Resin component processing method, resin component processing device, and resin component manufacturing method

By first irradiating the first light in the resin member to excite electrons, and then irradiating the second light, heating it in the wavelength region where the light absorption rate increases, the problem of low heating efficiency in the prior art is solved, and the resin is realized Efficient resin processing and bonding.

CN114929458BActive Publication Date: 2024-12-03LASER SYST INC +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080090664.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-27
Filing Date
2020-12-07
Publication Date
2024-12-03
Estimated Expiration
2040-12-07

AI Technical Summary

Technical Problem

In the prior art, resins are difficult to fully absorb light energy under near-infrared or infrared laser irradiation, resulting in low heating efficiency and difficult to process effectively.

Method used

By first irradiating the first light having a specific wavelength, the resin is electron-excited, and then irradiating the second light having a longer wavelength than the first light, the resin is heated in a wavelength region where the light absorption rate is increased.

Benefits of technology

It realizes efficient heating and fine processing of resin, improves laser irradiation accuracy and efficiency, and enables the resin to reach above the glass transition temperature, thereby achieving bonding or other processing needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114929458B_ABST
    Figure CN114929458B_ABST
Patent Text Reader

Abstract

The subject of the present invention is to provide a method for processing a resin component by sufficiently raising the temperature of only a desired area in a component containing resin by irradiation with light. Moreover, the subject of the present invention is to provide a processing device for a resin component and a method for manufacturing a resin component for performing the processing. The processing method of a resin component for solving the above-mentioned problem includes: a process of irradiating a first light of a first wavelength to electronically excite the resin to a first component containing resin; and a process of irradiating the resin electronically excited by the irradiation with a second light of a second wavelength, the second wavelength being a longer wavelength than the first wavelength. The second wavelength is included in the wavelength region where the light absorption rate of the resin increases by being electronically excited.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for processing a resin member, a device for processing a resin member, and a method for manufacturing a resin component. Background Art

[0002] In recent years, in the field of electronic devices and equipment, not only inorganic materials such as semiconductors and metals are used, but also devices and equipment that partially introduce organic materials (resins) in order to maximize their functions have attracted attention. When manufacturing such devices and equipment, it is necessary to join components containing resins to other components or to perform precision processing (cutting, forming grooves, etc.) on components containing resins.

[0003] As a processing method for components containing resin, laser cladding has attracted attention (for example, Patent Document 1). In this laser cladding method, at least one of two or more components (at least one of which contains resin) is irradiated with near-infrared or infrared laser. In the laser-irradiated portion, the temperature of the resin rises to above the glass transition temperature due to the photothermal effect. Then, multiple components are joined by bringing the melted resin of the laser-irradiated component into close contact with another component.

[0004] Furthermore, conventionally, processing has been performed in which a resin member is locally heated by irradiating a near-infrared or infrared laser to cut the resin member at a desired position or to form a groove at a desired position in the resin member.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2012-27447. Summary of the invention

[0008] Problem that the invention aims to solve

[0009] In order to heat the resin by laser irradiation, it is necessary to irradiate the resin with a laser in a wavelength range that the resin can absorb. However, general-purpose resins (such as polystyrene (hereinafter also referred to as "PS"), polymethyl methacrylate (hereinafter also referred to as "PMMA"), polyethylene terephthalate (hereinafter also referred to as "PET"), and polycarbonate (hereinafter also referred to as "PC") generally do not absorb in the visible light region. For example, PET has no substantial light absorption in a wide range of wavelengths from 400nm to 2200nm. In addition, polycarbonate also has no substantial light absorption in a wide range of wavelengths from 400nm to 1600nm. Therefore, in order to process PET and polycarbonate, it is necessary to irradiate with a laser with a wavelength longer than the above value.

[0010] In addition, the absorption coefficient of light in the near-infrared region (wavelength of about 800nm ​​to 2μm) of the resin is very small. Therefore, even when the resin is irradiated with a laser in the near-infrared region with high light intensity, absorption saturation (hereinafter, this phenomenon is also referred to as "absorption saturation") is likely to occur. Therefore, it is difficult to make the resin absorb light energy above the threshold. Therefore, there is room for improvement in the heating of resin using near-infrared or infrared lasers (photothermal reaction).

[0011] The present invention is completed in view of such a situation. That is, the purpose of the present invention is to provide a method for processing a resin component by efficiently raising the temperature of a component containing resin by irradiating light. In addition, its purpose is also to provide a processing device for a resin component for performing the processing and to provide a method for manufacturing a resin component.

[0012] Solutions to the problem

[0013] The present invention provides the following method for processing a resin member.

[0014] The processing method of the resin component includes: a process of irradiating a first component containing resin with a first light of a first wavelength to electronically excite the resin; and a process of irradiating the resin that is electronically excited by the irradiation of the first light with a second light of a second wavelength, wherein the second wavelength is a longer wavelength than the first wavelength, and a wavelength region of the second wavelength is included in a wavelength region where the light absorption rate of the resin increases due to the electronic excitation of the resin.

[0015] The present invention provides the following resin member processing apparatus.

[0016] The processing device of the resin component comprises: a first light irradiation system, which is used to irradiate the resin of the first component containing the resin with a first light of a first wavelength to excite the electrons of the resin; and a second light irradiation system, which is used to irradiate the resin of the first component with a second light of a second wavelength, wherein the second wavelength is a longer wavelength than the first wavelength, and the wavelength region of the second wavelength is included in the wavelength region where the light absorption rate of the resin increases due to the electronic excitation of the resin.

[0017] The present invention provides the following method for producing a resin component.

[0018] The manufacturing method of the resin component includes: a process of irradiating a first component containing resin with a first light of a first wavelength to electronically excite the resin; and a process of irradiating the resin that has been electronically excited by the irradiation with the first light with a second light of a second wavelength, wherein the second wavelength is a longer wavelength than the first wavelength, and a wavelength region of the second wavelength is included in a wavelength region where the light absorption rate of the resin increases due to the electronic excitation of the resin.

[0019] Effects of the Invention

[0020] According to the method for processing a resin member of the present invention, the member containing resin can be processed by sufficiently raising its temperature by irradiation with light.

[0021] Furthermore, according to the resin member processing apparatus of the present invention, it is possible to process the resin by irradiating a desired region with two or more types of light.

[0022] According to the method for manufacturing a resin component of the present invention, the resin component can be manufactured by sufficiently raising the temperature of a member containing resin by irradiation with light. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a schematic diagram showing an example of a processing apparatus for a resin member according to the present invention.

[0024] Figure 2A is a diagram schematically showing the wavelength region in which the light absorption rate increases due to the increase in resin temperature caused by electron excitation. Figure 2B This is a diagram schematically showing a wavelength region in which the light absorption rate increases due to the excited triplet state transiently presented by electron excitation.

[0025] Figure 3 This is a schematic diagram for explaining a method for manufacturing a resin component.

[0026] Figure 4 This is a diagram showing the relationship between the total output of laser light and the temperature of the PET plate when the PET plate is irradiated with laser light in Example 3 of the present invention.

[0027] Figure 5 This is a diagram showing the relationship between the total output of laser light and the temperature of the PC board when the PC board is irradiated with laser light in Example 3 of the present invention.

