Method for preparing electron transport layer material, QLED device and display device

By adding a silane coupling agent to the alcohol solvent to treat the metal oxide nanoparticles, a stable electron transport layer material is formed, which solves the problem of insufficient electron mobility and stability of the electron transport layer material in the existing technology, and significantly improves the performance of QLED Device performance and life.

CN114843428BActive Publication Date: 2024-10-29HEFEI FUNA TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210426914.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-21
Publication Date
2024-10-29
Estimated Expiration
2042-04-21

AI Technical Summary

Technical Problem

In the existing technology, when metal oxide nanoparticles are used as electron transport layer materials, their electron mobility and stability are insufficient, resulting in poor long-term performance of QLED devices and serious solution instability and agglomeration problems.

Method used

Add a silane coupling agent to the alcohol solvent, form a stable electron transport layer material through the first and second mixing processes, improve the stability and electron mobility of the metal oxide nanoparticles, and combine it with the metal through an appropriate amount of silane coupling agent The hydroxyl groups on the surface of oxide nanoparticles react to prevent agglomeration and condensation reactions and enhance the interlayer bonding force.

Benefits of technology

The electron mobility and stability of the electron transport layer are significantly improved, the service life of the QLED device is extended, and the luminous efficiency and structural stability are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114843428B_ABST
    Figure CN114843428B_ABST
Patent Text Reader

Abstract

The present invention proposes a method for preparing an electron transport layer material, a QLED device and a display device. The method for preparing an electron transport layer material comprises: providing an alcohol solvent, adding metal oxide nanoparticles to the alcohol solvent, performing a first mixing process to obtain a first solution, adding a silane coupling agent to the first solution, and performing a second mixing process to obtain a second solution. Thus, an electron transport layer material with high electron mobility can be obtained by a relatively simple method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of display, and in particular, to a method for preparing an electron transport layer material, a QLED device and a display apparatus. Background Art

[0002] Quantum dot light-emitting diodes (QLEDs) are gradually gaining favor in the business world in the field of new display technologies. This is because quantum dots have relatively excellent properties such as good color purity and stability of luminescence. A large number of scientific research results have been presented in the field of quantum dot light-emitting diode device research, among which the mobility of charges in different functional layers is an important technical parameter of QLED devices. QLED devices in related technologies mostly use metal oxide nanoparticles as materials for the electron transport layer, but the range of metal oxides that can be selected as materials for the electron transport layer in related technologies is relatively limited, and the performance of the device is also relatively limited, which cannot meet the long-term use requirements of QLED devices. The electron mobility and stability of the electron transport layer still need to be improved.

[0003] Therefore, the current methods for preparing electron transport layer materials, QLED devices and display apparatuses still need to be improved. Summary of the invention

[0004] In one aspect of the present invention, the present invention provides a method for preparing an electron transport layer material, comprising: providing an alcohol solvent, adding metal oxide nanoparticles to the alcohol solvent, performing a first mixing process to obtain a first solution, adding a silane coupling agent to the first solution, and performing a second mixing process to obtain a second solution. Thus, an electron transport layer material with high electron mobility can be obtained by a relatively simple method.

[0005] According to an embodiment of the present invention, the number of carbon atoms of the alcohol substance in the alcohol solvent is not greater than 6. This helps to form uniform surface ligands on the surface of the nanoparticles.

[0006] According to an embodiment of the present invention, the alcohol substance includes at least one of methanol, ethanol, propanol, isopropanol and butanol. This helps to control the particle size of the metal oxide.

[0007] According to an embodiment of the present invention, the metal oxide nanoparticles include at least one of ZnO, NiO, W2O3, Mo2O3, TiO2, SnO2, ZrO2 and Ta2O3, thereby helping to further improve the electron mobility of the electron transport layer.

[0008] According to an embodiment of the present invention, the silane coupling agent includes at least one of alkenyl silane, acryl alkoxy silane, epoxypropyl alkoxy silane, aminoalkyl silane, alkyl silane, aryl silane and aryl alkyl silane, thereby helping to improve the electron mobility of the electron transport layer.

[0009] According to an embodiment of the present invention, the silane coupling agent contains a halogen group, which helps to improve the interlayer bonding force between the electron transport layer and the light-emitting layer.

