Method for producing silicon single crystal
By limiting the quality and introduction of carbon impurities of silicon nitride powder, combined with the supplementary high-purity nitride film, the problems of carbon impurities control and high cost in nitrogen doping are solved, and low-cost low-carbon concentration specifications and high-efficiency nitrogen are achieved. Doping.
Patent Information
- Application Number
- CN202080096689.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-18
- Filing Date
- 2020-12-01
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-12-01
AI Technical Summary
During the manufacturing process of semiconductor devices, when using high-purity silicon nitride powder for nitrogen doping, there is a problem that carbon impurity concentration is difficult to control and costly, especially when manufacturing large-diameter crystals, it requires a large amount of silicon raw materials, resulting in low yield and high cost.
By limiting the carbon impurity quality in silicon nitride powder, controlling the carbon concentration in silicon single crystal below the allowable value, determining the upper limit of silicon nitride powder, and introducing silicon nitride powder before melting begins, through Cheklaus The base method is used to perform nitrogen doping, and combined with the supplement of high-purity nitride film, low-cost nitrogen doping is achieved.
While achieving low-carbon concentration specifications, low-cost nitrogen doping is achieved, production costs are reduced, and low-carbon impurity concentration of silicon single crystals is ensured, meeting the requirements of silicon single crystals for semiconductors.
Smart Images

Figure CN115103934B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a silicon single crystal. Background Art
[0002] Conventionally, the occurrence of slip (dislocation) of a silicon wafer due to heat treatment in a semiconductor device manufacturing process has sometimes become a factor that reduces the yield of final products.
[0003] Slip dislocation is a defect caused by the stress generated by the wafer's own weight or the stress generated by thermal deformation, as well as the application of high-temperature heat energy, which causes the silicon crystal structure to shift by several millimeters to several centimeters in length, starting from the mechanical damage caused when the silicon single crystal wafer contacts the supporting structure.
[0004] As a countermeasure against thermal stress generated by heat treatment in the process of manufacturing the semiconductor device, Patent Document 1 indicates that nitrogen doping is effective.
[0005] There are various methods for nitrogen doping. In the Czochralski method (CZ method), nitride is mixed in the melt. In order to obtain high-purity silicon wafers, the nitride used must be of high purity. In order to manage the nitrogen concentration contained in the silicon wafer, it is also important to accurately control the doping amount of nitride.
[0006] For example, as a nitrogen source, Patent Document 1 shows a silicon nitride powder sintered body (with a sintering aid added), a silicon powder molded product directly nitrided, or a material formed by blowing nitrogen or a nitrogen compound gas onto polycrystalline silicon before melting. However, the silicon nitride powder sintered body (with a sintering aid added) has a purity problem, and for the direct nitridation of silicon powder or raw materials before melting, the nitridation amount will vary if the temperature is not precisely controlled under the limitation of the surface reaction rate, so there is a problem of difficulty in concentration management.
[0007] In this regard, Patent Document 2 shows that a nitride film formed by nitriding a high-purity silicon wafer is used as a nitrogen source. In terms of purity, it is suitable as a nitrogen source in semiconductor silicon manufacturing, and since the thickness of the nitride film can be controlled by temperature control, concentration management can also be performed. However, in the case of manufacturing large-diameter crystals that use a large amount of silicon raw materials, a large number of silicon wafers with nitride films are required, which has a high cost technical problem.
[0008] As another nitrogen doping method, Patent Document 3 shows a method using high-purity silicon nitride powder. However, when a large amount of nitrogen doping is required, the following problem still exists: even in the high-purity silicon nitride powder obtained by the gas phase reaction of silicon tetrachloride, which is the highest purity silicon nitride available industrially, and ammonia, there are still carbon impurities contained in a relatively high concentration, which will have an adverse effect on achieving the low carbon concentration specification required for silicon single crystals for semiconductors, resulting in low yield and high cost problems.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent Application Laid-Open No. 60-251190
[0012] Patent Document 2: Japanese Patent Application Laid-Open No. 05-294780
[0013] Patent Document 3: Japanese Patent No. 5262257
[0014] Patent Document 4: Japanese Patent Application Laid-Open No. 11-195565 Summary of the invention
[0015] Technical Problems to be Solved by the Invention
[0016] As described above, in the conventional nitrogen doping method, for the method using a silicon wafer with a nitride film, there is a technical problem in terms of cost because a large number of silicon wafers with a nitride film are required when manufacturing large-diameter crystals that use a large amount of silicon raw materials. In addition, when using high-purity silicon nitride powder, there is a technical problem that carbon impurities contained in a relatively high concentration will have an adverse effect on achieving the low carbon concentration specification required for semiconductor silicon single crystals.
