %, or 55 to 80 mole %, or 60 to 80 mole %, or 50 to 75 mole %, or 55 to 75 mole %, or 60 to 75 mole %, or 65 to 75 mole % of ethylene glycol residues based on the total mole % of the diol component being 100 mole %.
[0086] In one embodiment, the diol component of the polyester composition useful in the present disclosure may contain up to 20 mol%, or up to 19 mol%, or up to 18 mol%, or up to 17 mol%, or up to 16 mol%, or up to 15 mol%, or up to 14 mol%, or up to 13 mol%, or up to 12 mol%, or up to 11 mol%, or up to 10 mol%, or up to 9 mol%, or up to 8 mol%, or up to 7 mol%, or up to 6 mol%, or up to 5 mol%, or up to 4 mol%, or up to 3 mol%, or up to 2 mol%, or up to 1 mol% or less of one or more modified diols (modified diols are defined as diols that are not ethylene glycol, diethylene glycol, neopentyl glycol, or 1,4-cyclohexanedimethanol). In certain embodiments, the polyester composition useful in the present disclosure may contain 10 mol% or less of one or more modified diols. In certain embodiments, the polyester useful in the present disclosure may contain 5 mol% or less of one or more modified diols. In certain embodiments, the polyester useful in the present disclosure may contain 3 mol% or less of one or more modified diols. In another embodiment, the polyesters useful in the present disclosure may contain 0 mole % of modifying diols. However, it is contemplated that some other diol residues may be formed in situ such that the amount of residues formed in situ is also an embodiment of the present disclosure.
[0087] In an embodiment, if used, the modified glycol for polyester as specified herein contains 2 to 16 carbon atoms. Examples of modified glycols include, but are not limited to, 1,2-propylene glycol, 1,3-propylene glycol, isosorbide, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, p-xylene glycol, polytetramethylene glycol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD), and mixtures thereof. In one embodiment, isosorbide is a modified glycol. In another embodiment, the modified glycol includes, but is not limited to, at least one of 1,3-propylene glycol and 1,4-butanediol. In one embodiment, 1,3-propylene glycol and / or 1,4-butanediol may be excluded. If 1,4- or 1,3-butanediol is used, more than 4 mol % or more than 5 mol % may be provided in one embodiment. In one embodiment, at least one modified glycol is 1,4-butanediol present in an amount of 5 to 25 mol %.
[0088] In one embodiment, a shrink film is provided, comprising a polyester composition, the polyester composition further comprising: 1,4-cyclohexanedimethanol residues present in an amount of 0.01 to about 10 mol %, diethylene glycol residues present in an amount of 2 to 9 mol %, neopentyl glycol residues present in an amount of 5 to 30 mol %, and ethylene glycol residues present in an amount of 60 mol % or more, based on the total mol % of the diol component being 100 mol %.
[0089] In some embodiments, polyesters according to the present disclosure may contain 0 to 10 mol%, e.g., 0.01 to 5 mol%, 0.01 to 1 mol%, 0.05 to 5 mol%, 0.05 to 1 mol%, or 0.1 to 0.7 mol% of one or more branching monomers (also referred to herein as branching agents) having 3 or more carboxyl substituents, hydroxyl substituents, or a combination thereof, based on the total mole percentage of diol or diacid residues, respectively. In certain embodiments, branching monomers or branching agents may be added before and / or during and / or after polymerization of the polyester. In some embodiments, the polyester(s) useful in the present disclosure may therefore be linear or branched.
[0090] Examples of branching monomers include, but are not limited to, polyfunctional acids or polyfunctional alcohols such as trimellitic acid, trimellitic anhydride, pyromellitic dianhydride, trimethylolpropane, glycerol, pentaerythritol, citric acid, tartaric acid, 3-hydroxyglutaric acid, and the like. In one embodiment, the branching monomer residues may include 0.1 to 0.7 mole % of one or more residues selected from at least one of the following: trimellitic anhydride, pyromellitic dianhydride, glycerol, sorbitol, 1,2,6-hexanetriol, pentaerythritol, trimethylolethane, and / or trimellitic acid. The branching monomers may be added to the polyester reaction mixture or blended with the polyester in the form of a concentrate as described, for example, in U.S. Pat. Nos. 5,654,347 and 5,696,176 (which are incorporated herein by reference for their disclosure of branching monomers).
[0091] The polyesters useful in the present disclosure may include at least one chain extender. Suitable chain extenders include, but are not limited to, multifunctional (including but not limited to difunctional) isocyanates, multifunctional epoxides, including, for example, epoxy novolacs and phenoloxy resins. In certain embodiments, the chain extender may be added at the end of the polymerization process or after the polymerization process. If added after the polymerization process, the chain extender may be incorporated by compounding or by addition during a conversion process, such as injection molding or extrusion.
[0092] The amount of chain extender used may vary depending upon the specific monomer composition used and the physical properties desired, but is typically from about 0.1 wt % to about 10 wt %, such as from about 0.1 to about 5 wt %, based on the total weight of the polyester.
[0093] Unless otherwise specified, it is contemplated that the polyester compositions useful in the present disclosure may have at least one intrinsic viscosity range described herein and at least one monomer range for the polyester compositions described herein. It is also contemplated that the polyester compositions useful in the present disclosure may have at least one intrinsic viscosity range described herein, unless otherwise specified. gUnless otherwise indicated, it is also contemplated that the polyester compositions useful in the present disclosure may have at least one intrinsic viscosity range described herein, at least one T range described herein, and at least one monomer range described herein. g range and at least one monomer range of the polyester compositions described herein.
[0094] For embodiments of the present disclosure, the polyesters useful for the present disclosure may exhibit at least one of the following intrinsic viscosities as measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.25 g / 50 ml at 25° C.: 0.50 to 1.2 dL / g; 0.50 to 1.0 dL / g; 0.50 to 0.90 dL / g; 0.50 to 0.80 dL / g; 0.55 to 0.80 dL / g; 0.60 to 0.80 dL / g; 0.65 to 0.80 dL / g; 0.70 to 0.80 dL / g; 0.50 to 0.75 dL / g; 0.55 to 0.75 dL / g; or 0.60 to 0.75 dL / g.
[0095] The glass transition temperature (Tg) of the polyesters was determined using a TA DSC 2920 from Thermal Analyst Instrument at a scan rate of 20°C / min.
[0096] In certain embodiments, the oriented or shrink film of the present disclosure comprises a polyester / polyester composition wherein the polyester has a Tg of 60 to 80° C.; 70 to 80° C.; or 65 to 80° C.; or 65 to 75° C. In certain embodiments, these Tg ranges may be met with or without the addition of at least one plasticizer during the polymerization process.
[0097] In embodiments of the present disclosure, certain oriented films and / or shrinkable films comprising the polyesters and / or polyester compositions useful in the present disclosure may have a unique combination of all of the following properties: good stretchability, controlled shrinkage properties, a certain toughness, a certain intrinsic viscosity, a certain glass transition temperature (Tg), a certain strain induced crystalline melting point, a certain flexural modulus, a certain density, a certain tensile modulus, a certain surface tension, good melt viscosity, good clarity, and good color.
[0098] In one embodiment, certain polyester compositions useful in the present disclosure may be visually clear.The term "visually clear" is defined herein as being appreciably absent of cloudiness, haziness, and / or muddiness upon visual inspection.
[0099] The polyester portion of the polyester composition useful in the present disclosure can be made by methods known in the literature, such as by a process in a homogeneous solution, by a transesterification process in a melt, and by a two-phase interface process. Suitable methods include, but are not limited to, a step of reacting one or more dicarboxylic acids with one or more diols at a temperature of 100° C. to 315° C. and a pressure of 0.1 to 760 mm Hg for a time sufficient to form a polyester. For methods of producing polyesters, see U.S. Pat. No. 3,772,405, which is incorporated herein by reference for disclosure of such methods.
[0100] As described in more detail in U.S. Pat. No. 2,720,507, which is incorporated herein by reference, polyesters can generally be prepared by condensing a dicarboxylic acid or a dicarboxylic acid ester with a diol in an inert atmosphere in the presence of a catalyst at elevated temperatures (which gradually increase during the condensation to temperatures as high as about 225° C. to 310° C.) and conducting the condensation under reduced pressure in the later stages of the condensation.
[0101] In some embodiments, in the process of making the polyester that can be used in the present disclosure, certain reagents that color the polymer, including toners or dyes, can be added to the melt. In one embodiment, a bluing toner is added to the melt to reduce the b* of the resulting polyester polymer melt phase product. Such bluing agents include (one or more) blue inorganic and organic toners and / or dyes. In addition, (one or more) red toners and / or dyes can also be used to adjust the a* color. (One or more) organic toners can be used, such as (one or more) blue and red organic toners, such as those (one or more) toners described in U.S. Patent Nos. 5,372,864 and 5,384,377, which are incorporated herein by reference in their entirety. (One or more) organic toners can be fed as a premixed composition. The premixed composition can be a pure blend of red and blue compounds, or the composition can be pre-dissolved or pulped in one of the raw materials of the polyester, such as ethylene glycol.
[0102] The total amount of toner components added may depend on the amount of yellow inherent in the base polyester and the effectiveness of the toner. In one embodiment, concentrations of up to about 15 ppm of combined organic toner components may be used, with a minimum concentration of about 0.5 ppm. In one embodiment, the total amount of bluing additive may be 0.5 to 10 ppm. In one embodiment, the toner(s) may be added to the esterification zone or the polycondensation zone. It is preferred that the toner(s) be added to the esterification zone or to the early stages of the polycondensation zone, such as in a prepolymerization reactor.
[0103] The present disclosure further relates to polymer blends. In one embodiment, the polymer blend comprises:
[0104] (a) 5 to 95 weight percent of a polyester composition of the present disclosure as described herein; and
[0105] (b) 5 to 95% by weight of at least one polymer component.
[0106] Suitable examples of polymer components include, but are not limited to, nylon; polyesters other than those described herein; polyamides, such as ZYTEL® from DuPont; polystyrene; polystyrene copolymers; styrene acrylonitrile copolymers; acrylonitrile butadiene styrene copolymers; poly(methyl methacrylate); acrylic copolymers; poly(ether-imides), such as ULTEM® (poly(ether-imide) from General Electric); polyphenylene ethers, such as poly(2,6-dimethylphenylene ether) or poly(phenylene ether) / polystyrene blends, such as NORYL 1000® (a blend of poly(2,6-dimethylphenylene ether) and polystyrene resin from General Electric); polyphenylene sulfide; polyphenylene sulfide / sulfone; poly(ester-carbonate); polycarbonate, such as LEXAN® (polycarbonate from General Electric); polysulfone; polysulfone ether; and poly(ether-ketone) of aromatic dihydroxy compounds; or mixtures of any of the foregoing polymers. In one embodiment, aliphatic-aromatic polyesters may be excluded from the polyester compositions useful in the present disclosure. The following polyesters that can be blended to make the polyester compositions of the present disclosure can be excluded as polymer components for additional blending if such blending exceeds the compositional range of the present disclosure: polyethylene terephthalate (PET), glycol-modified PET (PETG), glycol-modified poly(cyclohexylene dimethylene terephthalate) (PCTG), poly(cyclohexylene dimethylene terephthalate) (PCT), acid-modified poly(cyclohexylene dimethylene terephthalate) (PCTA), poly(butylene terephthalate) and / or diethylene glycol-modified PET (EASTOBOND™ copolyester).
[0107] The blends can be prepared by conventional processing techniques known in the art, such as melt blending or solution blending.
[0108] In embodiments, the polyester composition and polymer blend composition may also contain from 0.01 to 25% by weight of the total composition of commonly used additives such as colorants, (one or more) toners, dyes, mold release agents, flame retardants, plasticizers, glass bubbles, nucleating agents, stabilizers, including but not limited to UV stabilizers, heat stabilizers and / or reaction products thereof, fillers and impact modifiers. Examples of commercially available impact modifiers include but are not limited to ethylene / propylene terpolymers, functionalized polyolefins such as those containing methyl acrylate and / or glycidyl methacrylate, styrene-based block copolymer impact modifiers, and various acrylic core / shell impact modifiers. Residues of these additives are also contemplated as part of the polyester composition.
[0109] Reinforcement materials can be added to compositions useful in the present disclosure. Reinforcement materials can include, but are not limited to, carbon filaments, silicates, mica, clay, talc, titanium dioxide, wollastonite, glass flakes, glass beads and fibers, and polymer fibers and combinations thereof. In one embodiment, the reinforcement material comprises glass, such as fiberglass filaments, a mixture of glass and talc, a mixture of glass and mica, and a mixture of glass and polymer fibers.
[0110] In one embodiment, films and shrink films according to the present disclosure may contain 0.01 to 10 wt % of a polyester plasticizer. In one embodiment, the shrink film may contain 0.1 to 5 wt % of a polyester plasticizer. Typically, the shrink film may contain 90 to 99.99 wt % of a copolyester. In certain embodiments, the shrink film may contain 95 to 99.9 wt % of a copolyester.
[0111] In one aspect, the present disclosure relates to (one or more) shrink films and molded articles of the present disclosure comprising polyester compositions and / or polymer blends that can be used in the present disclosure. Methods of molding polyesters and / or blends into (one or more) films and / or sheets are well known in the art. Examples of (one or more) films and / or sheets that can be used in the present disclosure include, but are not limited to, (one or more) extruded films and / or sheets, (one or more) compression molded films, (one or more) calendered films and / or sheets, (one or more) solution cast films and / or sheets. In one aspect, methods of making films and / or sheets that can be used to make shrink films of the present disclosure include, but are not limited to, extrusion, compression molding, calendering, and solution casting.
[0112] In one embodiment, the polyester compositions useful in the present disclosure are made into films using any method known in the art for producing films from polyesters, such as solution casting, extrusion, compression molding, or calendaring.
[0113] In one embodiment, the formed film is subsequently oriented in one or more directions (e.g., uniaxially and / or biaxially oriented films). Such orientation of the film can be performed by any method known in the art using standard orientation conditions. For example, the oriented film of the present disclosure can be made from a film having a thickness of about 100 to 400 microns, such as an extruded, cast, or calendered film, which can be formed at T g To T g Orientation at a temperature of +55°C or 70°C to 125°C at a ratio of 5:1 to 3:1, for example, at a temperature of 100°C to 114°C at a ratio of 5:1 or 3:1, and can be oriented to a thickness of 20 to 80 microns. In one embodiment, orientation of the initial pre-shrink film can be carried out on a tenter frame according to these orientation conditions.
[0114] The shrink film of the present disclosure may have a shrink initiation temperature of about 55 to about 80° C., or about 55 to about 75° C., or about 55 to about 70° C. The shrink initiation temperature is the temperature at which shrinkage begins to occur.
[0115] In certain embodiments, the polyester compositions useful in the present disclosure may have a density of 1.6 g / cc or less, or 1.5 g / cc or less, or 1.4 g / cc or less, or from 1.1 g / cc to 1.5 g / cc, or from 1.2 g / cc to 1.4 g / cc, or from 1.2 g / cc to 1.35 g / cc.