[0010] According to an embodiment of the present invention, the volume fraction of the silane coupling agent in the second solution is 5%-30%. Thus, the electron mobility of the electron transport layer can be further improved.

[0011] According to an embodiment of the present invention, the mixing temperature of the second mixing process is (-5) to 5° C. Thus, the electron mobility of the electron transport layer can be further improved.

[0012] In another aspect of the present invention, the present invention proposes a QLED device, comprising: a substrate, an anode is provided on the substrate, and the anode is located on one side of the substrate; a hole transport layer, the hole transport layer is located on the side of the anode away from the substrate; a light-emitting layer, the light-emitting layer is located on the side of the hole transport layer away from the anode; an electron transport layer, the electron transport layer is located on the side of the light-emitting layer away from the hole transport layer; a cathode, the cathode is located on the side of the electron transport layer away from the light-emitting layer, wherein the material of the electron transport layer is the electron transport layer material prepared by the method described above. Thus, a QLED device with a long luminescence lifetime and structural stability can be obtained.

[0013] According to an embodiment of the present invention, the QLED device further comprises: a hole injection layer, the hole injection layer is located between the hole transport layer and the anode; a transition layer, the transition layer is located between the electron transport layer and the cathode, the material of the transition layer is metal oxide nanoparticles; and an encapsulation layer, the encapsulation layer is located on a side of the cathode away from the electron transport layer. Thus, the electron mobility in the QLED can be further improved.

[0014] According to an embodiment of the present invention, the thickness of the hole injection layer is 30-40 nm, the thickness of the hole transport layer is 25-35 nm, the thickness of the light emitting layer is 25-35 nm, the thickness of the electron transport layer is 35-45 nm, the thickness of the transition layer is 5-15 nm, and the thickness of the cathode is 130-170 nm. Thus, the luminous efficiency of the QLED device is further improved.

[0015] According to an embodiment of the present invention, the visible light reflectivity of the cathode is not less than 98%, thereby further improving the light emitting performance of the QLED device.

[0016] In another aspect of the present invention, the present invention provides a QLED device, comprising: a substrate including an anode, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, and a cathode arranged in sequence, wherein the electron transport layer contains a silane coupling agent and metal oxide nanoparticles. Thus, a QLED device with a long luminescence lifetime and structural stability can be obtained.

[0017] In another aspect of the present invention, the present invention provides a display device, comprising the aforementioned QLED device. Since the QLED device is the aforementioned one, the display device has all the features and advantages of the aforementioned QLED device, which will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0019] Figure 1 A schematic flow chart showing a method for preparing an electron transport layer material according to one embodiment of the present invention;

[0020] Figure 2 A schematic diagram of the structure of a QLED device according to an embodiment of the present invention is shown;

[0021] Figure 3 A schematic structural diagram of a QLED device according to yet another embodiment of the present invention is shown.

[0022] Figure 4 A schematic diagram of the mechanism of a QLED device according to an embodiment of the present invention is shown.

[0023] Description of reference numerals:

[0024] 100: substrate; 200: anode; 300: hole injection layer; 400: hole transport layer; 500: light emitting layer; 600: electron transport layer; 610: transition layer; 700: cathode; 800: encapsulation layer. DETAILED DESCRIPTION

[0025] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0026] This application is based on the inventor's discovery of the following problems:

[0027] At present, most electroluminescent QLEDs use metal oxide nanoparticles as materials for the production of electron transport layers. Metal oxide nanoparticles are usually dispersed in polar organic solvents to form ligands on the surface of the nanoparticles. The inventors found that after the metal oxide nanoparticles dispersed in the organic solvent are made into a solid film for the electron transport layer, a condensation reaction will occur between the surface ligands on the surfaces of adjacent metal oxide nanoparticles, and the condensation reaction will generate water. The product water of the condensation reaction will greatly destroy the stability of the electron transport layer. In addition, the alcohol solution of metal oxide nanoparticles is unstable and is greatly affected by external environments such as temperature, humidity, and vibration. The nanoparticles are prone to agglomeration, the solution becomes turbid or precipitated, and the uniformity of the formed electron transport layer is poor.

