A PVDF coated diaphragm and its preparation method and application
By using porous nanoceramic/PVDF composite agglomerates on lithium battery separators, the problems of poor heat resistance and insufficient air permeability of lithium battery separators at high temperatures are solved, and the cycle performance and capacity retention rate of lithium batteries are improved.
Patent Information
- Application Number
- CN202210991831.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-18
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-08-18
AI Technical Summary
Existing PVDF separators have poor heat resistance at high temperatures, causing congestion in the shuttle of lithium ions and affecting the cycle performance of lithium batteries. The dot-like coating method leads to increased air permeability, affecting the overall performance of the battery.
Porous nanoceramic/PVDF composite agglomerates are used as the organic layer. By forming randomly distributed porous nanoceramics/PVDF composite agglomerates on the separator, the resistance of lithium ion shuttle is reduced, and the adhesion force and air permeability of the separator and the pole piece are improved. .
It improves the cycle performance and capacity retention rate of lithium batteries, enhances the adhesion between the separator and the pole piece, and the porous nanoceramic/PVDF composite agglomerate has no effect on the breathability of the coating.
Smart Images

Figure CN115101894B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of secondary batteries, and in particular to a PVDF coated diaphragm and a preparation method and application thereof. Background Art
[0002] Lithium batteries can be divided into four parts from a structural point of view, positive and negative electrodes, electrolytes and diaphragms. Among them, the diaphragm acts as a barrier material between the positive and negative electrodes, providing a channel for the shuttle of lithium ions and blocking the passage of electrons, thereby preventing the contact and short circuit of the positive and negative electrodes. However, the diaphragm itself has poor heat resistance, and the diaphragm shrinks severely at high temperatures, which easily leads to short circuits due to contact between the positive and negative electrodes. In order to improve the heat resistance of the diaphragm, a heat-resistant layer is often coated on one or both sides of the diaphragm. For example, the Chinese invention patent application with publication number CN110571394A coats a ceramic layer on the base film to improve the thermal shrinkage of the diaphragm. Since the ceramic layer is not bonded to the pole piece, the battery is prone to softening. Organic coatings have been introduced in the industry, and an organic coating is coated on the ceramic layer or the base film layer to increase the adhesion between the diaphragm and the pole piece, thereby improving the hardness of the battery.
[0003] Since PVDF material has the characteristics of corrosion resistance, easy adhesion, and liquid retention, the lithium battery diaphragm coating industry uses PVDF as an organic coating to coat one or both sides of the diaphragm to increase the adhesion with the pole piece. PVDF coating can be divided into two types, oily coating and water-based coating. Among them, oily coating often uses acetone as a solvent to dissolve PVDF, and then coats and dries to form a film. Because acetone is volatile and burns easily. PVDF oily coating technology is extremely unsafe in mass production, so PVDF water-based coating is very popular. For example, the Chinese invention patent application with publication number CN111490213A uses a mixture of water-based PVDF emulsion and acrylate to coat one side of the base film to form a PVDF layer with neat and tight particle arrangement. However, since the primary particle size of PVDF is small, generally only at the nanometer level, this coating method will increase the overall air permeability time of the coating, resulting in an increase in the overall impedance value of the diaphragm, affecting the shuttling of lithium ions.
[0004] In order to improve the air permeability without affecting the adhesion between the diaphragm and the electrode, the existing technology uses air flow to crush the dried PVDF emulsion or spray-dry the PVDF emulsion to obtain secondary particle size PVDF powder at the micron level, which is then mixed with a binder to make a slurry. The secondary particle size PVDF is sprayed on the diaphragm using a point spraying method. The particle size of the sprayed points can generally reach several hundred microns. This ensures the adhesion between the diaphragm and the electrode while not affecting the air permeability of the coating. For example, the Chinese invention patent application with publication number CN114039170A adopts a dot coating method, mixing PVDF powder and a binder to make a slurry, and then coating the prepared slurry on the diaphragm in a dot-shaped arrangement with equal spacing; for example, the Chinese invention patent with publication number CN110911620A mixes PVDF emulsion and a binder, adds some additives, and then adds a small amount of non-spherical alumina, and sprays the slurry on the diaphragm by atomizer spraying or electrostatic spraying, thereby obtaining a non-continuous, highly adhesive dot-shaped PVDF diaphragm. The PVDF diaphragms prepared by these two patents maintain adhesion to the electrode and do not affect the overall air permeability of the diaphragm.