[0017] In view of the above technical problems, the present invention provides a nitrogen doping method for controlling the carbon impurity concentration brought by silicon nitride powder within an allowable range and implementing the target nitrogen doping at a low cost.
[0018] That is, an object of the present invention is to provide a method for producing single crystal silicon that can achieve a target nitrogen doping amount at low cost while achieving a low carbon concentration specification.
[0019] Technical means to solve technical problems
[0020] In order to solve the above-mentioned technical problems, the present invention provides a method for manufacturing a silicon single crystal, which is a method for manufacturing a silicon single crystal, comprising introducing silicon nitride powder into a raw material before melting begins and pulling a silicon single crystal doped with nitrogen by the Czochralski method. The method is characterized in that based on the amount of carbon impurities contained in the silicon nitride powder, the upper limit amount of silicon nitride powder that can be used is limited in a manner such that the carbon concentration in the silicon single crystal is below an allowable value, thereby doping with nitrogen.
[0021] For the single crystal manufacturing method of the present invention, by limiting the upper limit of the silicon nitride powder that can be used in a manner that makes the carbon concentration in the silicon single crystal below the allowable value based on the amount of carbon impurities contained in the silicon nitride powder, it is possible to determine the amount of silicon nitride powder introduced to achieve a carbon impurity concentration within the allowable range. Furthermore, for the single crystal manufacturing method of the present invention, compared to the case where only a silicon wafer with a nitride film is used as a nitrogen source, the same degree of nitrogen doping can be achieved at a lower cost. Therefore, according to the single crystal manufacturing method of the present invention, it is possible to achieve the target nitrogen doping amount at a low cost while achieving a low carbon concentration specification.
[0022] The upper limit of the amount of silicon nitride powder that can be used can be determined, for example, by satisfying the following formula (1):
[0023] {the upper limit amount [g] × (carbon impurity concentration in the silicon nitride powder [wt%] / 100) / carbon atomic weight [g / mol]} / silicon raw material addition amount [mol] ≤ 0.32 × 10 -6 (1)
[0024] By determining the upper limit of the amount of silicon nitride powder that can be used so as to satisfy the above formula (1), it is possible to produce single crystal silicon that complies with the low carbon concentration standard of 0.10 ppma or less generally required for semiconductor devices.
[0025] Alternatively, the upper limit of the amount of silicon nitride powder that can be used can also be determined, for example, by satisfying the following formula (2):
[0026] {the upper limit amount [g] × (carbon impurity concentration in the silicon nitride powder [wt%] / 100) / carbon atomic weight [g / mol]} / silicon raw material addition amount [mol] ≤ 0.16 × 10 -6 (2)
[0027] By determining the upper limit of the usable silicon nitride powder so as to satisfy the above formula (2), it is possible to meet the demand for silicon wafers with lower carbon concentrations, for example, to meet the low carbon concentration standard of 0.05 ppma or less.
[0028] The upper limit of the amount of silicon nitride powder that can be used can also be determined from the actual value of the carbon concentration in the silicon single crystal produced by doping the silicon nitride powder.
[0029] This makes it possible to more reliably achieve a carbon impurity concentration within the allowable range.
[0030] When the upper limit of the amount of silicon nitride powder that can be used is above the required nitrogen doping amount, only the silicon nitride powder is doped as a nitrogen source. When the upper limit is less than the required nitrogen doping amount, the missing nitrogen doping amount can be supplemented by using a silicon wafer with a high-purity nitride film to dope the raw material.
[0031] That is, the amount of the silicon nitride powder that is insufficient to achieve the required nitrogen doping amount can be supplemented by using a high-purity nitride film wafer obtained by nitriding a high-purity silicon wafer.
[0032] Therefore, even when the required nitrogen doping amount is high, the use amount of silicon wafers with high-purity nitride films can be minimized, and the required nitrogen doping amount can be achieved at low cost while achieving low carbon concentration specifications.
[0033] It is preferred that the silicon nitride powder be weighed in an amount not exceeding the above upper limit in a state where the silicon nitride powder is supported on a silicon wafer.
[0034] This can suppress the variation in the amount of introduction due to adhesion to a pharmaceutical weighing paper or the like during weighing, and can accurately introduce the weighed amount of silicon nitride powder into the raw material.
[0035] More preferably, the weighed silicon nitride powder is sandwiched between other silicon wafers to prepare a dopant, and the dopant is added to the raw material before melting, thereby performing nitrogen doping.