[0116] In one embodiment, the density of the film is reduced by introducing many small voids or holes in the film or shaped article. This method is called "voiding", and may also be referred to as "cavitating" or "microvoiding". The voids are obtained by incorporating about 1 to about 50% by weight of small organic or inorganic particles (including glass microspheres) or "inclusions" (referred to in the art as "voiding" or "cavitating" agents) into the matrix polymer and by stretching in at least one direction to orient the polymer. During the stretching process, small holes or voids are formed around the voiding agent. When voids are introduced into the polymer film, the resulting voided film not only has a lower density than a void-free film, but also becomes opaque and forms a paper-like surface. Such a surface also has the advantage of improved printability; that is, the surface is able to accept many inks at a significantly higher capacity than a void-free film. Typical examples of void-containing films are described in U.S. Pat. Nos. 3,426,754; 3,944,699; 4,138,459; 4,582,752; 4,632,869; 4,770,931; 5,176,954; 5,435,955; 5,843,578; 6,004,664; 6,287,680; 6,500,533; 6,720,085; U.S. Patent Application Publication Nos. 2001 / 0036545; 2003 / 0068453; 2003 / 0165671; 2003 / 0170427; Japanese Patent Application Nos. 61-037827; 63-193822; 2004-181863; European Patent No. 0 581 970 B1 and European patent application No. 0 214 859 A2.
[0117] In certain embodiments, the extruded film is oriented while being stretched. Oriented films or shrinkable films of the present disclosure may be made of films having any thickness, depending on the desired end use. In one embodiment, a desirable condition is that the oriented film and / or shrinkable film may be printed with ink for use in applications including labels, photosensitive films that may be attached to substrates such as paper, and / or other applications in which it may be useful. It may be desirable to coextrude polyesters that may be used in the present disclosure with another polymer, such as PET, to make films that may be used to make oriented films and / or shrinkable films of the present disclosure. An advantage of the latter approach is that a tie layer may not be required in some embodiments.
[0118] In one embodiment, the uniaxially and biaxially oriented films of the present disclosure may be made from films having a thickness of about 100 to 400 microns, such as extruded, cast, or calendered films, which may be formed at the T of the film. g To T gThe film can be stretched at a temperature of +55°C at a ratio of 6.5:1 to 3:1, and can be stretched to a thickness of 20 to 80 microns. In one embodiment, the orientation of the initially extruded film can be carried out on a tenter according to these orientation conditions. The shrink film of the present disclosure can be made from the oriented film of the present invention.
[0119] In certain embodiments, the shrink films of the present disclosure have a gradual shrinkage with little wrinkling. In certain embodiments, the shrink films of the present disclosure have a shrinkage in the cross direction of no more than 40% per 5°C temperature increment.
[0120] In certain embodiments of the present disclosure, when immersed in 65°C water for 10 seconds, the shrink film of the present disclosure has a shrinkage of 10% or less, or 5% or less, or 3% or less, or 2% or less in the machine direction, or no shrinkage. In certain embodiments of the present disclosure, when immersed in 65°C water for 10 seconds, the shrink film of the present disclosure has a shrinkage of -10% to 10%, -5% to 5%, or -5% to 3%, or -5% to 2%, or -4% to 4%, or -3% to 4%, or -2% to 4%, or -2% to 2.5%, or -2% to 2%, or 0 to 2% in the machine direction, or no shrinkage. Negative machine direction shrinkage percentages refer to machine direction growth here. Positive machine direction shrinkage refers to shrinkage in the machine direction.
[0121] In certain embodiments of the present disclosure, the shrink film of the present disclosure has a shrinkage rate of 50% or more, or 60% or more, or 70% or more in the main shrinking direction when immersed in 95° C. water for 10 seconds.
[0122] In certain embodiments of the present disclosure, the shrink film of the present disclosure has a shrinkage of 50 to 90% in the main shrink direction and 10% or less, or -10% to 10% in the machine direction when immersed in 95°C water for 10 seconds.
[0123] In one embodiment, the polyesters useful in the present disclosure are formed into films using any method known in the art for producing films from polyesters, such as solution casting, extrusion, compression molding, or calendaring. The extruded (or formed) film is then oriented in one or more directions (e.g., a uniaxially and / or biaxially oriented film). Such orientation of the film can be performed by any method known in the art using standard orientation conditions. For example, the uniaxially oriented film of the present disclosure can be made from a film having a thickness of about 100 to 400 microns, such as an extruded, cast, or calendared film, which can be formed at the T of the film. g To T g It is stretched at a temperature of +55°C at a ratio of 6.5:1 to 3:1, and it can be stretched to a thickness of 20 to 80 microns. In one embodiment, orientation of the initially extruded film can be carried out on a tenter frame according to these orientation conditions.
[0124] In certain embodiments of the present disclosure, the shrink film of the present disclosure has a shrinkage in the cross direction of no more than 40% per 5°C temperature increment.
[0125] In certain embodiments of the present disclosure, the shrink film of the present disclosure may have a shrink initiation temperature of about 55 to about 80° C., or about 55 to about 75° C., or 55 to about 70° C. The shrink initiation temperature is the temperature at which shrinkage begins to occur.
[0126] In certain embodiments of the present disclosure, the shrink film of the present disclosure may have a shrinkage initiation temperature of 55°C to 70°C.
[0127] In certain embodiments of the present disclosure, the shrink film of the present disclosure may have a percent strain at break greater than 200% at a stretching speed of 500 mm / min in a direction perpendicular to the main shrinking direction according to ASTM method D882.
[0128] In certain embodiments of the present disclosure, the shrink film of the present disclosure may have a percent strain at break greater than 300% at a stretching speed of 500 mm / min in a direction perpendicular to the main shrinking direction according to ASTM method D882.
[0129] In certain embodiments of the present disclosure, the shrink film of the present disclosure may have a tensile stress at break (break stress) of 20 to 400 MPa; or 40 to 260 MPa; or 42 to 260 MPa as measured according to ASTM method D882.
[0130] In certain embodiments of the present disclosure, the shrink film of the present disclosure may have a shrink force of 4 to 18 MPa, or 4 to 15 MPa, depending on the stretching conditions and the desired end use, as measured by ISO Method 14616. For example, certain labels made for plastic bottles may have a shrink force of 4 to 8 MPa, and certain labels made for glass bottles may have a shrink force of 10 to 14 MPa as measured by ISO Method 14616 at 80°C using a Shrink Force Tester manufactured by LabThink.
[0131] In one embodiment of the present disclosure, the polyester composition may be formed by reacting monomers by known methods for making polyesters which are generally referred to as reactor grade compositions.
[0132] In one embodiment of the present disclosure, the polyester compositions of the present disclosure can be formed by blending polyesters such as polyethylene terephthalate (PET), glycol-modified PET (PETG), glycol-modified poly(cyclohexylene dimethylene terephthalate) (PCTG), poly(cyclohexylene dimethylene terephthalate) (PCT), acid-modified poly(cyclohexylene dimethylene terephthalate) (PCTA), poly(butylene terephthalate) and / or diethylene glycol-modified PET (EASTOBOND™ copolyester) to achieve the monomer ranges of these compositions.
[0133] In certain embodiments, the polyester composition and polymer blend composition may also contain 0.01 to 25% by weight of common additives such as colorants, (one or more) toners, dyes, release agents, flame retardants, plasticizers, glass bubbles, nucleating agents, stabilizers, including but not limited to UV stabilizers, heat stabilizers and / or reaction products thereof, fillers and impact modifiers, based on the total composition. Examples of commercially available impact modifiers include but are not limited to ethylene / propylene terpolymers, functionalized polyolefins such as those containing methyl acrylate and / or glycidyl methacrylate, styrene-based block copolymer impact modifiers, and various acrylic core / shell impact modifiers. Residues of these additives are also contemplated as part of the polyester composition.
[0134] Reinforcement materials can be added to the polyester compositions useful in the present disclosure. Reinforcement materials can include, but are not limited to, carbon filaments, silicates, mica, clay, talc, titanium dioxide, wollastonite, glass flakes, glass beads and fibers, and polymer fibers and combinations thereof. In one embodiment, the reinforcement material comprises glass, such as fiberglass filaments, a mixture of glass and talc, a mixture of glass and mica, and a mixture of glass and polymer fibers.
[0135] Molded articles, which may or may not consist of or contain a shrink film, may also be made from any of the polyester compositions disclosed herein and are included within the scope of the present disclosure.
[0136] Typically, the shrink film according to the present disclosure may contain 0.01 to 10 wt % of a polyester plasticizer. In one embodiment, the shrink film may contain 0.1 to 5 wt % of a polyester plasticizer. Typically, the shrink film may contain 90 to 99.99 wt % of a copolyester. In certain embodiments, the shrink film may contain 95 to 99.9 wt % of a copolyester.
[0137] In one embodiment, when having a pre-oriented thickness of about 100 to 400 microns and subsequently oriented on a tenter frame at a temperature of Tg to Tg + 55°C at a ratio of 6.5:1 to 3:1 to a thickness of about 20 to about 80 microns, the shrink film of the present disclosure may have one or more of the following properties:
[0138] (1) When immersed in 95°C water for 10 seconds, the amount of shrinkage in the main shrinkage direction or transverse direction is greater than 60% (or greater than 70%), and the shrinkage in the machine direction is 10% or less (or -5% to 4%);
[0139] (2) a shrinkage onset temperature of about 55°C to about 70°C;
[0140] (3) a percent strain at break of greater than 200%, or from 200 to 600%, or from 200 to 500%, or from 226 to 449%, or from 250 to 455% in the cross direction or in the machine direction or in both directions at a tensile speed of 500 mm / min according to ASTM method D882;
[0141] (4) A shrinkage of not more than 40% per 5°C temperature increment; and / or
[0142] (5) a strain-induced crystalline melting point greater than 200°C. Any combination of these properties or all of these properties may be present in the shrink film of the present disclosure. The shrink film of the present disclosure may have a combination of two or more of the above shrink film properties. The shrink film of the present disclosure may have a combination of three or more of the above shrink film properties. The shrink film of the present disclosure may have a combination of four or more of the above shrink film properties. In certain embodiments, properties (1)-(2) are present. In certain embodiments, properties (1)-(5) are present. In certain embodiments, properties (1)-(3) are present, and so on.
[0143] The shrinkage percentages herein are based on an initially formed film having a thickness of about 20 to 80 microns that has been oriented on a tenter frame at a temperature of Tg to Tg + 55° C. at a ratio of 6.5:1 to 3:1, such as oriented at a ratio of 5:1 at a temperature of 70° C. to 85° C. In one embodiment, the shrinkage properties of the oriented film used to make the shrink film of the present disclosure are not adjusted by annealing the film at a temperature above the temperature at which it is oriented.
[0144] The shape of the film that can be used to make the oriented film or shrink film of the present disclosure is not limited in any way. For example, it can be a flat film or a film that has been formed into a tube. In order to produce the shrink film that can be used in the present disclosure, the polyester is first formed into a flat film and then "uniaxially stretched", which means that the polyester film is oriented in one direction. The film can also be "biaxially oriented", which means that the polyester film is oriented in two different directions; for example, the film is stretched in the machine direction and in a direction different from the machine direction. Usually, but not always, the two directions are substantially perpendicular. For example, in one embodiment, the two directions are in the longitudinal or machine direction ("MD") of the film (the direction in which the film is produced on the film making machine) and the transverse ("TD") direction of the film (the direction perpendicular to the MD of the film). The biaxially oriented film can be sequentially oriented, simultaneously oriented, or oriented by some combination of simultaneous and sequential stretching.
[0145] The film can be oriented by any common method, such as roller stretching, long gap stretching, tenter stretching, and tubular stretching. By using any of these methods, sequential biaxial stretching, simultaneous biaxial stretching, uniaxial stretching, or a combination of these can be performed. For the biaxial stretching mentioned above, stretching in the machine direction and the transverse direction can be performed simultaneously. Stretching can also be performed first in one direction and then in the other direction to produce effective biaxial stretching. In one embodiment, the film is initially heated to its glass transition temperature (T g ) above 5°C to 80°C for stretching the film. In one embodiment, the film may be initially heated to its T g The film may be oriented at 10°C to 30°C or more. In one embodiment, the stretching rate is 5 to 20 inches (12.7 to 50.8 centimeters) per second. The film may then be oriented, for example, in the machine direction, the transverse direction, or both directions, to 2 to 6 times the original measurement. The film may be oriented as a single film layer, or may be coextruded with another polyester, such as PET (polyethylene terephthalate), as a multilayer film and then oriented.
[0146] In one embodiment, the present disclosure includes a manufactured or shaped article comprising a shrink film of any shrink film embodiment of the present disclosure. In another embodiment, the present disclosure includes a manufactured or shaped article comprising an oriented film of any oriented film embodiment of the present disclosure.
[0147] In certain embodiments, the present disclosure includes, but is not limited to, shrink films applied to containers, plastic bottles, glass bottles, packaging, battery packs, hot-fill containers, and / or industrial articles, or other applications. In one embodiment, the present disclosure includes, but is not limited to, oriented films applied to containers, packaging, plastic bottles, glass bottles, photosensitive substrates such as paper, battery packs, hot-fill containers, and / or industrial articles, or other applications.
[0148] In certain embodiments of the present disclosure, the shrink film of the present disclosure can be formed into a label or sleeve. The label or sleeve can then be applied to a finished product, such as a container wall, a battery pack, or applied to a sheet or film.
[0149] The oriented films or shrink films of the present disclosure can be applied to shaped articles, such as sheets, films, tubes, bottles, and are commonly used in various packaging applications. For example, films and sheets made from polymers such as polyolefins, polystyrene, poly(vinyl chloride), polyesters, polylactic acid (PLA) are often used to make shrink labels for plastic beverage or food containers. For example, the shrink films of the present disclosure can be used in many packaging applications, wherein the shrink films applied to shaped articles exhibit properties such as good printability, high opacity, higher shrink force, good texture, and good stiffness.
[0150] The combination of improved shrink properties and improved toughness provides new commercial options including, but not limited to, shrink films for containers, plastic bottles, glass bottles, packaging, battery packs, hot fill containers and / or industrial articles or other applications.
[0151] In one aspect of the present disclosure, the disclosed polyester compositions can be used as (one or more) thermoformed and / or thermoformable films or sheets. The present disclosure also relates to manufactured articles comprising (one or more) thermoformed films and / or sheets of the present disclosure. In one embodiment, the polyester compositions of the present disclosure can be used as films and sheets that are easily formed into shaped articles or molded articles. In one embodiment, the (one or more) films and / or sheets of the present disclosure can be processed into molded articles or molded parts by thermoforming. The polyester compositions of the present disclosure can be used in various molding and extrusion applications.
[0152] Furthermore, in one embodiment, the polyester composition and polyester blend composition useful for the thermoforming sheet(s) of the present disclosure may also contain 0.1 to 25 wt % of the total composition of commonly used additives such as colorants, mold release agents, flame retardants, plasticizers, nucleating agents, stabilizers, including but not limited to UV stabilizers, heat stabilizers, fillers, and impact modifiers.
[0153] In one embodiment, reinforcing materials may be included in the thermoformed film(s) or sheet(s) comprising the polyester composition of the present disclosure. For example, suitable reinforcing materials may include carbon filaments, silicates, mica, clay, talc, titanium dioxide, wollastonite, glass flakes, glass beads and fibers, and polymer fibers and combinations thereof.
[0154] In one embodiment, the thermoformed film or sheet is a multilayer film or sheet.In one embodiment, at least one layer of the multilayer film or sheet is a foamed or expanded polymer or polyester layer.