[0028] Figure 6 This is a graph showing the relationship between the total output of laser light and the temperature of the PMMA plate when the PMMA plate is irradiated with laser light in Example 3 of the present invention. DETAILED DESCRIPTION

[0029] The present invention relates to a processing method for a resin component, a processing device for a resin component used in the processing method, and a method for manufacturing a resin component using the processing method. Below, taking an embodiment of the present invention as an example, the processing method for a component, the processing device, and the method for manufacturing a resin component are described, but the present invention is not limited to the embodiment.

[0030] 1. Processing method of resin components

[0031] In a method for processing a resin member according to an embodiment of the present invention, the following steps are performed: a step of irradiating a first member containing a resin with a first light of a first wavelength to electronically excite the resin (first light irradiation step); and a step of irradiating the resin electronically excited by the irradiation with the first light with a second light of a second wavelength (second light irradiation step), the second wavelength being a wavelength longer than the first wavelength. In addition, the second wavelength is a wavelength included in a wavelength region where the light absorption rate of the resin increases due to the electronic excitation of the resin.

[0032] As described above, in the method of irradiating near-infrared light or infrared light to the resin to excite the resin vibration, absorption saturation easily occurs, making it difficult to sufficiently increase the temperature of the resin.

[0033] In contrast, in this embodiment, the first light having the first wavelength is irradiated to excite the electrons of the resin of the first component to be processed. The electron excitation mentioned here refers to the excitation of the electrons of the chromophore of the polymer as the resin, mainly with π-π * Transition or n-π * The electrons corresponding to the transition are excited. If the electrons of the resin are excited, a wavelength region where the light absorption rate increases will be generated. Therefore, in the present embodiment, a second light of a second wavelength contained in the wavelength region where the light absorption rate increases is also irradiated. By irradiating the resin with the second light, the temperature of the resin is sufficiently increased, and the first component becomes processable. In addition, in the present specification, the wavelength region where the light absorption rate of the resin increases can be any wavelength region where the light absorption rate of the resin increases compared to before the irradiation of the first light, and this wavelength region also includes a wavelength region where there is no light absorption before the irradiation of the first light but newly shows light absorption through the irradiation of the first light.

[0034] Here, the wavelength region where the light absorption rate increases by electronically exciting the resin includes two wavelength regions. The first wavelength region where the light absorption rate increases is a wavelength region that exists on the longer wavelength side than the first wavelength (first light) used to make the resin electronically transition, and where the light absorption rate increases due to the temperature rise of the resin caused by electronic excitation. This wavelength region is also called a "tropical zone" and is explained by Urbach's law.

[0035] Urbach's law states that the shape A of the low energy side (long wavelength side) of the absorption spectrum of a substance is expressed by the following formula.

[0036] [Formula 1]

[0037] A(E, T) = A0exp(σ(E-E0) / kT)

[0038] In the above formula, A0 represents a proportionality constant, and σ represents a steepness coefficient. σ represents a value close to 1. E represents the photon energy of light absorbed by a substance, and is represented by E=h(c / λ). The photon energy of the light is related to the wavelength λ of the light to be absorbed. In addition, h in the formula is Planck's constant, and c is the speed of light. In addition, the above E0 is the energy level of the substance, k is the Boltzmann constant, and T is the absolute temperature.

[0039] According to the above-mentioned Urbach law, as the temperature of the substance rises, the end of the low energy side of the absorption spectrum moves to the long wavelength side. Therefore, light absorption occurs even in a wavelength region where little or no absorption occurs at low temperatures. That is, as in the present embodiment, when the resin electrons are excited by irradiation with the first light, the temperature of the resin increases, thereby increasing the light absorption rate even in a wavelength region on the long wavelength side compared to the wavelength region where the resin can normally absorb light.

[0040] The second wavelength region where the light absorption rate increases is located on the longer wavelength side than the first wavelength (first light) for causing electron transition in the resin and where the light absorption rate increases due to the excited triplet state transiently presented by electron excitation.

[0041] Among organic substances, there are many that have no light absorption in the visible light region in the ground state, but have absorption in the visible light region in the excited state and have a large absorption coefficient. For example, The Journal of Physical Chemistry 1993, Vol. 97, pp. 6753-6759 (published by the American Chemical Society) shows the absorption spectrum of the excited triplet state of PET. As mentioned above, PET has no light absorption in the wavelength range of 400nm to 2200nm in the ground state. However, the document shows that if PET is in the excited triplet state, there is a light absorption band in the wavelength range of 390nm to 550nm.

[0042] In addition, Macromolecules, Vol. 27, No. 14, 1994 (published by the American Chemical Society) shows the absorption spectrum of the excited triplet state of polycarbonate. In this document, polycarbonate also has no light absorption in the wavelength range of 400nm to 1600nm in the ground state. However, this document shows that if polycarbonate is made into an excited triplet state, there is a light absorption band in the wavelength range of 350nm to 500nm. That is, as in the present embodiment, if the resin electrons are excited by irradiation with the first light, the resin becomes an excited triplet state, thereby presenting a new wavelength region capable of light absorption on the long wavelength side compared to the wavelength region in which the resin can usually absorb light.

[0043] Here, the processing method of the resin component of the present embodiment can be applied to a method of heating and processing a first component containing resin, and can be applied to various methods. For example, it can be applied to a method of joining a first component containing resin to other components. In addition, it can also be applied to a method of cutting or forming a groove in a first component containing resin. Below, taking the method of joining a first component containing resin to a second component as an example, the first light irradiation process and the second light irradiation process and the joining process of the present embodiment are described, but the processing method of the present embodiment is not limited to the joining method.

[0044] (First Light Irradiation Step)

[0045] In this process, the first light having a first wavelength is irradiated to the first member containing the resin. Here, the resin contained in the first member can be any resin that can be electronically excited by irradiation with light (first light), and examples thereof include polyethylene terephthalate (PET), polystyrene, polymethyl methacrylate (PMMA), polycarbonate (PC), etc. In addition, the resin may not have absorption caused by electronic excitation for the wavelength of the second light (second wavelength) described later.

[0046] Among the above-mentioned resins, polyethylene terephthalate (PET), polycarbonate (PC), or polymethyl methacrylate (PMMA) is preferred because it is easily excited by electrons when irradiated with the first light and the light absorption rate on the long wavelength side is easily increased. In addition, the first member may contain at least a resin in the region joined to the second member described later, and may also contain components other than the resin.

[0047] In addition, the shape of the first member is not particularly limited, and may be, for example, a flat plate or a three-dimensional structure. In addition, the bonding surface of the first member with the second member may be a flat surface or a curved surface.

[0048] The transmittance of the light (the first light and the second light) of the first member can be appropriately selected according to the direction of the irradiated light (the first light and the second light). For example, when the first light and the second light are irradiated from the side of the first member joining the second member, the first member may not be transmittant to the first light and the second light. On the other hand, when the first light and the second light are irradiated from the opposite side of the first member joining the second member, it is preferred that the first member be transmittant to the first light and the second light.