[0028] The present application aims to solve one of the technical problems in the related art to a certain extent.

[0029] In one aspect of the present application, the present invention provides a method for preparing an electron transport layer material, by adding a silane coupling agent to an alcohol solvent of metal oxide nanoparticles, so that the stability of the metal oxide solution forming the electron transport layer is improved, and the electron transport layer formed by the solution has a high electron mobility. In addition, the method of the present invention is simple to operate and easy to repeat.

[0030] For ease of understanding, the principle of the method for preparing the electron transport layer material in the present application having the aforementioned beneficial effects is explained below:

[0031] The inventors found that the presence of hydroxyl groups in the surface ligands can reduce the size of metal oxide nanoparticles and prevent the aggregation of metal oxide nanoparticles, thereby improving the stability of the metal oxide solution. In addition, the smaller the metal oxide nanoparticles, the higher the electron mobility of the formed electron transport layer. In the related art, since the condensation reaction consumes a large number of hydroxyl groups on the surface of the metal oxide, the metal oxide nanoparticles in the solution are prone to agglomeration, which causes the metal oxide solution to become turbid or precipitate. Moreover, when the QLED device is operating normally under voltage, electrons flow through the electron transport layer, which will further intensify the condensation reaction process, thereby accelerating the destruction of the entire device and significantly shortening its life.

[0032] In the present application, the inventors significantly improved the stability of the metal oxide solution by adding an appropriate amount of silane coupling agent to the alcohol solution of the metal oxide. Figure 4By adding an appropriate amount of silane coupling agent to the alcohol solution of metal oxide, the silane coupling agent will easily undergo dehydration condensation with the hydroxyl groups on the surface of the metal oxide nanoparticles, thereby being grafted on the surface of the metal oxide nanoparticles. Compared with the number of hydroxyl groups consumed by the surface ligand condensation reaction between the metal oxide nanoparticles, the number of hydroxyl groups consumed by the silane coupling agent grafted on the surface of the metal oxide nanoparticles is extremely small and can be ignored. Due to the steric hindrance effect of the organic long chain of the silane coupling agent, the agglomeration between the metal oxide nanoparticles can be effectively blocked, making the dispersion of the nanoparticles more uniform and the alcohol solution of the metal oxide more stable. In addition, the addition of the silane coupling agent greatly reduces the number of hydroxyl ligands consumed on the surface of the metal oxide nanoparticles due to the condensation reaction, effectively ensuring that the particle size of the metal oxide is within the nanometer size range, thereby improving the structural stability of the electron transport layer, effectively alleviating the problem of reduced device life caused by dehydration condensation during normal operation of the device, and significantly improving the service life of the QLED device. In summary, the solution stability of the metal oxide formed by this method is relatively high, and the electron transport layer formed by the solution has a relatively high electron mobility.

[0033] When special instructions are required, Figure 4 The -X in represents a halogen group. It is understood that Figure 4 The connection between the silane coupling agent and the electron transport layer and the light emitting layer is only schematically explained. In actual situations, the volume of the silane coupling agent is extremely small, and there is no obvious silane coupling agent layer structure between the electron transport layer and the light emitting layer.

[0034] Specifically, refer to Figure 1 The preparation of the electron transport layer material in this application includes the following steps:

[0035] S100: Provide alcohol solvent

[0036] According to some embodiments of the present invention, the type of alcohol substance in the alcohol solvent is not particularly limited as long as it can form ligands on the surface of the nanoparticles. For example, the number of carbon atoms of the alcohol substance in the alcohol solvent may be no more than 6. Specifically, the carbon chain length of the alcohol substance may be a low alcohol of 1-4. Thus, hydroxyl ligands can be formed on the surface of the metal oxide nanoparticles.

[0037] According to some embodiments of the present invention, the type of alcohol substance is not particularly limited, and specifically, the alcohol substance may include at least one of methanol, ethanol, propanol, isopropanol and butanol. The alcohol substance forms hydroxyl ligands on the surface of the metal oxide, which can control the particle size of the metal oxide nanoparticles to a certain extent and prevent the metal oxide from aggregating and settling.

