Electrophoretic galvanized iron product and surface treatment method thereof

By forming a chemical conversion film and an electrophoretic resin film layer on galvanized iron products, the electrophoretic surface treatment process of galvanized iron products is simplified, the process complex and pollution problems are solved, the water and chemical raw materials are saved, and the product performance is improved and lifespan.

CN114875395BActive Publication Date: 2024-11-26WEIFANG GUOYI ALUMINUM +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210331802.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-31
Publication Date
2024-11-26
Estimated Expiration
2042-03-31

AI Technical Summary

Technical Problem

The electrophoretic surface treatment process of existing galvanized iron products is complex, resulting in a large amount of wastewater and solid waste pollution, consuming a large amount of chemical raw materials and water, and increasing production costs.

Method used

The chemical conversion film and electrophoretic resin film layers are connected through chemical bonds to simplify the process flow, and the chemical conversion film of zinc oxalate, zinc fluoride and zinc oxide are formed by de-oiling and polishing chemical conversion and electrophoresis, combining electrophoretic resin Film layer to improve adhesion and product life.

Benefits of technology

It significantly reduces water and solid waste, saves chemical raw materials, improves the product's corrosion resistance, pollution resistance and adhesion, extends the product's life, and reduces the environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114875395B_ABST
    Figure CN114875395B_ABST
Patent Text Reader

Abstract

The present invention discloses an electrophoretic galvanized iron product and a surface treatment method thereof, wherein the surface of the galvanized iron product is provided with an electrophoretic resin film layer formed by electrophoresis, and a layer of chemical conversion film is further provided between the surface of the galvanized iron product and the electrophoretic resin film layer; the chemical conversion film is a chemical conversion film formed after the galvanized iron product undergoes degreasing chemical conversion; the chemical conversion film is a chemical conversion film containing zinc oxalate, zinc fluoride, and zinc oxide. The present invention pre-treats the surface of the electrophoretic galvanized iron product by first using a one-step degreasing chemical conversion method, which can remove oil stains and natural oxide films on the surface of the galvanized iron product, and forms a layer of chemical conversion protective film of zinc oxalate, zinc oxide, and zinc fluoride on the surface of the product, thereby improving the corrosion resistance, anti-pollution, and surface bonding ability of the product, and greatly solving the problem of low adhesion between the organic film and the product, thereby improving the performance index of the product and increasing the life of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a galvanized iron product, in particular to a surface treatment technology of an electrophoresis galvanized iron product. Background Art

[0002] At present, the electrophoretic surface treatment process of galvanized iron products is as follows: pre-treatment: the galvanized iron workpiece is degreased, washed with hot water, surface conditioned, and washed with water in sequence, then phosphated, washed with water, and then immersed in an electrolyte for electrophoretic treatment to obtain high corrosion resistance on the surface of the galvanized iron product.

[0003] At present, the electrophoretic surface treatment process of galvanized iron products is complicated. A large amount of wastewater and solid waste, including a large amount of hazardous waste, is generated during the production process, which brings a large amount of pollutants to the environment. It also consumes a large amount of chemical raw materials and water, which has always restricted the development of the industry.

[0004] Therefore, the current electrophoretic treatment process for galvanized iron products has many problems such as complex process flow, large amount of water washing resulting in large amount of water waste and water pollution, and consumption of large amount of chemical raw materials, which leads to increased production costs. Summary of the invention

[0005] The first technical problem to be solved by the present invention is: in view of the shortcomings of the prior art, an electrophoretic galvanized iron product is provided, in which the chemical conversion film and the electrophoretic resin film layers of the electrophoretic galvanized iron product are linked by chemical bonds, thereby increasing the bonding force between the resin paint and the chemical conversion film layers, and the paint film has strong adhesion, which also greatly solves the problem of low adhesion between the organic film and the product, thereby increasing the life of the product.

[0006] The second technical problem to be solved by the present invention is: in view of the shortcomings of the prior art, a surface treatment method for electrophoretic galvanized iron products is provided. The treatment method has a short process flow, the treatment liquid can be recycled without replacement, a large amount of water and chemical raw materials are saved, and the product performance is better.

[0007] To solve the above-mentioned first technical problem, the technical solution of the present invention is:

[0008] An electrophoretic galvanized iron product, wherein the surface of the galvanized iron product is provided with an electrophoretic resin film layer formed by electrophoresis, and a layer of chemical conversion film is also provided between the surface of the galvanized iron product and the electrophoretic resin film layer; the chemical conversion film is a chemical conversion film formed after the galvanized iron product undergoes oil removal and chemical conversion; the chemical conversion film is a chemical conversion film containing zinc oxalate, zinc fluoride, and zinc oxide.