[0049] The wavelength of the first light irradiated in this process (first wavelength) can be any wavelength that can excite the resin electrons in the first member, and can be appropriately selected according to the type of resin. For example, if it is polyethylene terephthalate (PET) or polycarbonate (PC), the wavelength region of the first wavelength is preferably below 410nm, for example, it can be set to a laser with a wavelength of 375nm or a laser with a wavelength of 405nm.

[0050] Here, the first light is particularly preferably a laser. If the first light is a laser, its irradiation area can be controlled to be very small, and the first light can be irradiated in a precise pattern. In addition, the laser can be a continuously oscillating laser or a pulsed oscillating laser. From the viewpoint of being able to continuously irradiate the first light to the desired area, a continuously oscillating laser is more preferred.

[0051] In addition, at this time, the output of the laser light source is preferably 10mW to 500mW. For example, for polyethylene terephthalate (PET), it is more preferably 100mW to 400mW. For example, for polycarbonate (PC), it is preferably 30mW to 250mW, and more preferably 30mW to 200mW. For example, for polymethyl methacrylate (PMMA), it is more preferably 100mW to 400mW. By irradiating the first light with the above output, the resin electrons can be efficiently excited. In addition, preferably, the light intensity at the focusing position of the first light is 0.01kW / cm 2 More preferably, 0.01 kW / cm 2 ~1.00kW / cm 2 .

[0052] Furthermore, preferably, the accumulated light amount of the first light at the focusing position of the first light is 0.2 mJ / cm 2 ~35.0mJ / cm 2 When the accumulated light amount of the first light is within this range, the temperature of the resin can be sufficiently increased by electron excitation to generate the above-mentioned hot zone or the above-mentioned excited triplet state.

[0053] Furthermore, when the first light is irradiated, the temperature of the region irradiated with the first light may be measured, and the intensity of the first light may be adjusted based on the temperature.

[0054] (Second Light Irradiation Step)

[0055] In this process, the resin excited by the electrons by the irradiation of the first light is irradiated with the second light of the second wavelength, and the second wavelength is longer than the wavelength of the first light. The timing of irradiating the second light can be any period during which the resin is excited by the electrons by the irradiation of the first light, and can be slightly staggered from the irradiation of the first light, but generally speaking, it is preferred to irradiate the first light and the second light simultaneously.

[0056] The wavelength of the second light irradiated in this process (second wavelength) only needs to be a wavelength that is longer than the first wavelength and is included in the wavelength region where the light absorption rate of the resin increases due to the electronic excitation of the resin. As described above, the wavelength region where the light absorption rate increases due to the electronic excitation of the resin can be a wavelength region that exists on the longer wavelength side than the first wavelength (first light) and causes the temperature of the resin to increase due to the electronic excitation. In addition, as described above, the wavelength region where the light absorption rate increases due to the electronic excitation of the resin can be a wavelength region that exists on the longer wavelength side than the first wavelength (first light) and increases the light absorption rate due to the transiently presented excited triplet state caused by the electronic excitation. The second light can be light of a wavelength contained in one of the above-mentioned wavelength regions.

[0057] Here, the wavelength region in which the light absorption rate increases due to the temperature rise of the resin caused by electron excitation is present on the longer wavelength side than the first wavelength (first light), for example Figure 2A The wavelength region indicated by the dotted line in FIG. In addition, the wavelength region in which the light absorption rate increases due to the transiently present excited triplet state caused by electron excitation is present on the longer wavelength side than the first wavelength (first light), for example, Figure 2B The dotted line in the figure shows the wavelength region. Figure 2A and Figure 2B In FIG. 8 , the wavelength region indicated by the solid line is the original absorption wavelength region of the resin.

[0058] The wavelength region in which the light absorption rate of the resin increases due to the electronic excitation of the resin varies depending on the type of resin. Therefore, the second wavelength is appropriately selected in accordance with the type of resin. For example, in the case of polyethylene terephthalate (PET), polycarbonate (PC), etc., preferably, the wavelength region of the second wavelength is greater than 400 nm and less than 550 nm, for example, a laser with a wavelength of 405 nm or a laser with a wavelength of 450 nm can be used.

[0059] Here, the second light is also preferably a laser. If the second light is a laser, its irradiation area can be controlled to be very small, and the second light can be irradiated in a precise pattern. In addition, the laser can be a continuously oscillating laser or a pulsed oscillating laser. From the viewpoint of being able to continuously irradiate the desired area with the second light, a continuously oscillating laser is more preferred.

[0060] In addition, at this time, the output of the light source from the laser is preferably 30mW to 1200mW. For example, for polyethylene terephthalate (PET), it is more preferably 100mW to 1000mW. For example, for polycarbonate (PC), it is more preferably 50mW to 500mW. For example, for polymethyl methacrylate (PMMA), it is more preferably 100mW to 500mW. By irradiating the second light with the above output, the temperature of the resin in the first component can be efficiently increased. In addition, preferably, the light intensity at the focusing position of the second light is 0.01kW / cm 2 More preferably, 0.01 kW / cm 2 ~2.00kW / cm 2 .

[0061] The accumulated light intensity at the focusing position of the second light may be an amount of light that can heat the first member (resin) to a temperature above the glass transition temperature of the resin in the first member. For example, 0.2 mJ / cm 2 ~65.0mJ / cm 2 When the accumulated light amount of the second light is within this range, the temperature of the resin is sufficiently increased, and the first member and the second member can be easily firmly bonded to each other.

[0062] Here, the second light may be irradiated from a direction coaxial with the first light or from a different direction. In addition, in this process, the temperature of the area irradiated with the second light (and the first light) may be measured and the intensity of the second light may be adjusted according to the temperature.

[0063] (Joining process)

[0064] The bonding process is a process of bonding the region (resin) of the first member irradiated with the first light and the second light to the second member. In addition, the bonding process may be performed after the first member is subjected to the first light irradiation process and the second light irradiation process. That is, after the first member is subjected to the first light irradiation process and the second light irradiation process, the temperature of the resin in the first member is sufficiently increased, and then the first member is overlapped and bonded with the second member prepared separately (prepared in the preparation process).

[0065] On the other hand, the bonding process may be performed simultaneously with the above-mentioned first light irradiation process and the second light irradiation process (especially simultaneously with the second light irradiation process). In the case where the bonding process and the first light irradiation process and the second light irradiation process are performed simultaneously, the above-mentioned first member and the second member are overlapped in advance so that the first light and the second light are focused on their interface, thereby enabling the first light irradiation process, the second light irradiation process and the bonding process to be performed simultaneously.

[0066] Furthermore, in the joining step, the first member and the second member may be pressed against each other as necessary.

[0067] Here, the type of the second component is not particularly limited as long as it is a component that can be bonded to the first component, and can be appropriately selected according to the purpose. For example, it can be the same resin as the first component, or it can be a different resin. In addition, when the second component contains a resin, it is also possible to heat up not only the resin in the first component but also the resin in the second component by irradiating the first light and the second light. On the other hand, the second component can also be an inorganic material such as metal or ceramic.

[0068] The shape of the second member is not particularly limited, and may be, for example, a flat plate or a three-dimensional structure. In addition, the bonding surface of the second member to the first member may be a flat surface or a curved surface.

