Aluminum product with weather-resistant paint film protective layer and surface treatment method thereof

By forming chemical conversion film and paint film protective layer with chemical bond links on the surface of aluminum products, the problems of complex processes, waste of water and insufficient weathering performance in the prior art are solved, and efficient surface treatment is achieved, which significantly reduces wastewater and solid waste. The corrosion resistance and adhesion of the product are improved, and meet the anti-corrosion requirements of special industries.

CN114752927BActive Publication Date: 2024-11-26WEIFANG GUOYI ALUMINUM +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210333348.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-31
Publication Date
2024-11-26
Estimated Expiration
2042-03-31

AI Technical Summary

Technical Problem

The surface treatment process of existing aluminum products is complex, resulting in a lot of water waste and pollution, and the weather resistance is insufficient, which cannot meet the anti-corrosion requirements of special industries such as the automobile industry.

Method used

Using a weather-resistant paint film protective layer process that connects chemical bonds between the chemical conversion film and the paint film, a chemical conversion film containing aluminum oxalate, aluminum fluoride, zirconium salt or titanium salt is used, and protected by degreasing and polishing, electrophoresis or spraying layer, reduces washing steps, improves adhesion and corrosion resistance.

Benefits of technology

It significantly reduces the amount of wastewater and solid waste, improves the corrosion resistance and adhesion of aluminum products, meets the weather resistance requirements of special industries, extends the product life, and passes 1,000-hour acid salt spray test to meet the national standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114752927B_ABST
    Figure CN114752927B_ABST
Patent Text Reader

Abstract

The present invention discloses a weather-resistant paint film protective layer aluminum product and a surface treatment method thereof, wherein the surface of the aluminum product is provided with a paint film protective layer, and is characterized in that: a layer of chemical conversion film is also provided between the surface of the aluminum product and the paint film protective layer; the chemical conversion film is a chemical conversion film formed after the aluminum product is degreased, polished and chemically converted; the chemical conversion film is a chemical conversion film containing aluminum oxalate, aluminum fluoride, sodium aluminum hexafluoride, zirconium salt or titanium salt and zirconium-titanium complex salt. The present invention pre-treats the surface of electrophoretic or spray-painted aluminum products by first using a degreasing chemical conversion liquid, and the degreasing and chemical conversion are completed in one step, forming a layer of chemical conversion protective film on the surface of the product, thereby improving the corrosion resistance, anti-pollution, and surface bonding ability of the product, and improving the filamentary corrosion resistance of the aluminum product, and can meet the corrosion resistance quality requirements of special fields such as automotive parts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an aluminum product, and in particular to a surface treatment technology of the aluminum product. Background Art

[0002] At present, the electrophoretic surface treatment process of aluminum alloy products refers to the process of curing water-soluble color paint or varnish by electrophoresis treatment to form a film layer. The commonly used treatment process is to remove oil (surfactant, sulfuric acid or hydrofluoric acid, etc.), wash with water, wash with alkali (sodium hydroxide), wash with water (two steps), pickle, wash with water (two steps), oxidize to form a film, wash with water, wash with pure water, and then electrophoretically form a film. Another treatment process is to remove oil (surfactant, sulfuric acid or hydrofluoric acid, etc.), wash with water, wash with alkali (sodium hydroxide), wash with water (two steps), pickle, wash with water (two steps), passivate, wash with pure water, then electrophoretically form a film, and finally solidify. These two treatment processes are complicated in the whole process, and a large amount of wastewater and solid waste are generated in the production process, including a large amount of hazardous waste. Not only is the production process complicated and the production control requirements are high, but also a large amount of pollutants are brought to the environment. In addition, the second treatment process is not oxidized, and the electrophoretic coating has low adhesion and poor corrosion resistance. In short, the problems existing in the current aluminum product surface treatment technology are that environmental issues have always restricted the development of the industry. The spray painting process of aluminum alloy products refers to the process of using organic solvent-based or water-soluble solvent-based polyvinylidene fluoride (PVDF) paint as a film layer. Most of the aluminum products are pre-treated by degreasing, alkali washing, pickling, water washing, chemical conversion to film (chromization and chromium-free passivation), water washing, and drying steps, and then primer, barrier paint, topcoat, varnish, and curing steps. The electrophoresis or spray painting process of the prior art is not only complicated, but also requires 2-3 water washings between the degreasing, pickling, alkali washing, and chemical conversion to film (chromization / chromium-free passivation) processes of aluminum products, which consumes a lot of water, and consumes a lot of chemical raw materials and water. In addition, about 2 to 6 kg of Al per ton of pre-treatment is washed away and discharged, causing great waste.

