Silver electroplating composition and method for electroplating silver having a low coefficient of friction
By using a silver plating composition containing a silver ion source and a specific sulfide compound, the wear resistance and friction coefficient problems of the silver film are solved, and the deposition of a low friction coefficient and high durability silver layer is achieved, suitable for dense interconnection Electronic components connector.
Patent Information
- Application Number
- CN202210274957.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-03-29
- Filing Date
- 2022-03-21
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-03-21
AI Technical Summary
Silver films are highly susceptible to poor wear resistance, especially in connectors with repeated fit and separation cycles, resulting in adverse wear performance and their high coefficient of friction leads to pin failure in dense interconnections.
Silver electroplating compositions containing silver ion sources and specific sulfide compounds, such as HO(CH2)2-S-(CH2)2OH, are used to deposit silver without the use of lubricants, providing low coefficient of friction and improved Wear resistance, by co-deposition with sulfonated anionic polymer or its salt, and control the pH of the composition to be less than 7.
It is achieved without the use of lubricant, a high durable silver layer with a friction coefficient of 1 or less is deposited, significantly improving the wear resistance and cold welding resistance of the silver, and reducing wear and friction losses.
Abstract
Description
Technical Field
[0001] The present invention relates to silver electroplating compositions and methods for electroplating silver having a low coefficient of friction. More specifically, the present invention relates to silver electroplating compositions and methods for electroplating silver having a low coefficient of friction and improved wear resistance, and wherein the silver electroplating compositions are preferably free of cyanide. Background Art
[0002] Silver film is very susceptible to poor wear resistance due to low hardness, poor resistance to lateral displacement and significant degree of cold welding (wherein two silver contacts can be combined under use conditions to hinder removal). Poor wear performance is disadvantageous for connectors where repeated mating and separation cycles are required. In addition, as interconnection becomes denser and more refined, the force required for embedding and mating electronic components is proportional to the natural high friction coefficient of silver (COF is about 1.5). This may cause pin failure, especially when the pin becomes smaller and the spacing is denser. Despite these challenges, silver still has the potential to become a very attractive connector finish. Silver itself has one of the lowest contact resistance values among pure metals, and it is significantly cheaper than gold (dominant industrial substitute). Therefore, in order to effectively utilize silver, it is highly desirable to have a silver finish with low COF that is wear-resistant and cold-resistant.
[0003] Therefore, there is a need for a silver electroplating composition that is stable and deposits silver having a low coefficient of friction and improved wear resistance. Summary of the invention
[0004] The present invention relates to a silver electroplating composition comprising a silver ion source, a sulfide compound having the following formula:
[0005] HO(CH2)2-S-(CH2)2OH (I),
[0006] A sulfonated anionic polymer, a salt thereof, or a mixture thereof capable of co-depositing with silver to provide a silver deposit comprising a coefficient of friction of 1 or less without the use of a lubricant, and having a pH of less than 7.
[0007] The present invention also relates to a method for electroplating silver on a substrate, the method comprising:
[0008] a) providing a substrate;
[0009] b) contacting the substrate with a silver electroplating composition comprising a source of silver ions, a sulfide compound having the formula:
[0010] HO(CH2)2-S-(CH2)2OH (I),
[0011] a sulfonated anionic polymer, a salt thereof, or a mixture thereof capable of co-depositing with silver to provide a silver deposit comprising a coefficient of friction of 1 or less without the use of a lubricant, and a pH of less than 7; and
[0012] c) applying an electric current to the silver electroplating composition and the substrate to electroplate a silver deposit on the substrate.
[0013] The present invention further relates to an article comprising a silver layer adjacent to a surface of a substrate, wherein the silver layer comprises at least 99 metal basis % silver and has a coefficient of friction of 1 or less without the use of a lubricant. DETAILED DESCRIPTION
[0014] As used throughout the specification, the abbreviations have the following meanings unless the context clearly indicates otherwise: °C = degrees Celsius; g = gram; mg = milligram; L = liter; mL = milliliter; mm = millimeter; cm = centimeter; μm = micrometer; DI = deionized; A = ampere; ASD = ampere / dm 2 = plating speed; DC = direct current; N = Newton; COF = coefficient of friction; rpm = revolutions per minute; s = seconds; TDE = 2,2'-thiodiethanol; NSFC = naphthalenesulfonic acid formaldehyde condensate; and M n = Number average molecular weight.