[0038] S200: Adding metal oxide nanoparticles to alcohol solvent

[0039] According to some embodiments of the present invention, metal oxide nanoparticles are added to the alcohol solvent in this step to form ligands on the surface of the metal oxide. The type of metal oxide nanoparticles is not particularly limited. Specifically, the metal oxide nanoparticles may include at least one of ZnO, NiO, W2O3, Mo2O3, TiO2, SnO2, ZrO2 and Ta2O3. The above metal oxide nanoparticles have good electron mobility in the nanoscale range due to the quantum size effect.

[0040] S300: Performing the first mixing process

[0041] According to some embodiments of the present invention, in this step, the alcohol solvent to which the metal oxide nanoparticles are added is subjected to a first mixing treatment. Specifically, the first mixing treatment can be a stirring treatment. The temperature of the stirring treatment is not particularly limited as long as the temperature is not higher than the boiling point of the alcohol solvent. For example, the first mixing treatment can be carried out at room temperature.

[0042] S400: Add silane coupling agent to the first solution

[0043] According to some embodiments of the present invention, the volume of the silane coupling agent added to the first solution is not particularly limited. It is understandable that the second mixing treatment does not affect the volume of the silane coupling agent and the alcohol solvent in the solution, so the volume fraction of the silane coupling agent in the second solution is the same as the volume fraction of the silane coupling agent added to the first solution. For example, the volume fraction of the silane coupling agent in the second solution can be 5%-30%. When the volume fraction of the silane coupling agent in the second solution is less than 5%, the modification effect of the silane coupling agent on the metal oxide nanoparticles is not obvious, and precipitation will still occur in the solution of the metal oxide. After the adjacent metal oxides are powered on, the formed electron transport layer will still undergo condensation reaction to generate water, which significantly damages the device life; when the volume fraction of the silane coupling agent in the second solution is greater than 30%, the amount of silane coupling agent grafted on the surface of the metal oxide has reached the maximum amount that can be grafted on its surface, and the free silane coupling agent in the remaining solvent will remain in the electron transport layer after the subsequent formation of the electron transport layer, resulting in a decrease in the electron mobility of the electron transport layer.

[0044] According to some embodiments of the present invention, the solution stability of the metal oxide and the electron mobility of the formed electron transport layer can be effectively improved by adding a silane coupling agent. The type of silane coupling agent is not particularly limited. For example, the silane coupling agent can include at least one of alkenyl silane, acryl alkoxy silane, epoxypropyl alkoxy silane, aminoalkyl silane, alkyl silane, aryl silane and aryl alkyl silane. When the silane coupling agent belongs to the above type, it can undergo a dehydration condensation reaction with the hydroxyl groups on the surface of the metal oxide nanoparticles, thereby being grafted on the metal oxide nanoparticles. The steric hindrance effect of the silane coupling agent makes it difficult for adjacent metal oxide nanoparticles to agglomerate, effectively avoiding the condensation reaction between the surface ligands of adjacent metal oxide nanoparticles to consume hydroxyl groups.

[0045] According to some embodiments of the present invention, the structure of the silane coupling agent is not particularly limited. Figure 4 Silane coupling agents may contain halogen groups. When the material forming the light-emitting layer or the surface ligands of the material forming the light-emitting layer contain halogen, the halogen groups of the silane coupling agent may react with the halogen groups in the material forming the light-emitting layer, thereby improving the interlayer bonding force between the electron transport layer and the quantum dot light-emitting layer, thereby improving the structural stability of the QLED device.

[0046] S500: Performing the second mixing process

[0047] According to some embodiments of the present invention, a second mixing treatment is performed in this step to obtain a second solution. The method of the second mixing treatment is not particularly limited, for example, the second mixing treatment may be a stirring treatment. According to some embodiments of the present invention, the mixing temperature of the second mixing treatment is not particularly limited, for example, the mixing temperature of the second mixing treatment may be (-5) to 5°C, preferably, the temperature of the second mixing treatment may be 0°C. Under lower temperature conditions, the silane coupling agent can be more uniformly grafted on the surface of the metal oxide, so that the metal oxide nanoparticles are not prone to condensation reactions with adjacent metal oxide nanoparticles in all directions.