[0069] The transmittance of light (the first light and the second light) to the second component can be appropriately selected according to the timing of the bonding process and the direction of the irradiated light (the first light and the second light). For example, in the case where the first light irradiation process and the second light irradiation process are not performed simultaneously with the bonding process, the second component may not be transmittance to the first light and the second light. In addition, even in the case where the first light irradiation process and the second light irradiation process are performed in a state where the first component and the second component are overlapped, when the first light and the second light are irradiated from the first component side, the second component may not be transmittance to the first light and the second light. On the other hand, in the case where the first light irradiation process and the second light irradiation process are performed in a state where the first component and the second component are overlapped, and the first light and the second light are irradiated from the second component side, it is preferred that the second component is transmittance to the first light and the second light.

[0070] (other)

[0071] In the above description, the irradiation of two wavelengths of light, the first light and the second light, is described. However, in the present embodiment, light of three or more wavelengths may be irradiated. For example, the second light having a wavelength equivalent to the tropical zone generated by the irradiation of the first light is irradiated, and further the third light having a wavelength equivalent to the absorption wavelength region of the excited triplet state generated by the irradiation of the first light is irradiated, so that the temperature of the resin in the first component can be further efficiently raised.

[0072] In addition, in the above, a method of joining a first component to a second component by irradiating a first light is described, but the present embodiment may also be a method of, for example, melting a desired portion of the first component to cut the first component into a desired shape, or heating a portion of the first component to form a desired recess, etc.

[0073] In the above description, the following case is described, that is, by irradiation with the first light, the resin contained in the first member is electronically excited, and the second light included in the wavelength region where the light absorption rate of the resin increases due to the electronic excitation is irradiated. However, in this embodiment, when irradiating with the first light, the first member absorbs the first light, and the second light having a second wavelength included in the wavelength region where the resin in the first member exhibits light absorption due to the light absorption is irradiated.

[0074] (Effect)

[0075] In the above method, the first light is used to excite the electrons of the resin, and the second light contained in the wavelength region where the electron excitation causes increased light absorption is irradiated. In this way, by combining the two wavelengths of light that the resin can absorb for irradiation, the resin can absorb more light energy and can be efficiently heated. Moreover, the laser with a shorter wavelength such as a laser with a wavelength of 375nm or a laser with a wavelength of 405nm used as the first light can narrow the irradiation range compared with the laser with a longer wavelength such as near infrared and infrared, so the irradiation accuracy of the laser can be improved. Therefore, compared with the use of lasers with a longer wavelength such as near infrared and infrared to process resin components, delicate processing can be performed.

[0076] In addition, sometimes the light absorption rate of the resin in the wavelength region where the light absorption rate increases due to electron excitation is significantly greater than the light absorption rate of the first light. Therefore, by the above method, the resin can absorb a lot of light energy by irradiation with the second light, and as a result, the resin temperature can be efficiently raised.

[0077] In general, the oscillation wavelength of a high-output laser irradiation system is usually 400nm to 1600nm. In addition, in order to avoid internal damage caused by its short wavelength, a laser irradiation system with an oscillation wavelength of less than 400nm is generally low-output. In the above method, the second wavelength of the second light can be set to exceed 400nm. Therefore, a high-output laser irradiation system can also be used.

[0078] 2. Processing equipment

[0079] The above-mentioned processing method can be performed by the following processing device including a first light irradiation system for irradiating the first light of the above-mentioned first wavelength and a second light irradiation system for irradiating the second light of the above-mentioned second wavelength. However, the device for performing the above-mentioned processing method is not limited to this device. In addition, in the following description, a device for joining the first member and the second member is described, but the processing device may also be, for example, a cutting device or a cutting device for the first member.

[0080] Figure 1An example of a processing device according to this embodiment is shown. Figure 1 As shown, the processing device 100 includes: an XY stage for mounting the first member 111 and the second member 112, a first light irradiation system 120, a second light irradiation system 130, a lens 140, a temperature measurement unit 150, and a light quantity control unit 160. In addition, as required, a support unit (not shown) and a position control unit (not shown) for controlling the relative position of the first member 111 and the second member 112 may also be included.

[0081] The first light irradiation system 120 is a light irradiation system for irradiating the first light 123, and can be configured to include, for example, a first laser light source 121 and a first reflecting mirror (dichroic mirror) 122. The first laser light source 121 can be, for example, a laser that oscillates a laser with a wavelength of 375 nm or a laser with a wavelength of 405 nm.

[0082] The second light irradiation system 130 is a light irradiation system for irradiating the second light 133, and may include, for example, a second laser light source 131 and a second reflecting mirror 132. The second laser light source 131 may be, for example, a laser that oscillates laser light of a wavelength of 405 nm or 450 nm.

[0083] The type of lens 140 is not particularly limited as long as it can focus the first light 123 emitted from the first light irradiation system 120 and the second light 133 emitted from the second light irradiation system 130 to the contact portion between the first member 111 and the second member 112. The focusing point diameter can be appropriately selected according to the bonding pattern.

[0084] The XY stage 110 can be any structure that supports the first member 111 and the second member 112, and can be the same as the XY device of a general laser irradiation device. In addition, the XY stage 110 can also be linked with a support portion (not shown) for controlling the relative position of the first member 111 and the second member 112. The support portion can be any structure that can support the first member 111 and / or the second member 112 and move them in a desired positional relationship. In addition, the structure of the position control portion (not shown) for adjusting the position of the support portion and the position of the XY stage 110 is not particularly limited, and can be a computer or the like.

[0085] In addition, the temperature measuring unit 150 is not particularly limited in its temperature measuring method as long as it can measure the temperature at the irradiation position (the contact position between the first member 111 and the second member 112) of the first light irradiation system 123 and the second light irradiation system 130. The temperature measuring unit 150 can be set as a radiation type thermometer, for example.

[0086] The light intensity control unit 160 is not particularly limited in structure as long as it can obtain the temperature measured by the temperature measurement unit 150 and adjust the output of the first light irradiation system 120 and the second light irradiation system 130 based on the temperature. For example, it can be a computer. In addition, it is also possible to use a computer as both the light intensity control unit 160 and the above-mentioned position control unit.

[0087] When the first member 111 and the second member 112 are joined together using the processing apparatus 100, the first member 111 is arranged on the XY stage 110 ( Figure 1 Then, the first light 123 is emitted from the first light irradiation system 120. At this time, the first light 123 is focused onto the resin ( Figure 1 In the embodiment, at the contact portion between the first component 111 and the second component 112).

[0088] In addition, the second light 133 is emitted from the second light irradiation system 130 substantially simultaneously with the irradiation of the first light 123 by the first light irradiation system 120. Then, the second light 133 is focused onto the resin ( Figure 1 In the embodiment, at the contact portion between the first component 111 and the second component 112).

[0089] Then, the temperature of the resin irradiated with the first light and the second light is measured by the temperature measuring unit 150. The light quantity control unit 160 determines whether the temperature measured by the temperature measuring unit 150 is equal to or higher than the glass transition temperature of the resin in the first member 111, and adjusts the light output of the first light irradiation system 120 and the second light irradiation system 130 based on the determination result. At this time, the position control unit (not shown) can also move the XY stage 110 as needed, so as to irradiate the first light 123 and the second light 133 in a desired pattern.