[0005] However, in the above technical solution, PVDF materials generally use α-crystal form, and the crystal region of α-crystal form can be divided into shaped region and amorphous region. The shaped region accounts for about 40% of the α-crystal form PVDF used for the diaphragm. Lithium ions can only pass through the amorphous region, but not the shaped region. Therefore, when PVDF powder is coated in a dotted manner, PVDF powder gathers at one point, of which 40% is the shaped region, and lithium ions cannot pass through, which will inevitably cause congestion of lithium ion shuttle in the dotted area of PVDF, thereby affecting the overall cycle performance of the battery. Summary of the invention
[0006] The purpose of this application is to provide a PVDF coated diaphragm and its preparation method and application, which can reduce the congestion of lithium ions when shuttling through point-aggregated PVDF without changing the bonding effect between PVDF and the electrode, thereby reducing the internal resistance of the battery and improving the cycle performance.
[0007] To achieve the above-mentioned purpose, the embodiment of the present application adopts the following technical scheme: a PVDF coated diaphragm, comprising: a base film, the base film adopts a porous film; a heat-resistant layer, the heat-resistant layer is arranged on at least one side surface of the base film; an organic layer, the organic layer is arranged on the heat-resistant layer, the organic layer includes a porous nano-ceramic / PVDF composite agglomerate, a binder and a defoaming agent, and the porous nano-ceramic / PVDF composite agglomerate is formed by agglomeration of porous nano-ceramics and PVDF particles.
[0008] In the above technical scheme, the embodiment of the present application forms a randomly distributed organic layer on the diaphragm by using porous nano-ceramic / PVDF composite agglomerates. The porous nano-ceramics in the porous nano-ceramic / PVDF composite agglomerate particles can provide channels for the shuttle of lithium ions, reduce the resistance of lithium ions passing through the aggregated point-like PVDF, and thus improve the cycle performance of the battery. The presence of porous nano-ceramics provides storage space for the electrolyte and increases the capacity retention rate of the battery. The high specific surface tension of porous nano-ceramics can play a certain adsorption role when bonding with the pole piece, thereby increasing the adhesion between the diaphragm and the pole piece and enhancing the hardness of the battery. The porous nano-ceramics provides a channel for the conduction of gas, and the coated porous nano-ceramic / PVDF composite agglomerate coating has no effect on the overall air permeability of the coated diaphragm.
[0009] Further, according to an embodiment of the present application, the base film is one of a PP film, a PE film, or a composite film of a PP film and a PE film.
[0010] Further, according to an embodiment of the present application, the thickness of the base film is 5-16µm.
[0011] Further, according to an embodiment of the present application, the heat-resistant layer includes ceramics, a stabilizer, glue and a wetting agent.
[0012] Further, according to an embodiment of the present application, the particle size of the ceramic is 0.5-1.2µm.
[0013] Further, according to an embodiment of the present application, the added amount of the stabilizer is 0.2-2wt% of the ceramic.
[0014] Further, according to an embodiment of the present application, the amount of glue added is 1-10wt% of the ceramic.
[0015] Further, according to an embodiment of the present application, the added amount of the wetting agent is 0.2-2wt% of the ceramic.
[0016] Further, according to an embodiment of the present application, the mass ratio of the porous nano-ceramics to the PVDF particles is 1-3:10.
[0017] Further, according to an embodiment of the present application, the particle size of the porous nanoceramic is 150-350 nm, the pore size is 10-80 nm, and the porosity is 50-80%.
[0018] Further, according to an embodiment of the present application, the crystal form of the PVDF particles is α-crystal form, and the particle size is 150-300nm.
[0019] Further, according to an embodiment of the present application, the particle size of the porous nano-ceramic / PVDF composite agglomerates is 3-10µm.
[0020] Further, according to an embodiment of the present application, the added amount of the binder is 3-10wt% of the porous nano-ceramic / PVDF composite agglomerate.
[0021] Further, according to an embodiment of the present application, the added amount of the defoaming agent is 0.5-3wt% of the porous nano-ceramic / PVDF composite agglomerate.
[0022] In order to achieve the above object, the present application also discloses a method for preparing a PVDF coated diaphragm, comprising the following steps:
[0023] Coating the heat-resistant layer: coating the heat-resistant layer slurry on at least one side of the base film;
[0024] Coating the organic layer: taking the porous nano-ceramic / PVDF composite agglomerate, the binder, and water, mixing them, and stirring at high speed; adding the defoaming agent, stirring slowly, and obtaining the organic layer slurry; using air gun spraying or high-speed centrifugation to spray the organic layer slurry on the heat-resistant layer.