[0048] The above-mentioned preparation method can obtain a metal oxide dispersion liquid for preparing an electron transport layer material with high stability, so that an electron transport layer with high electron mobility can be prepared by the dispersion liquid. The method for preparing the electron transport layer can be spin coating. Specifically, the metal oxide dispersion liquid is spin coated to form a film, and a structurally stable electron transport layer can be obtained after drying.

[0049] In another aspect of the present invention, reference Figure 2, the present invention proposes a QLED device, including: a substrate 100, an anode 200 is arranged on the substrate 100, and the anode 200 is located on one side of the substrate 100; a hole transport layer 400, the hole transport layer 400 is located on the side of the anode 200 away from the substrate 100; a light-emitting layer 500, the light-emitting layer 500 is located on the side of the hole transport layer 400 away from the anode 200; an electron transport layer 600, the electron transport layer 600 is located on the side of the light-emitting layer 500 away from the hole transport layer 400; a cathode 700, the cathode 700 is located on the side of the electron transport layer 600 away from the light-emitting layer 500, wherein the material of the electron transport layer 600 is the electron transport layer material prepared by the aforementioned method. Since the material of the formed electron transport layer is prepared by the aforementioned preparation method, the QLED device has all the characteristics and advantages of the aforementioned preparation method, which will not be repeated here. In summary, the electron mobility of the electron transport layer in the QLED device is high, and the device life is long; the interlayer bonding force between the electron transport layer and the light-emitting layer is high, and the structural stability of the device is high.

[0050] According to some embodiments of the present invention, reference Figure 3 The structure of the QLED device is not particularly limited. For example, the QLED device may include: a hole injection layer 300, which is located on the side of the anode 200 away from the substrate 100 and between the hole transport layer 400 and the anode 200; a transition layer 610, which is located between the electron transport layer 600 and the cathode 700. Preferably, the material forming the transition layer 610 may be metal oxide nanoparticles, and preferably, the material forming the transition layer may be LiF. The provision of the transition layer may eliminate the interface defect states between the electron transport layer and the cathode, reduce the effective barrier height of the interface, and further improve the cathode electron injection.

[0051] According to some embodiments of the present invention, reference Figure 3 The structure of the QLED device is not particularly limited. For example, the QLED device may include: an encapsulation layer 800, which is located on a side of the cathode 700 away from the electron transport layer 600. The provision of the encapsulation layer can prevent external water vapor from entering the interior of the QLED device, thereby improving the service life of the QLED device. The material forming the encapsulation layer is not particularly limited. For example, the material forming the encapsulation layer may be a UV resin.

[0052] According to some embodiments of the present invention, the thickness of each layer in the QLED device is not particularly limited. For example, the thickness of the hole injection layer may be 30-40nm, preferably, the thickness of the hole injection layer is 35nm; the thickness of the hole transport layer may be 25-35nm, preferably, the thickness of the hole transport layer is 30nm; the thickness of the light-emitting layer may be 25-35nm, preferably, the thickness of the light-emitting layer is 30nm; the thickness of the electron transport layer may be 35-45nm, preferably, the thickness of the electron transport layer is 40nm; the thickness of the transition layer may be 5-15nm, preferably, the thickness of the transition layer is 10nm; the thickness of the cathode may be 130-170nm, preferably, the thickness of the cathode is 150nm.

[0053] According to some embodiments of the present invention, the type of material forming the light-emitting layer is not particularly limited. For example, the quantum dot material forming the light-emitting layer may contain halogens, or the surface of the quantum dot material forming the light-emitting layer may be modified with halogen groups. Thus, when the silane coupling agent on the surface of the material forming the electron transport layer also contains halogen groups, the interlayer bonding force between the electron transport layer and the quantum dot light-emitting layer can be effectively improved, thereby improving the structural stability of the QLED device.

[0054] According to some embodiments of the present invention, the material forming the cathode is not particularly limited, for example, the visible light reflectivity of the cathode may be not less than 98%. When the visible light reflectivity of the cathode is high, the external ambient light has less effect on the light-emitting effect of the QLED device, thereby preventing the contrast of the display device from decreasing due to the external ambient light, thereby affecting the display effect.