[0155] One aspect of the present disclosure is a method of making molded or formed parts and articles using thermoforming.Any thermoforming technique or method known to those skilled in the art can be used to produce the molded or formed articles of the present disclosure.
[0156] In one embodiment, the thermoforming process can be carried out in several ways, such as taught in "Technology of Thermoforming"; Throne, James; Hanser Publishers; 1996; pages 16-29, which are incorporated herein by reference. In some embodiments, it is a positive thermoforming process, in which gas or air pressure is applied to the softened sheet, and the sheet is then stretched and drawn out like a bubble, and a male mold is introduced into the bubble from the inside. Vacuum is then applied to allow the part to be further drawn and follow the male mold surface. In this thermoforming process, biaxial stretching / orientation is mainly completed in one step with gas or air pressure applied to the softened sheet. The molding step is then completed by vacuum and male mold to freeze the orientation into the sheet to achieve a good balance of physical and appearance properties. In other embodiments, it is a negative thermoforming process in which a vacuum or physical plug is applied to the heat softened sheet and the sheet is stretched and drawn to near final part dimensions, then positive air pressure from the inside or further external vacuum from the outside pulls the sheet and causes it to follow an external negative mold, fixing the orientation into the polymer and forming the sheet into an article.
[0157] In some embodiments, the bubbles generated are further shaped, sometimes with the aid of a plunger, after which the sheet is covered and shaped on the raised male mold, and then the corners and shelf guides, etc., are pulled into the mold by applying a vacuum. In some embodiments, after being removed from the mold, the molded part or molded article can be trimmed, punched, and corner cut as needed.
[0158] In other embodiments, thermoforming is a process in which a film or sheet of the polyester composition of the present disclosure is heated to a temperature sufficient to deform it, and then the heated film or sheet is made to follow the contours of the mold by means such as vacuum assistance, gas pressure assistance, and matched mold assistance. In another embodiment, the heated film or sheet is placed in a mold and forced to follow the contours of the mold by, for example, applying gas pressure, applying a vacuum, plunger assistance, or using a matched mold. In some embodiments, thermoforming produces thin-walled articles.
[0159] In one embodiment, the thermoforming method molds the film or sheet into the desired shape by pressing the male mold into the heated film or sheet. In this embodiment, thermoforming involves supporting the male mold of the product between the surface or countertop equipped with vacuum. In this embodiment, the heat from an external heat source, such as a hot air blower, a heat lamp or other radiant heat source, is directed at the film or sheet. In this embodiment, the film or sheet is heated to a softening point. In this embodiment, a vacuum is then applied to the countertop and below the countertop and around the mold, and the heat-softened film or sheet is pulled toward the countertop, so that the softened film or sheet is contacted with the mold surface. In this embodiment, the vacuum pulls the softened film or sheet to close contact with the contour of the mold surface and follows the contour of the mold surface. Therefore, the film or sheet then presents the shape of the mold. In this embodiment, after the film or sheet cools, it hardens, and the resulting product or parts can be taken out from the mold.
[0160] In one embodiment, the thermoforming process comprises: forming a film or sheet from the polyester composition of the present disclosure; heating the film or sheet until it softens and positioning it over a mold; drawing the preheated film or sheet onto the heated mold surface; cooling the film or sheet; and then removing or separating the molded article or part from the mold cavity, or optionally, heat setting the formed film or sheet by maintaining the film or sheet in contact with the heated mold for a period of time sufficient to partially crystallize the film or sheet.
[0161] In one embodiment, the thermoforming method comprises: forming a film or sheet from the polyester composition of the present disclosure; heating the film or sheet to a temperature of 100°C. g or above; applying gas, vacuum and / or physical pressure to the heat softened film or sheet and stretching the film or sheet to approximately the final part size; causing the sheet to conform to the mold shape by vacuum or pressure; cooling the film or sheet to below the T of the polyester g temperature; and then removing or separating the thermoformed article or part from the mold.
[0162] Films and sheets for use in thermoforming processes can be made by any conventional method known to those skilled in the art. In one embodiment, the film or sheet is formed by extrusion. In one embodiment, the film or sheet is formed by calendaring. In one embodiment, during the thermoforming process, the film or sheet is heated to a temperature of about 100°C above the T of the polyester. g In one embodiment, the temperature is higher than the T of the polyester. g In one embodiment, in order to achieve a shorter molding time, heating of the film or sheet is necessary before positioning over the thermoforming mold. In one embodiment, the sheet must be heated to above its T gand below a temperature at which it would sag excessively while positioned over the mold cavity. In one embodiment, the molded film or sheet is cooled to below the T of the polyester prior to removal from the mold. g In one embodiment, the thermoforming process may include vacuum assistance, air assistance, mechanical plunger assistance, or matching molds. In some embodiments, the mold is heated to the T of the film or sheet. g The selection of the optimum mold temperature depends on the type of thermoforming equipment, the configuration and wall thickness of the molded article, and other factors.
[0163] In some embodiments, the heated film or sheet is stretched by establishing and withdrawing a vacuum.
[0164] In one embodiment, heat setting is a process of heat-inducing partial crystallization of a polyester film or sheet without significant orientation. In one embodiment, heat setting is achieved by maintaining the film or sheet in contact with a heated mold surface for a sufficient time to achieve a level of crystallinity that provides adequate physical properties for the finished part. In one embodiment, the level of crystallinity should be from about 10 to about 30%.
[0165] In one embodiment, the heat-set components can be removed from the mold cavity by known removal means. For example, in one embodiment, backblowing is used and involves breaking the vacuum established between the mold and the formed film or sheet by introducing compressed air. In some embodiments, the molded article or molded part is then trimmed and the grinding waste is recovered.
[0166] In some embodiments, the addition of nucleating agent provides faster crystallization in the thermoforming process, and therefore provides faster molding. In one embodiment, nucleating agent, such as fine-grained inorganic or organic materials, can be used. For example, in one embodiment, suitable nucleating agent includes talcum, titanium dioxide, calcium carbonate and immiscible or crosslinked polymer. In one embodiment, nucleating agent is used in an amount of about 0.01% to about 20% based on the weight of the product. In one embodiment, other conventional additives such as pigment, dye, plasticizer, anti-cracking agent and stabilizer can be used according to the needs of thermoforming. In some embodiments, anti-cracking agent improves impact strength, and nucleating agent provides faster crystallization. In some embodiments, crystallization is necessary to achieve high temperature stability.
[0167] In one embodiment, the polyester composition of the present disclosure is foamed with a chemical and / or physical foaming agent, the foamed polyester is extruded into a sheet or film, and the foamed polyester film or sheet is thermoformed to make a foamed polyester film or sheet. Before foaming, additives for providing enhanced properties for the foamed polyester film can be added to the polyester. Some examples of additives include slip agents, anti-blocking agents, plasticizers, fluorescent whitening agents, and ultraviolet inhibitors. In one embodiment, the foamed polyester film can be extruded or laminated on one or both sides using conventional techniques to enhance its properties. In one embodiment, the coating material can be a printed surface rather than the foam film itself providing a product label.
[0168] The composition of the present disclosure can be used as molded or formed plastic parts or as solid plastic articles. The composition of the present disclosure can be used as thermoformed parts or products. The composition is suitable for any application requiring transparent hard plastics. Examples of such parts include disposable knives, forks, spoons, plates, cups, straws and eyeglass frames, toothbrush handles, toys, car decorations, tool handles, camera parts, parts of electronic devices, razor parts, ink pen holders, disposable syringes, bottles, etc. In one embodiment, the composition of the present disclosure can be used as plastics, films, fibers and sheets. In one embodiment, the composition can be used as plastics for making bottles, bottle caps, eyeglass frames, cutlery, disposable cutlery, cutlery handles, shelves, shelf dividers, electronic housings, electronic equipment housings, computer monitors, printers, keyboards, pipelines, automotive parts, automotive interior parts, automotive decorations, logos, thermoformed letters, sidings, toys, thermally conductive plastics, ophthalmic lenses, tools, tool handles and appliances. In another embodiment, the compositions of the present disclosure are suitable for use as films, sheets, fibers, molded articles, shaped articles, molded parts, molded components, medical devices, dental trays, dental appliances, containers, food containers, shipping containers, packaging, bottles, bottle caps, eyeglass frames, cutlery, disposable cutlery, cutlery handles, shelves, shelf dividers, furniture components, electronic housings, electronic equipment housings, computer monitors, printers, keyboards, pipes, toothbrush handles, automotive parts, automotive interior parts, automotive decoration, signs, outdoor signs, skylights, multi-wall films, multi-layer films, insulation parts, insulation articles, insulation containers, thermoformed letters, siding, toys, toy parts, trays, food trays, dental trays, thermally conductive plastics, ophthalmic lenses and frames, tools, tool handles and utensils, health care products, commercial food service products, boxes, films for graphic arts applications, plastic films for plastic glass laminates, promotional displays, skylights, smoke vents, laminated cards, fenestrations, glazing, dividers, ceilings, lighting, machine covers guards), graphic arts, lenses, extruded laminated sheets or films, decorative laminates, office furniture, face masks, medical packaging, signage holders on point-of-sale shelves, and shelf price holds.
[0169] The present thermoformable or thermoformable compositions can be used to form films, molded articles, molded parts, shaped articles, formed parts and sheets. The method of forming the thermoformable or thermoformable compositions into films, molded articles, molded parts, shaped articles, formed parts and sheets can be according to any method known in the art. Examples of molded articles include, but are not limited to, medical devices, medical packaging, health care products, commercial food service products such as trays, containers, food trays, cups, storage boxes, bottles, food processors, blenders and mixer bowls, utensils, water bottles, fresh-keeping trays, washing machine parts, refrigerator parts, vacuum cleaner parts, ophthalmic lenses and frames, and toys.
[0170] The present disclosure further relates to manufactured articles comprising film(s) and / or sheets comprising the polyester compositions described herein.In embodiments, the films and / or sheets of the present disclosure may be any thickness desired for the intended application.
[0171] The present disclosure further relates to (one or more) films and / or sheets described herein. Methods for forming the polyester composition into (one or more) films and / or sheets include any method known in the art. Examples of (one or more) films and / or sheets of the present disclosure include, but are not limited to, (one or more) extruded films and / or sheets, (one or more) calendered films and / or sheets, (one or more) compression molded films and / or sheets, (one or more) solution cast films and / or sheets. Methods for making films and / or sheets include, but are not limited to, extrusion, calendering, compression molding, wet block processing, dry block processing, and solution casting.
[0172] The present disclosure further relates to molded or shaped articles as described herein. Methods of forming the polyester composition into molded or shaped articles include any known methods in the art. Examples of molded or shaped articles of the present disclosure include, but are not limited to, thermoformed or thermoformable articles, injection molded articles, extrusion molded articles, injection blow molded articles, injection stretch blow molded articles, and extrusion blow molded articles. Methods of making molded articles include, but are not limited to, thermoforming, injection molding, extrusion, injection blow molding, injection stretch blow molding, and extrusion blow molding. The methods of the present disclosure may include any thermoforming methods known in the art. The methods of the present disclosure may include any blow molding methods known in the art, including, but not limited to, extrusion blow molding, extrusion stretch blow molding, injection blow molding, and injection stretch blow molding.
[0173] The present disclosure includes any injection blow molding manufacturing method known in the art. Although not limited thereto, a typical description of the injection blow molding (IBM) manufacturing method includes: 1) melting a composition in a reciprocating screw extruder; 2) injecting the molten composition into an injection mold to form a partially cooled tube (i.e., a preform) closed at one end; 3) moving the preform into a blow mold having a desired finished shape around the preform and closing the blow mold around the preform; 4) blowing air into the preform to stretch and expand the preform to fill the mold; 5) cooling the molded product; 6) ejecting the product from the mold.
[0174] The present disclosure includes any injection stretch blow molding manufacturing method known in the art. Although not limited thereto, a typical description of the injection stretch blow molding (ISBM) manufacturing method includes: 1) melting a composition in a reciprocating screw extruder; 2) injecting the molten composition into an injection mold to form a partially cooled tube (i.e., a preform) closed at one end; 3) moving the preform into a blow mold having a desired finished shape around the preform and closing the blow mold around the preform; 4) stretching the preform using an internal stretch rod and blowing air into the preform to stretch and expand the preform to fill the mold; 5) cooling the molded product; 6) ejecting the product from the mold.
[0175] The present disclosure includes any extrusion blow molding manufacturing method known in the art. Although not limited thereto, a typical description of an extrusion blow molding manufacturing method includes: 1) melting a composition in an extruder; 2) extruding the molten composition through a die to form a tube (i.e., a parison) of molten polymer; 3) clamping a mold having a desired finished shape around the parison; 4) blowing air into the parison to stretch and expand the extrudate to fill the mold; 5) cooling the molded article; 6) ejecting the article from the mold; and 7) removing excess plastic (commonly referred to as flash) from the article.
[0176] In another aspect of the present disclosure, it has been discovered that the polyester resins of the present disclosure can be produced from recycled copolyesters and / or recycled polyesters.
[0177] One embodiment of the present disclosure is a method of producing a polyester composition from recycled polyester, comprising:
[0178] (a) introducing terephthalic acid (TPA); and ethylene glycol (EG); and recycled polyester including recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG into a paste tank to form a slurry, which is stirred and heated at a temperature of up to 150° C.;
[0179] (b) transferring the paste tank slurry to the first reaction zone;
[0180] (c) introducing into the first reaction zone at least one additional diol comprising 1,4-cyclohexanedimethanol (CHDM), neopentyl glycol (NPG), or diethylene glycol (DEG), optionally in the presence of an esterification catalyst and / or stabilizer, and optionally adding additional terephthalic acid (TPA); and ethylene glycol (EG) to a total diol:TPA molar ratio of 1:1 to 4:1;
[0181] (d) reacting TPA and EG with the at least one additional diol in a first reaction zone at a melt temperature of at least 200° C. to form a first esterification product comprising oligomers and unreacted TPA, EG, and additional diol(s);
[0182] (e) conveying the first esterification product to a second reaction zone;
[0183] (f) further reacting the first esterification product and optionally additionally added diol in a second reaction zone at a melt temperature of at least 200° C. to form a second esterification product comprising a polyester oligomer, optionally in the presence of an esterification catalyst and / or a stabilizer;
[0184] (g) passing the second esterification product to a third reaction zone; and
[0185] (h) polycondensing the second esterification product in a third reaction zone, optionally in the presence of a polycondensation catalyst and / or a stabilizer, to form a polymeric product comprising a polyester.
[0186] One embodiment of the present disclosure is a method of producing a polyester composition from recycled polyester, comprising:
[0187] (a) introducing terephthalic acid (TPA) or its ester; and ethylene glycol (EG); and recycled polyester including one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG into a paste tank to form a slurry, which is stirred and heated at a temperature of up to 150° C.;
[0188] (b) transferring the paste tank slurry to the first reaction zone;
[0189] (c) introducing into the first reaction zone at least one additional diol comprising 1,4-cyclohexanedimethanol (CHDM), neopentyl glycol (NPG) or diethylene glycol (DEG), and optionally adding additional recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG; and optionally adding additional terephthalic acid (TPA); and ethylene glycol (EG) to a total diol:TPA molar ratio of 1:1 to 4:1, optionally in the presence of an esterification catalyst and / or stabilizer;
[0190] (d) reacting TPA and EG with the at least one additional diol in a first reaction zone at a melt temperature of at least 200° C. to form a first esterification product comprising oligomers and unreacted TPA, EG, and additional diol(s);
[0191] (e) conveying the first esterification product to a second reaction zone;
[0192] (f) further reacting the first esterified product in a second reaction zone at a melt temperature of at least 200° C., optionally in the presence of an esterification catalyst and / or stabilizer and optionally adding additional diols comprising one or more of CHDM, NPG or DEG and / or additional recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG to form a second esterified product comprising polyester oligomers;
[0193] (g) passing the second esterification product to a third reaction zone; and
[0194] (h) polycondensing the second esterification product in a third reaction zone, optionally in the presence of a polycondensation catalyst and / or a stabilizer, to form a polymeric product comprising a polyester.