[0036] Thus, the deviation of the introduced amount due to scattering or adhesion to the medicine weighing paper during weighing can be suppressed, and the weighed amount of silicon nitride powder can be introduced into the raw material more accurately. That is, in the single crystal manufacturing method of the above preferred embodiment, the silicon nitride powder can be accurately weighed to a target amount that can achieve a carbon impurity concentration within an allowable range, and the target amount of silicon nitride powder can be accurately introduced into the raw material.
[0037] Effects of the Invention
[0038] As described above, according to the single crystal production method of the present invention, it is possible to achieve a target nitrogen doping amount at low cost while achieving a low carbon concentration specification. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 FIG. 1 is a schematic cross-sectional view showing an example of a crystal manufacturing apparatus capable of implementing the silicon single crystal manufacturing method of the present invention. DETAILED DESCRIPTION
[0040] The present invention relates to a method for manufacturing a silicon single crystal, and more specifically, to a method for manufacturing a silicon single crystal such as a silicon wafer, a silicon epitaxial wafer, an SOI wafer, and a heteroepitaxial wafer. From another perspective, the present invention relates to a method for manufacturing a nitrogen-doped silicon single crystal by using a CZ method for implementing nitrogen doping.
[0041] As described above, a method for producing single crystal silicon that can achieve a target nitrogen doping amount at low cost while meeting low carbon concentration specifications has been sought.
[0042] The inventors of the present invention have conducted in-depth research on the above-mentioned technical problems, and found that by limiting the upper limit of the amount of silicon nitride powder that can be used so that the carbon concentration in the silicon single crystal is below the allowable value, and introducing the silicon nitride powder into the raw material before melting begins to dope nitrogen under this limitation, it is possible to achieve the target nitrogen doping amount at a low cost while achieving the low carbon concentration specification, thereby completing the present invention.
[0043] That is, the present invention is a method for manufacturing a silicon single crystal, which is a method for manufacturing a silicon single crystal, wherein silicon nitride powder is introduced into a raw material before melting begins, and a silicon single crystal doped with nitrogen is pulled by the Czochralski method. The method is characterized in that based on the amount of carbon impurities contained in the silicon nitride powder, the upper limit amount of silicon nitride powder that can be used is limited in a manner such that the carbon concentration in the silicon single crystal is below an allowable value, thereby doping with nitrogen.
[0044] Hereinafter, the present invention will be described in detail, but the present invention is not limited thereto.
[0045] <Silicon Single Crystal Manufacturing Method>
[0046] First, through Figure 1 An example of the structure of a crystal manufacturing apparatus capable of implementing the silicon single crystal manufacturing method of the present invention is described. Figure 1 As shown, the crystal manufacturing apparatus 100 comprises: a main chamber 1 and a pulling chamber 2 connected to the upper part of the main chamber 1 for storing the growing silicon single crystal 3. A quartz crucible 5 for containing a raw material melt 4 and a graphite crucible 6 for supporting the quartz crucible 5 are provided inside the main chamber 1. In addition, a heater 7 as a main heat source is arranged concentrically with the quartz crucible 5 and the graphite crucible 6. An insulating member 8 is arranged outside the heater 7. In addition, a gas outflow port 9 is provided in the main chamber 1, and a gas inlet 10 is provided in the pulling chamber 2, so as to introduce or discharge an inert gas (for example, argon gas) into or out of the main chamber 1 and the pulling chamber 2. A cylindrical gas rectifying cylinder 11 is arranged above the surface of the raw material melt 4 in a manner surrounding the silicon single crystal 3 being pulled. In addition, an insulating member 12 is arranged facing each other above the melt surface of the raw material melt 4. In addition, a magnetic field applying device 13 is arranged on the outer periphery of the main chamber 1.
[0047] Next, the method for producing a silicon single crystal of the present invention will be described in more detail.
[0048] In the silicon single crystal manufacturing method of the present invention, first, as an example, using Figure 1 The crystal production apparatus 100 shown in the figure supplies silicon raw material into the quartz crucible 5 to prepare for the growth of silicon single crystal. After the silicon raw material is heated and melted, the growth axis direction of the silicon single crystal can be set to, for example, <100> While applying a magnetic field using the magnetic field applying device 13, a silicon single crystal is grown, and the silicon single crystal is pulled up using a conventional CZ method, thereby manufacturing a silicon single crystal.
[0049] In the present invention, silicon nitride (Si3N4) powder is introduced into the raw material before melting begins, and a silicon single crystal is pulled by the Czochralski method.