[0025] Further, according to an embodiment of the present application, the thickness of the heat-resistant layer is 1-4µm.
[0026] Further, according to an embodiment of the present application, the spraying particle size of the organic layer is 50-400µm, and the spraying coverage is 8-25%.
[0027] Further, according to the embodiment of the present application, the porous nano-ceramic / PVDF composite agglomerate is prepared by the following method:
[0028] Add deionized water and dispersant into the reactor and stir evenly; introduce nitrogen repeatedly to exhaust oxygen, and after the replacement is qualified, introduce VDF into the reactor; increase the temperature and pressure to a constant temperature and pressure, and then inject initiator and emulsifier to carry out polymerization reaction;
[0029] After the reaction is completed, the unreacted VDF is recycled, and the polymer emulsion is condensed, washed, and separated to obtain PVDF emulsion;
[0030] The porous nano-ceramics are added into the PVDF emulsion, stirred evenly, dried, and air flow crushed to obtain the porous nano-ceramics / PVDF composite agglomerates.
[0031] In order to achieve the above objectives, the embodiments of the present application also disclose an application of a PVDF coated diaphragm in a lithium battery.
[0032] Compared with the prior art, the present application has the following beneficial effects: the present application forms a randomly distributed organic layer on the diaphragm by using porous nano-ceramic / PVDF composite agglomerates. The porous nano-ceramics in the porous nano-ceramic / PVDF composite agglomerate particles can provide a channel for the shuttle of lithium ions, reduce the resistance of lithium ions passing through the aggregated point-like PVDF, and thus improve the cycle performance of the battery. The presence of porous nano-ceramics provides storage space for the electrolyte and increases the capacity retention rate of the battery. The high specific surface tension of porous nano-ceramics can play a certain adsorption role when bonded to the pole piece, thereby increasing the adhesion between the diaphragm and the pole piece and enhancing the hardness of the battery. The porous nano-ceramics provides a channel for the conduction of gas, and the coated porous nano-ceramic / PVDF composite agglomerate coating has no effect on the overall air permeability of the coated diaphragm. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The present application is further described below in conjunction with the accompanying drawings and embodiments.
[0034] Figure 1 It is a schematic diagram of the structure of the porous nano-ceramic / PVDF composite agglomerate in this application.
[0035] Figure 2 It is a schematic diagram of the structure of porous nanoceramics. DETAILED DESCRIPTION
[0036] In order to make the purpose and technical solution of the present invention clearly and completely described, and the advantages more clearly understood, the embodiments of the present invention are further described in detail with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are part of the embodiments of the present invention, rather than all of the embodiments, and are only used to explain the embodiments of the present invention, and are not used to limit the embodiments of the present invention. All other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] In the description of the present invention, it should be noted that the terms "center", "middle", "upper", "lower", "left", "right", "inner", "outer", "top", "bottom", "side", "vertical", "horizontal" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "one", "first", "second", "third", "fourth", "fifth", "sixth" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0038] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0039] For the purpose of simplicity and illustration, the principles of the embodiments are mainly described by reference to examples. In the following description, many specific details are proposed to provide a thorough understanding of the embodiments. However, it is obvious that for those of ordinary skill in the art, these embodiments may not be limited to these specific details in practice. In some instances, known methods and structures are not described in detail to avoid making these embodiments unnecessarily difficult to understand. In addition, all embodiments can be used in combination with each other.
[0040] The present application discloses a PVDF coated diaphragm, including a base film, a heat-resistant layer and an organic layer. The base film is a porous film, specifically one of a PP film, a PE film, or a composite film of a PP film and a PE film, with a thickness of 5-16µm.
[0041] The heat-resistant layer is arranged on at least one side of the base film, with a thickness of 1-4µm, and includes ceramics, stabilizers, glue and wetting agents. Among them, the ceramics specifically use one or more of aluminum oxide, silicon oxide, boehmite, titanium oxide, zirconium oxide, aluminum hydroxide, etc., with a particle size of 0.5-1.2µm. The stabilizer specifically uses one or more of gelatin, hydroxyethyl cellulose, methyl cellulose, xanthan gum, β-cyclodextrin, sodium carboxymethyl cellulose, etc., and the addition amount is 0.2-2wt% of the ceramic. The glue specifically uses one or more of acrylic acid, acrylic polymer, styrene-butadiene rubber, polystyrene, polyacrylate, etc., and the addition amount is 1-10wt% of the ceramic. The wetting agent specifically uses one or more of sodium dodecyl sulfate, fatty alcohol, sodium salt of butyl naphthalene sulfonate, nonylphenol polyoxyethylene ether, etc., and the addition amount is 0.2-2wt% of the ceramic.