[0195] One embodiment of the present disclosure is a method of producing a polyester composition from recycled polyester, comprising:
[0196] (a) introducing terephthalic acid (TPA); and ethylene glycol (EG); and a recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG into a paste tank to form a slurry, which is stirred and heated at a temperature of up to 150° C.;
[0197] (b) transferring the paste tank slurry to the first reaction zone;
[0198] (c) introducing into the first reaction zone at least one additional diol comprising 1,4-cyclohexanedimethanol (CHDM), neopentyl glycol (NPG), or diethylene glycol (DEG), and optionally adding additional recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA, or recycled PCTG; and optionally adding additional terephthalic acid (TPA); and ethylene glycol (EG) to a total diol:TPA molar ratio of 1:1 to 4:1, optionally in the presence of an esterification catalyst and / or stabilizer;
[0199] (d) reacting TPA and EG with the at least one additional diol in a first reaction zone at a melt temperature of at least 200° C. to form a first esterification product comprising oligomers and unreacted TPA, EG, and additional diol(s);
[0200] (e) conveying the first esterification product to a second reaction zone;
[0201] (f) further reacting the first esterified product in a second reaction zone at a melt temperature of at least 200° C., optionally in the presence of an esterification catalyst and / or stabilizer and optionally adding additional diols comprising one or more of CHDM, NPG or DEG and / or additional recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG to form a second esterified product comprising polyester oligomers;
[0202] (g) passing the second esterification product to a third reaction zone; and
[0203] (h) polycondensing the second esterified product in a third reaction zone, optionally in the presence of a polycondensation catalyst and / or stabilizer, and optionally adding additional recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA, or recycled PCTG to form a polymeric product comprising a polyester.
[0204] One embodiment of the present disclosure is a method of producing a polyester composition from recycled polyester, comprising:
[0205] (a) terephthalic acid (TPA); and ethylene glycol (EG) are introduced into a paste tank to form a slurry, which is stirred and heated at a temperature of up to 150° C.;
[0206] (b) transferring the paste tank slurry to the first reaction zone;
[0207] (c) introducing into the first reaction zone at least one additional diol comprising 1,4-cyclohexanedimethanol (CHDM), neopentyl glycol (NPG) or diethylene glycol (DEG), optionally in the presence of an esterification catalyst and / or stabilizer, and adding a recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG; and optionally adding additional terephthalic acid (TPA); and ethylene glycol (EG) to a total diol:TPA molar ratio of 1:1 to 4:1;
[0208] (d) reacting TPA and EG with the at least one additional diol in a first reaction zone at a melt temperature of at least 175° C. to form a first esterification product comprising oligomers and unreacted TPA, EG, and additional diol(s);
[0209] (e) conveying the first esterification product to a second reaction zone;
[0210] (f) further reacting the first esterified product in a second reaction zone at a melt temperature of at least 200° C., optionally in the presence of an esterification catalyst and / or stabilizer and optionally adding additional diols comprising one or more of CHDM, NPG or DEG and / or additional recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG to form a second esterified product comprising polyester oligomers;
[0211] (g) passing the second esterification product to a third reaction zone; and
[0212] (h) polycondensing the second esterified product in a third reaction zone, optionally in the presence of a polycondensation catalyst and / or stabilizer, and optionally adding additional recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA, recycled PCTG, recycled PCTM, or recycled PETM to form a polymerization product comprising polyester.
[0213] One embodiment of the present disclosure is a method of producing a polyester composition from recycled polyester, comprising:
[0214] (a) introducing terephthalic acid (TPA); and ethylene glycol (EG); and recycled polyester including one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG into a paste tank to form a slurry, which is stirred and heated at a temperature of up to 150° C.;
[0215] (b) transferring the paste tank slurry to the first reaction zone;
[0216] (c) introducing into the first reaction zone at least one additional diol including 1,4-cyclohexanedimethanol (CHDM), neopentyl glycol (NPG) or diethylene glycol (DEG), and adding additional recycled polyester including one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG; and optionally adding additional terephthalic acid (TPA); and ethylene glycol (EG) to a total diol:TPA molar ratio of 1:1 to 4:1, optionally in the presence of an esterification catalyst and / or stabilizer;
[0217] (d) reacting TPA and EG with the at least one additional diol in a first reaction zone at a melt temperature of at least 200° C. to form a first esterification product comprising oligomers and unreacted TPA, EG, and additional diol(s);
[0218] (e) conveying the first esterification product to a second reaction zone;
[0219] (f) further reacting the first esterified product in a second reaction zone at a melt temperature of at least 200° C., optionally in the presence of an esterification catalyst and / or stabilizer and adding additional diols comprising one or more of CHDM, NPG or DEG and / or additional recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG to form a second esterified product comprising polyester oligomers;
[0220] (g) passing the second esterification product to a third reaction zone; and
[0221] (h) polycondensing the second esterified product in a third reaction zone, optionally in the presence of a polycondensation catalyst and / or stabilizer, and optionally adding additional recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA, or recycled PCTG to form a polymeric product comprising a polyester.
[0222] One embodiment of the present disclosure is a method of producing a polyester composition from recycled polyester, comprising:
[0223] (a) introducing terephthalic acid (TPA); and ethylene glycol (EG); and recycled polyester including one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG into a paste tank to form a slurry, which is stirred and heated at a temperature of up to 150° C.;
[0224] (b) transferring the paste tank slurry to the first reaction zone;
[0225] (c) introducing into the first reaction zone at least one additional diol comprising 1,4-cyclohexanedimethanol (CHDM), neopentyl glycol (NPG), or diethylene glycol (DEG), optionally in the presence of an esterification catalyst and / or stabilizer, and optionally adding additional recycled PET, recycled PETG, recycled PCT, recycled PCTA, or recycled PCTG; and optionally terephthalic acid (TPA); and ethylene glycol (EG) to a total diol:TPA molar ratio of 1:1 to 4:1;
[0226] (d) reacting TPA and EG with the at least one additional diol in a first reaction zone at a melt temperature of at least 200° C. to form a first esterification product comprising oligomers and unreacted TPA, EG, and additional diol(s);
[0227] (e) conveying the first esterification product to a second reaction zone;
[0228] (f) further reacting the first esterified product in a second reaction zone at a melt temperature of at least 200° C., optionally in the presence of an esterification catalyst and / or stabilizer and optionally adding additional diols comprising one or more of CHDM, NPG or DEG and / or additional recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG to form a second esterified product comprising polyester oligomers;
[0229] (g) passing the second esterification product to a third reaction zone; and
[0230] (h) polycondensing the second esterified product in a third reaction zone and adding additional recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG, optionally in the presence of a polycondensation catalyst and / or stabilizer, to form a polymerization product comprising polyester.
[0231] One embodiment of the present disclosure is a method of producing a polyester composition from recycled polyester, comprising:
[0232] (a) introducing terephthalic acid (TPA); and ethylene glycol (EG); and recycled polyester including one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG into a paste tank to form a slurry, which is stirred and heated at a temperature of up to 150° C.;
[0233] (b) transferring the paste tank slurry to the first reaction zone;
[0234] (c) introducing into the first reaction zone at least one additional diol comprising 1,4-cyclohexanedimethanol (CHDM), neopentyl glycol (NPG), or diethylene glycol (DEG), optionally in the presence of an esterification catalyst and / or stabilizer, and adding additional recycled PET, recycled PETG, recycled PCT, recycled PCTA, or recycled PCTG; and optionally terephthalic acid (TPA); and ethylene glycol (EG) to a total diol:TPA molar ratio of 1:1 to 4:1;
[0235] (d) reacting TPA and EG with the at least one additional diol in a first reaction zone at a melt temperature of at least 200° C. to form a first esterification product comprising oligomers and unreacted TPA, EG, and additional diol(s);
[0236] (e) conveying the first esterification product to a second reaction zone;
[0237] (f) further reacting the first esterified product in a second reaction zone at a melt temperature of at least 200° C., optionally in the presence of an esterification catalyst and / or a stabilizer and adding additional diols comprising one or more of CHDM, NPG or DEG and / or additional recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG to form a second esterified product comprising polyester oligomers;
[0238] (g) passing the second esterification product to a third reaction zone; and
[0239] (h) polycondensing the second esterified product in a third reaction zone and adding additional recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG, optionally in the presence of a polycondensation catalyst and / or stabilizer, to form a polymerization product comprising polyester.
[0240] In one embodiment, the recycled polyester and / or copolyester can be recycled as manufacturing scrap or industrial waste or post-consumer recycled (PCR) waste. Typically, PCR or recycled waste is articles made from polyester or copolyester that have been used and discarded. Today, PET is recycled by mechanical methods and incorporated into new PET bottles and other PET articles as a blend with virgin material.
[0241] Copolyesters with recycled content and copolyesters made from recycled content contain dicarboxylic acid monomer residues, diol (diol or glycol) monomer residues and repeating units. Therefore, the term "monomer residue" as used herein refers to the residue of dicarboxylic acid, diol (diol or glycol) or hydroxycarboxylic acid. "Repeat unit" as used herein refers to an organic structure having 2 monomer residues bonded via carbonyl groups. The copolyesters of the present disclosure contain acid residues (100 mol %) and diol residues (100 mol %) in substantially equal molar proportions, which react substantially in equal proportions to make the total mole number of repeating units equal to 100 mol %. Therefore, the mole percentages provided in the present disclosure can be based on the total mole number of acid residues, the total mole number of diol residues, or the total mole number of repeating units. For example, a copolyester containing 30 mol % monomer (which can be a dicarboxylic acid, a diol or a hydroxycarboxylic acid) based on the total repeating units means that the copolyester contains 30 mol % monomer in a total of 100 mol % repeating units. Therefore, there are 30 moles of monomer residues in every 100 moles of repeating units. Similarly, a copolyester containing 30 mole % dicarboxylic acid monomers based on total acid residues means that the polyester contains 30 mole % dicarboxylic acid monomers out of a total of 100 mole % acid residues. Thus, in the latter case, there are 30 moles of dicarboxylic acid monomer residues for every 100 moles of acid residues.
[0242] The term "polyester" as used herein includes "homopolymers" and "homopolyesters" and "copolyesters" and refers to a synthetic polymer prepared by the polycondensation of at least one diacid component comprising one or more difunctional carboxylic acids and at least one diol component comprising one or more difunctional hydroxyl compounds. The term "copolyester" as used herein means a polyester formed by the polycondensation of at least 3 different monomers, such as a dicarboxylic acid with two or more diols, or in another example, a diol with two or more different dicarboxylic acids. Typically, the difunctional carboxylic acid is a dicarboxylic acid and the difunctional hydroxyl compound is a dihydric alcohol, such as a glycol and a diol. Alternatively, the difunctional carboxylic acid can be a hydroxycarboxylic acid, such as p-hydroxybenzoic acid, and the difunctional hydroxyl compound can be an aromatic nucleus with 2 hydroxyl substituents, such as hydroquinone. The term "residue" as used herein refers to any organic structure incorporated into a polymer by a polycondensation reaction involving the corresponding monomers. The dicarboxylic acid residue can be derived from a dicarboxylic acid monomer or its associated acyl halide, ester, salt, anhydride or mixture thereof. For example, in one embodiment, for the copolyesters of the present disclosure, the diacid component is supplied as terephthalic acid or isophthalic acid.
[0243] The recycled polyester and / or copolyester can be repolymerized into the copolyester using any polycondensation reaction conditions known in the art. They can be manufactured by continuous, semi-continuous and intermittent operation modes and can utilize various reactor types. Examples of suitable reactor types include, but are not limited to, stirred tanks, continuous stirred tanks, slurry reactors, tubular reactors, scraped film reactors, falling film reactors or extrusion reactors. The term "continuous" as used herein refers to a method in which reactants are introduced in an uninterrupted manner and products are removed simultaneously. For economic reasons, the method is advantageously operated as a continuous process and produces excellent coloring of the polymer, because the appearance of the copolyester may deteriorate if allowed to stay in the reactor for too long at elevated temperatures.
[0244] The copolyesters disclosed herein are prepared by procedures known to those skilled in the art. The reaction of the diol component and the dicarboxylic acid component can be carried out using conventional copolyester polymerization conditions. For example, when the copolyester is prepared by means of an ester exchange reaction, such as from the ester form of the dicarboxylic acid component, the reaction process may include two steps. In the first step, the diol component and the dicarboxylic acid component, such as terephthalic acid, react at an elevated temperature of about 150° C. to about 250° C. at a pressure of about 0.0 kPa gauge to about 414 kPa gauge (60 pounds per square inch, "psig") for about 0.5 to about 8 hours. The temperature for the transesterification reaction is about 180° C. to about 230° C. for about 1 to about 4 hours, while the pressure is about 103 kPa gauge (15 psig) to about 276 kPa gauge (40 psig). Thereafter, the reaction product is heated at a higher temperature and reduced pressure to form a copolyester while eliminating the diol, which is easily volatilized and removed from the system under these conditions.
[0245] The second step or polycondensation step is continued for about 0.1 to about 6 hours, or about 0.2 to about 2 hours, at a higher vacuum and a temperature of typically about 230°C to about 350°C, or about 250°C to about 310°C, or about 260°C to about 290°C, until a polymer having the desired degree of polymerization as determined by intrinsic viscosity is obtained. The polycondensation step may be conducted at a reduced pressure of about 53 kPa (400 Torr) to about 0.013 kPa (0.1 Torr). Agitation or appropriate conditions are used in both stages to ensure adequate heat transfer and surface renewal of the reaction mixture, and to remove water, excess diol or alcohol to promote reaction and polymerization. The reaction rates of both stages are enhanced by appropriate catalysts, such as alkoxytitanium compounds, alkali metal hydroxides and alcoholates, salts of organic carboxylic acids, alkyl tin compounds, metal oxides, and the like. A three-stage manufacturing procedure similar to that described in U.S. Pat. No. 5,290,631 may also be used, particularly when a mixed monomer feed of acid and ester is used.
[0246] In order to ensure that the reaction of the diol component and the dicarboxylic acid component by the transesterification reaction is driven to completion, it is sometimes necessary to use about 1.05 to about 2.5 moles of the diol component relative to 1 mole of the dicarboxylic acid component, and then remove the excess diol in a subsequent step. However, those skilled in the art will understand that the ratio of the diol component to the dicarboxylic acid component generally depends on the design of the reactor used for the reaction process in which it occurs.