[0050] Here, the upper limit amount of the silicon nitride powder to be introduced is limited based on the amount of carbon impurities contained in the silicon nitride powder so that the carbon concentration in the silicon single crystal becomes equal to or less than the allowable value.
[0051] As described above, even high-purity silicon nitride powder has a high concentration of carbon impurities. However, in the single crystal manufacturing method of the present invention, the upper limit of the amount of silicon nitride powder that can be used is limited based on the amount of carbon impurities contained in the silicon nitride powder so that the carbon concentration in the silicon single crystal is below the allowable value, and the amount of silicon nitride powder introduced that can achieve a carbon impurity concentration within the allowable range can be determined.
[0052] Furthermore, in the single crystal manufacturing method of the present invention, by using silicon nitride powder to implement nitrogen doping on the basis of controlling the upper limit amount of silicon nitride powder that can be used in the above manner, the same level of nitrogen doping can be achieved at a lower cost compared to the case where only a silicon wafer with a nitride film is used as a nitrogen source.
[0053] Therefore, according to the single crystal manufacturing method of the present invention, it is possible to achieve a required nitrogen doping amount at a low cost while achieving a low carbon concentration specification.
[0054] In the single crystal production method of the present invention, it is preferred that the silicon nitride powder be weighed in an amount not exceeding the upper limit amount specified above, with the silicon nitride powder being supported on a silicon wafer.
[0055] When silicon nitride powder is weighed with pharmaceutical weighing paper or the like in the same manner as conventional dopants, silicon nitride powder with a small particle size will adhere to and remain on the surface of the pharmaceutical weighing paper, thereby causing deviations in the amount of nitrogen doping. In response to this, by weighing the silicon nitride powder while it is supported on a silicon wafer, it is possible to suppress deviations in the amount of introduction caused by adhesion (residue) on the pharmaceutical weighing paper or the like during weighing.
[0056] In the silicon single crystal manufacturing device of the present invention, it is more preferred that: the silicon nitride powder weighed in a state of being carried on a silicon wafer is clamped with other silicon wafers to form a dopant, and the dopant is added to the raw material before melting begins (for example, on the raw material carried in the quartz crucible 5).
[0057] For example, the high-purity silicon nitride powder obtained by the gas phase reaction of silicon tetrachloride and ammonia is a microparticle of about several μm to 100 μm. It will be difficult to dissolve all the silicon nitride powder used in the melt due to the scattering during operation or melting process. Therefore, it is difficult to control the doping amount of nitride, resulting in a technical problem of deviation in the doping amount. For this technical problem, patent document 4 discloses a method of spreading silicon nitride powder on the bottom of a crucible for doping, but since silicon nitride powder will scatter when adding polysilicon raw material after adding silicon nitride to the bottom of the crucible, this method is not an effective solution. That is, there is the following problem in the prior art: when weighing silicon nitride powder on a pharmaceutical weighing paper instead of on a silicon wafer, when doping or moving to the silicon wafer that clamps the silicon nitride powder, some silicon nitride powder will inevitably remain on the pharmaceutical weighing paper and the silicon nitride powder will scatter, making it difficult to accurately dope the weighed amount.
[0058] In this regard, by manufacturing the dopant in the above-mentioned manner and adding the dopant to the raw material before melting begins, it is possible to suppress the deviation in the amount of introduction caused by the dopant scattering during operation or in the process of melting the raw material, or adhering (residing) on pharmaceutical weighing paper during weighing, so that the weighed amount of silicon nitride powder can be accurately introduced into the raw material.
[0059] When using high-purity silicon nitride powder that is easily scattered due to its small particle size and easily adheres to and remains on pharmaceutical weighing paper, it is more effective to weigh it on the silicon wafer in the above-mentioned manner and dope it in a sandwiched form.
[0060] That is, in the above preferred embodiment of the present invention, by using the dopant produced in the above manner, a target amount of silicon nitride powder capable of achieving a carbon impurity concentration within an allowable range can be accurately weighed and the target amount of silicon nitride powder can be accurately introduced into the raw material.
[0061] In the single crystal production method of the present invention, the upper limit of the amount of silicon nitride powder that can be used can be determined, for example, by satisfying the following formula (1):
[0062] {the upper limit amount [g] × (carbon impurity concentration in the silicon nitride powder [wt%] / 100) / carbon atomic weight [g / mol]} / silicon raw material addition amount [mol] ≤ 0.32 × 10 -6 (1)
[0063] By finding the upper limit of the amount of silicon nitride powder that can be used in a manner that satisfies the above formula (1), it is possible to manufacture single crystal silicon that complies with the low carbon concentration specification of 0.10 ppma or less that is generally required for semiconductor devices. That is, based on the above formula (1), the amount of silicon nitride powder that can be used can be limited so that the carbon concentration in the silicon wafer is 0.10 ppma or less, thereby doping the silicon nitride powder.