[0003] Aluminum products prepared by existing surface treatment processes can meet the requirements of general aluminum products. However, in some special industries, such as the automotive industry, auto parts and automobile shells are exposed to the sun, rain, and even salt, alkali, and acid mist for a long time. This puts higher requirements on the surface corrosion resistance and weather resistance of aluminum products. The current pre-treatment processes cannot meet the international standards (ISO4628-3) after acid salt spray resistance tests.

[0004] Therefore, the current electrophoretic or painting process for aluminum products has the problems of complex process flow, large amount of water washing resulting in large amount of water waste and water pollution, and also waste of some chemical raw materials, resulting in increased production costs, especially poor weather resistance, which cannot meet the surface corrosion protection requirements of special industries. Summary of the invention

[0005] The first technical problem to be solved by the present invention is: in view of the shortcomings of the prior art, a weather-resistant paint film protective layer aluminum product is provided, in which the chemical conversion film and the paint film protective layer of the aluminum product are linked by chemical bonds, thereby increasing the bonding strength between the paint film and the chemical conversion film layer. The paint film has strong adhesion, improves the corrosion resistance of the paint film, and greatly solves the problem of low adhesion between the organic film and the product. It mainly solves the problem of filamentous corrosion under the paint coating and increases the life of the product.

[0006] The second technical problem to be solved by the present invention is: in view of the shortcomings of the prior art, a surface treatment method for aluminum products with a weather-resistant paint film protective layer is provided. The chemical conversion film and the paint film layer of the treated aluminum products are linked by chemical bonds, which increases the bonding force between the film paint and the chemical conversion film layer. The paint film has strong adhesion, improves the corrosion resistance of the paint film, and greatly solves the problem of low adhesion between the organic film and the product. It mainly solves the problem of filamentous corrosion under the paint film and increases the life of the product.

[0007] To solve the above-mentioned first technical problem, the technical solution of the present invention is:

[0008] A weather-resistant paint film protective layer aluminum product, the surface of the aluminum product is provided with a paint film protective layer, characterized in that: a layer of chemical conversion film is also provided between the surface of the aluminum product and the paint film protective layer; the chemical conversion film is a chemical conversion film formed after the aluminum product is degreased, polished and chemically converted; the chemical conversion film is a chemical conversion film containing aluminum oxalate, aluminum fluoride, sodium aluminum hexafluoride, zirconium salt or titanium salt and zirconium-titanium complex salt.

[0009] As a preferred technical solution, the zirconium salt includes NaZrF3(OH)2·H2O and NaZrF3O·2H2O; and the titanium salt is Al2O3·4AlOF·TiO·H2O.

[0010] As an improved technical solution, the thickness of the chemical conversion film is 0.01 to 20 μm.

[0011] As an improved technical solution, the chemical conversion film is a film with uniform irregular morphology.

[0012] As an improved technical solution, the paint film protective layer is an electrophoretic paint protective layer or a spray paint protective layer formed by electrophoresis or spray painting.

[0013] To solve the above second technical problem, the present invention adopts the following two parallel technical solutions:

[0014] The first one:

[0015] The surface treatment method of the weather-resistant paint film protective layer aluminum product comprises the following steps:

[0016] (1) Chemical conversion for degreasing and polishing: The aluminum product to be treated is placed in a chemical conversion solution for degreasing and polishing, and reacted for 1 min to 48 h, and a uniform chemical conversion film is covered on the surface of the aluminum product and the low-lying parts of the product; the chemical conversion solution for degreasing and polishing comprises the following components: 5 to 80 g / L of oxalic acid, 0.1 to 4 g / L of ammonium bifluoride (equivalent to ammonium fluoride and hydrogen fluoride in fluorine content), 10 to 60 g / L of one or two of fluorozirconic acid or fluorotitanic acid or their salts, 0.003 to 0.008 g / L of a surfactant, and 0.05 to 0.15 g / L of an additive;

[0017] (2) Electrophoresis: The aluminum product after chemical conversion is sequentially washed with water and pure water, and then electrophoresed in a resin electrophoretic paint to form an electrophoretic resin film layer on the chemical conversion film;

[0018] (3) Curing: The aluminum product after electrophoresis is cured at 120-240°C.