[0055] In another aspect of the present invention, the present invention provides a QLED device, comprising: a substrate containing an anode, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, and a cathode arranged in sequence, wherein the electron transport layer contains a silane coupling agent and metal oxide nanoparticles. The electron transport layer in the QLED device has a high electron mobility and a long device life; the interlayer bonding force between the electron transport layer and the light-emitting layer is high, and the structural stability of the device is high.

[0056] In another aspect of the present invention, the present invention provides a display device, comprising the aforementioned QLED device. Since the QLED device is the aforementioned QLED device, the display device has all the features and advantages of the aforementioned QLED device, which will not be described in detail here.

[0057] The scheme of the present application is described below by specific examples. It should be noted that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in this area or the product instructions are used. The reagents or instruments used are not specified by the manufacturer, and are all conventional products that can be obtained commercially.

[0058] Experimental Example 1:

[0059] 1. Preparation of electron transport layer material solution

[0060] Ethanol solution is selected as the alcohol solvent, ZnO nanoparticles are selected as the metal oxide nanoparticles, and dimethylvinyl chloride silane is selected as the silane coupling agent.

[0061] The specific steps are as follows:

[0062] (1) Obtaining a first solution: adding 200 mg of metal ZnO nanoparticles to 10 ml of ethanol solvent, stirring until a transparent solution is formed;

[0063] (2) Obtaining a second solution: Add 1 ml of the silane coupling agent solution to 3 ml of the first solution, and stir and mix at 0° C. for 1 h to form a uniform solution for later use.

[0064] 2. Preparation of QLED devices

[0065] (1) depositing a hole injection layer on the surface of the transparent anode substrate having the anode, and then performing an annealing treatment, wherein the thickness of the hole injection layer is 35 nm, the annealing temperature is 160° C., and the annealing time is 15 min;

[0066] (2) depositing a hole transport layer on the surface of the hole injection layer away from the anode, and then performing annealing treatment, the thickness of the hole transport layer is 30 nm, the annealing temperature is 150° C., and the annealing time is 10 min;

[0067] (3) depositing a light-emitting layer on the surface of the hole transport layer away from the hole injection layer, and then performing an annealing treatment, wherein the material forming the light-emitting layer contains Cl element, the thickness of the light-emitting layer is 30 nm, the annealing temperature is 250° C., and the annealing time is 60 min;

[0068] (4) spin coating the surface of the light-emitting layer away from the hole transport layer to form an electron transport layer, the spin coating solution is the second solution prepared in step 1, and the thickness of the electron transport layer is 40 nm;

[0069] (5) depositing a transition layer on the side of the electron transport layer away from the light-emitting layer, and then performing an annealing treatment, wherein the thickness of the transition layer is 10 nm, the annealing temperature is 80° C., and the annealing time is 30 min;

[0070] (6) depositing a cathode on the side of the transition layer away from the electron transport layer, the cathode thickness is 150 nm, and the cathode reflectivity to visible light is 98%;

[0071] (7) UV resin is coated on the side of the cathode away from the transition layer, and UV light is applied to form an encapsulation layer. UV lamp power 0.2W / cm 2 , UV irradiation time is 10s.

[0072] Example 2

[0073] The preparation method of Example 2 is the same as that of Example 1, except that the silane coupling agent added when preparing the solution of the electron transport layer material in Example 2 is dimethoxymethylvinylsilane.

[0074] Comparative Example 1

[0075] The preparation method in Comparative Example 1 is the same as that in Example 1, except that no silane coupling agent is added when preparing the solution of the electron transport layer material in Comparative Example 1, that is, the first solution in the present application is directly used to prepare the electron transport layer.

[0076] The QLEDs in the above-mentioned Examples 1 and 2 and Comparative Example 1 were tested respectively to determine their brightness at 100 cd / m 2 The time when the brightness decreases to 50% of the initial brightness.