[0064] In addition, although the carbon concentration standard in the crystal used in the single crystal manufacturing method of the present invention is a limitation on the carbon impurity concentration originating from silicon nitride powder in the silicon melt, if the limitation based on the above formula (1) is implemented, a silicon wafer with an allowable carbon concentration can be obtained using a grown crystal with a solidification rate of 80% by weight of the raw material, wherein the carbon concentration is the carbon concentration in the crystal that takes into account the segregation phenomenon during the growth of the silicon single crystal as shown in the following formula (3).
[0065] Carbon concentration in crystal = k0 × carbon concentration in melt (raw material melt) × (1-g) (k0-1) (3)
[0066] k0: segregation coefficient, g: solidification rate (= weight of grown crystal / weight of added raw materials)
[0067] Alternatively, for example, in the manufacture of silicon wafers having a carbon concentration standard of 0.05 ppma or less, by adjusting (limiting) the upper limit of the amount of silicon nitride powder that can be used so as to satisfy the following formula (2), it is possible to meet the demand for silicon wafers with lower carbon concentrations.
[0068] {the upper limit amount [g] × (carbon impurity concentration in the silicon nitride powder [wt%] / 100) / carbon atomic weight [g / mol]} / silicon raw material addition amount [mol] ≤ 0.16 × 10 -6 (2)
[0069] The amount of silicon raw material added in the above formulas (1) and (2) is the sum of the amount of silicon raw material (mol) before melting added to, for example, the quartz crucible 5 and the amount of silicon contained in the dopant in the silicon wafer sandwiching the silicon nitride powder. In addition, as a typical example of the carbon atomic weight, it is 12.01 [g / mol].
[0070] In addition, since the above formulas (1) and (2) are example formulas for calculating the upper limit amount of silicon nitride powder that can be used, the lower limit of the value of the ratio {the upper limit amount [g] × (carbon impurity concentration in the silicon nitride powder [wt%] / 100) / carbon atomic weight [g / mol]} / silicon raw material addition amount [mol] in the above formulas (1) and (2) is not particularly limited, and the missing nitrogen doping amount can be supplemented by, for example, using other nitrogen sources such as silicon wafers with high-purity nitride films.
[0071] The upper limit of the amount of silicon nitride powder that can be used can also be determined based on the actual value of the carbon concentration in the silicon single crystal produced by doping the silicon nitride powder. This makes it possible to more reliably achieve a carbon impurity concentration within the allowable range.
[0072] When the upper limit of the usable silicon nitride powder is above the required nitrogen doping amount, only the silicon nitride powder is used as a nitrogen source for doping, and when the upper limit is less than the required nitrogen doping amount, the missing nitrogen doping amount can be supplemented by doping the raw material with a silicon wafer with a high-purity nitride film. That is, the part where the amount of the silicon nitride powder (the upper limit that can be used) is insufficient to reach the required nitrogen doping amount can be supplemented by a wafer with a high-purity nitride film obtained by nitriding a high-purity silicon wafer.
[0073] Therefore, even when the required nitrogen doping amount is high, the use amount of silicon wafers with high-purity nitride films can be minimized, thereby achieving the required nitrogen doping amount at low cost while achieving low carbon concentration specifications.
[0074] As the silicon wafer with a high-purity nitride film, for example, the silicon wafer with a high-purity nitride film described in Patent Document 2 can be used.
[0075] The required nitrogen doping amount (required nitrogen atom doping amount in the melt) can be determined, for example, by taking into account the influence of the segregation of nitrogen atoms on the nitrogen atom concentration in the target silicon single crystal.
[0076] The silicon wafer used in the weighing of silicon nitride powder and the manufacture of dopants is not particularly limited as long as it can carry silicon nitride powder. If a silicon wafer with a smaller diameter is used, lower costs can be achieved. For the diameter of the silicon wafer used in the weighing of silicon nitride powder and the manufacture of dopants, when the diameter is, for example, 3 inches or more and 12 inches or less, since the weight is less than 128g, a conventional electronic balance can be used to weigh silicon nitride with sufficient measurement accuracy, and a diameter of 3 inches or more and 8 inches or less, or a small piece obtained by cutting a silicon wafer with a diameter of 4 to 12 inches can be used. Thus, while weighing silicon nitride with sufficient measurement accuracy, silicon nitride can be weighed in a manner that conforms to the sample chamber size of the electronic balance or the weight specification that can be measured. In addition, when using a cut small piece, in order to avoid the influence of contamination during cutting, it is more preferable to use a cleaned / mirror-etched small piece. Furthermore, in the weighing of silicon nitride powder and the manufacture of dopants, the above-mentioned silicon wafer with a high-purity nitride film used as a dopant can be used.