[0015] The term "adjoining" means direct contact such that the two metal layers have a common interface. The abbreviation "N" means Newton, which is the SI unit of force and is equal to the force imparting an acceleration of 1 meter / second / second to a mass of 1 kilogram and is equal to 100,000 dynes. The term "coefficient of friction" is a value showing the relationship between the friction force between two objects and the normal force between the objects involved; and is mathematically given by COF=F 摩擦 / F 垂直 Indicates that F 摩擦 is the friction force, COF is the coefficient of friction, and F 垂直is the perpendicular or normal force, where the perpendicular or normal force is the force applied between the two articles perpendicular to the direction of relative motion between the two articles when the friction between the two articles is measured. The term "metal-based" means that no more than 0.1% of the product is trace metal, and the remainder is the product. The term "lubricant" refers to one or more additional compounds applied to the surface to reduce the COF (an example of a commonly used lubricant is octadecyl mercaptan). The term "tribology" means the science and engineering of surfaces that interact in relative motion, and includes the study and application of the principles of lubrication, friction and wear. The term "wear resistance" means the resistance to the loss of material from a surface by mechanical action. The term "minimum wear" means that for a length greater than 250 μm, the formation of a wear groove (material loss) is less than 10% of the width of the wear mark. The term "wear groove" is a depression in the silver layer having a profile depth greater than 1 / 3 of the local average thickness of the high-durability silver deposit, excluding the contact area directly subjected to the tribological measurement method. The term "local average thickness" means the thickness of the silver layer within a radius of 1000 μm around the edge of the wear groove. The term "cold welding" means a solid-state welding process in which a connection occurs without melting or heating at the interface of the two parts to be welded, and there is no molten liquid or molten phase at the joint. The term "aqueous" means water or water-based. Throughout the specification, the terms "composition" and "bath" are used interchangeably. Throughout the specification, the terms "deposit" and "layer" are used interchangeably. Throughout the specification, the terms "electroplating", "plating" and "deposition" are used interchangeably. The term "matte" means dull or without luster. Throughout the specification, the term "a / an" can refer to both the singular and the plural. Unless otherwise stated, all percentage (%) values and ranges indicate weight percentages. All numerical ranges are inclusive and can be combined in any order, except that it is logical for this numerical range to be limited to add up to 100%.
[0016] The present invention relates to a silver electroplating composition comprising a silver ion source, a sulfide compound having the following formula:
[0017] HO(CH2)2-S-(CH2)2OH(I),
[0018] Sulfonated anionic polymers, salts thereof, or mixtures thereof capable of co-depositing with silver to provide a silver deposit comprising a coefficient of friction of 1 or less without a lubricant, and a pH of less than 7. Sulfonated anionic polymers capable of co-depositing with silver to provide a silver deposit comprising a coefficient of friction of 1 or less include, but are not limited to, naphthalenesulfonic acid formaldehyde condensates and poly-acrylic acid-co-vinyl sulfonic acid. Salts include, but are not limited to, sodium salts of naphthalenesulfonic acid formaldehyde condensates and sodium salts of polyacrylic acid-co-vinyl sulfonic acid.
[0019] Preferably, the silver electroplating composition of the present invention comprises HO(CH2)2-S-(CH2)2OH(I) or thiodiethanol in combination with one or more of naphthalenesulfonic acid formaldehyde condensate and poly-acrylic acid-co-vinylsulfonic acid and salts thereof, to enable electroplating of a high durability silver deposit on a substrate with a coefficient of friction (COF) of 1 or less without a lubricant. More preferably, the silver electroplating composition of the present invention comprises thiodiethanol in combination with naphthalenesulfonic acid formaldehyde condensate and salts thereof. Preferably, the silver electroplating composition does not contain cyanide.
[0020] The sulfide is included in the silver electroplating composition in an amount of preferably 10-300 g / L, more preferably 20-275 g / L, even more preferably 35-200 g / L.
[0021] Naphthalenesulfonic acid formaldehyde condensate and poly-acrylic acid-co-vinylsulfonic acid and salts thereof are contained in the silver electroplating composition in an amount of preferably 2-100 g / L, more preferably 2-35 g / L, even more preferably 2-25 g / L.
[0022] The aqueous acidic silver electroplating composition of the present invention comprises a silver ion source. The silver ion source can be provided by a silver salt, such as but not limited to silver halide, silver gluconate, silver citrate, silver lactate, silver nitrate, silver sulfate, silver alkane sulfonate, silver alkanol sulfonate or a mixture thereof. When a silver halide is used, preferably the halide is a chloride. Preferably, the silver salt is silver sulfate, silver alkane sulfonate, silver nitrate, or a mixture thereof, more preferably, the silver salt is silver sulfate, silver methane sulfonate, or a mixture thereof. Silver salts are generally commercially available or can be prepared by methods described in the literature. Preferably, the silver salt is readily soluble in water. Preferably, the silver salt is included in the composition to provide a silver ion concentration of at least 10 g / L, more preferably, the silver salt is included in the composition in an amount to provide a silver ion concentration of 10 g / L to 100 g / L, further preferably, the silver salt is included in the composition in an amount to provide a silver ion concentration of 20 g / L to 80 g / L, even more preferably, the silver salt is included in the composition in an amount to provide a silver ion concentration of 20 g / L to 60 g / L, and most preferably, the silver salt is included in the composition in an amount to provide a silver ion concentration of 30 g / L to 60 g / L.