[0247] When the copolyester is prepared by direct esterification, for example from the acid form of the dicarboxylic acid component, the copolyester is made by reacting a dicarboxylic acid or a mixture of dicarboxylic acids with a diol component or a mixture of diol components. The reaction is carried out at a pressure of about 7 kPa gauge (1 psig) to about 1379 kPa gauge (200 psig), or less than 689 kPa (100 psig) to produce a low molecular weight linear or branched copolyester product having an average degree of polymerization of about 1.4 to about 10. The temperature used during the direct esterification reaction is about 180° C. to about 280° C., or about 220° C. to about 270° C. This low molecular weight polymer can then be polymerized by a polycondensation reaction.
[0248] In some embodiments, suitable glycols include, but are not limited to, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, polyethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, neopentyl glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, terephthalyol, 1,4-cyclohexanedimethanol, 2,2,4,4-tetramethylcyclobutane-1,3-diol, polytetramethylene glycol, isosorbide, or mixtures thereof.
[0249] In some embodiments, copolyesters including the following diacids are suitable for use in a repolymerization process or a polymerization process to make new copolyesters with recycled content: terephthalic acid, isophthalic acid, trimellitic anhydride (or acid), naphthalene dicarboxylic acid, and 1,4-cyclohexane dicarboxylic acid.
[0250] In some embodiments, copolyesters including the following diols are suitable for use in a repolymerization process or a polymerization process to make new copolyesters with recycled content: ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, polyethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, neopentyl glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, terephthalylinol, 1,4-cyclohexanedimethanol, 2,2,4,4-tetramethylcyclobutane-1,3-diol, polytetramethylene glycol, isosorbide, or mixtures thereof.
[0251] In one embodiment, recycled scrap comprising terephthalate polyesters and / or copolyesters may be used in the repolymerization process. In one embodiment, any conventionally prepared terephthalate polyester or copolyester may be used in the repolymerization process. In one embodiment, suitable terephthalate polyesters and / or copolyesters include poly(ethylene terephthalate) (PET), glycol-modified polyethylene terephthalate (PETG), poly(cyclohexylene dimethylene terephthalate), glycol-modified poly(cyclohexylene dimethylene terephthalate) (PCTG), acid-initiated (acid) poly(cyclohexylene dimethylene terephthalate) (PCTA), poly(butylene terephthalate) (PBT), poly(propylene terephthalate) (PPT), polytrimethylene terephthalate (PTT), polycyclohexanedimethylene terephthalate (PCT), polyethylene naphthalate (PEN), TMCD-modified poly(ethylene terephthalate) (PETM), TMCD-modified poly(cyclohexylene dimethylene terephthalate) (PCTM), and mixtures thereof. In one embodiment, the terephthalate polyester is poly(ethylene terephthalate) (PET). In one embodiment, the copolyester is PETG. In one embodiment, the copolyester is PCT. In one embodiment, the copolyester is PCTG. In one embodiment, the copolyester is PCTA. In one embodiment, the copolyester is PCTM. In one embodiment, the copolyester is PETM.
[0252] In one embodiment, a mixture of terephthalate polyesters and copolyesters is combined and polymerized together. In one embodiment, PET and PETG are combined and polymerized together. In one embodiment, PET and PETM are combined and polymerized together. In one embodiment, PET and PCT are combined and polymerized together. In one embodiment, PET and PCTA are combined and polymerized together. In one embodiment, PET and PCTG are combined and polymerized together. In one embodiment, PET and PCTM are combined and polymerized together. In one embodiment, PET and PETG and PETM are combined and polymerized together. In one embodiment, PET and PETG and PCTM are combined and polymerized together. In one embodiment, PET, PETG, PCTM, and PETM are combined and polymerized together.
[0253] In one embodiment, copolyesters suitable for use in the present disclosure are prepared from monomers such as dimethyl terephthalate (DMT), terephthalic acid (TPA), isophthalic acid (IPA), 1,4-cyclohexanedicarboxylic acid (CHDA), ethylene glycol (EG), diethylene glycol (DEG), neopentyl glycol (NPG), 1,4-cyclohexanedimethanol (CHDM), and 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD).
[0254] One embodiment of the present disclosure is directed to a method of preparing a copolyester having a high level of recycled content by repolymerizing waste or post-consumer polyesters including terephthalate-containing polyesters (e.g., PET) and / or copolyesters (e.g., PETG) with water or an alcohol or glycol and using the recycled monomers to prepare the copolyesters containing a high mole percentage of recycled monomer residues.
[0255] In one aspect of the present disclosure, a high molecular weight copolyester containing a diol and a diacid component, wherein the diol component comprises ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, polyethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, neopentyl glycol, 1,4-butanediol, 1,5-pentanediol, dimethyl 1,4-cyclohexanedicarboxylate, dimethyl trans-1,4-cyclohexanedicarboxylate, 1,6-hexanediol, terephthalylenol, 1,4-cyclohexanedimethanol, 2,2,4,4-tetramethylcyclobutane-1,3-diol, polytetramethylene glycol, hexanediol, Diacids, isosorbide and mixtures thereof, and the diacid component includes dimethyl terephthalate, terephthalic acid, isophthalic acid (IPA), trimellitic anhydride (or trimellitic acid), salts of 5-(sulfo)isophthalic acid (SIPA), naphthalene dicarboxylic acid, 1,4-cyclohexane dicarboxylic acid and mixtures thereof; when a depolymerization aid or solvent such as water, alcohol or excess diol is introduced under conditions where a reversible transesterification reaction can occur, depolymerization by hydrolysis, alcoholysis or glycolysis will occur, thereby reducing the chain length (molecular weight) of the polymer. With sufficient solvent, the reaction will proceed to the extent that the mixture is mainly composed of the monomer, i.e., the diester of the diol and the acid component. In one aspect, the diols of the mixture include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, polyethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, neopentyl glycol, 1,4-butanediol, 1,5-pentanediol, dimethyl 1,4-cyclohexanedicarboxylate, trans-dimethyl 1,4-cyclohexanedicarboxylate, 1,6-hexanediol, terephthalyol, 1,4-cyclohexanedimethanol, 2,2,4,4-tetramethylcyclobutane-1,3-diol, polytetramethylene glycol, adipic acid, isosorbide, and mixtures thereof. In one embodiment, the diols of the mixture include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, neopentyl glycol, 1,4-butanediol, 1,5-pentanediol, 1,4-cyclohexanedimethanol, 2,2,4,4-tetramethylcyclobutane-1,3-diol, and mixtures thereof. In one embodiment, the diols of the mixture include ethylene glycol, neopentyl glycol, 1,4-cyclohexanedimethanol, 2,2,4,4-tetramethylcyclobutane-1,3-diol, and mixtures thereof. These recycled monomers can then be used to prepare copolyesters containing a high mole percentage of recycled monomer residues.
[0256] The present invention relates to methods for using recycled polyethylene terephthalate (PET) and recycled glycol-modified polyethylene terephthalate copolyesters (PETG), especially post-consumer waste, in the production of linear high molecular weight copolyesters. There is an increasing demand for using higher amounts of recycled materials in plastic products. This demand for recycled content has led to the need to develop new methods and processes for capturing existing plastic waste streams and converting them into new plastic products. The recycling of PETG waste is of particular interest. In recent years, due to the problems encountered in the processing of these combined waste streams, legislation has attempted to separate recycled glycol-modified PET (PETG) waste from recycled polyethylene terephthalate (PET) waste with resin identification code (RIC) 1. In addition, a large amount of PETG that can be recycled and converted into new plastic products is not currently recycled. In particular, shrink films made from PETG contain inks and other contaminants that must be removed from the recycling stream to produce high-quality transparent recycled PET (rPET). In addition, medical packaging is made of a large proportion of PETG, and there is currently no recycling stream for this material. The present invention provides a method for utilizing recycled PETG and recycled PETG as a reactive intermediate in conjunction with PET in the production of copolyesters useful in making extruded and injection molded products such as shrinkable films, fibers, durable goods and other shaped articles and items.
[0257] There is currently a very well defined and large-scale mechanical recycling process whereby polyethylene terephthalate (PET) products are recycled and converted into semi-crystalline recycled PET (rPET) and further incorporated into new plastic products. Diol modification of PET with other diols such as 1,4-cyclohexanediol, diethylene glycol, butanediol or neopentyl glycol is a very common process used to improve the clarity of PET, improve toughness and reduce crystallinity. These diol-modified materials are often referred to as diol-modified PET or PETG. Although the chemical composition of these materials is very similar to PET, modification with diols other than ethylene glycol produces materials that are difficult to recycle in PET recycling processes. New methods must be created to recycle and reuse these PETG materials.
[0258] The method described in the present disclosure uses recycled PETG as a raw material feed to make a variety of new copolyester resins. In this method, recycled PETG (rPETG) is introduced as a paste together with ethylene glycol and terephthalic acid to feed the transesterification reactor at the beginning of the manufacturing process for producing new copolyesters. During the process of the method, the added diol breaks down the rPETG into its original acid and diol residue starting materials, new diols and acids are added, and then the mixture is esterified and polymerized to produce new copolyesters. This method has the advantage of using recycled PETG as a raw material without the need for further purification of the acid and diol produced. In addition, this method is advantageous because it provides a method for using rPETG that currently has no mechanical recycling stream and is therefore thrown into landfills.
[0259] In addition, rPETG (or rPCTG, or rPCTM, or rPETM, or rPCTA, or rPCTG, or rPCT) contains two or more higher value monomers that are not present in rPET, such as CHDM, TMCD, DEG and NPG. The PETG product made by this method behaves the same as virgin PETG and can be used in exactly the same applications without sacrificing any performance due to the addition of recycled materials. Traditionally, rPETG is blended with virgin materials to form physical blends. These blends often lose performance in terms of mechanical properties or color and appearance, and often cannot be used in the same applications as virgin materials.
[0260] It has become a commercial requirement to use previously used, particularly post-consumer PET, in the synthesis of new PET for the manufacture of water and carbonated beverage bottles. Several chemical treatment techniques are known to facilitate the regeneration and recycling of previously used polyester materials. These techniques are used to depolymerize the recycled polyester material, thereby reducing the polyester material to its monomer and / or oligomer components. The monomer and / or oligomer components are then repolymerized to produce the recycled polyester material.
[0261] One known depolymerization technique is to subject recycled PET to methanolysis. According to the methanolysis process, rPET is reacted with methanol to produce dimethyl terephthalate (DMT) and ethylene glycol (EG). DMT and EG can be easily purified and then used to produce recycled polyester materials containing PET. However, most conventional commercial PET production facilities around the world are designed to use terephthalic acid (TPA), and some smaller-scale facilities use DMT, but most facilities are not designed to use TPA and DMT as monomer feedstocks at the same time. Therefore, additional processing is usually required to convert DMT into TPA, which is required as a feedstock for many such facilities, and in either case, further purification of the diols and DMT / TPA is required.
[0262] Another known depolymerization technology is hydrolysis, whereby the recycled PET is reacted with water to depolymerize the rPET into TPA and EG. However, it is known that it is very difficult and expensive to remove certain types of contaminants that are typically present in recycled PET from TPA. In addition, for those facilities designed to use DMT as a feedstock, TPA must be converted to DMT, and further purification of diols and DMT / TPA is required.
[0263] Glycolysis can also be used to depolymerize recycled PET. Glycolysis occurs when rPET is reacted with EG, thereby producing bis(2-hydroxyethyl)terephthalate (BHET) and / or its oligomers. Glycolysis has some significant advantages over methanolysis or hydrolysis, primarily because BHET can be used as a feedstock for DMT-based or TPA-based PET production processes without requiring major modifications to the production facility or further purification. Another significant advantage offered by the glycolysis technology is that it is not necessary to remove the glycol from the depolymerization solvent.
[0264] Previously known glycolysis processes include separate complete glycolysis of post-consumer rPET and subsequent addition of a portion of the glycolysis product to a polycondensation process. Such a glycolysis process is described in U.S. Pat. No. 5,223,544. Such a process requires high pressure and a large excess of ethylene glycol. These requirements reduce reactor efficiency by reducing the potential production capacity of the reactor.
[0265] It has generally been found that high temperatures and large excesses of EG are required in these glycolysis processes to dissolve the polyester molecules so that they can subsequently be broken down into their component parts, such as BHET and its oligomers. High temperatures and excess EG result in the production of large amounts of diethylene glycol as a by-product. The diethylene glycol thus produced cannot be easily removed from the BHET, and therefore, if the BHET is subsequently used to produce recycled PET, the resulting PET product has an excessive diethylene glycol content, rendering the polymer unacceptable for many commercial uses.
[0266] Other known processes involving glycolysis require that a heel of BHET oligomers having a degree of polymerization greater than 10 remain in the reactor at the end of the reaction run in order to dissolve the post-consumer rPET, which is insoluble in most solvents. These procedures are described in U.S. Pat. No. 4,609,680. Thus, there is clearly still a need in the art for a glycolysis process that can efficiently process previously used post-consumer rPET in the manufacture of new packaging grade PET.
[0267] The present disclosure provides solutions to the above problems. In particular, the method of the present disclosure provides an efficient and economical process for producing packaging grade polyester products using recycled polyester and / or recycled copolyester, including recycled PET, recycled PETG, recycled PETM and recycled PCTM or a mixture of these materials.
[0268] In one embodiment, the viscosity of the material in the paste zone and the viscosity of the material leaving the paste zone is greatly reduced when using rPETG (and rPC™ or a blend with rPET) compared to using rPET alone. In one embodiment, TPA dissolves faster in rPET than in EG alone. In one embodiment, TPA can dissolve faster in rPETG, rPETM or rPC™.
[0269] In one embodiment, TPA is completely replaced by recycled polyester or copolyester.
[0270] In one embodiment, composition control of the final polyester product is performed by a combination of recycling the feed and adding components to the first reaction zone.
[0271] In one embodiment of the present disclosure, the copolyester is made in two main stages. The first stage reacts the initial materials to form monomers and / or oligomers. If the starting materials entering the first stage include acid end groups, such as TPA or isophthalic acid, the first stage is called esterification. The esterification stage can be a single step or can be divided into multiple steps. The second stage further reacts the monomers and / or oligomers to form the final copolyester product. The second stage is generally referred to as the polycondensation stage. The polycondensation stage can be a single step or can be divided into a pre-polycondensation (or prepolymerization) step and a final (or refining) polycondensation step.
[0272] Figure 6 A process flow diagram showing the manufacture of polyester or copolyester such as PETG according to various embodiments of the present disclosure is shown. Although the flow diagram ( Figure 6 ) show the reaction zones as separate vessels, which are typically continuous stirred tank reactors (CSTRs), but these vessels may be integrated units with multiple esterification zones (with appropriate partitioning and controls). Likewise, although the reaction zones are shown as separate vessels, which are typically wiped film or thin film type CSTRs, these vessels may be combined in one or more integrated units with multiple polycondensation zones (with appropriate partitioning and controls). Various other types of esterification and polycondensation reactors and reactor arrangements are known in the art and may be adapted for use in accordance with the present disclosure.
[0273] refer to Figure 6In one embodiment, a paste consisting of a 2:1 molar ratio of EG and TPA with recycled copolyester and / or polyester is fed to the location marked as the paste tank. Additional EG is fed to the first reaction zone or reactor 1 and based on the target final composition of the copolyester at the same location, other glycols such as CHDM, TMCD, NPG and DEG may also be fed to the first reaction zone, and optionally, additional recycled materials may be added. In one embodiment, these raw materials may be added separately and / or directly to the first reaction zone. In some embodiments, the recycled copolyester and / or polyester is fed to at least one of the following locations: a paste tank, zone #1, zone #2, or a refining zone. In some embodiments, the recycled copolyester and / or polyester is fed to at least one of the following locations: a paste tank, zone #1, zone #2, or a refining zone.