[0090] also, Figure 1 In the manufacturing apparatus shown in FIG. 1 , the first light 123 and the second light 133 are irradiated from the same direction. However, the first light 123 and the second light 133 may be irradiated from different directions. Figure 1 In the device shown, the first light 123 and the second light 133 are irradiated while the first component 111 and the second component 112 are arranged in contact with each other. However, it is also possible to arrange only the first component 111 on the XY stage 110 and irradiate the first light 123 and the second light 133, and then overlap the second component 112 on the first component 111 through the above-mentioned support portion to connect them.

[0091] 3. Manufacturing method of resin parts

[0092] The method for manufacturing a resin component of the present invention includes the following steps: a step of irradiating a first light of a first wavelength that electronically excites a resin of a first member containing a resin; and a step of irradiating a second light of a second wavelength that is longer than the first wavelength to the resin electronically excited by the irradiation of the first light. Here, the wavelength region of the second wavelength only needs to be included in the wavelength region in which the light absorption rate of the resin increases due to the electronic excitation of the resin contained in the first member, but preferably, the wavelength region of the second wavelength is a wavelength region in which the light absorption rate of the resin increases due to the increase in the temperature of the resin caused by the electronic excitation of the resin contained in the first member.

[0093] Examples of resin parts manufactured by the method for manufacturing resin parts of the present invention include parts manufactured by processing resin, parts manufactured by cutting resin, parts formed by forming grooves in resin, parts formed by joining resin to resin, etc. Parts manufactured by cutting resin and parts formed by forming grooves in resin include, for example, resin containers such as beverage containers and food containers, reflectors for backlight sources, etc. As parts formed by joining resin to resin, for example, tubes for passing gas or liquid can be listed. In addition, the resin part can also include an area composed of materials other than resin in a part thereof. That is, examples of resin parts also include: parts formed by joining resin to metal or ceramic other than resin, etc. As parts formed by joining resin to metal or ceramic other than resin, for example, mechanical parts such as decorative screws, electronic devices such as fuses and connectors, etc. can be listed.

[0094] Here, Figure 3 An example of a method for manufacturing a resin component of the present invention is shown. The manufacturing method includes a method of performing a first light irradiation step and a second light irradiation step on a first member 211 containing resin. As the first member 211, the same member as the first member 111 can be used.

[0095] The manufacturing method includes, for example, a method for manufacturing a resin component by performing the above-mentioned first light irradiation process and the second light irradiation process on a first member 211 containing a resin, forming a groove of a desired shape in the first member 211. In addition, the manufacturing method of the resin component includes, for example, a method for manufacturing a resin component by performing the above-mentioned first light irradiation process and the second light irradiation process on a first member 211 containing a resin, cutting the first member 211 into a desired shape. In addition, the device (resin component manufacturing device) 200 used in the manufacturing method of the resin component is the same as the above-mentioned processing device 100 except that the first member 211 is irradiated with the first light and the second light and the first member 211 is processed as desired. The same structure as the above-mentioned processing device 100 is given the same figure mark, and the detailed description is omitted.

[0096] As another example of the method for manufacturing a resin component of the present invention, there can be cited a method in which, in addition to the above-mentioned process of irradiating the first light and the process of irradiating the second light, a process of preparing a second member and a process of bringing the area of ​​the first member irradiated with the first light and the second light into contact with the second member to join the first member and the second member can be performed. According to this method, the first member and the second member can be joined, and a resin component formed by joining resin to resin, or a resin component formed by joining resin to metal or ceramic other than resin, etc. can be manufactured. As an example of the first member and the second member in the case of manufacturing a resin component formed by joining resin to resin, a resin tube can be cited as the first member and the second member, respectively, and the resin component is a tube formed by joining resin tubes. In the case of manufacturing a resin component formed by joining resin to metal other than resin, as an example of the first member, a resin head can be cited, and as an example of the second member, a metal screw portion can be cited, and the resin component is a decorative screw formed by joining a resin head to a metal screw portion. In addition, when manufacturing a resin component formed by bonding a resin to a metal other than a resin, examples of the first member include a resin housing and a resin case, and examples of the second member include a metal terminal. In addition, the step of irradiating the second light and the step of bonding the first member to the second member may be performed simultaneously.

[0097] Here, the first light irradiation step, the second light irradiation step, and the bonding step in the manufacturing method of the resin component of the present invention are the same as the steps described in the processing method of the resin component described above. In addition, the first component and the second component used in the manufacturing method of the resin component may be the same as the first component and the second component described in the processing method of the resin component described above. Therefore, the detailed description thereof is omitted.

[0098] Example

[0099] Hereinafter, the present invention will be described in detail with reference to Examples; however, the present invention is not limited to these Examples.

[0100] (Reference Example 1) Verification of Increased Light Absorption Rate (Temperature Zone)

[0101] The absorption spectra of the PET sheet (thickness 1 mm) in the wavelength range of 350nm to 500nm were measured at room temperature and 65°C, and these were compared. As a result, in the absorption spectrum measured at 65°C, the light absorptivity on the long wavelength side increased compared to the absorption spectrum measured at room temperature, and the absorbance in the wavelength region of 380nm and above increased in particular. From this result, it can be confirmed that the light absorption increased (tropical zone) occurred in the PET sheet.

[0102] (Reference Example 2) Verification of Temperature Increase of Resin Accompanied by Laser Irradiation

[0103] A semiconductor laser with a wavelength of 405 nm was irradiated to each of the PET plate, PMMA plate, and PC (polycarbonate) plate at an output of 300 mW, and the temperature of the laser irradiated portion was measured. As a result, almost no temperature rise was found in the PET plate and PMMA plate. In addition, a temperature rise was found in the PC (polycarbonate) plate, but it did not rise to a temperature required for resin processing such as welding. From this result, it can be seen that PET, PMMA, and PC (polycarbonate) do not substantially absorb light with a wavelength of 405 nm.

[0104] In this specification, “substantially no light absorption” includes the case of slight light absorption. In addition, “no light absorption” is used with the same meaning as “substantially no light absorption”. For example, when the laser light is irradiated with a laser light having an output of 300 mW, the resin is assumed to have substantially no light absorption when the laser light is not absorbed and the temperature of the resin exceeds the glass transition temperature as in Reference Example 2.

[0105] (Comparative Example 1)

[0106] The PET plate was irradiated with a semiconductor laser (continuous oscillation type) with a wavelength of 375 nm, and the temperature of the irradiated area was measured. In addition, the focusing light irradiation system was set to a single lens (f = 40 mm to 100 mm), and the focusing point diameter was set to less than 1 mm. In addition, the temperature measurement was set to real-time measurement using a radiation type thermometer. The results are shown in Table 1.

[0107] ·result

[0108] [Table 1]

[0109]

[0110] When resins are joined (welded), the temperature of the resin of at least one of the components must exceed its glass transition temperature (T g ). The glass transition temperature of PET is 70°C. In contrast, as shown in Table 1, when a semiconductor laser with a wavelength of 375nm was irradiated to a PET plate alone, even if the output was increased, the temperature of the resin was only 67.5°C. In other words, the glass transition temperature of PET was not reached. In addition, even when two PET plates were overlapped and placed in contact with each other and 400mW of a 375nm wavelength laser was focused, they could not be joined.