[0019] Second type:

[0020] The surface treatment method of the weather-resistant paint film protective layer aluminum product comprises the following steps:

[0021] (1) Chemical conversion for degreasing and polishing: The aluminum product to be treated is placed in a chemical conversion solution for degreasing and polishing, and reacted for 1 minute to 48 hours, so that a uniform chemical conversion film is covered on the surface of the aluminum product and the low-lying parts of the product; the chemical conversion solution for degreasing and polishing comprises the following components: 5 to 80 g / L of oxalic acid, 0.1 to 4 g / L of ammonium bifluoride (equivalent to ammonium fluoride and hydrogen fluoride in fluorine content), 10 to 60 g / L of one or two of fluorozirconic acid or fluorotitanic acid or their salts, 0.003 to 0.008 g / L of a surfactant, 0.05 to 0.15 g / L of an additive, and 5 to 200 g / L of a chromium-free passivation resin;

[0022] (2) Painting: The aluminum product after chemical conversion is dried or dripped without water washing and then sprayed with paint to form a protective paint film on the chemical conversion film;

[0023] (3) Curing: The painted aluminum product is cured at 120-240°C.

[0024] As an improved technical solution, the surfactant includes one or more of alkylphenol polyoxyethylene ether, octylphenol polyoxyethylene ether, nonylphenol polyoxyethylene ether, glycerol fatty acid ester, and sorbitan fatty acid ester.

[0025] As an improved technical solution, the auxiliary agent includes one or more of sodium nitrite, sodium oxalate, sodium fluoride, sodium carbonate, sodium sulfate, and sodium hydroxide.

[0026] As an improved technical solution, the temperature of the degreasing and polishing chemical conversion liquid is 10-40°C.

[0027] In the process of chemical conversion treatment of aluminum products for oil removal, grease enters the treatment liquid, and under the joint action of oxalic acid, fluoride ions, ammonium ion surfactants, additives, etc., a transparent fiber with a length of about 30 mm and a specific gravity of less than 1 is generated. The main component is polyester. The fiber removal tank liquid will not be updated due to the increase in grease concentration by regular filtration. The inventor has used this method for four years and the tank liquid is clear and not turbid. The precipitation caused by foreign impurities every year (the amount is very small) can be removed by pouring the tank. There is no pollution without emission. The difference between the present invention and the prior art is that the tank liquid does not need to be replaced and updated, and the flocculent fibers polymerized by grease can be removed by regular filtration, which ensures the clarity of the tank liquid and sustainable reuse, solving the environmental protection problem. Fluozirconic acid, fluorotitanic acid and their salts in the chemical conversion liquid are precipitated in the form of sol-gel during the film formation process. The self-repairing ability of zirconium and titanium ions slows down the growth rate of filamentous corrosion and greatly improves the weather resistance of the product.

[0028] The presence of F ions in the chemical conversion solution of the present invention reduces the chemical energy of AI, making it easier to generate AI. 3+, The concentration of oxalic acid is about 30 times that of hydrogen fluoride and ammonia, and it also ensures AI 3+ It can generate aluminum oxalate and participate in film formation. F ions also act as a catalyst in the reaction process.

[0029] As an improved technical solution, the Al in the chemical conversion solution 3+ The equilibrium concentration is less than 1g / L.