[0009] As an improved technical solution, the unit area weight of the chemical conversion film is 10 to 500 mg / m 2 .

[0010] As an improved technical solution, the chemical conversion film is a uniform regular crystal morphology film (see attached Figure 1 , 2 , 3).

[0011] To solve the above second technical problem, the technical solution of the present invention is:

[0012] A surface treatment method for electrophoretic galvanized iron products comprises the following steps:

[0013] (1) Degreasing and polishing chemical conversion: the galvanized iron product to be treated is placed in a degreasing and polishing chemical conversion solution, reacted for 1 to 20 minutes, and a uniform chemical conversion film is covered on the surface of the galvanized iron product; the degreasing and polishing chemical conversion solution comprises the following components: 5 to 30 g / L oxalic acid, 1 to 6 g / L ammonium bifluoride (equivalent to ammonium fluoride and hydrogen fluoride in fluorine content), and 0.003 to 0.008 g / L surfactant;

[0014] (2) Electrophoresis: After the galvanized iron product has been chemically converted, it is washed with water and then electrophoresed in a resin electrophoretic paint to form an electrophoretic resin film layer on the chemical conversion film.

[0015] As an improved technical solution, the surfactant includes one or more of alkylphenol polyoxyethylene ether, octylphenol polyoxyethylene ether, nonylphenol polyoxyethylene ether, glycerol fatty acid ester, and sorbitan fatty acid ester.

[0016] In the process of chemical conversion treatment of degreasing and polishing galvanized iron products of the present invention, grease enters the treatment liquid, and a transparent fiber is generated under the joint action of oxalic acid, fluoride ion, and ammonia ion surfactants. The main component is polyester. By filtering and removing fibers regularly, the tank liquid will not be updated due to the increase in grease concentration. The inventor uses this method to make the tank liquid clear and free of turbidity. The precipitation caused by foreign impurities every year (the amount is very small) can be removed by emptying the tank. There is no pollution without emission. The difference between the present invention and the prior art is that the tank liquid does not need to be replaced and updated, and the flocculent fibers polymerized by grease can be removed by regular filtration, which ensures the clarity and sustainable reuse of the tank liquid and solves the environmental protection problem.

[0017] The presence of F ions in the chemical conversion solution of the present invention reduces the chemical energy of Zn, making it easier to generate Zn 2+ The concentration of oxalic acid is about 20 times that of ammonium hydrogen fluoride, and it also ensures that Zn 2+ It can generate zinc oxalate and participate in film formation. F ions also act as a catalyst in the reaction process.

[0018] As an improved technical solution, the Zn in the chemical conversion solution 2+ The equilibrium concentration is less than 0.8g / L.

[0019] As an improved technical solution, the working temperature of the oil removal chemical conversion liquid is 10-60°C.

[0020] Due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0021] The present invention pre-treats the surface of electrophoretic galvanized iron products by first adopting a one-step degreasing chemical conversion method, so that oil stains and natural oxide films on the surface of the galvanized iron products can be removed, and zinc ions generated by fluorine ions and zinc oxide on the surface of the galvanized iron products and zinc ions are captured by oxalic acid and precipitated on the surface of the products, forming a chemical conversion protective film of zinc oxalate, zinc oxide and zinc fluoride on the surface of the products, thereby improving the corrosion resistance, pollution resistance and surface bonding ability of the products. Through SEM+EDS detection and analysis, the chemical conversion film has a uniform and regular intercrystalline structure morphology as shown in the attached drawings (1, 2, 3), and the chemical composition is shown in the attached drawings. Figure 4 , 5 It can produce good adhesion between the chemical conversion film and the electrophoretic resin paint layer, and also greatly solve the problem of low adhesion between the organic film and the product, thereby improving the performance indicators of the product and increasing the life of the product.