[0077] In addition, the method for producing a silicon single crystal of the present invention can also be used to remove Figure 1 The present invention can be implemented by an apparatus other than the crystal manufacturing apparatus 100. For example, the silicon single crystal manufacturing method of the present invention can also be implemented by an apparatus that does not include a magnetic field applying apparatus.
[0078] Example
[0079] Hereinafter, the present invention will be described in more detail using Examples and Comparative Examples, but the present invention is not limited thereto.
[0080] (Comparative Example 1)
[0081] In Comparative Example 1, the following conditions were used so that the nitrogen atomic concentration in the crystal at the position where the curing rate was 10% was 1×10 14 atoms / cm 3 , 5×10 14 atoms / cm 3 , 1×10 15 atoms / cm 3 and 2×10 15 atoms / cm 3 Four silicon single crystals (300 mm in diameter) were pulled up in this manner.
[0082] First, a silicon raw material and a silicon wafer with a nitride film as a nitrogen source are added to a quartz crucible with a diameter of 32 inches (800 mm). The silicon wafer with a nitride film used here is a silicon wafer with a nitride film made by directly nitriding an 8-inch PW (mirror-polished wafer with a diameter of 200 mm) and making the nitride film thickness 750 nm. After adding polycrystalline silicon as a silicon raw material to the quartz crucible, doping is performed in the form of a nitride film silicon wafer supported on the raw material.
[0083] At this time, the number of wafers with nitride films used was such that the nitrogen atomic concentration in the crystal at the position where the curing rate was 10% was 1×10 14 , 5×10 14 , 1×10 15 , 2×10 15 atoms / cm 3 The number of silicon single crystals were 8.9, 44.3, 88.6 and 177.3 respectively.
[0084] In addition, the total weight of the added silicon raw material including the silicon wafer with the nitride film was 400 kg.
[0085] Next, the silicon raw material and the silicon wafer with the nitride film are melted to prepare a raw material melt, and a silicon single crystal is pulled and grown from the raw material melt.
[0086] After that, samples with a thickness of 2 mm were collected from the positions where the solidification rate of the grown silicon single crystal was 10% and 80%, and the samples were plane-polished. In addition, the carbon concentration of the sample from the position where the solidification rate was 80% was measured by FTIR. Furthermore, the nitrogen atomic concentration of the sample from the position where the solidification rate was 10% was measured by SIMS.
[0087] (Example 1)
[0088] In Example 1, four silicon single crystals were pulled up and evaluated in the same manner as in Comparative Example 1 except that a dopant produced by sandwiching silicon nitride powder between silicon wafers was used as a nitrogen source.
[0089] In Example 1, when weighing silicon nitride powder, the silicon nitride powder is weighed on a 4-inch (100 mm in diameter) silicon wafer, and after weighing, the silicon nitride powder is clamped with other wafers to produce a dopant, and the dopant is carried on the silicon raw material.
[0090] Based on the previously measured carbon impurity concentration of 0.2 wt % of the silicon nitride powder used, the carbon concentration in the silicon crystal when the curing rate is 80% is 0.05 ppma or less so as to satisfy the formula: {the upper limit amount [g] × (carbon impurity concentration in the silicon nitride powder [wt %] / 100) / carbon atomic weight [g / mol]} / silicon raw material addition amount [mol] ≤ 0.16 × 10 -6 (2) was used to calculate the upper limit of the amount of silicon nitride powder that can be used. The upper limit of the amount of silicon nitride powder that can be used was 13.684 g. On the other hand, the nitrogen atomic concentration in the crystal at the position where the curing rate was 10% was 1×10 14 , 5×10 14 , 1×10 15 , 2×10 15 atoms / cm 3 The nitrogen doping amounts required for each silicon single crystal, calculated in terms of silicon nitride powder, are 1.323 g, 6.613 g, 13.226 g, and 26.452 g, respectively.