[0030] Due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0031] The present invention pre-treats the surface of aluminum products by first using a degreasing chemical conversion liquid to remove oil stains and natural oxidation on the surface of the aluminum products. The fluorine ions and aluminum ions generated by aluminum trioxide and aluminum on the surface of the aluminum products are captured by oxalic acid and precipitated in the low-lying areas on the surface of the products, filling the mechanical lines of the products. A chemical conversion protective film of aluminum oxalate, aluminum oxide, aluminum fluoride, sodium aluminum hexafluoride, zirconium salt or titanium salt and zirconium-titanium complex salt is formed on the surface of the products, thereby improving the corrosion resistance, pollution resistance and surface bonding ability of the products. The morphology of the chemical conversion film is shown in the attached figure after SEM+EDS detection and analysis. Figure 1-3, which can produce good adhesion between the chemical conversion film and the paint layer, and also greatly solve the problem of low adhesion between the organic film and the product, thus improving the performance indicators of the product and increasing the life of the product. Zirconium salt or titanium salt and zirconium-titanium complex salt play a repairing role in the chemical conversion film, which significantly improves the resistance of aluminum products to filiform corrosion in special industries with high quality requirements, such as automotive parts. After 1000 hours of acid salt spray test, it meets the national standard, proving that the filiform corrosion phenomenon has been significantly improved.

[0032] The present invention completes degreasing and chemical conversion in one step, simplifies the steps, and saves the water washing step between each step in the prior art. During electrophoresis, only the water washing before electrophoresis is retained, and the painting is directly carried out without water washing during painting. Compared with the prior art, wastewater is reduced by 80%, solid waste is reduced by 90%, and there is no heavy metal discharge. The weight of the product after pre-treatment is not only not reduced, but increased by more than 0.5 kg per ton of product, and the adhesion between the product and the paint film is significantly increased, which greatly improves the corrosion resistance of the product, and has good adhesion, resistance to boiling, resistance to salt spray test, and acid and alkali resistance. Chromium-free passivation resin is easier to fill at the bottom of the hole formed by the pore-forming effect of fluoride ions, solving the weak point of corrosion resistance at the bottom of the hole. It can also obtain a morphology state that is easy to be firmly combined with the electrophoretic film, and effectively blocks the diffusion process of corrosion under the film. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0034] Figure 1 This is a surface morphology image of a chemical conversion film with a chemical conversion time of 5 minutes detected by SEM of the present invention, which is magnified 5,000 times;

[0035] Figure 2 This is a surface morphology image of a chemical conversion film with a chemical conversion time of 5 minutes detected by SEM of the present invention, which is magnified 5,000 times;

[0036] Figure 3 This is a surface morphology image of a chemical conversion film with a chemical conversion time of 5 minutes detected by SEM of the present invention, which is magnified 5,000 times;

[0037] Figure 4 Yes Figure 1 EDS analysis energy spectrum of a certain point in the image;

[0038] Figure 5 Yes Figure 1 EDS analysis energy spectrum of a certain point in the image;

[0039] Figure 6 Yes Figure 1 EDS analysis energy spectrum of a certain point in the image;

[0040] Figure 7 Yes Figure 1EDS analysis energy spectrum of a certain point in the image;

[0041] Figure 8 Yes Figure 2 EDS analysis energy spectrum of a certain point in the image;

[0042] Fig. 9 Yes Figure 2 EDS analysis energy spectrum of a certain point in the image;

[0043] Fig.10 Yes Figure 2 EDS analysis energy spectrum of a certain point in the image;

[0044] Fig.11 Yes Figure 2 EDS analysis energy spectrum of a certain point in the image;

[0045] Fig.12 Yes Figure 2 EDS analysis energy spectrum of a certain point in the image;

[0046] Fig.13 This is the filiform corrosion test effect diagram of sample 1;

[0047] Fig.14 This is the filiform corrosion test effect diagram of sample 2;

[0048] Fig.15 , Fig.16 yes Fig.14 An enlarged view of the two marked filamentary corrosion points. DETAILED DESCRIPTION

[0049] The present invention will be further described below in conjunction with the accompanying drawings and Examples. It should be understood that these embodiments are only intended to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0050] like Figure 1-Figure 3 As shown, Figure 1 , Figure 2 , Figure 3 The chemical conversion film obtained by the oil removal chemical conversion of the present invention is uniform and irregular in shape, and has a large surface area when combined with the paint film. The chemical conversion film and the paint film are chemically bonded to obtain the maximum chemical conversion film-paint film bonding force, improve adhesion and impact resistance, alkali resistance, and salt spray resistance, and can more effectively solve the corrosion defects under the film. The aluminum product after the surface treatment of the present invention has excellent adhesion after cross-cutting, impact, and bending tests.