[0022] The surface treatment method of the present invention completes degreasing and chemical conversion in one step, and the steps are simplified. In addition, the water washing step between each step in the prior art is saved, and only the water washing before electrophoresis is retained. Compared with the prior art, waste water is reduced by 80%, solid waste is reduced by 90%, and no heavy metal is discharged. The weight of the product before treatment is not only not reduced, but increased by more than 0.5 kg per ton of product, and the adhesion between the product and the electrophoretic film is significantly increased, which greatly improves the corrosion resistance of the product. The product not only has good adhesion, resistance to boiling water, resistance to salt spray tests, and resistance to acid and alkali, but also can obtain a morphology that is easy to be firmly combined with the electrophoretic film, and effectively blocks the diffusion process of corrosion under the film. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0024] Figure 1 This is a surface morphology image of a chemical conversion film with a chemical conversion time of 5 minutes detected by SEM of the present invention, which is magnified 855 times;

[0025] Figure 2 This is a surface morphology image of a chemical conversion film with a chemical conversion time of 5 minutes detected by SEM of the present invention, which is magnified 315 times;

[0026] Figure 3 This is a surface morphology image magnified 1000 times of a chemical conversion film with a chemical conversion time of 5 minutes detected by SEM of the present invention;

[0027] Figure 4 Yes Figure 3EDS analysis energy spectrum of a certain point in the image;

[0028] Figure 5 Yes Figure 3 EDS analysis energy spectrum of a certain point in the image;

[0029] Figure 6 It is a schematic diagram of the chemical conversion and film formation principle of the present invention. DETAILED DESCRIPTION

[0030] The present invention will be further described below in conjunction with the accompanying drawings and Examples. It should be understood that these embodiments are only intended to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0031] As attached Figure 1-3 As shown, the films generated by chemical conversion in the present invention all have uniform intercrystalline morphology, and have a large surface area when combined with the paint film. The chemical conversion film and the electrophoretic resin paint are chemically bonded to obtain the maximum chemical conversion film-paint film bonding force (see Chemical Principles Figure 6 ), improve adhesion and impact resistance, alkali resistance, salt spray resistance, and can more effectively solve the corrosion defects under the film.

[0032] Respectively Figure 3 Select any two points of the chemical conversion film for EDS analysis; Figure 4 , Figure 5 The energy spectrum of , and the analysis results are shown in Table 1 and Table 2.

[0033] Table 1

[0034] element Line Type Apparent concentration k ratio Wt% Wt%Sigma Standard sample label C K-line system 13.74 0.13742 10.77 0.17 C Vit N K-line system 4.08 0.00727 0.49 0.22 BN O K-line system 152.82 0.51424 28.64 0.25 <![CDATA[SiO2]]> F K-line system 1.78 0.00349 0.22 0.07 <![CDATA[CaF2]]> Na K-line system 0.00 0.00000 0.00 0.29 Albite Mg K-line system 0.04 0.00028 0.02 0.07 MgO Al K-line system 0.40 0.00291 0.17 0.08 <![CDATA[Al2O3]]> Si K-line system 0.20 0.00158 0.09 0.09 <![CDATA[SiO2]]> P K-line system 0.16 0.00088 0.05 0.12 GaP S K-line system 0.19 0.00161 0.09 0.15 <![CDATA[FeS2]]> Ti K-line system 0.01 0.00011 0.01 0.01 Ti Cu L Line 0.64 0.00640 0.43 0.30 Cu Zn L Line 89.00 0.89003 59.04 0.38 Zn Total 100.00

[0035] Table 2

[0036]

[0037]

[0038] Example 1

[0039] An electrophoretic galvanized iron product, wherein the surface of the electrophoretic galvanized iron product is provided with an electrophoretic resin film layer formed by electrophoresis, and a layer of chemical conversion film is further provided between the surface of the galvanized iron product and the electrophoretic resin film layer; the chemical conversion film is a chemical conversion film formed after the galvanized iron product undergoes oil removal and chemical conversion; the chemical conversion film is a chemical conversion film containing zinc oxalate, zinc fluoride, and zinc oxide, and the unit area weight of the chemical conversion film is 50 mg / m 2 .

[0040] Example 2

[0041] An electrophoretic galvanized iron product, wherein the surface of the electrophoretic galvanized iron product is provided with an electrophoretic resin film layer formed by electrophoresis, and a layer of chemical conversion film is further provided between the surface of the galvanized iron product and the electrophoretic resin film layer; the chemical conversion film is a chemical conversion film formed after the galvanized iron product is chemically converted after degreasing; the chemical conversion film is a chemical conversion film containing zinc oxalate, zinc fluoride, and zinc oxide, and the unit area weight of the chemical conversion film is 150 mg / m 2 .

[0042] Example 3

[0043] An electrophoretic galvanized iron product, wherein the surface of the electrophoretic galvanized iron product is provided with an electrophoretic resin film layer formed by electrophoresis, and a layer of chemical conversion film is further provided between the surface of the galvanized iron product and the electrophoretic resin film layer; the chemical conversion film is a chemical conversion film formed after the galvanized iron product undergoes oil removal and chemical conversion; the chemical conversion film is a chemical conversion film containing zinc oxalate, zinc fluoride, and zinc oxide, and the unit area weight of the chemical conversion film is 20 mg / m 2 .