[0274] The reaction mixture is heated in the first reaction zone by means of a recirculation loop including a heat exchanger. Esterification occurs in the first reaction zone to form a first esterified product comprising copolyester monomers, oligomers, or both and unreacted TPA, EG, and other glycols, such as CHDM, TMCD, NPG, or DEG. The reaction product of the first reaction zone is then transferred to the second reaction zone. Further esterification occurs in the second reaction zone to form a second esterified product comprising additional copolyester monomers, oligomers, or both.
[0275] In some embodiments, the average chain length of the monomers and / or oligomers exiting the esterification stage may be less than 25, 1 to 20, or 5 to 15.
[0276] In one embodiment, the second reaction zone is optional.In some embodiments, the product is passed from the first reaction zone to the third reaction zone.
[0277] The reaction product of the second reaction zone is then sent to the third reaction zone. In some embodiments, polycondensation occurs in the third reaction zone to form a prepolymer product comprising a copolyester oligomer, optionally in the presence of a polycondensation catalyst. In some embodiments, polycondensation occurs in the third reaction zone without the need for a polycondensation catalyst to form a prepolymer product comprising a copolyester oligomer. In some embodiments, the catalyst residue remaining in the copolyester and the polyester is recovered and is enough to serve as a polycondensation catalyst. In some embodiments, the third reaction zone is converted into an oligomer with an average chain length of 2 to 40, 5 to 35, or 10 to 30 by the monomer leaving the esterification stage.
[0278] The prepolymer product is then conveyed to one or more reaction zones or refining zones. Additional polycondensation occurs in the refining zone, optionally in the presence of a polycondensation catalyst, to form a copolyester having a desired average chain length or IV. The copolyester is then removed from the refining zone for subsequent processing, such as forming into pellets by an extruder connected to an underwater pelletizer.
[0279] In one embodiment, the temperature in the paste tank is between 120-180°C.
[0280] In one embodiment, the temperature in the glycolysis and transesterification zone is 200-300°C.
[0281] In one embodiment, the reacting step is performed at a melt temperature of at least 253° C., at least 255° C., or at least 257° C. In one embodiment, additionally or alternatively, the reacting step is performed at a melt temperature of no greater than 290° C., no greater than 285° C., no greater than 280° C., no greater than 275° C., no greater than 270° C., or no greater than 265° C. In various embodiments, the reacting step is performed at a melt temperature of 250 to 270° C., or 257 to 265° C.
[0282] In one embodiment, the reacting step is conducted at a pressure of 25 to 40 psi, or 30 to 40 psig.
[0283] In one embodiment, the esterification step is performed at a melt temperature of at least 253° C., at least 255° C., or at least 257° C. In one embodiment, additionally or alternatively, the esterification step is performed at a melt temperature of no greater than 290° C., no greater than 285° C., no greater than 280° C., no greater than 275° C., no greater than 270° C., or no greater than 265° C. In various embodiments, the esterification step is performed at a melt temperature of 250 to 270° C., or 257 to 265° C.
[0284] In one embodiment, the esterification step (d) is conducted at a pressure of 8 to 20 psig.
[0285] In one embodiment, the average residence time of the reactants in the reaction step is 2 hours or less, 1.75 hours or less, 1.5 hours or less, 1.25 hours or less, 1 hour or less, or 0.75 hour or less. In various embodiments, the average residence time of the reactants in the reaction step is 30 to 40 minutes.
[0286] In one embodiment, the average residence time of the reactants in the esterification step is 2 hours or less, 1.75 hours or less, 1.5 hours or less, 1.25 hours or less, 1 hour or less, or 0.75 hours or less. In various embodiments, the average residence time of the reactants in the esterification step (d) is 30 to 40 minutes.
[0287] In various embodiments, the total molar ratio of EG:TPA introduced into the process is from 2.3:1 to 3.0:1.
[0288] In various embodiments, the total molar ratio of EG:TPA introduced into the process is from 2.3:1 to 2.71:1.
[0289] The temperature, pressure and average residence time of the reaction step in the first reaction zone are those described above.
[0290] In various embodiments, the reacting step in the first reaction zone is conducted at a melt temperature of 250 to 270°C and a pressure of 25 to 40 psi.
[0291] In various embodiments, the reacting step in the first reaction zone is conducted at a melt temperature of 257 to 265°C and a pressure of 30 to 40 psi.
[0292] The temperature, pressure and average residence time for the esterification step in the second reaction zone are those described above.
[0293] In various embodiments, the esterification step in the second reaction zone is conducted at a melt temperature of 250 to 270°C and a pressure of 8 to 20 psi.
[0294] In various embodiments, the esterification step in the second reaction zone is conducted at a melt temperature of 257 to 265°C and a pressure of 8 to 20 psi.
[0295] The polycondensation catalyst that can be used for the method of the present disclosure is not particularly limited. Examples of such catalysts include titanium-based compounds, antimony-based compounds, and germanium-based compounds. Titanium catalysts are very efficient and provide high polycondensation rates at low catalyst levels. The polycondensation catalyst can be added during the esterification stage or the polycondensation stage. In one embodiment, they are added to the first reaction zone along with the feed. In one embodiment, the catalyst is added in the range of 1 to 500 ppm based on the weight of the copolyester. In one embodiment, in the case of titanium, the catalyst can be added in the range of 1 to 50 ppm based on the weight of the copolyester.
[0296] In one embodiment, catalyst selection is influenced by the catalyst from the recycled feed. Specific catalytic advantages are achieved by the combination of the catalyst from the feed and the catalyst added to the first reaction zone and the second reaction zone. Catalysts that may be from rPET include Sb and Li / Al. Catalysts from rPETG can be Ti, Co, Ge and Sb. Catalysts from rPETM and rPCTM include Co.
[0297] In some embodiments, phosphorus compounds are usually added with catalysts to improve thermal stability. Phosphorus compounds that can be used as heat stabilizers include phosphoric acid, phosphorous acid, phosphonic acid, phosphinic acid, phosphous acid and their various esters and salts. The ester can be an alkyl, branched alkyl, substituted alkyl, difunctional alkyl, alkyl ether, aryl and substituted aryl. In some embodiments, suitable heat stabilizers include triphenyl phosphate Merpol A. In one embodiment, phosphorus is added in the range of 0 to 100 ppm based on the weight of the copolyester.
[0298] In various embodiments, one or more other additives may be added to the starting materials, copolyesters and / or copolyester monomers / oligomers at one or more locations within the process. In various embodiments, suitable additives may include, for example, trifunctional or tetrafunctional comonomers such as trimellitic anhydride, trimethylolpropane, pyromellitic dianhydride, pentaerythritol or other polyacids or polyols; crosslinking agents or other branching agents; colorants; toners; pigments; carbon black; glass fibers; fillers; impact modifiers; antioxidants; UV absorber compounds; oxygen scavenging compounds; etc.
[0299] The processes according to the present disclosure are particularly suitable for use on an industrial scale. For example, in one embodiment, they can be implemented on a commercial production line capable of operating at a rate of 500 to 30,000 lbs / hr polymer.
[0300] In another aspect, the present disclosure relates to copolyesters made by the process of the present disclosure.
[0301] In still further accordance with the above process, the new polyester product may contain glycol units of ethylene glycol, diethylene glycol, and 1,4-cyclohexanedimethanol, wherein the 1,4-cyclohexanedimethanol units constitute up to about 25 mole % of the total glycol units and diethylene glycol constitutes up to 15 mole % of the total glycol units. In this case, the 1,4-cyclohexanedimethanol and diethylene glycol units may be added directly to a portion of the ethylene glycol component in the first reaction mixture or derived from a portion of post-consumer poly(ethylene terephthalate) or glycol-modified poly(ethylene terephthalate) flake material.
[0302] In various embodiments, the copolyester comprises:
[0303] (a) a diacid component comprising 60 to 100 mole % of residues of terephthalic acid, isophthalic acid, or mixtures thereof; and
[0304] (b) a diol component comprising 0-96.5 mol % of residues of ethylene glycol and 3.5 to 100 mol % of residues of 1,4-cyclohexanedimethanol,
[0305] The diacid component is calculated based on 100 mol % of the total diacid residues in the copolyester, and the diol component is calculated based on 100 mol % of the total diol residues in the copolyester.
[0306] In various embodiments, the copolyester comprises:
[0307] (a) a diacid component comprising from 90 to 100 mole percent of residues of terephthalic acid; and
[0308] (b) a diol component comprising 50 to 96.5 mol % of residues of ethylene glycol and 3.5 to 50 mol % of residues of 1,4-cyclohexanedimethanol,
[0309] The diacid component is calculated based on 100 mol % of the total diacid residues in the copolyester, and the diol component is calculated based on 100 mol % of the total diol residues in the copolyester.
[0310] In various embodiments, the copolyester comprises:
[0311] (a) a diacid component comprising from 90 to 100 mole percent of residues of terephthalic acid; and
[0312] (b) a diol component comprising 0 to 50 mol % of residues of ethylene glycol and 50 to 100 mol % of residues of 1,4-cyclohexanedimethanol,
[0313] The diacid component is calculated based on 100 mol % of the total diacid residues in the copolyester, and the diol component is calculated based on 100 mol % of the total diol residues in the copolyester.
[0314] In various embodiments, the copolyester comprises:
[0315] (a) a diacid component comprising from 60 to 100 mole % of residues of terephthalic acid; and
[0316] (b) a diol component comprising 65 to 85 mole % of residues of ethylene glycol and 25 to 35 mole % of residues of 1,4-cyclohexanedimethanol,
[0317] The diacid component is calculated based on 100 mol % of the total diacid residues in the copolyester, and the diol component is calculated based on 100 mol % of the total diol residues in the copolyester.
[0318] In various embodiments, the copolyester has an intrinsic viscosity of 0.4 to 1.5 dL / g, or 0.5 to 1.2 dL / g, or 0.6 to 0.9 dL / g.
[0319] In various other embodiments, the copolyester comprises:
[0320] (a) a diacid component comprising 100 mole % of residues of terephthalic acid, isophthalic acid, or mixtures thereof;
[0321] (b) a diol component comprising 0 to 96.5 mole % of residues of ethylene glycol, 3.5 to 100 mole % of residues of 1,4-cyclohexanedimethanol, and 0 to 0.4 mole % of residues of trimellitic anhydride; and
[0322] wherein the copolyester has an intrinsic viscosity (IV) of 0.4 to 1.5 dL / g,
[0323] wherein all weight percentages are based on the total weight of the copolyester; and
[0324] The diacid component is calculated based on 100 mol % of the total diacid residues in the copolyester, and the diol component is calculated based on 100 mol % of the total diol residues in the copolyester.
[0325] In one embodiment, the present disclosure includes a manufactured or shaped article comprising a shrink film of any shrink film embodiment of the present disclosure. In another embodiment, the present disclosure includes a manufactured or shaped article comprising an oriented film of any oriented film embodiment of the present disclosure.
[0326] In certain embodiments, the present disclosure includes, but is not limited to, shrink films applied to containers, plastic bottles, glass bottles, packaging, battery packs, hot-fill containers, and / or industrial articles, or other applications. In one embodiment, the present disclosure includes, but is not limited to, oriented films applied to containers, packaging, plastic bottles, glass bottles, photosensitive substrates such as paper, battery packs, hot-fill containers, and / or industrial articles, or other applications.
[0327] In certain embodiments of the present disclosure, the shrink film of the present disclosure can be formed into a label or sleeve. The label or sleeve can then be applied to a finished product, such as a container wall, a battery pack, or applied to a sheet or film.
[0328] The oriented films or shrink films of the present disclosure can be applied to shaped articles, such as sheets, films, tubes, bottles, and are commonly used in various packaging applications. For example, films and sheets made from polymers such as polyolefins, polystyrene, poly(vinyl chloride), polyesters, polylactic acid (PLA) are often used to make shrink labels for plastic beverage or food containers. For example, the shrink films of the present disclosure can be used in many packaging applications, wherein the shrink films applied to shaped articles exhibit properties such as good printability, high opacity, higher shrink force, good texture, and good stiffness.
[0329] The combination of improved shrink properties and improved toughness provides new commercial options including, but not limited to, shrink films for containers, plastic bottles, glass bottles, packaging, battery packs, hot fill containers and / or industrial articles or other applications.
[0330] Additionally, the materials of the present disclosure can be extruded into sheets, and the sheets can be further thermoformed into three-dimensional articles.The materials of the present disclosure can be converted into molded articles, films, shrinkable films, oriented films, blow molded articles, and blown film articles.
[0331] The present disclosure includes and explicitly contemplates and discloses any and all combinations of the embodiments, features, characteristics, parameters and / or ranges mentioned herein. That is, the subject matter of the present disclosure can be defined by any combination of the embodiments, features, characteristics, parameters and / or ranges mentioned herein.
[0332] Any process / method, apparatus, compound, composition, embodiment or component of the present disclosure may be modified by the transitional terms "comprising," "consisting essentially of," or "consisting of," or variations of these terms.
[0333] As used herein, the indefinite articles "a" and "an" refer to one or more, unless the context clearly indicates otherwise. Similarly, singular forms of nouns include their plural forms and vice versa, unless the context clearly indicates otherwise.
[0334] Although attempts have been made to make it precise, the numerical values and ranges described herein should be considered approximate unless the context otherwise indicates. These values and ranges may deviate from their specified numbers depending on the desired properties that the present disclosure seeks to obtain and the changes caused by the standard deviations present in the measurement technology. In addition, the ranges described herein are intended and explicitly contemplated to include all subranges and numerical values within the specified ranges. For example, the range 50 to 100 is intended to include all numerical values within the range, including subranges such as 60 to 90, 70 to 80, etc.
[0335] Any two numerical values of the same property or parameter reported in the examples may define a range. These numerical values may be rounded to the nearest thousandth, hundredth, tenth, integer, ten, hundredth or thousand to define the range.
[0336] The contents of all documents cited herein, including patents and non-patent documents, are incorporated herein by reference in their entirety. If any incorporated subject matter contradicts any disclosure herein, the disclosure herein shall take precedence over the incorporated content.
[0337] The present disclosure can be further illustrated by the following examples, but it should be understood that these examples are included for illustrative purposes only and are not intended to limit the scope of the present disclosure. Unless otherwise indicated, parts are parts by weight, temperatures are in ° C (Celsius) or at room temperature, and pressures are equal to or close to atmospheric pressure. Example
[0338] The present disclosure may be further illustrated by the following examples of its embodiments, but it is to be understood that these examples are included for illustration purposes only and are not intended to limit the scope of the present disclosure unless expressly specified otherwise.
[0339] Comparative Example 1
[0340] The shrink film properties of a standard polyester shrink film resin (Sample SPR) are shown in Table 1 (this standard resin is commercially available from Eastman Chemical Company). The shrink film made using this standard shrink film resin is Comparative Example #1.