[0051] Respectively Figure 1Select 4 points, corresponding to Figure 4-7 The energy spectrum of the analysis results are shown in Tables 1 to 4 below; Figure 2 Choose any 5 points to perform EDS analysis; Figure 8-12 The energy spectra and analysis results are shown in Tables 5 to 9 below.

[0052] Table 1

[0053] element Line Type Apparent concentration k ratio Wt% Wt%Sigma Standard sample label C K-line system 1.06 0.01064 9.52 0.63 C Vit N K-line system 0.29 0.00052 0.27 0.24 BN O K-line system 0.58 0.00197 0.55 0.10 <![CDATA[SiO2]]> F K-line system 0.30 0.00059 0.10 0.07 <![CDATA[CaF2]]> Mg K-line system 3.19 0.02119 1.80 0.06 MgO Al K-line system 137.55 0.98792 87.38 0.67 <![CDATA[Al2O3]]> Ar K-line system 0.21 0.00205 0.24 0.05 Ar(v) Zr L Line 0.09 0.00092 0.14 0.13 Zr Total 100.00

[0054] Table 2

[0055] element Line Type Apparent concentration k ratio Wt% Wt%Sigma Standard sample label C K-line system 1.10 0.01103 9.83 0.51 C Vit N K-line system 0.02 0.00004 0.02 0.23 BN O K-line system 0.74 0.00250 0.70 0.10 <![CDATA[SiO2 <!-- 4 -->]]> F K-line system 0.06 0.00012 0.02 0.06 <![CDATA[CaF2]]> Mg K-line system 3.26 0.02161 1.83 0.06 MgO Al K-line system 137.63 0.98851 87.44 0.56 <![CDATA[Al2O3]]> Zr L Line 0.11 0.00105 0.16 0.12 Zr Total 100.00

[0056] Table 3

[0057] element Line Type Apparent concentration k ratio Wt% Wt%Sigma Standard sample label C K-line system 0.90 0.00903 8.28 0.52 C Vit N K-line system 0.10 0.00018 0.09 0.25 BN O K-line system 0.57 0.00193 0.54 0.11 <![CDATA[SiO2]]> F K-line system 0.47 0.00093 0.16 0.07 <![CDATA[CaF2]]> Mg K-line system 3.05 0.02025 1.74 0.06 MgO Al K-line system 138.18 0.99242 88.89 0.57 <![CDATA[Al2O3]]> Cr K-line system 0.30 0.00299 0.30 0.10 Cr Zr L Line 0.00 0.00000 0.00 0.14 Zr Total 100.00

[0058] Table 4

[0059] element Line Type Apparent concentration k ratio Wt% Wt%Sigma Standard sample label C K-line system 1.27 0.01270 10.84 0.55 C Vit N K-line system 0.12 0.00021 0.10 0.25 BN O K-line system 1.45 0.00488 1.33 0.12 <![CDATA[SiO2]]> F K-line system 0.38 0.00074 0.12 0.07 <![CDATA[CaF2]]> Mg K-line system 3.27 0.02166 1.81 0.06 MgO Al K-line system 136.88 0.98312 85.26 0.60 <![CDATA[Al2O3]]> Si K-line system 0.32 0.00251 0.42 0.06 <![CDATA[SiO2]]> Zr L Line 0.07 0.00074 0.11 0.14 Zr Total 100.00

[0060] Table 5

[0061] element Line Type Apparent concentration k ratio Wt% Wt%Sigma Standard sample label C K-line system 0.42 0.00418 4.28 0.49 C Vit N K-line system 0.00 0.00000 0.00 0.25 BN O K-line system 0.55 0.00184 0.53 0.11 <![CDATA[SiO2]]> F K-line system 0.13 0.00025 0.04 0.07 <![CDATA[CaF2]]> Na K-line system 0.00 0.00000 0.00 0.04 Albite Mg K-line system 3.39 0.02247 2.02 0.06 MgO Al K-line system 137.02 0.98415 93.13 0.50 <![CDATA[Al2O3]]> Zr L Line 0.00 0.00000 0.00 0.15 Zr Total 100.00