[0044] Example 4

[0045] (1) Degreasing and polishing chemical conversion: The galvanized iron product to be treated is placed in a degreasing and polishing chemical conversion solution at a temperature of 28°C and reacted for 12 minutes. The surface of the galvanized iron product is covered with a uniform chemical conversion film; the degreasing and polishing chemical conversion solution contains: 30 g / L oxalic acid, 2 g / L ammonium bifluoride, and 0.004 g / L surfactant alkylphenol polyoxyethylene ether. The chemical conversion solution contains Zn 2+ The equilibrium concentration is 0.1 g / L.

[0046] (2) Electrophoresis: After the chemical conversion, the galvanized iron product is washed with water, and then electrophoresed in a resin electrophoretic paint to form an electrophoretic resin film layer on the chemical conversion film, which is then cured.

[0047] Example 5

[0048] (1) Degreasing and polishing chemical conversion: The galvanized iron product to be treated is placed in a degreasing and polishing chemical conversion solution at a temperature of 20°C and reacted for 4 minutes. The surface of the galvanized iron product is covered with a uniform chemical conversion film; the degreasing and polishing chemical conversion solution contains: 18 g / L oxalic acid, 1.4 g / L ammonium bifluoride, and 0.005 g / L of surfactant sorbitan fatty acid ester. The Zn 2+ The equilibrium concentration is 0.2 g / L.

[0049] (2) Electrophoresis: After the chemical conversion, the galvanized iron product is washed with water, and then electrophoresed in a resin electrophoretic paint to form an electrophoretic resin film layer on the chemical conversion film, which is then cured.

[0050] Example 6

[0051] (1) Degreasing and polishing chemical conversion: The galvanized iron product to be treated is placed in a degreasing and polishing chemical conversion solution at a temperature of 16°C and reacted for 6.5 minutes. The surface of the galvanized iron product is covered with a uniform chemical conversion film; the degreasing and polishing chemical conversion solution contains: 10 g / L oxalic acid, 1 g / L ammonium bifluoride, and 0.0035 g / L of surfactant octylphenol polyoxyethylene ether. The chemical conversion solution contains Zn 2+ The equilibrium concentration is 0.15 g / L.

[0052] (2) Electrophoresis: After the chemical conversion, the galvanized iron product is washed with water, and then electrophoresed in a resin electrophoretic paint to form an electrophoretic resin film layer on the chemical conversion film, which is then cured.

Claims

1. A surface treatment method for electrophoretic galvanized iron products, wherein the surface of the galvanized iron products is provided with an electrophoretic resin film layer formed by electrophoresis, characterized in that: A layer of chemical conversion film is also arranged between the surface of the galvanized iron product and the electrophoretic resin film layer; the chemical conversion film is a uniform regular crystal morphology film; the chemical conversion film is a chemical conversion film formed after the galvanized iron product undergoes oil removal and chemical conversion; the chemical conversion film is a chemical conversion film containing zinc oxalate, zinc fluoride, and zinc oxide; comprising the following steps: (1) Chemical conversion for degreasing and polishing: The galvanized iron product to be treated is placed in a chemical conversion solution for degreasing and polishing, and the reaction is carried out for 1 to 20 minutes, and a uniform chemical conversion film is formed on the surface of the galvanized iron product; the chemical conversion solution for degreasing and polishing comprises the following components: 5 to 30 g / L of oxalic acid, 1 to 6 g / L of ammonium bifluoride, and 0.003 to 0.008 g / L of a surfactant; the surfactant comprises one or more of alkylphenol polyoxyethylene ether, octylphenol polyoxyethylene ether, nonylphenol polyoxyethylene ether, glycerol fatty acid ester, and sorbitan fatty acid ester; Zn in the chemical conversion solution 2+ The equilibrium concentration is less than 0.8 g / L; (2) Electrophoresis: After the chemical conversion of the galvanized iron product, the product is washed with water and then electrophoresed in a resin electrophoretic paint to form an electrophoretic resin film layer on the chemical conversion film.

2. The surface treatment method of electrophoretic galvanized iron products according to claim 1, characterized in that: The weight per unit area of ​​the chemical conversion film is 10 to 500 mg / m².

3. The surface treatment method of electrophoretic galvanized iron products according to claim 1, characterized in that: The temperature of the degreasing and polishing chemical conversion liquid is 10-60°C.

4. An electrophoretic galvanized iron product obtained by the surface treatment method for electrophoretic galvanized iron products as described in any one of claims 1 to 3.