[0042] The organic layer is disposed on the heat-resistant layer by spraying, and the organic layer includes porous nano-ceramic / PVDF composite aggregates, a binder and a defoamer. Figure 1-2As shown, the particle size of the porous nanoceramic / PVDF composite agglomerate is 3-10µm, which is agglomerated by porous nanoceramic 1 and PVDF particles 2, and porous nanoceramic 1 has holes 3. The porous nanoceramic in the porous nanoceramic / PVDF composite agglomerate particles can provide a channel for the shuttle of lithium ions, reduce the resistance of lithium ions passing through the aggregated point-like PVDF, and thus improve the cycle performance of the battery. The presence of porous nanoceramics provides storage space for electrolytes and increases the capacity retention rate of the battery. The high specific surface tension of porous nanoceramics can play a certain adsorption role when bonding with the pole piece, thereby increasing the bonding force between the diaphragm and the pole piece and enhancing the hardness of the battery. The porous nanoceramic provides a channel for the conduction of gas, and the coated porous nanoceramic / PVDF composite agglomerate coating has no effect on the overall air permeability of the coated diaphragm.
[0043] Further, the mass ratio of porous nano-ceramics to PVDF particles is 1-3:10. The porous nano-ceramics specifically adopt one or more of porous nano-alumina, porous nano-silicon oxide, porous nano-titanium oxide, porous coordination polymer, porous nano-boehmite, porous nano-aluminum hydroxide, porous nano-zinc oxide, etc., with a particle size of 150-350nm, a pore size of 10-80nm, and a porosity of 50-80%. The PVDF particles adopt a primary particle size PVDF material with an α-crystal form, a crystallinity of about 40%, and a particle size of 150-300nm.
[0044] Specifically, the porous nano-ceramic / PVDF composite agglomerate is prepared by the following method:
[0045] Select a suitable reactor, add deionized water and dispersant and stir evenly;
[0046] Repeatedly introduce nitrogen to exhaust oxygen, and after the replacement is qualified, introduce VDF into the reactor;
[0047] The temperature and pressure are raised to a constant temperature and pressure, and then the initiator and emulsifier are introduced to carry out the polymerization reaction. During this period, VDF can be introduced to control the reaction pressure;
[0048] After the reaction is completed, the unreacted VDF is recycled, and the polymer emulsion is condensed, washed, and separated to obtain PVDF emulsion;
[0049] The porous nano-ceramics are added into the PVDF emulsion, stirred evenly, dried, and air flow crushed to obtain the porous nano-ceramics / PVDF composite agglomerates.
[0050] Further, the binder is specifically one or more of styrene-butadiene rubber, polystyrene, polyacrylate, acrylic acid, acrylonitrile, etc., and the added amount is 3-10wt% of the porous nano-ceramic / PVDF composite agglomerate. The defoamer is specifically one or more of polydimethylsiloxane, dimethyl polysiloxane, dimethyl silicone oil, emulsified silicone oil, etc., and the added amount is 0.5-3wt% of the porous nano-ceramic / PVDF composite agglomerate.
[0051] The present application also discloses a method for preparing a PVDF coated diaphragm, comprising the following steps:
[0052] Coating the heat-resistant layer: take ceramic, deionized water, and dispersant and stir at high speed for 40 minutes; add stabilizer and stir at high speed for 60 minutes; add binder, vacuum -0.7MPa, and stir at high speed for 60 minutes; add wetting agent and stir at low speed for 30 minutes to obtain heat-resistant layer slurry; coat the heat-resistant layer slurry on at least one side of the base film;
[0053] Coating the organic layer: Mix the porous nano-ceramic / PVDF composite aggregate, binder and water, stir at high speed; add defoamer, stir slowly to obtain organic layer slurry; spray the organic layer slurry on the heat-resistant layer by air gun spraying or high-speed centrifugation. The spraying particle size of the organic layer is 50-400µm, and the spraying coverage is 8-25%.
[0054] The technical scheme and effects of the present application are further described below by listing embodiments and comparative examples, but the present application is not limited to these embodiments.