[0062] Table 6

[0063] element Line Type Apparent concentration k ratio Wt% Wt%Sigma Standard sample label C K-line system 0.33 0.00330 3.46 0.53 C Vit N K-line system 0.10 0.00017 0.09 0.28 BN O K-line system 0.42 0.00141 0.41 0.11 <![CDATA[SiO2]]> F K-line system 0.07 0.00014 0.02 0.08 <![CDATA[CaF2]]> Na K-line system 0.07 0.00031 0.03 0.04 Albite Mg K-line system 3.46 0.02296 2.09 0.07 MgO Al K-line system 136.07 0.97730 93.89 0.60 <![CDATA[Al2O3]]> Zr L Line 0.00 0.00000 0.00 0.16 Zr Total 100.00

[0064] Table 7

[0065] element Line Type Apparent concentration k ratio Wt% Wt%Sigma Standard sample label C K-line system 0.39 0.00385 3.95 0.51 C Vit N K-line system 0.13 0.00024 0.12 0.26 BN O K-line system 0.46 0.00155 0.44 0.11 <![CDATA[SiO2]]> F K-line system 0.21 0.00041 0.07 0.08 <![CDATA[CaF2]]> Na K-line system 0.00 0.00000 0.00 0.04 Albite Mg K-line system 3.53 0.02342 2.11 0.07 MgO Al K-line system 137.00 0.98396 93.24 0.59 <![CDATA[Al2O3]]> Zr L Line 0.04 0.00039 0.07 0.15 Zr Total 100.00

[0066] Table 8

[0067] element Line Type Apparent concentration k ratio Wt% Wt%Sigma Standard sample label C K-line system 0.49 0.00490 4.96 0.52 C Vit N K-line system 0.08 0.00015 0.08 0.26 BN O K-line system 0.50 0.00167 0.48 0.11 <![CDATA[SiO2]]> F K-line system 0.04 0.00007 0.01 0.07 <![CDATA[CaF2]]> Na K-line system 0.03 0.00014 0.01 0.04 Albite Mg K-line system 3.53 0.02341 2.10 0.07 MgO Al K-line system 136.17 0.97805 92.31 0.59 <![CDATA[Al2O3]]> Zr L Line 0.03 0.00030 0.05 0.15 Zr Total 100.00

[0068] Table 9

[0069]

[0070]

[0071] Example 1

[0072] A weather-resistant paint film protective layer aluminum product, the surface of the aluminum product is provided with an electrophoretic paint protective layer formed by electrophoresis, and a chemical conversion film with a thickness of 0.2μm is also provided between the surface of the aluminum product and the electrophoretic paint protective layer; the chemical conversion film is a chemical conversion film formed after the aluminum product is degreased, polished and chemically converted; the chemical conversion film is a chemical conversion film containing aluminum oxalate, aluminum fluoride, sodium aluminum hexafluoride, zirconium salt or titanium salt and zirconium-titanium complex salt.

[0073] Example 2

[0074] A weather-resistant paint film protective layer aluminum product, the surface of the aluminum product is provided with an electrophoretic paint protective layer formed by electrophoresis, and a chemical conversion film with a thickness of 2.0 μm is also provided between the surface of the aluminum product and the electrophoretic paint protective layer; the chemical conversion film is a chemical conversion film formed after the aluminum product is degreased, polished and chemically converted; the chemical conversion film is a chemical conversion film containing aluminum oxalate, aluminum fluoride, sodium aluminum hexafluoride, zirconium salt or titanium salt Al2O3·4AlOF·TiO·H2O including NaZrF3(OH)2·H2O and NaZrF3O·2H2O, and zirconium-titanium complex salt.

[0075] Example 3

[0076] A weather-resistant paint film protective layer aluminum product, the surface of the aluminum product is provided with a spray paint protective layer formed by spray painting, and a layer of chemical conversion film with a thickness of 4.0 μm is also provided between the surface of the aluminum product and the spray paint protective layer; the chemical conversion film is a chemical conversion film formed after the aluminum product is degreased, polished and chemically converted; the chemical conversion film is a chemical conversion film containing aluminum oxalate, aluminum fluoride, sodium aluminum hexafluoride, zirconium salt or titanium salt Al2O3·4AlOF·TiO·H2O including NaZrF3(OH)2·H2O and NaZrF3O·2H2O, and zirconium-titanium complex salt.