[0091] According to the calculation results, the nitrogen atomic concentration at the position where the curing rate is 10% is 1×10 14 atoms / cm 3 , 5×10 14 atoms / cm 3 , and 1×10 15 atoms / cm 3 When producing silicon single crystals, since the upper limit of the amount of silicon nitride powder that can be used is greater than the nitrogen doping amount required for the target nitrogen doping, only 1.323 g, 6.613 g, and 13.226 g of silicon nitride powder were used as nitrogen sources. 15 atoms / cm 3When preparing a silicon single crystal, since the upper limit of the amount of silicon nitride powder that can be used is less than the nitrogen doping amount required for the target nitrogen doping, 13.684 g of silicon nitride powder and 85.6 silicon wafers with nitride films were used as nitrogen sources. As the silicon wafer with nitride film, the same silicon wafer with nitride film as that used in Comparative Example 1 was used. In Example 1, the total weight of the added raw materials including the silicon wafer with dopant and the silicon wafer with nitride film was 400 kg.
[0092] (result)
[0093] The evaluation results of Example 1 and Comparative Example 1 are shown in Table 1 below.
[0094] [Table 1]
[0095]
[0096] For the four silicon single crystals obtained in Example 1 and Comparative Example 1, it was confirmed that the nitrogen concentration at the position where the solidification rate of the pulled silicon single crystal was 10% measured by SIMS reached the target value. In addition, as shown in Table 1, it was also confirmed that the nitrogen atomic concentration at the position where the solidification rate was 10% was 1×10 14 atoms / cm 3 , 5×10 14 atoms / cm 3 , and 1×10 15 atoms / cm 3 The nitrogen doping cost required for the growth of silicon single crystals is reduced by more than 99%, and the nitrogen atomic concentration is 2×10 15 atoms / cm 3 Silicon single crystals can also reduce nitrogen doping costs by 51%.
[0097] Furthermore, it was confirmed that the carbon concentration at the position where the solidification rate of the same silicon single crystal obtained in Example 1 was 80% was the same as that of the silicon wafer with a nitride film, and that it could be used to manufacture semiconductor devices without any problem.
[0098] (Example 2)
[0099] In Example 2, which was confirmed as an additional test, only silicon nitride powder (doping amount of silicon nitride powder was 26.452 g) was used as a nitrogen source to perform the curing process. The nitrogen atomic concentration at the position where the curing rate was 10% was 2×10 15 atoms / cm 3 The doping amount satisfies the formula (1): {upper limit [g] × (carbon impurity concentration in the silicon nitride powder [wt%] / 100) / carbon atomic weight [g / mol]} / silicon raw material addition amount [mol] ≤ 0.32 × 10 -6(1) The upper limit is below. At this time, the nitrogen concentration reaches the target value, and the carbon concentration can be kept below 0.05 ppma until the curing rate reaches 60%. In addition, although the carbon concentration at the curing rate of 80% is 0.09 ppma, which is greater than 0.05 ppma, it meets the low carbon concentration specification of 0.10 ppma or less generally required for semiconductor devices.
[0100] By comparing Example 1 and Example 2, it can be seen that although the low carbon concentration specification can be achieved by limiting the upper limit value in a manner that satisfies formula (1), a more stringent low carbon concentration specification can be met when the upper limit value is limited in a manner that satisfies formula (2) compared to the case where the upper limit value is limited in a manner that satisfies formula (1).
[0101] Therefore, in order to meet the low carbon concentration specifications of silicon wafers with high yield and low cost, when the amount of silicon nitride powder that can be used is calculated for the nitrogen atom concentration in the target silicon single crystal as shown in the present invention, and the amount of silicon nitride powder that can be used is insufficient to achieve the required nitrogen atom doping amount in the melt, it is preferred to dope silicon nitride powder with a silicon wafer with a high-purity nitride film as a nitrogen source.
[0102] (Example 3)
[0103] In Example 3, four silicon single crystals were pulled up in the same manner as in Example 1 except for the following points, and the same evaluation was performed.
[0104] In Example 3, the same amount of silicon nitride powder as that weighed in Example 1 is weighed using pharmaceutical weighing paper, the weighed silicon nitride powder is added to the bottom of the crucible, and then polycrystalline silicon is added as silicon raw material, melted, and a silicon single crystal is pulled.
[0105] The nitrogen concentration at the position where the solidification rate of the four silicon single crystals obtained in Example 3 was 10% as measured by SIMS was within the allowable range, but was lower than the nitrogen concentration of the corresponding four silicon single crystals obtained in Example 1.