[0055] [Example 1]
[0056] Preparation of porous nano-ceramic / PVDF composite agglomerates: Select a suitable reactor, add 4000 parts of deionized water and 2 parts of polyvinyl alcohol and stir evenly; repeatedly introduce nitrogen to exhaust oxygen, and after the replacement is qualified, introduce 1000 parts of VDF into the reactor; increase the temperature and pressure to 85°C and 3.0MPa, and then inject 5 parts of diisopropyl peroxydicarbonate and 1.5 parts of perfluorooctanoic acid agent, and VDF can be introduced during the reaction to control the reaction pressure; after the reaction is completed, the unreacted VDF is recycled The polymer emulsion is condensed, washed and separated to obtain a PVDF emulsion with a solid content of 20% and a particle size of 250nm; 1000 parts of the emulsion PVDF are added with 25 parts of porous nanoceramics with a particle size D50 of 180nm, a pore size of 50nm and a porosity of 55% (porous nanoceramics: PVDF = 1.25:10), stirred evenly, dried, and the air flow crushing intensity is controlled to obtain a porous nanoceramics / PVDF composite agglomerate with a particle size D50 of 4.55µm.
[0057] Coating the heat-resistant layer: Mix 200 parts of aluminum oxide and 400 parts of deionized water, and stir at high speed for 40 minutes; add 1.5 parts of methyl cellulose and stir at high speed for 60 minutes; add 12 parts of polyacrylate, vacuum -0.7MPa, and stir at high speed for 60 minutes; add 1 part of sodium dodecyl sulfate as a moistener and stir at low speed for 30 minutes to obtain the heat-resistant layer slurry. Use micro-gravure technology to coat the finished slurry on the Enjie 7µm diaphragm, and after baking and winding, a 2µm heat-resistant layer coated diaphragm is obtained.
[0058] Coating the organic layer: 100 parts of the obtained porous nano-ceramic / PVDF composite aggregate, 8 parts of acrylonitrile, and 400 parts of deionized water were mixed and stirred at high speed for 180 minutes; 1 part of dimethyl polysiloxane was added and stirred at low speed for 30 minutes to obtain an organic layer slurry; the organic layer slurry was sprayed on the heat-resistant layer by an air gun spraying method, and the spraying surface density was obtained by adjusting the spraying flow rate and air pressure to 0.5 g / m 2 , PVDF coated diaphragm with a particle size of 320µm and a coverage of 23%.
[0059] [Example 2]
[0060] In the step of preparing porous nano-ceramic / PVDF composite agglomerates, 1000 parts of the emulsion are added with 40 parts of porous nano-ceramics (porous nano-ceramics: PVDF=2:10) with a particle size D50 of 320 nm, a pore size of 15 nm, and a porosity of 78%, stirred evenly, dried, and porous nano-ceramics / PVDF composite agglomerates with a particle size D50 of 6.08 µm are obtained by adjusting the air flow crushing intensity;
[0061] In the step of coating the organic layer, the spraying flow rate and air pressure were adjusted to obtain a spraying surface density of 0.5 g / m 2 , a PVDF coated diaphragm with a particle size of 150 μm and a coverage of 18%, and the remaining steps are the same as in Example 1.
[0062] [Example 3]
[0063] In the step of preparing porous nano-ceramic / PVDF composite agglomerates, 1000 parts of the emulsion are added with 58 parts of porous nano-ceramics with a particle size D50 of 220 nm, a pore size of 75 nm, and a porosity of 65% (porous nano-ceramics: PVDF = 2.9:10), stirred evenly, dried, and porous nano-ceramics / PVDF composite agglomerates with a particle size D50 of 7.54 µm are obtained by adjusting the air flow crushing intensity;
[0064] In the step of coating the organic layer, the spraying flow rate and air pressure were adjusted to obtain a spraying surface density of 0.5 g / m 2 , a PVDF coated diaphragm with a particle size of 250 μm and a coverage of 12%, and the remaining steps are the same as in Example 1.
[0065] [Comparative Example 1]
[0066] In the step of preparing the porous nano-ceramic / PVDF composite agglomerate of Example 1, without adding porous nano-ceramic, the PVDF emulsion is directly dried, the air flow crushing strength is controlled, and the secondary particle size PVDF with a particle size D50 of 7.52 μm is obtained; then 100 parts of the secondary particle size PVDF with a D50 of 7.52 μm and 28 parts of porous nano-ceramic with a particle size D50 of 220 nm, a pore size of 75 nm, and a porosity of 65% are taken (porous nano-ceramic: PVDF = 2.8:10);
[0067] In the step of coating the organic layer, the spraying flow rate and air pressure were adjusted to obtain a spraying surface density of 0.5 g / m 2 , a coated diaphragm mixed with secondary particle size PVDF and porous nano-ceramics with a particle size of 240 μm and a coverage of 12%, and the rest is the same as Example 1.