[0077] Example 4

[0078] (1) Degreasing and polishing chemical conversion: The aluminum product to be treated is placed in a degreasing and polishing chemical conversion solution at a temperature of 20° C. and reacted for 5 minutes. A uniform chemical conversion film is covered on the surface of the aluminum product and the low-lying parts of the product. The degreasing and polishing chemical conversion solution contains the following components: 18 g / L oxalic acid, 1.4 g / L ammonium bifluoride, 50 g / L fluorozirconic acid, 0.005 g / L surfactant alkylphenol polyoxyethylene ether, and 0.12 g / L auxiliary agent sodium nitrite;

[0079] (2) Electrophoresis: The aluminum product after chemical conversion is washed with water and then with pure water, and then electrophoresed in a resin electrophoretic paint to form an electrophoretic resin film layer on the chemical conversion film, and finally cured;

[0080] (3) Curing: The aluminum product after electrophoresis is cured at 200°C.

[0081] Example 5

[0082] (1) Chemical conversion for degreasing and polishing: The aluminum product to be treated is placed in a degreasing and polishing chemical conversion solution at a temperature of 30°C and reacted for 2 hours, and a uniform chemical conversion film is covered on the surface of the aluminum product and the low-lying parts of the product; the degreasing and polishing chemical conversion solution comprises the following components: 40 g / L oxalic acid, 1.8 g / L ammonium bifluoride, 20 g / L fluorotitanic acid, 0.004 g / L surfactant octylphenol polyoxyethylene ether, and 0.10 g / L auxiliary agent sodium oxalate;

[0083] (2) Electrophoresis: The aluminum product after chemical conversion is washed with water and then with pure water, and then electrophoresed in a resin electrophoretic paint to form an electrophoretic resin film layer on the chemical conversion film, and finally cured for 30 minutes;

[0084] (3) Curing: The aluminum product after electrophoresis is cured at 160°C.

[0085] Example 6

[0086] (1) Chemical conversion for degreasing and polishing: The aluminum product to be treated is placed in a degreasing and polishing chemical conversion solution at a temperature of 25° C. and reacted for 6.5 minutes. A uniform chemical conversion film is covered on the surface of the aluminum product and the low-lying parts of the product. The degreasing and polishing chemical conversion solution comprises the following components: 20 g / L oxalic acid, 2.5 g / L ammonium bifluoride, 22 g / L of fluorozirconic acid and fluorotitanic acid, 0.006 g / L of surfactant glycerol fatty acid ester, and 0.12 g / L of auxiliary agent sodium fluoride.

[0087] (2) Electrophoresis: The aluminum product after chemical conversion is washed with water and then with pure water, and then electrophoresed in a resin electrophoretic paint to form an electrophoretic resin film layer on the chemical conversion film, and finally enters a curing furnace for curing at 210° C. for 25 minutes;

[0088] (3) Curing: The aluminum product after electrophoresis is cured at 150°C.

[0089] Example 7

[0090] (1) Chemical conversion for degreasing and polishing: The aluminum product to be treated is placed in a degreasing and polishing chemical conversion solution at a temperature of 22° C. and reacted for 30 minutes. A uniform chemical conversion film is formed on the surface of the aluminum product and the low-lying parts of the product. The degreasing and polishing chemical conversion solution comprises the following components: 25 g / L oxalic acid, 2.5 g / L ammonium bifluoride, 45 g / L fluorozirconic acid, 0.004 g / L surfactant octylphenol polyoxyethylene ether, 0.08 g / L auxiliary sodium oxalate, and 80 g / L chromium-free passivation resin.

[0091] (2) Painting: The aluminum product after chemical conversion is dried or dripped without water washing and then sprayed with paint to form a protective paint film on the chemical conversion film;

[0092] (3) Curing: The painted aluminum product is cured at 140°C.