[0111] (Example 1)

[0112] Condition 1

[0113] Two PET plates, a PET plate and a PC (polycarbonate) plate, and a PET plate and a PMMA plate were overlapped and arranged. At the overlapping portion, a 400mW laser 1 (wavelength 375nm) was focused on the portion, and a 1000mW laser 2 (wavelength 405nm) was focused on the portion. The irradiation of these lasers was performed from the PET plate side.

[0114] Furthermore, temperature measurement was performed in the following manner using the following types of laser light and a focused light irradiation system.

[0115] Laser 1: 375nm wavelength semiconductor laser (continuous oscillation type)

[0116] Laser 2: 405nm wavelength semiconductor laser (continuous oscillation type)

[0117] Converging light irradiation system: Use a single lens (f=40mm~100mm) for converging light irradiation, and the focal point diameter is less than 1mm.

[0118] Temperature measurement: Real-time measurement using a radiation thermometer.

[0119] Result 1

[0120] After the laser irradiation, the PET plates were observed to be bonded (welded) to each other, the PET plates to the PC plates, and the PET plates to the PMMA plates. In the above-mentioned Comparative Example 1, the PET plates could not be welded to each other by irradiating the laser with a wavelength of 375 nm alone. On the other hand, when the laser with a wavelength of 375 nm and the laser with a wavelength of 405 nm were used in combination, the two resin plates could be welded.

[0121] The results show that the resin (mainly PET) was electronically excited by the irradiation of the 375nm laser, and a new light absorption band appeared on the longer wavelength side (near 405nm) than the 375nm wavelength. Therefore, it can be said that the temperature of PET exceeded its glass transition point by the irradiation of the two lasers, thus achieving welding.

[0122] Condition 2

[0123] Two PC boards and a PC board and a PMMA board were arranged so as to overlap. For the overlapping portion, a 200mW laser 1 (wavelength 375nm) was focused on the portion, and a 500mW laser 2 (wavelength 405nm) was focused on the portion. In addition, the laser irradiation to the overlapping portion of the PC board and the PMMA board was irradiated from the PMMA board side.

[0124] Furthermore, temperature measurement was performed in the following manner using the following types of laser light and a focused light irradiation system.

[0125] Laser 1: 375nm wavelength semiconductor laser (continuous oscillation type)

[0126] Laser 2: 405nm wavelength semiconductor laser (continuous oscillation type)

[0127] Converging light irradiation system: Use a single lens (f=40mm~100mm) for converging light irradiation, and the focal point diameter is less than 1mm.

[0128] Temperature measurement: Real-time measurement using a radiation thermometer.

[0129] Result 2

[0130] After the laser irradiation, the overlapping portions of the PC sheets and the overlapping portions of the PC sheet and the PMMA sheet were observed, and it was confirmed that they were both joined (welded).

[0131] According to the results, the resin (mainly PC) was electronically excited by the irradiation of the laser with a wavelength of 375nm, and a new light absorption band appeared on the longer wavelength side (near the wavelength of 405nm) than the wavelength of 375nm. Therefore, it can be said that the temperature of PC exceeded its glass transition point by the irradiation of the two lasers, thus achieving welding.

[0132] Condition 3

[0133] Two PMMA plates were placed so as to overlap each other, and at the overlapping portion, 400 mW of laser light 1 (wavelength 375 nm) was focused on the portion, and at the same time, 1000 mW of laser light 2 (wavelength 405 nm) was focused on the portion.

[0134] Furthermore, temperature measurement was performed in the following manner using the following types of laser light and a focused light irradiation system.

[0135] Laser 1: 375nm wavelength semiconductor laser (continuous oscillation type)

[0136] Laser 2: 405nm wavelength semiconductor laser (continuous oscillation type)

[0137] Converging light irradiation system: Use a single lens (f=40mm~100mm) for converging light irradiation, and the focal point diameter is less than 1mm.

[0138] Temperature measurement: Real-time measurement using a radiation thermometer.

[0139] Result 3

[0140] After the above laser irradiation, the overlapping parts of the PMMA plates were observed and confirmed to be joined (welded). According to the results, the resin (PMMA) was electronically excited by the irradiation of the laser with a wavelength of 375nm, and a new light absorption band appeared on the longer wavelength side (near the wavelength of 405nm) than the wavelength of 375nm. Therefore, it can be said that the temperature of PMMA exceeded its glass transition point by the irradiation of the two lasers, thus achieving welding.

[0141] (Example 2)

[0142] Condition 1

[0143] A PET plate (thickness 1 mm) was irradiated with laser 1 (wavelength 375 nm) with an output of 200 mW to raise the temperature of the irradiated portion to 40° C. In addition, while irradiating with laser 1, the same irradiated portion was irradiated with laser 2 (semiconductor laser with a wavelength of 405 nm) with an output of 500 mW, and the temperature of the irradiated portion was measured.

[0144] Furthermore, temperature measurement was performed in the following manner using the following types of laser light and a focused light irradiation system.

[0145] Laser 1: 375nm wavelength semiconductor laser (continuous oscillation type)

[0146] Laser 2: 405nm wavelength semiconductor laser (continuous oscillation type)

[0147] Converging light irradiation system: Use a single lens (f=40mm~100mm) for converging light irradiation, and the focal point diameter is less than 1mm.

[0148] Temperature measurement: Real-time measurement using a radiation thermometer.

[0149] Result 1

[0150] The temperature of the PET plate rises to 110° C. (rise temperature ΔT=85° C.) by irradiation with the laser beam 2. This temperature exceeds the glass transition temperature (70° C.) of PET, and it can be said that PET can be processed.

[0151] Condition 2

[0152] The PET plate (thickness 1 mm) was irradiated with the following laser 1 (wavelength 375 nm) with an output of 200 mW, and the irradiated portion was heated to 60°C. In addition, while irradiating with laser 1, the same irradiated portion was irradiated with laser 2 (wavelength 405 nm) with an output of 500 mW, and the temperature of the irradiated portion was measured. In addition, the type of laser, the type of focusing light irradiation system, and the temperature measurement method were the same as those in condition 1.

[0153] Result 2

[0154] The temperature of the irradiated portion rises to 125° C. (rising temperature ΔT=100° C.) by irradiation with the laser beam 2. This temperature exceeds the glass transition temperature (70° C.) of PET, and it can be said that PET can be processed.

[0155] (Example 3)

[0156] Condition 1

[0157] A PET plate (thickness 1 mm) was irradiated with laser light using the following five methods, and the temperature of the irradiated area was measured. Figure 4 The relationship between the temperature of the irradiated part and the total laser output is shown in FIG. Figure 4 In the embodiment, method 4 and method 5 are shown as embodiments in which two lasers with different wavelengths are combined for irradiation and the temperature of the irradiated part is measured. As comparative examples, method 1, method 2 and method 3 are shown as comparative examples in which only one laser is irradiated and the temperature of the irradiated part is measured.