[0341] The shrinkage properties are shown in Figure 2 The shrinkage was measured in the main shrinkage direction (TD direction) and in the direction perpendicular to the main shrinkage direction (MD direction) at a temperature of 60 to 95°C. The strain-induced crystalline melting point (SICMP) was measured on the stretched film using a differential scanning calorimeter (DSC). Figure 1 ). The pellet samples can also be crystallized in an oven at 170°C for 2 hours to evaluate the crystallinity in the sample. The strain-induced crystalline melting point is measured on the first heating at a heating rate of 20°C / min, but the resins described in this disclosure generally do not have a crystalline melting point that can be measured on the second heating of a DSC procedure at a heating rate of 20°C / min.
[0342] Table 1
[0343] Resin Sample SPR value PTA content (mol%) 100 EG content (mol%) 65 CHDM (mol%) 23 DEG content (mol%) 12 Film thickness (micrometer) 50 Ultimate shrinkage (at 95°C) 80 Contraction force (Mpa) 6 Tg (℃) 70 Strain induced crystallization melting point (℃) 160 Elongation at break (%, at 300mm / min) 450 Elongation at break (%, at 500mm / min) 30
[0344] The Association for Plastic Recyclers (APR) has established a test (PET-CG-03) for measuring whether a material is compatible with existing recycling processes. Using this test method, labels (minimum 3% by weight) and bottles are ground to ¼" to ½" flake size. The bottle flakes are then blended 50:50 with control bottle flakes without labels. The samples are then elutriated in a setting that allows no more than 1.2% of the PET to be labeled. The flakes are washed with 0.3% Triton X-100 and 1.0% caustic at 88°C for 15 minutes. The flakes are then washed with water after all floating material has been removed and then strained to remove excess water. The flakes are again elutriated as before. Two pounds of washed flakes are then placed in a Teflon-lined baking tray for each washed sample and flakes are added to a layer thickness of 1.5 inches. The tray containing the flakes is placed in a circulating oven at 208°C for 1-1 / 2 hours. The flakes are cooled and then passed through a screen with 0.0625-inch openings. As the material passes through the sieve, there should not be any material that clumps and therefore becomes too large to pass through the sieve. This test is followed by extrusion / granulation and molding steps to ensure the quality of the flakes.
[0345] The film samples described in Table 1 produced >1 wt% agglomerated PET flakes using this APR test and are therefore approved for recycling of PET. Therefore, labels made with this type of resin must be removed prior to the PET recycling process to eliminate agglomeration of the processed PET flakes. However, the crystallizable film compositions of the present disclosure provide advantages to recycling processes because the crystallizable films are more compatible with recycling processes and can be recycled with PET flakes.
[0346] The crystallizable compositions described in the present disclosure are designed to be compatible with recycling processes. In order to be compatible with recycling processes, crystallizable films are designed in such a way that they do not become "sticky" during the drying step at 208°C as described in the APR test. However, the film must also meet the performance criteria typically required of shrinkable films (high ultimate shrinkage, low to negative MD shrinkage, etc.). In order to meet these two requirements - recyclability and good shrinkage properties, the polyester composition must be amorphous, that is, the composition does not contain crystallinity when measured using the second heating of DSC with a heating rate of 20°C / minute. However, after stretching, the film made from the optimized polyester resin composition should contain a broad strain-induced crystalline melting peak above 200°C as measured during the first heating of the DSC run at a heating rate of 20°C / minute. This level of strain-induced crystallinity prevents sticking to the recycled PET flakes during the drying step. Therefore, the optimized polyester resin composition of the present disclosure can be described as amorphous but crystallizable.
[0347] The following examples further illustrate how the polyesters of the present disclosure may be made and evaluated, and are intended to be illustrative only and not intended to limit the scope thereof. Unless otherwise indicated, parts are by weight, temperatures are in °C (Celsius) or at room temperature, and pressures are at or near atmospheric pressure.
[0348] The present invention may be further illustrated by the following examples of preferred embodiments thereof, but it is to be understood that these examples are included for illustrative purposes only and are not intended to limit the scope of the present disclosure unless expressly specified otherwise.
[0349] Example 1
[0350] In order to better understand these performance goals, a series of copolyesters with various CHDM and DEG contents were made using procedures well known to those skilled in the art of making polyesters. Once synthesized, the resin was ground into a powder and then pressed into 10 mil film samples using a heated press. The pressed film was then stretched using a Bruckner Film Stretcher so that shrink film properties could be measured. The ground sample was crystallized in a forced air oven at 170°C for 2 hours so that the crystalline melting point could be measured. This crystalline sample was used as a proxy for the strain-induced crystalline melting peak that would exist after stretching. Table 2 is a summary of the experimental details. Comparative Example 1 (Film #L-1 / Resin Sample SPR) was also made and evaluated as a control.
[0351] Table 2
[0352] membrane# EG CHDM DEG Amorphous monomer content IV (dL / g) Tg(℃), second heating Tm(℃), second heating Tm after heat treatment (℃) Tm(C) after stretching L-1 65 23 12 35 0.91 77 none 165 N / A L-2 72 23 5 28 0.824 77 none 187 182 L-3 76 19 5 24 0.926 76 none 188 194 L-4 76 16 8 24 0.922 74 none 189 194 L-5 79 16 5 21 0.781 76 none 206 205 L-6 82 16 2 18 0.924 78 none 206 208
[0353] The data in Table 2 show that the resin samples with an amorphous monomer content (in this case, DEG + CHDM) less than 24 have a crystalline melting peak above 200°C after heat treatment. The composition of Film #L-5 was subsequently scaled up to a larger reactor and used to make shrink film in a commercial tenter. The shrink properties of this film are shown together with the sample of Comparative Example 1 (resin SPR). Figure 3 The composition of membrane A is the same as membrane #L-5.
[0354] Table 3
[0355] SPR A (CZ-2) PTA content (mol%) 100 100 EG content (mol%) 64 76 CHDM (mol%) 23 17 DEG content (mol%) 12 6 Total amorphous monomer content 35 23 Film thickness (micrometer) 50 50 Ultimate shrinkage (at 95°C) 80 63 MD shrinkage at 75C (%) -5 7 Contraction force (Mpa) 8.5 8 Tg (℃) 69 74 Strain induced crystallization melting point (℃) 161 194 Elongation at break (%, at 300mm / min) 459 451 Elongation at break (%, at 500mm / min) 35 580
[0356] Table 3 is a summary of the comparison of Sample SPR and Film Sample A. Based on this data, the Film A composition did not shrink in a similar manner to Comparative Example #1. The ultimate shrinkage (shrinkage in the main shrink direction or TD at 95C) was 17% lower than Comparative Example #1. In addition, the shrinkage of Sample A in the direction perpendicular to the main shrink direction (MD shrinkage) was actually positive (7%) compared to Comparative Example #1. Positive MD shrinkage is not preferred.
[0357] Example 2
[0358] Neopentyl glycol (NPG) is another diol monomer capable of forming an amorphous copolyester composition. It is believed that the addition of NPG in place of CHDM can reduce MD shrinkage. To study this effect in more detail, another resin sample similar in composition but containing NPG in place of CHDM was prepared. This new resin sample was then blended with the resin used to make L-5 to study the effect of monomer substitution. These resins were extruded into 10 mil films and then stretched on a Bruckner film stretcher. Testing of these films revealed the following results. When the CHDM content was less than 8 mol%, the MD shrinkage at 75°C was 0%. As the CHDM content was further reduced, the MD shrinkage became negative, indicating that the film grew rather than shrunk. In addition, the effect of amorphous monomer content was confirmed. All samples shown in Table 4 had an amorphous monomer content of >23. Subsequently, the strain-induced crystalline melting points of these compositions were <200°C. This strain-induced crystalline melting point of <200°C was too low to pass the APR test. Generally, the strain-induced crystalline melting point should be >200°C to pass the APR test. From this study it was determined that the amorphous monomer must be further reduced to ensure a strain induced crystalline melting point > 200°C and in some cases the CHDM content should be less than 10 mol% to ensure that films made with the resin shrink little in the direction perpendicular to the main shrinkage direction (MD direction).
[0359] Table 4
[0360] membrane# CHDM (mol%) NPG (mol%) DEG (mol%) EG (mol%) Amorphous monomer content (mol%) MD% at 75℃ Tm (first heating) (℃) 1 0 16 8.0 76.0 24 -0.5 189 2 8.6 7.8 7.6 76.0 24 -1.5 191 3 10.1 6.3 7.4 76.2 24 0 191 4 11.8 4.6 7.2 76.4 24 0.5 192 5 14.4 2.1 7.0 76.5 24 2 193 6 (L-5) 16.3 0 7.0 76.7 23 4 193
[0361] Example 3
[0362] A series of resins were then made, extruded into 10 mil films using a 2.5" Davis and Standard extruder, stretched, and then evaluated for their shrink film properties to compare shrink properties and crystallinity. Details of these resin compositions and the properties of shrink films made from these resin compositions are shown in Table 5. From this analysis, an optimized resin composition was designed to obtain a low MD shrinkage at 75°C and a strain-induced crystalline melting point of >200°C. This optimized resin composition contained 10 mol% NPG and 5 mol% CHDM and 5 mol% DEG. Again, it was determined that resins containing <20 mol% amorphous monomer content had a strain-induced crystalline melting point equal to or greater than 200°C. In addition, when the CHDM monomer content was less than 10 mol%, the MD shrinkage was also minimized.
[0363] Table 5
[0364] N M (-058) I (-059) I (106) GP (C-A17) PTA content (mol%) 100 100 100 100 100 EG content (mol%) 80 79 79 76 71 NPG (mol%) 10 0 16 16 26 CHDM (mol%) 5 15 0 0 0 DEG content (mol%) 5 5 5 8 3 Total amorphous monomer content 20 20 21 24 29 Film thickness (micrometer) 50 50 50 50 50 Ultimate shrinkage (% at 95°C) 59 57 65 59 79 MD shrinkage at 75℃(%) 1.5 4 0 0 -5 Contraction force (Mpa) 9 9 9 8 10 Tg (℃) 75 76 74 71 76 Strain induced crystallization melting point (℃) 200 201 196 187 177 Elongation at break (%, at 300mm / min) 588 643 552 619 380 Elongation at break (%, at 500mm / min) 675 636 493 505 367
[0365] Table 6
[0366] N I(-045) I(-059) I(106) GP (C-A17) O (-063) PTA content (mol%) 100 100 100 100 100 100 EG content (mol%) 80 78 79 76 71 79 NPG (mol%) 10 16 16 16 26 13 CHDM (mol%) 5 0 0 0 0 3 DEG content (mol%) 5 6 5 8 3 6 Total amorphous monomer content 20 22 21 24 29 22 Film thickness (micrometer) 50 50 50 50 50 50 Ultimate shrinkage (at 95°C) 66 71 72 71 79 70 MD shrinkage at 75C (%) 2 -2 -2 -1 -5 -0.5 Contraction force (Mpa) 11 9 9.7 10 10 9.5 Tg (℃) 75 71 73.5 71 75.7 73 Strain induced crystallization melting point (℃) 200 189 194 189 177 195 Elongation at break (%, at 300mm / min) 588 648 656 626 380 Elongation at break (%, at 500mm / min) 675 690 532 712 357
[0367] Example 4
[0368] Several of these resins were then tested in a caking test mimicking the APR procedure to evaluate the effect of melting point (Tm) on caking. The parameters for the caking test were as follows:
[0369] ~135 g PET flake per sample; ~3.4 g shrink film in shrunk state (2.5% film and flake)
[0370] Place PET sheet + film in aluminum pan to a depth of 1.5 inches
[0371] - Place the tray with the slices in a forced air oven at 208°C oven temperature for 1.5 hours.
[0372] The results from these experiments are described in Table 7.
[0373] Table 7
[0374] membrane Tm (℃) Score (1-10, 10 is no lumps) 045 188 5 059 196 4 058 201 8 Comparative Example 1 (SPR) 165 2
[0375] Comparative Example 2
[0376] Films made from these compositions with an amorphous monomer content of less than 20 (and therefore a DEG content of less than 12) are also extremely tough. The toughness of these films was measured using ASTM D882. Films with an elongation at break greater than 300% at pull rates of 300 mm / min and 500 mm / min are considered tough.
[0377] Other film configurations can be used to make these crystallizable polyester shrink film resins. For example, a multilayer film can be made so that the core layer of the film is made of an amorphous shrink film resin (e.g., Comparative Example #1) and the skin layer is made of a crystallizable shrink film resin of the present disclosure. Under this structure, the shrink film properties are more similar to the core layer properties, but the skin layer provides a certain degree of crystallinity so that the amount of agglomeration in the recycling process can be reduced. Blends of various commercial resin compositions can also be made to replicate the resin composition of reactor-grade resins. In each case, the performance of the resulting shrink film must be evaluated for effectiveness in shrink film applications. These shrink film concepts are described in Table 12. These films were made on a commercial tenter and their performance in these shrink film applications was evaluated.
[0378] Standard Sample E21, Sample E12, Sample SP and Sample SPR were evaluated. All standard samples evaluated are commercially available from Eastman Chemical Company. Sample E226, Sample E213, Sample E2616 were made in the laboratory using procedures known to those skilled in the art of making copolyesters.
[0379] Table 12
[0380] Measured shrink film properties Core layer Covering SPR Sample SPR none E21 Sample SPR Sample E21 Sample E213 Cap Sample SPR Sample E213
[0381] Table 13
[0382] Blend components (%) Sample SP Sample E226 Sample E12 Sample E21 Sample E2616 Blend #1 20 40 4 36 Blend #2 40 60 Blend #3 50 50 Blend #4 60 40
[0383] Table 14
[0384] Measured shrink film properties Sample SPR Sample E21 Covering Sample E213 Covering Blended Monolayer #1 #2 #3 #4 PTA content (mol%) 100 100 100 100 100 100 100 EG content (mol%) 65 67 67 79 81 79 78 NPG (mol%) 0 0 1.2 13 11 13.5 15.5 CHDM (mol%) 23 20.8 22 3 3 2.4 2.1 DEG content (mol%) 12 11 11 5 5.1 4.6 4.3 Total amorphous monomer content 35 31.5 33.5 21 18.6 20.5 21.9 Film thickness (micrometer) 50 50 50 50 50 50 50 Ultimate shrinkage (% at 95C) 79 76 77 71 59 64 68 MD shrinkage at 75C (%) -5 2 -4 6 2.5 1.5 0 Contraction force (Mpa) 5.9 6.4 6.7 10.3 8.2 9.2 9.5 Tg (℃) 69 69.5 69.1 73.2 75 75.5 75.5 Strain induced crystallization melting point (℃) 160 156, 239 159 234 225 225 224
[0385] As can be seen in these blending examples, many of the properties of the resulting shrink films meet the desired properties of the compositions of the present disclosure. However, two of the film examples have significant MD shrinkage at 75°C. However, the strain-induced crystalline melting points of these examples are higher (235-240°C). This higher strain-induced crystalline melting point can be advantageous in applications where a higher melting point is desired, but these higher melting points come with higher MD shrinkage, so a balance of properties must be achieved.
[0386] Experimental details:
[0387] The resin samples were dried in a dehumidified dryer at 60°C and then blended and extruded into films using two different methods. In the lab-scale extruder process, films with a thickness of 10 mils (250 microns) were extruded using a 2.5" Davis and Standard extruder. Once extruded, the films were cut and stretched on a BrucknerKaro 4 tenter frame at a temperature 10-15°C above Tg to a final thickness of about 5:1 stretch ratio and 50 microns. In the commercial process, films were made on a commercial tenter line where the extruded films were stretched directly after extrusion. These films were stretched to a thickness of about 5:1 stretch ratio and 50 microns under approximately the same conditions as the films made using the lab-scale process.