[0068] [Comparative Example 2]
[0069] In the step of preparing porous nano-ceramic / PVDF composite agglomerates in Example 1, the porous ceramic is not added, the emulsion is directly dried, and the air flow crushing intensity is adjusted to obtain pure secondary particle size PVDF with a particle size of 4.58 μm;
[0070] In the step of coating the organic layer, the spraying flow rate and air pressure were adjusted to obtain a spraying surface density of 0.5 g / m 2 A pure secondary particle size PVDF coated diaphragm with a particle size of 340 μm and a coverage of 22%, and the remaining steps are the same as Example 1.
[0071] [Comparative Example 3]
[0072] In the step of preparing the porous nano-ceramic / PVDF composite agglomerate in Example 1, 1000 parts of the emulsion were added with 40 parts of nano-ceramic with a particle size of 320 μm (nano-ceramic: PVDF = 2:10), stirred evenly, dried, and the modified secondary particle size PVDF with a particle size of 6.05 μm was obtained by adjusting the air flow crushing strength;
[0073] In the step of coating the organic layer, the spraying flow rate and air pressure were adjusted to obtain a spraying surface density of 0.5 g / m 2 , a nano-ceramic / PVDF composite agglomerate-coated diaphragm with a particle size of 160 μm and a coverage of 19%, and the remaining steps are the same as in Example 1.
[0074] [Comparative Example 4]
[0075] Coating the heat-resistant layer: Mix 200 parts of aluminum oxide and 400 parts of deionized water, and stir at high speed for 40 minutes; add 1.5 parts of methyl cellulose and stir at high speed for 60 minutes; add 12 parts of polyacrylate, vacuum -0.7MPa, and stir at high speed for 60 minutes; add 1 part of sodium dodecyl sulfate as a moistener and stir at low speed for 30 minutes to obtain the heat-resistant layer slurry. Use micro-gravure technology to coat the finished slurry on the Enjie 7µm diaphragm, and after baking and winding, a 2µm heat-resistant layer coated diaphragm is obtained.
[0076] [Agglomerate particle size]
[0077] The agglomerates obtained in the embodiment and the comparative example were dispersed in ethanol, and ultrasonic treatment was performed at 800W and 40KHz for 30 min, followed by stirring at a high speed of 2000rpm for 60 min. The particle size of the agglomerates before and after the treatment was tested, and the particle size change rate (particle size change rate = |(particle size after treatment - particle size before treatment)| / particle size before treatment) was less than 1%. The particle size tester was Battersize2000, and the refractive index was selected to be 1.42.
[0078] The calculation results of the test machine are summarized in Table 1.
[0079] Table 1
[0080]
[0081] It can be seen from Table 1 that after ultrasound and high-speed shearing, the particle size change rate of the agglomerates is less than 1%, so it can be seen that the agglomerates exist stably as hard agglomerates.
[0082]
Composite diaphragm performance
[0083] The following performance tests were performed on the composite diaphragms prepared in Examples 1-3 and Comparative Examples 1-4.
[0084] Air permeability: the time required for 100 ml of gas to pass through a membrane of a fixed area;
[0085] Liquid storage performance: Take a 10cm*10cm diaphragm and immerse it in a lithium salt electrolyte (EC:EMC:DEC=3:5:2, LiPF6, 1Mol / L) at 60℃ for 24h. Weigh the mass of the diaphragm before and after immersion. Liquid storage rate = mass after immersion / mass before immersion*100%;
[0086] Adhesion performance: Adhesion between the coated diaphragm and the positive electrode sheet at 3MPa, 5min, 90℃. The positive electrode sheet is composed of 100 parts of lithium manganese oxide + 85 parts of lithium iron phosphate + 8 parts of conductive carbon black + 7 parts of PVDF;
[0087] Ionic conductivity performance: In an argon glove box, the diaphragm was made into a 2016 button battery, and an appropriate amount of electrolyte (EC:EMC:DEC=3:5:2, LiPF6, 1Mol / L) was added. The AC impedance test in the electrochemical workstation showed that σ=L / (Rb*A), where σ is the ionic conductivity (S cm -1 ); L is the thickness of the diaphragm (cm); Rb is the intrinsic resistance of the diaphragm (Ω); A is the effective area (cm 2 );
[0088] Capacity retention rate: The battery is cycled 180 times at 0.3C charge and discharge, and the capacity before and after the test cycle is measured. Capacity retention rate = capacity after cycle / capacity before cycle.
[0089] The test and calculation results are summarized in Table 2.