[0158] Method 1 (comparative example): irradiation with laser 1 (wavelength 375 nm) only

[0159] Method 2 (comparative example): irradiation with laser 2 (wavelength 405 nm) only

[0160] Method 3 (Comparative Example): Irradiation with Laser 3 (wavelength 450nm) only

[0161] Method 4 (Example): Simultaneous irradiation with equal output of laser 1 (wavelength 375 nm) and laser 2 (wavelength 405 nm)

[0162] Method 5 (Example): Simultaneous irradiation with equal output of laser 1 (wavelength 375nm) and laser 3 (wavelength 450nm)

[0163] Regarding method 4 and method 5 using two types of lasers, the total output of the two lasers is represented by the sum of the outputs. For example, when the total output in method 4 is 200 mW, the outputs of laser 1 and laser 2 are each 100 mW.

[0164] Furthermore, temperature measurement was performed in the following manner using the following types of laser light and a focused light irradiation system.

[0165] Laser 1: 375nm wavelength semiconductor laser (continuous oscillation type)

[0166] Laser 2: 405nm wavelength semiconductor laser (continuous oscillation type)

[0167] Laser 3: 450nm wavelength semiconductor laser (continuous oscillation type)

[0168] Converging light irradiation system: Use a single lens (f=40mm~100mm) for converging light irradiation, and the focal point diameter is less than 1mm.

[0169] Temperature measurement: Real-time measurement using a radiation thermometer.

[0170] Result 1

[0171] like Figure 4 As shown in FIG. 1 , in method 2 in which laser 2 (wavelength 405 nm) was irradiated alone and in method 3 in which laser 3 (wavelength 450 nm) was irradiated alone, the temperature of the PET plate was almost unchanged. On the other hand, in method 4 in which laser 1 (wavelength 375 nm) and laser 2 (wavelength 405 nm) were irradiated in combination, and in method 5 in which laser 1 (wavelength 375 nm) and laser 3 (wavelength 450 nm) were irradiated in combination, the temperature of the PET plate increased significantly. Regarding method 1 in which laser 1 (wavelength 375 nm) was irradiated alone, a temperature increase was confirmed, but as will be described later, the light conversion efficiency of ultraviolet region laser light such as laser 1 is low, and therefore, a relatively large power is required in method 1.

[0172] Condition 2

[0173] A PC plate (thickness 5 mm) was irradiated with laser light in the following five methods, and the temperature of the irradiated portion was measured. Figure 5 The relationship between the temperature of the irradiated part and the total laser output is shown. Specifically, Figure 5 In the embodiment, method 4 and method 5 are shown as embodiments in which two lasers with different wavelengths are combined for irradiation and the temperature of the irradiated part is measured. As comparative examples, method 1, method 2 and method 3 are shown as comparative examples in which only one laser is irradiated and the temperature of the irradiated part is measured.

[0174] Method 1 (comparative example): irradiation with laser 1 (wavelength 375 nm) only

[0175] Method 2 (comparative example): irradiation with laser 2 (wavelength 405 nm) only

[0176] Method 3 (Comparative Example): Irradiation with Laser 3 (wavelength 450nm) only

[0177] Method 4 (Example): Simultaneous irradiation with equal output of laser 1 (wavelength 375 nm) and laser 2 (wavelength 405 nm)

[0178] Method 5 (Example): Simultaneous irradiation with equal output of laser 1 (wavelength 375nm) and laser 3 (wavelength 450nm)

[0179] Regarding method 4 and method 5 using two lasers, the total output of the two lasers is represented by the sum of the outputs. For example, when the total output in method 4 is 50 mW, the outputs of laser 1 and laser 2 are each 25 mW.

[0180] Furthermore, temperature measurement was performed in the following manner using the following types of laser light and a focused light irradiation system.

[0181] Laser 1: 375nm wavelength semiconductor laser (continuous oscillation type)

[0182] Laser 2: 405nm wavelength semiconductor laser (continuous oscillation type)

[0183] Laser 3: 450nm wavelength semiconductor laser (continuous oscillation type)

[0184] Converging light irradiation system: Use a single lens (f=40mm~100mm) for converging light irradiation, and the focal point diameter is less than 1mm.

[0185] Temperature measurement: Real-time measurement using a radiation thermometer.

[0186] Result 2

[0187] like Figure 5 As shown, in method 2 in which laser 2 (wavelength 405nm) was irradiated alone and method 3 in which laser 3 (wavelength 450nm) was irradiated alone, the temperature of the PC board was almost unchanged. On the other hand, in method 4 in which laser 1 (wavelength 375nm) and laser 2 (wavelength 405nm) were irradiated in combination, and in method 5 in which laser 1 (wavelength 375nm) and laser 3 (wavelength 450nm) were irradiated in combination, the temperature of the PC board increased significantly. Regarding method 1 in which laser 1 (wavelength 375nm) was irradiated alone, a temperature increase was confirmed, but as described later, the light conversion efficiency of ultraviolet region lasers such as laser 1 is low, and therefore, a relatively large power is required in method 1.

[0188] Condition 3

[0189] A PMMA plate (thickness 5 mm) was irradiated with laser light in the following five methods, and the temperature of the irradiated portion was measured. Figure 6 The relationship between the temperature of the irradiated part and the total laser output is shown. Specifically, Figure 6 In the embodiment, method 4 and method 5 are shown as embodiments in which two lasers with different wavelengths are combined for irradiation and the temperature of the irradiated part is measured. As comparative examples, method 1, method 2 and method 3 are shown as comparative examples in which only one laser is irradiated and the temperature of the irradiated part is measured.

[0190] Method 1 (comparative example): irradiation with laser 1 (wavelength 375 nm) only

[0191] Method 2 (comparative example): irradiation with laser 2 (wavelength 405 nm) only

[0192] Method 3 (Comparative Example): Irradiation with Laser 3 (wavelength 450nm) only

[0193] Method 4 (Example): Simultaneous irradiation with equal output of laser 1 (wavelength 375 nm) and laser 2 (wavelength 405 nm)

[0194] Method 5 (Example): Simultaneous irradiation with equal output of laser 1 (wavelength 375nm) and laser 3 (wavelength 450nm)

[0195] Regarding method 4 and method 5 using two lasers, the total output of the two lasers is represented by the sum of the outputs. For example, when the total output in method 4 is 200 mW, the outputs of laser 1 and laser 2 are each 100 mW.

[0196] Furthermore, temperature measurement was performed in the following manner using the following types of laser light and a focused light irradiation system.

[0197] Laser 1: 375nm wavelength semiconductor laser (continuous oscillation type)

[0198] Laser 2: 405nm wavelength semiconductor laser (continuous oscillation type)

[0199] Laser 3: 450nm wavelength semiconductor laser (continuous oscillation type)

[0200] Converging light irradiation system: Use a single lens (f=40mm~100mm) for converging light irradiation, and the focal point diameter is less than 1mm.

[0201] Temperature measurement: Real-time measurement using a radiation thermometer.