[0388] In a lab-scale pressed film process, the resin is dried overnight (about 12 hours) under vacuum in an oven set to a temperature slightly below the Tg of the material. After drying, 8.00 grams of the resin is weighed out and placed between two metal plates according to the following configuration: Plate – Kapton film – Resin surrounded by a square 10 mil shim – Kapton film – Plate. Before inserting the configuration into the press, the press platens are heated to about 100°C above the Tm of the resin. The configuration is then inserted between the platens of the press and enough force is applied to the plates to completely melt the resin. The resin is allowed to melt for 3 minutes and then the pressure is increased to 12,000 psi for 1.5 minutes. A "bubble bump" procedure was then performed: the pressure was released from 12,000 psi to 0 psi and increased to 13,000 psi; the pressure was immediately released again to 0 psi and increased to 14,000 psi; repeated in 1000 psi increments until 16,000 psi was reached, and the pressure was allowed to remain at 16,000 psi for 1.5 minutes. After this, the resin / plate configuration was removed from the press and removed from the shim using a blade. The result was a 6x6 10 mil film ready to be stretched on a Bruckner.
[0389] The diol content of the extruded film compositions was determined by NMR. All NMR spectra were recorded on a JEOL Eclipse Plus 600 MHz NMR spectrometer using chloroform-trifluoroacetic acid (70-30 vol / vol) for polymers or 60 / 40 (wt / wt) phenol / tetrachloroethane with deuterated chloroform added for locking for oligomer samples. The acid component of the polymer blends used in the examples herein was 100 mol % terephthalic acid. The total mole percent of the diol component was equal to 100 mol % and the total mole percent of the acid component was equal to 100 mol %.
[0390] The intrinsic viscosity of the polyesters is determined herein in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25°C and is reported in dL / g.
[0391] Shrinkage is measured herein by placing a 100 mm x 100 mm square film sample in water at 65°C to 95°C for 10 seconds without restraining the shrinkage in any direction. The % shrinkage is then calculated by the following equation:
[0392] %Shrinkage rate = [(100mm-length after shrinkage) / 100mm]x100%.
[0393] Shrinkage is measured in the direction perpendicular to the main shrinkage direction (machine direction, MD) and also in the main shrinkage direction (transverse direction, TD).
[0394] For the examples herein, shrinkage force was measured in MPa using a LabThink FST-02 Thermal Shrinkage Tester.
[0395] For the examples herein, stretched film properties were measured using ASTM method D882. The films were evaluated using multiple film stretching speeds (300 mm / min and 500 mm / min).
[0396] The glass transition temperature and strain-induced crystalline melting point (T and T, respectively) of the polyesters were determined using a TA DSC 2920 from Thermal Analyst Instrument at a scanning rate of 20 °C / min. g and T m ). Tm was measured during the first heating of the stretched sample and T was measured during the second heating step. g Alternatively, samples can be crystallized in a forced air oven at 170°C for 2 hours and then analyzed by DSC. For all samples, there is generally no crystalline melting point during the second heating of the DSC scan at a heating rate of 20°C / min.
[0397] The disclosure has been described in detail with particular reference to preferred embodiments thereof, but it will be understood that variations and modifications can be effected within the spirit and scope of the disclosure.
[0398] Laboratory scale process results:
[0399] General procedure: A mixture of 53.16 g PTA, 62.21 g EG, 2.97 g DEG, 11.52 g CHDM and 18.86 g rPET was placed in a 500 ml flask equipped with a nitrogen inlet, a metal stirrer and a short path distillation column. In addition, 0.14 ml of Ti catalyst solution (target 16 ppmTi) and 1 ml of Mn solution (target 45 ppmMn) were added to the flask. The flask was placed in a Wood's metal bath heated to 200°C. The stirring speed was set to 200 RPM at the beginning of the experiment. The contents of the flask were heated at 200°C for 60 minutes, and then the temperature was gradually increased to 250°C over 300 minutes. The reaction mixture was then heated to 270°C for 20 minutes, while the stirrer was slowed to 100 rpm and vacuum was gradually applied to 0.4 Torr. The temperature was then increased to 278°C over 20 minutes and the stirring was reduced to 60 rpm, and the mixture was kept under these conditions for 120 minutes. After this hold, the mixture was returned to atmospheric pressure and heating was stopped. The polymer was then removed from the flask for analysis. Example 1 was performed with rPET 100% replacing TPA. Example 2 was performed with rPET 20% replacing TPA.
[0400] In one aspect of the present disclosure, given a reasonably constant supply of rPET, Figure 7 The predicted amounts of Sb and other residual catalysts and additives are shown in . In some embodiments, Figure 7 This shows that the amount of antimony that must be added to the system can be balanced based on the amount of rPET fed to the process. For example, if 100 ppm of Sb is desired in the final product, 60% rPET can be fed into the process or 20% rPET can be fed and 60 ppm of Sb added to the system.
[0401] Laboratory Resin Characterization:
[0402] .
[0403] The resins made in both cases were similar in all key performance criteria. The two materials had similar color, IV and composition, regardless of the amount of rPET added.
[0404] Pilot plant process results:
[0405] Resin samples (A1 and A2) were made by adding 7.3 wt% recycled PET by weight to a reactor containing 45.7 wt% ethylene glycol, 0.7 wt% diethylene glycol, 9.8 wt% cyclohexanedimethanol, and 36.4 wt% terephthalic acid. Ti catalyst was added at 30 ppm. The glycol to acid ratio was 3.3, with ethylene glycol and cyclohexanedimethanol making up the excess. The reaction mixture was held at 250-255°C and 25-30 psig for 3-3.5 hours. Phosphorus was added at 21 ppm, and the reaction mixture was then heated to 270°C and stirred under vacuum until the target melt viscosity was reached.
[0406] The control resin sample (B) was made using the same method, except that rPET or DEG were not added to the reaction mixture and 50 ppm of Ti catalyst was used. 44.1 wt % ethylene glycol, 10.5 wt % cyclohexanedimethanol and 45.5 wt % terephthalic acid were loaded into the reactor. The ratio of glycol to acid was 2.9, with ethylene glycol and cyclohexanedimethanol making up the excess. The CHDM excess was the same as in the previous example, while the EG excess was reduced.
[0407] The characterization of the resins is described in the table below.
[0408] Pilot Plant Resin Characterization:
[0409] .
[0410] Resin Examples A1 and A2 were combined to make Resin A. Resins A and B were dried in a dehumidified dryer at 60°C for 4-6 hours. Films having a thickness of 10 mils (250 microns) were then extruded using a 2.5" Davis and Standard extruder. Once extruded, the films were cut and stretched on a Bruckner Karo 4 tenter frame to a final thickness of 50 microns. The films were stretched at a ratio of 5:1, a stretch rate of 100% / second, and a stretch temperature of 5-15°C above the Tg of the extruded film. Characterization of the shrinkable films made in this manner is described in the table below.
[0411] Examples A and B: Shrinkable films made from resin compositions made from rPET
[0412] .
[0413] Resins A and B have very similar compositions, IVs, and colors. Shrinkable films made with these resins also have very similar properties. These results demonstrate that incorporating rPET into the resin manufacturing process does not affect the final properties of the resin or articles made from the resin.
[0414] Commercial scale process:
[0415] Resin samples were also produced on a commercial manufacturing facility to demonstrate the utility of the present invention.
[0416] In a commercial scale process, 5% recycled PET is added to a slurry tank along with terephthalic acid and ethylene glycol. The slurry tank is stirred for more than 30 minutes to achieve thorough mixing. This slurry is then added to reaction zone 1 along with catalyst, additional ethylene glycol, diethylene glycol, and cyclohexanediol. This mixture is reacted at a pressure of 35+psig at above 235°C for at least 1 hour to simultaneously depolymerize the PET and react the monomers. The monomers and oligomers from reaction zone 1 are then conveyed to reaction zone 2 where they are further reacted while separating out additional glycols, but maintaining the reaction temperature. This material enters reaction zone 3 for refining at higher temperatures and deeper vacuum conditions. Characterization of the final product (Example C) is shown in the table below, compared to another copolyester resin (Example D) of the same composition that was also made in a commercial process without the addition of rPET.
[0417] Commercial Process Resin Characterization:
[0418] .
[0419] Resins C and D were dried in a dehumidified dryer at 60°C for 4-6 hours. Films having a thickness of 10 mils (250 microns) were then extruded using a 2.5" Davis and Standard extruder. Once extruded, the films were cut and stretched on a Bruckner Karo 4 tenter frame to a final thickness of 50 microns. The films were stretched at a ratio of 5:1, a stretch rate of 100% / sec, and a stretch temperature of 5-15°C above the Tg of the extruded film. Characterization of the shrinkable films made in this manner is described in the table below.
[0420] Examples C and D: Shrinkable films made from resin compositions made from rPET
[0421] .
[0422] Resins C and D have very similar compositions, IVs, and colors. Shrinkable films made with these resins also have very similar properties. These results demonstrate that incorporating rPET into the resin manufacturing process does not affect the final properties of the resin or articles made from the resin.
[0423] The disclosure has been described in detail with particular reference to specific embodiments thereof, but it will be understood that variations and modifications can be effected within the spirit and scope of the disclosure.
Claims
1. A method for producing a polyester composition from recycled polyester, comprising: (a) introducing terephthalic acid (TPA); and ethylene glycol (EG); and recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG into a paste tank to form a slurry, which is stirred and heated at a temperature of 150° C. or less; (b) transferring the paste tank slurry to the first reaction zone; (c) introducing into the first reaction zone, in the presence of an esterification catalyst and / or stabilizer, at least one additional diol comprising 1,4-cyclohexanedimethanol (CHDM), neopentyl glycol (NPG), or diethylene glycol (DEG), and adding additional recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA, or recycled PCTG; and optionally adding additional terephthalic acid (TPA); and ethylene glycol (EG) to a total diol:TPA molar ratio of 1:1 to 4:1; (d) reacting the TPA and EG and the recycled polyester with the at least one additional diol in the first reaction zone at a melt temperature of at least 200° C. to form an esterification product comprising oligomers and unreacted TPA, EG, and the at least one additional diol; (e) optionally conveying the esterification product to a second reaction zone; (f) further reacting the esterification product in the presence of an esterification catalyst and / or stabilizer, optionally in the second reaction zone at a melt temperature of at least 200° C. and adding additional diols comprising one or more of CHDM, NPG or DEG and / or additional recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG to form a resulting esterification product comprising polyester oligomers; (g) transferring the resulting esterified product from the one or more reaction zones to a third reaction zone; and (h) polycondensing the obtained esterification product in the third reaction zone in the presence of a polycondensation catalyst and / or a stabilizer and adding additional recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG to form a polymerization product comprising polyester, wherein the polyester comprises: (a) a dicarboxylic acid component comprising: (i) 70 to 100 mole percent of terephthalic acid residues; (ii) 0 to 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having 20 or less carbon atoms; and (b) a diol component comprising: 75 mol % or more of ethylene glycol residues, and Greater than 0 and less than or equal to 20 mol% of other diols, the other diols are composed of: (i) 0.1 to less than 24 mole % neopentyl glycol residues; (ii) 0.1 to less than 24 mole percent of 1,4-cyclohexanedimethanol residues; (iii) 1 to less than 10 mole % of the total diethylene glycol residues in the final polyester composition; The total mole % of the diol component is 100 mole %.
2. A method for producing a polyester composition from recycled polyester, comprising: (a) terephthalic acid (TPA); and ethylene glycol (EG) are introduced into a paste tank to form a slurry, which is stirred and heated at a temperature of 150° C. or less; (b) transferring the paste tank slurry to the first reaction zone; (c) introducing into the first reaction zone at least one additional diol comprising 1,4-cyclohexanedimethanol (CHDM), neopentyl glycol (NPG) or diethylene glycol (DEG) in the presence of an esterification catalyst and / or stabilizer, and adding a recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG; and optionally adding additional terephthalic acid (TPA); and ethylene glycol (EG) to a total diol:TPA molar ratio of 1:1 to 4:1; (d) reacting the TPA and EG and the recycled polyester with the at least one additional diol in the first reaction zone at a melt temperature of at least 175° C. to form an esterification product comprising oligomers and unreacted TPA, EG, and the at least one additional diol; (e) optionally conveying the esterification product to a second reaction zone; (f) further reacting the esterification product in the presence of an esterification catalyst and / or stabilizer, optionally in the second reaction zone at a melt temperature of at least 200° C. and adding additional diols comprising one or more of CHDM, NPG or DEG and / or additional recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA or recycled PCTG to form a resulting esterification product comprising polyester oligomers; (g) conveying the resulting esterified product to a third reaction zone; and (h) polycondensing the resulting esterification product in the third reaction zone in the presence of a polycondensation catalyst and / or a stabilizer and optionally adding additional recycled polyester comprising one or more of recycled PET, recycled PETG, recycled PCT, recycled PCTA, recycled PCTG, recycled PCTM or recycled PETM to form a polymer product comprising polyester, wherein the polyester comprises: (a) a dicarboxylic acid component comprising: (i) 70 to 100 mole percent of terephthalic acid residues; (ii) 0 to 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having 20 or less carbon atoms; and (b) a diol component comprising: 75 mol % or more of ethylene glycol residues, and Greater than 0 and less than or equal to 20 mol% of other diols, the other diols are composed of: (i) 0.1 to less than 24 mole % neopentyl glycol residues; (ii) 0.1 to less than 24 mole percent of 1,4-cyclohexanedimethanol residues; (iii) 1 to less than 10 mole % of the total diethylene glycol residues in the final polyester composition; The total mole % of the diol component is 100 mole %.
3. A method of introducing or establishing recycled content in a polyester produced by the method of claim 1, comprising: a. obtaining a recycled monomer quota or credit for at least one recycled monomer including TPA, EG, DMT, CHDM, NPG or DEG, b. converting the recovered monomers in a synthesis process to produce polyesters, c. marking at least a portion of said polyester as corresponding to at least a portion of said recycled monomer quota or credit, and optionally d. Offering for sale or selling polyesters containing or obtained with recycled monomer content corresponding to such designation.
4. The process according to claim 3, wherein the amount of recycled polyester added to the process is 5-100% based on the amount of TPA required.
5. The method according to any one of claims 1-2, wherein the esterification catalyst comprises one or more of Mn, Ti, Zn, Co, Ge or Al.
6. The method according to any one of claims 1-2, wherein the polycondensation catalyst comprises one or more of Sn, Sb, Ti, Li / Al, Al, Ge, Pb, Zn, Co, Bi, Cd, Ca or Ni.
7. The method according to any one of claims 1-2, wherein the method further comprises adding a catalyst or an additive by adding recycled polyester, wherein the catalyst or the additive is a component of the recycled polyester.
8. The method according to any one of claims 1-2, wherein the method further comprises adding a catalyst or additive by adding recycled polyester, wherein the catalyst or additive is Sb, Ti, Co, Mn, Li, Al, P.
Citation Information
Patent Citations
Microporous polymeric films and process for their manufacture
EP0214859A2
Biaxially oriented, laminated polyester film
EP0581970B1
Synthetic resin film for printing
JP1986037827A
Shrinkable film
JP1988193822A
Heat shrinkable polyester type film roll and its manufacturing process
JP2004181863A