[0106] In Example 3, the silicon nitride powder adhered to the pharmaceutical weighing paper during weighing, and a small amount of silicon nitride powder was scattered when added to the bottom of the crucible. Therefore, in Example 3, the actual amount of nitrogen doped was less than the amount of silicon nitride powder to be doped with the weighed amount.
[0107] In contrast, in Examples 1 and 2, the doping amount of the weighed silicon nitride powder is sufficiently consistent with the actual doping amount, that is, the deviation of the doping amount due to scattering or adhesion during weighing can be suppressed.
[0108] In addition, although the nitrogen doping amount achieved in Example 3 is lower than that in Example 1, it is within the allowable range as shown above. In addition, the nitrogen doping cost of Example 3 is the same as that of Example 1, which can significantly reduce the cost compared with Comparative Example 1. In addition, it is confirmed that the carbon concentration of the silicon single crystal obtained in Example 3 at the position where the solidification rate is 80% is the same as that of the silicon wafer with a nitride film, and it can be used to manufacture semiconductor devices without any problems. That is, even in Example 3, it is possible to achieve the target nitrogen doping amount at a low cost while achieving the low carbon concentration specification.
[0109] As described above, according to the present invention, the carbon impurity concentration brought by silicon nitride powder can be controlled within the allowable range, and a low-cost nitrogen doping method can be implemented. That is, according to the present invention, a method for manufacturing single crystal silicon that can achieve a target nitrogen doping amount at a low cost while achieving a low carbon concentration specification can be provided.
[0110] In addition, the present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are examples, and technical solutions having substantially the same structure and achieving the same technical effects as the technical concept described in the claims of the present invention are all included in the protection scope of the present invention.
Claims
1. A method for producing a silicon single crystal, comprising introducing silicon nitride powder into a raw material before melting begins and pulling a silicon single crystal doped with nitrogen by the Czochralski method, It is characterized in that Based on the amount of carbon impurities contained in the silicon nitride powder, the upper limit of the amount of silicon nitride powder that can be used is limited so that the carbon concentration in the silicon single crystal is below the allowable value, thereby doping with nitrogen. The upper limit amount of the silicon nitride powder is determined so as to satisfy the following formula (1): {the upper limit amount [g] × (carbon impurity concentration in the silicon nitride powder [wt%] / 100) / carbon atomic weight [g / mol]} / silicon raw material addition amount [mol] ≤ 0.32 × 10 -6 (1).
2. The method for producing a silicon single crystal according to claim 1, It is characterized in that The upper limit amount of the silicon nitride powder is determined so as to satisfy the following formula (2): {the upper limit amount [g] × (carbon impurity concentration in the silicon nitride powder [wt%] / 100) / carbon atomic weight [g / mol]} / silicon raw material addition amount [mol] ≤ 0.16 × 10 -6 (2).
3. The method for producing a silicon single crystal according to claim 1, It is characterized in that The upper limit amount of the silicon nitride powder is obtained based on an actual value of carbon concentration in a silicon single crystal produced by doping the silicon nitride powder.
4. The method for producing a silicon single crystal according to any one of claims 1 to 3, It is characterized in that When the upper limit is above the required nitrogen doping amount, only the silicon nitride powder is doped as a nitrogen source. When the upper limit is less than the required nitrogen doping amount, the missing nitrogen doping amount is supplemented by doping the raw material with the nitrogen doping amount using a silicon wafer with a high-purity nitride film.
5. The method for producing a silicon single crystal according to any one of claims 1 to 3, It is characterized in that The silicon nitride powder is weighed to an amount not exceeding the upper limit in a state where the silicon nitride powder is supported on a silicon wafer.
6. The method for producing a silicon single crystal according to claim 4, It is characterized in that The silicon nitride powder is weighed to an amount not exceeding the upper limit in a state where the silicon nitride powder is supported on a silicon wafer.
7. The method for producing a silicon single crystal according to claim 5, It is characterized in that The dopant is prepared by sandwiching the weighed silicon nitride powder between other silicon wafers, The dopant is added to the raw material before melting begins, thereby doping with nitrogen.
8. The method for producing a silicon single crystal according to claim 6, It is characterized in that The dopant is prepared by sandwiching the weighed silicon nitride powder between other silicon wafers, The dopant is added to the raw material before melting begins, thereby doping with nitrogen.
Citation Information
Patent Citations
Preparation of silicon single crystal
JP1985251190A
Method for manufacturing silicon single crystals
JP1993294780A
Built crystal substrate and liquid built crystal growing method
CN101118940A
Manufacturing method of epitaxial water and epitaxial wafer
CN108511317A
Method for measuring carbon concentration in monocrystalline silicon
CN110199057A