[0090] Table 2
[0091]
[0092] As can be seen from Table 2, compared with Comparative Example 4, coating a layer of porous nano-ceramic / PVDF composite agglomerates on the heat-resistant layer of Examples 1-3 has no effect on the overall air permeability of the coating. Compared with Comparative Example 4, coating a layer of secondary particle size PVDF on the heat-resistant layer of Comparative Examples 1-3 increases the overall air permeability of the coating by about 10s / 100cc. In Comparative Example 1, the porous nano-ceramic and the secondary particle size PVDF are mixed and coated, and the porous nano-ceramic cannot enter the interior of the secondary particle size PVDF agglomerates. Therefore, the secondary particle size PVDF agglomerates hinder the passage of gas, so its air permeability is relatively high.
[0093] In Examples 1-3, since the porous nanoceramics are doped in the agglomerates, the porous nanoceramics provide a certain space for electrolyte storage, so the porous nanoceramics / PVDF composite agglomerates sprayed diaphragms in the examples have better liquid storage performance than the comparative examples. In Comparative Example 1, since there are porous nanoceramics and secondary particle size PVDF, the liquid storage performance is better; in Comparative Example 4, since there is only a heat-resistant layer and no PVDF layer, its liquid storage performance is poor; in Comparative Example 2, pure secondary particle size PVDF is selected, and the liquid storage performance is also relatively good; in Comparative Example 3, since the secondary particle size PVDF is doped with nanoceramics, the nanoceramics have no liquid storage performance, so the overall liquid storage performance is worse than that of Comparative Example 2.
[0094] The adhesion between the coated diaphragm and the pole piece in Examples 1-3 is slightly stronger than that in Comparative Example 2, which is related to the porous nano-ceramics. The porous nano-ceramics have a large specific surface tension. When the porous nano-ceramics / PVDF composite agglomerates are bonded to the pole piece, the porous nano-ceramics increase the adsorption effect between the diaphragm and the pole piece. Comparative Example 3 has a weaker adhesion to the pole piece than Comparative Example 2 because the surface adsorption of nano-ceramics is not strong. In Comparative Example 1, although the porous nano-ceramics have an adsorption effect on the pole piece, when the porous nano-ceramics are dispersed around the secondary particle size PVDF, the adhesion between PVDF and the pole piece is hindered, so its overall adhesion is poor.
[0095] In Examples 1-3, since porous nanoceramics are doped in the agglomerates, a large channel is provided for the shuttling of lithium ions, which improves the congestion of lithium ions when the secondary particle size PVDF is aggregated. Therefore, the deterioration of ionic conductivity is not obvious relative to Comparative Example 4. In Comparative Example 1, although porous nanoceramics are added, the porous nanoceramics can only be dispersed around the secondary particle size PVDF and cannot enter the interior of the secondary particle size PVDF, which cannot improve the congestion of the secondary particle size PVDF for ion shuttling. Therefore, its ionic conductivity deteriorates significantly relative to Comparative Example 4. Comparative Examples 2 and Comparative Examples 3 have a more obvious deterioration of ionic conductivity relative to Comparative Example 4 because the shaped area in the secondary particle size PVDF hinders the shuttling of lithium ions.
[0096] In Examples 1-3, since the porous nano-alumina can store a certain amount of electrolyte, the capacity retention rate of the battery is improved, and the porous nano-ceramic / PVDF composite agglomerates improve the congestion phenomenon of ion conduction, thereby alleviating the attenuation of the cycle. In Comparative Example 1, the medium-porous nano-ceramics cannot improve the congestion phenomenon of ion conduction caused by the secondary particle size PVDF, so its capacity retention rate is also relatively low. In Comparative Example 4, there is only a heat-resistant layer, and the overall liquid storage performance is poor, so the capacity retention rate is poor. In Comparative Examples 2 and 3, the overall liquid storage performance is much worse than that of the embodiments, so their overall capacity retention rates are poor compared to the embodiments.
[0097] Therefore, the present application adds porous nano-ceramics to the PVDF emulsion to obtain porous nano-ceramics / PVDF composite agglomerates, and uses the porous nano-ceramics / PVDF composite agglomerates to prepare a coated diaphragm, which has no effect on the air permeability of the coating, slightly increases the adhesion performance of the coated diaphragm with the electrode, improves the liquid storage performance of the diaphragm, and thus improves the cycle performance of the diaphragm. The porous nano-ceramics provide a large-aperture channel for lithium ion shuttling, thereby improving the ionic conductivity of the coated diaphragm.