[0077] The test results show that the life of the QLED device in Example 1 is 10200h, the life of the QLED device in Example 2 is 8600h, and the life of the QLED device in Comparative Example 1 is 7500h. Compared with the QLED device in Comparative Example 1 in which the electron transport layer is not treated with a silane coupling agent, the addition of a silane coupling agent containing only Cl in Example 2 has increased the life of the QLED device by 14.7%, and the addition of a silane coupling agent containing the same halogen group as the light-emitting layer has increased the life of the QLED device by 36%. It can be seen that the life of the QLED device can be significantly improved by the addition of a silane coupling agent, and when the silane coupling agent and the light-emitting layer contain the same halogen group, the life of the QLED device can be further improved.

[0078] In the description of the present invention, the orientation or position relationship indicated by the terms "upper" and "lower" etc. is based on the orientation or position relationship shown in the drawings and is only for the convenience of describing the present invention rather than requiring the present invention to be constructed and operated in a specific orientation. Therefore, it should not be understood as a limitation on the present invention.

[0079] In the description of this specification, the description with reference to the terms "one embodiment", "another embodiment", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment are included in at least one embodiment of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples, unless they are contradictory. In addition, it should be noted that in this specification, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated.

[0080] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing an electron transport layer material, characterized in that: include: Provide alcohol solvent, adding metal oxide nanoparticles to the alcohol solvent, performing a first mixing process to obtain a first solution, adding a silane coupling agent to the first solution, performing a second mixing process to obtain a second solution, The silane coupling agent contains a halogen group. When the material forming the light-emitting layer or the surface ligand of the material forming the light-emitting layer contains a halogen, the halogen group of the silane coupling agent reacts with the material forming the light-emitting layer or the halogen group in the surface ligand of the material forming the light-emitting layer, thereby improving the interlayer bonding force between the electron transport layer and the quantum dot light-emitting layer. The mixing temperature of the second mixing treatment is (-5)~5°C, The volume fraction of the silane coupling agent in the second solution is 5%-30%.

2. The method according to claim 1, characterized in that The carbon number of the alcohol substance in the alcohol solvent is not more than 6.

3. The method according to claim 2, characterized in that The alcohol substance includes at least one of methanol, ethanol, propanol, isopropanol and butanol.

4. The method according to claim 1, characterized in that: The metal oxide nanoparticles include at least one of ZnO, NiO, W2O3, Mo2O3, TiO2, SnO2, ZrO2 and Ta2O3.

5. The method according to claim 1, characterized in that The silane coupling agent includes at least one of alkenyl silane, acryl alkoxy silane, epoxypropyl alkoxy silane, aminoalkyl silane, alkyl silane, aryl silane and aryl alkyl silane.

6. A QLED device, characterized in that: include: A substrate, wherein an anode is disposed on the substrate and the anode is located on one side of the substrate; A hole transport layer, the hole transport layer is located on a side of the anode away from the substrate; A light-emitting layer, the light-emitting layer is located on a side of the hole transport layer away from the anode; An electron transport layer, the electron transport layer is located on a side of the light-emitting layer away from the hole transport layer; a cathode, the cathode being located on a side of the electron transport layer away from the light-emitting layer, Wherein, the material of the electron transport layer is an electron transport layer material prepared by the method according to any one of claims 1 to 5.

7. The QLED device according to claim 6, characterized in that The QLED device further comprises: A hole injection layer, the hole injection layer is located between the hole transport layer and the anode; A transition layer, the transition layer is located between the electron transport layer and the cathode, and the material of the transition layer is metal oxide nanoparticles; The encapsulation layer is located on a side of the cathode away from the electron transport layer.

8. The QLED device according to claim 7, characterized in that The thickness of the hole injection layer is 30-40nm, the thickness of the hole transport layer is 25-35nm, the thickness of the light-emitting layer is 25-35nm, the thickness of the electron transport layer is 35-45nm, the thickness of the transition layer is 5-15nm, and the thickness of the cathode is 130-170nm.

9. The QLED device according to claim 8, characterized in that The visible light reflectivity of the cathode is not less than 98%.

10. A display device, characterized in that: A QLED device comprising any one of claims 6-9.

Citation Information

Patent Citations

  • Silane functionalized buffer layers and electronic devices comprising the same

    CN105074952A

  • Optoelectronic devices comprising solution-processable metal oxide buffer layers

    CN107251256A

  • Composite film and preparation method and application thereof

    CN109935731A

  • Carrier transport material and preparation method thereof, and QLED device