[0093] Example 8

[0094] (1) Degreasing and polishing chemical conversion: The aluminum product to be treated is placed in a degreasing and polishing chemical conversion solution at a temperature of 20° C. and reacted for 20 minutes. A uniform chemical conversion film is covered on the surface of the aluminum product and the low-lying parts of the product. The degreasing and polishing chemical conversion solution comprises the following components: 40 g / L oxalic acid, 3 g / L ammonium bifluoride, 40 g / L fluorotitanic acid, 0.006 g / L surfactant glycerol fatty acid ester, 0.13 g / L auxiliary sodium nitrite, and 120 g / L chromium-free passivation resin;

[0095] (2) Painting: The aluminum product after chemical conversion is dried or dripped without water washing and then sprayed with paint to form a protective paint film on the chemical conversion film;

[0096] (3) Curing: The painted aluminum product is cured at 180°C.

[0097] Comparative test example

[0098] The aluminum sample was subjected to the degreasing and polishing chemical conversion and electrophoresis of Example 4 to obtain Sample 1.

[0099] The same aluminum sample was degreased, polished and chemically converted by the same steps as in Example 4 (the difference is that the degreasing, polishing and chemical conversion liquid does not contain fluorozirconic acid, and the rest is the same), and then subjected to electrophoresis to obtain comparative sample 2.

[0100] Sample 1 and sample 2 were subjected to filiform corrosion test at the same time. After 1000h acid salt spray test, Fig.13 and Fig.14 The samples are compared with those of sample 1 and sample 2 respectively. Fig.15 and Fig.16 They are Fig.14 The magnified effect diagram of the two filamentary corrosion points marked in the figure. The experiment shows that the sample with added fluorozirconic acid has no filamentary corrosion phenomenon, the corrosion width is good after the salt spray test, the cross-cut adhesion is good, and the addition of fluorozirconic acid significantly improves the filamentary corrosion phenomenon.

Claims

1. A surface treatment method for an aluminum product with a weather-resistant paint film protective layer, wherein the surface of the aluminum product is provided with a paint film protective layer, characterized in that: A layer of chemical conversion film is also arranged between the surface of the aluminum product and the paint film protective layer; the chemical conversion film is a chemical conversion film formed after the aluminum product is degreased, polished and chemically converted; the chemical conversion film is a chemical conversion film containing aluminum oxalate, aluminum fluoride, sodium aluminum hexafluoride, zirconium salt or titanium salt and zirconium-titanium complex salt; comprising the following steps: (1) Chemical conversion for degreasing and polishing: the aluminum product to be treated is placed in a degreasing and polishing chemical conversion liquid, and reacted for 1 minute to 48 hours, so that a uniform chemical conversion film is covered on the surface of the aluminum product and the low-lying parts of the product; the composition of the degreasing and polishing chemical conversion liquid is: 5 to 80 g / L of oxalic acid, 0.1 to 4 g / L of ammonium bifluoride, 10 to 60 g / L of one or two of fluorozirconic acid or fluorotitanic acid or their salts, 0.003 to 0.008 g / L of surfactant, 0.05 to 0.15 g / L of additive, and 5 to 200 g / L of chromium-free passivation resin; (2) Painting: The aluminum product after chemical conversion is dried without washing or dripped dry before painting to form a protective paint film on the chemical conversion film; (3) Curing: The painted aluminum products are cured at 120-240°C.

2. The surface treatment method of aluminum products with weather-resistant paint film protective layer according to claim 1, characterized in that: The surfactant includes one or more of alkylphenol polyoxyethylene ether, octylphenol polyoxyethylene ether, nonylphenol polyoxyethylene ether, glycerol fatty acid ester, sorbitan fatty acid ester; the auxiliary agent includes one or more of sodium nitrite, sodium oxalate, sodium fluoride, sodium carbonate, sodium sulfate, and sodium hydroxide.

3. The surface treatment method of aluminum products with weather-resistant paint film protective layer according to claim 1, characterized in that: The temperature of the degreasing and polishing chemical conversion liquid is 10-40°C.

4. The surface treatment method of aluminum products with weather-resistant paint film protective layer according to claim 1, characterized in that: The zirconium salt includes NaZrF3(OH)2•H2O and NaZrF3O•2H2O; the titanium salt is Al2O3•4AlOF•TiO•H2O.

5. The surface treatment method of aluminum products with weather-resistant paint film protective layer according to claim 1, characterized in that: The thickness of the chemical conversion film is 0.01 to 20 μm.