[0098] Although the above describes the illustrative specific implementation methods of the present application so that technicians in this technical field can understand the present application, the present application is not limited to the scope of the specific implementation methods. For ordinary technicians in this technical field, as long as various changes are within the spirit and scope of the present application defined and determined by the attached claims, all application creations using the concept of the present application are protected.
Claims
1. A PVDF coated diaphragm, characterized in that: include: A base membrane, wherein the base membrane is a porous film; A heat-resistant layer, the heat-resistant layer being disposed on at least one side surface of the base film; An organic layer, the organic layer is arranged on the heat-resistant layer, the organic layer comprises a porous nano-ceramic / PVDF composite agglomerate, a binder and a defoamer, the porous nano-ceramic / PVDF composite agglomerate is formed by agglomerating porous nano-ceramic and PVDF particles; The porous nano-ceramic / PVDF composite agglomerate is prepared by the following method: Add deionized water and dispersant into the reactor and stir evenly; introduce nitrogen repeatedly to exhaust oxygen, and after the replacement is qualified, introduce VDF into the reactor; increase the temperature and pressure to a constant temperature and pressure, and then inject initiator and emulsifier to carry out polymerization reaction; After the reaction is completed, the unreacted VDF is recycled, and the polymer emulsion is condensed, washed, and separated to obtain PVDF emulsion; The porous nano-ceramics are added into the PVDF emulsion, stirred evenly, dried, and air flow crushed to obtain the porous nano-ceramics / PVDF composite agglomerates.
2. A PVDF coated diaphragm according to claim 1, characterized in that: The base film is a PP film, a PE film, or a composite film of a PP film and a PE film.
3. A PVDF coated diaphragm according to claim 1, characterized in that: The thickness of the base film is 5-16 μm.
4. A PVDF coated diaphragm according to claim 1, characterized in that: The heat-resistant layer comprises ceramics, a stabilizer, glue and a wetting agent.
5. A PVDF coated diaphragm according to claim 4, characterized in that: The particle size of the ceramic is 0.5-1.2 μm.
6. A PVDF coated diaphragm according to claim 4, characterized in that: The stabilizer accounts for 0.2-2 wt % of the ceramic.
7. A PVDF coated diaphragm according to claim 4, characterized in that: The glue accounts for 1-10wt% of the ceramic.
8. A PVDF coated diaphragm according to claim 4, characterized in that: The wetting agent accounts for 0.2-2 wt % of the ceramic.
9. A PVDF coated diaphragm according to claim 1, characterized in that: The mass ratio of the porous nano-ceramics to the PVDF particles is 1-3:
10.
10. A PVDF coated diaphragm according to claim 1, characterized in that: The porous nano-ceramic has a particle size of 150-350 nm, a pore size of 10-80 nm, and a porosity of 50-80%.
11. A PVDF coated diaphragm according to claim 1, characterized in that: The PVDF particles have an α-crystal form and a particle size of 150-300 nm.
12. A PVDF coated diaphragm according to claim 1, characterized in that: The particle size of the porous nano-ceramic / PVDF composite agglomerate is 3-10 μm.
13. A PVDF coated diaphragm according to claim 1, characterized in that: The binder accounts for 3-10 wt % of the porous nano-ceramic / PVDF composite agglomerate.
14. A PVDF coated diaphragm according to claim 1, characterized in that: The defoaming agent accounts for 0.5-3wt% of the porous nano-ceramic / PVDF composite agglomerate.
15. A method for preparing a PVDF coated diaphragm as claimed in claim 1, characterized in that: The following steps are involved: Coating the heat-resistant layer: coating the heat-resistant layer slurry on at least one side of the surface of the base film; Coating the organic layer: taking the porous nano-ceramic / PVDF composite agglomerate, a binder, and water, mixing them, and stirring at high speed; adding a defoaming agent, stirring slowly, and obtaining an organic layer slurry; using an air gun spraying or a high-speed centrifugal method to spray the organic layer slurry on the heat-resistant layer.
16. The method for preparing a PVDF coated diaphragm according to claim 15, characterized in that: The thickness of the heat-resistant layer is 1-4 μm.
17. The method for preparing a PVDF coated diaphragm according to claim 15, characterized in that: The spraying particle size of the organic layer is 50-400µm, and the spraying coverage is 8-25%.
18. Use of a PVDF coated diaphragm as claimed in any one of claims 1 to 14 or a PVDF coated diaphragm prepared by the method for preparing a PVDF coated diaphragm as claimed in any one of claims 15 to 17 in a lithium battery.