[0202] Result 3

[0203] like Figure 6As shown, in method 2 in which laser 2 (wavelength 405 nm) was irradiated alone and method 3 in which laser 3 (wavelength 450 nm) was irradiated alone, the temperature of the PMMA plate was almost unchanged. On the other hand, in method 4 in which laser 1 (wavelength 375 nm) and laser 2 (wavelength 405 nm) were irradiated in combination, and in method 5 in which laser 1 (wavelength 375 nm) and laser 3 (wavelength 450 nm) were irradiated in combination, the temperature of the PMMA plate increased significantly. Regarding method 1 in which laser 1 (wavelength 375 nm) was irradiated alone, a temperature increase was confirmed, but as will be described later, the light conversion efficiency of ultraviolet region lasers such as laser 1 is low, and therefore, a relatively large power is required in method 1.

[0204] According to the results 1 to 3 in Example 3, it can be seen that light in the visible light region that is not originally absorbed by the resin can also be used in the processing method of the present invention. In addition, in general, the light conversion efficiency of the laser in the ultraviolet region is low. Therefore, in order to make the laser in the ultraviolet region high output, a relatively large power is required. In the processing method of the present invention, since the output of such a laser in the ultraviolet region with low light conversion efficiency can be reduced, the power consumption can be suppressed and the resin component can be processed extremely efficiently. In addition, since the ultraviolet region laser element has low light conversion efficiency, its temperature is easy to rise, and the temperature rise may cause damage to the element. As a countermeasure against such temperature rise causing damage to the element, it is possible to consider using multiple ultraviolet region laser elements, while suppressing damage to each ultraviolet region laser element, and setting it to the desired output. However, in the processing method of the present invention, since the output of the laser in the ultraviolet region required for processing can be suppressed, the number of ultraviolet region laser elements can be reduced.

[0205] Furthermore, the temperature of the resin can be raised without including a light absorber in the resin or applying a light absorber to the surface of the resin. Therefore, the cost of resin processing can be suppressed compared to the case of using a light absorber.

[0206] This application claims priority based on Japanese Patent Application No. 2019-239647 filed on December 27, 2019. The contents described in the specification and drawings of that application are all cited in the specification of this application.

[0207] Industrial Applicability

[0208] According to the processing method of the present invention, only a desired region of a member containing resin can absorb a sufficient amount of light to increase its temperature and process the member. Therefore, the present invention is a very useful technology for manufacturing various electronic devices and equipment, for example.

[0209] Description of Reference Numerals

[0210] 100 Processing equipment

[0211] 110XY stage

[0212] 111, 211 First Component

[0213] 112 Second Component

[0214] 120 First light irradiation system

[0215] 121 First Laser Source

[0216] 122 First Reflector

[0217] 123 First Light

[0218] 130 Second light irradiation system

[0219] 131 Second laser light source

[0220] 132 Second Reflector

[0221] 133 Second Light

[0222] 140 Lens

[0223] 150 Temperature measurement unit

[0224] 160 Light intensity control unit

[0225] 200 Resin parts manufacturing equipment

Claims

1. A method for processing a resin component, comprising: irradiating a first member including a resin with a first light having a first wavelength for exciting electrons of the resin; as well as a step of irradiating the resin that has been electronically excited by the irradiation of the first light with a second light having a second wavelength, the second wavelength being a wavelength longer than the first wavelength, The wavelength region of the second wavelength is included in a wavelength region where the light absorption rate of the resin increases due to the electronic excitation of the resin. The second wavelength is greater than 400 nm and less than 550 nm.

2. The method for processing a resin member according to claim 1, wherein: Also includes the step of preparing a second component, The method further includes bonding the first member to the second member by bringing the region of the first member irradiated with the first light and the second light into contact with the second member.

3. The method for processing a resin member according to claim 2, wherein: The step of irradiating the second light and the step of bonding the first member and the second member are performed simultaneously.

4. The method for processing a resin member according to any one of claims 1 to 3, wherein: The wavelength region of the second wavelength is a wavelength region in which the light absorption rate of the resin increases due to an increase in the temperature of the resin caused by electron excitation of the resin.

5. The method for processing a resin member according to any one of claims 1 to 3, wherein: The wavelength region of the second wavelength is a wavelength region in which the light absorption rate of the resin increases due to the triplet excited state of the resin caused by the electron excitation of the resin.

6. The method for processing a resin member according to any one of claims 1 to 3, wherein: The resin does not have absorption due to electron excitation with respect to the light of the second wavelength when not irradiated with the first light.

7. The method for processing a resin member according to any one of claims 1 to 3, wherein: The step of irradiating the first light and the step of irradiating the second light are performed simultaneously.

8. The method for processing a resin member according to any one of claims 1 to 3, wherein: The first light and the second light are laser beams.

9. The method for processing a resin member according to any one of claims 1 to 3, wherein: The first wavelength is less than 410 nm.

10. The method for processing a resin member according to any one of claims 1 to 3, wherein: In the process of irradiating the first light and the process of irradiating the second light, the temperature of the area of ​​the first component irradiated with the first light and the second light is measured, and the intensity of the first light and the second light is adjusted according to the temperature of the area of ​​the first component irradiated with the first light and the second light.

11. A resin component processing device comprising: a first light irradiation system for irradiating the resin of the first member containing the resin with first light of a first wavelength for exciting electrons of the resin; and a second light irradiation system for irradiating the resin of the first member with second light of a second wavelength, the second wavelength being a longer wavelength than the first wavelength, The wavelength region of the second wavelength is included in a wavelength region where the light absorption rate of the resin increases due to the electronic excitation of the resin. The second wavelength is greater than 400 nm and less than 550 nm.

12. The resin member processing device according to claim 11, wherein: It also has a position control unit for controlling the relative position of the first member and the second member, The position control section joins the second member to the first member irradiated with the first light and the second light by the first light irradiation system and the second light irradiation system, respectively.

13. The resin member processing device according to claim 11, wherein: In a state where the first member and the second member are arranged so as to be in contact with each other, the first light and the second light are irradiated from the first light irradiation system and the second light from the second light irradiation system, respectively, to the interface between the first member and the second member.

14. The resin member processing device according to any one of claims 11 to 13, wherein: The wavelength region of the second wavelength is a wavelength region in which the light absorption rate of the resin increases due to an increase in the temperature of the resin caused by electron excitation of the resin.

15. The resin member processing device according to any one of claims 11 to 13, wherein: The wavelength region of the second wavelength is a wavelength region in which the light absorption rate of the resin increases due to the triplet excited state of the resin caused by the electron excitation of the resin.

16. The resin member processing device according to any one of claims 11 to 13, wherein: The first light irradiation system and the second light irradiation system simultaneously irradiate the first light and the second light.

17. The resin member processing device according to any one of claims 11 to 13, wherein: The first light irradiation system and the second light irradiation system respectively emit laser light.

18. The resin member processing device according to any one of claims 11 to 13, wherein: The first wavelength is less than 410 nm.

19. The resin member processing device according to any one of claims 11 to 13, wherein: It also has a temperature measurement unit and a light intensity control unit. The temperature measuring unit measures the temperature of a region of the first member irradiated with the first light and the second light. The light amount control unit adjusts the intensities of the first light and the second light according to the temperature measured by the temperature measurement unit.