[0023] Optionally, the silver electroplating composition of the present invention may contain an acid. Such acids include, but are not limited to, organic acids such as acetic acid, citric acid, malonic acid, arylsulfonic acid, alkanesulfonic acid (such as methanesulfonic acid, ethanesulfonic acid and propanesulfonic acid), arylsulfonic acid (such as benzenesulfonic acid, toluenesulfonic acid, 5-sulfosalicylic acid); and inorganic acids such as sulfuric acid, aminosulfonic acid, hydrochloric acid, phosphoric acid, hydrobromic acid and fluoroboric acid. Water-soluble salts of the aforementioned acids may also be included in the silver electroplating composition of the present invention. Preferably, the acid is acetic acid, citric acid, 5-sulfosalicylic acid, alkanesulfonic acid, arylsulfonic acid, aminosulfonic acid or its salt, and more preferably, the acid is acetic acid, citric acid, methanesulfonic acid, aminosulfonic acid or its salt. Most preferably, the acid is methanesulfonic acid. Such salts include, but are not limited to, methanesulfonates, sulfamates, citrates, sodium and potassium salts of acids (such as sodium acetate and potassium acetate, disodium hydrogen citrate, sodium dihydrogen citrate, trisodium citrate, tripotassium citrate, dipotassium citrate, dipotassium hydrogen citrate and potassium dihydrogen citrate). Most preferably, the salt is sodium methanesulfonate or potassium methanesulfonate. A mixture of acids can be used. Acids are generally commercially available or can be prepared by methods known in the literature. Such acids can be included in an amount that provides a desired conductivity and pH.
[0024] Preferably, the acid or salt thereof is included in an amount of at least 5 g / L, more preferably from 10 g / L to 250 g / L, even more preferably from 30 g / L to 150 g / L, most preferably from 30 g / l to 125 g / L.
[0025] Optionally, inorganic bases such as sodium hydroxide and potassium hydroxide and organic bases such as various types of amines can be used to adjust the pH of the silver electroplating composition of the present invention. Preferably, the alkaline pH regulator is selected from potassium hydroxide or sodium hydroxide. The pH regulator can be added in an amount required to maintain the desired pH range.
[0026] The pH of the silver electroplating composition is less than 7. Preferably, the pH is 0 to 6.5, more preferably, the pH is 0 to 6, even more preferably, the pH is 0 to 5, and most preferably, the pH is 0 to 3.
[0027] Optionally, the silver electroplating composition of the present invention comprises one or more grain refiners. Preferably, the grain refiner is a thiol compound. Such thiol compounds include, but are not limited to, thiol compounds selected from one or more of the following: thiomalic acid, 2-mercaptosuccinic acid, 3-mercapto-1-propanesulfonic acid, 1-[2-(dimethylamino)ethyl]-1H-tetrazole-5-thiol, and salts thereof. Salts of thiol compounds include, but are not limited to, alkali metal salts such as sodium, potassium, lithium, and cesium; ammonium salts; and tetraalkylammonium salts. Preferably, the thiol compound is selected from one or more of 2-mercaptosuccinic acid, 3-mercapto-1-propanesulfonic acid, and 3-mercapto-1-sodium propanesulfonate. More preferably, the thiol compound is selected from one or more of 2-mercaptosuccinic acid and 3-mercapto-1-sodium propanesulfonate, and most preferably, the thiol compound is 2-mercaptosuccinic acid.
[0028] Preferably, the grain refiner is included in an amount of 5 g / L or more, more preferably, the thiol compound is included in an amount of 10 g / L to 100 g / L, further preferably 15 g / L to 90 g / L, even more preferably 20 g / L to 90 g / L, most preferably 30 g / L to 90 g / L.
[0029] Optionally, the silver electroplating composition of the present invention may contain one or more brighteners. Such brighteners include, but are not limited to, amines such as alkyl, alkylene, alkyl alcohol, alkanol or alkylaryl amines, and alkylene polyamines and polyalkylene polyimines, as disclosed in US 4,246,077; heterocyclic nitrogen compounds such as 4-amino-1,2,4-triazole; and sulfonate-containing brighteners such as aminosulfonic acid, 5-sulfosalicylic acid, 3-(1-pyridyl)-1-propanesulfonate and naphthalenetrisulfonic acid.
[0030] Nickel salts can also be included in aqueous acidic silver electroplating compositions in an amount sufficient to provide a desired bright and uniform silver deposit. Such nickel brighteners are substantially not incorporated into silver, so that binary alloys are deposited. Nickel ion sources include, but are not limited to, nickel sulfate and nickel sulfate hexahydrate and nickel sulfate heptahydrate, nickel sulfamate and nickel sulfamate tetrahydrate nickel sulfamate, nickel chloride and nickel chloride hexahydrate, nickel acetate and nickel acetate tetrahydrate, nickel nitrate, nickel nitrate hexahydrate, and mixtures thereof. More preferably, the nickel ion source is nickel sulfamate and nickel sulfamate tetrahydrate nickel sulfamate, and most preferably, the nickel ion source is nickel sulfamate. Such nickel salts are commercially available, or can be prepared by methods well known in the art.
[0031] Preferably, when brighteners are included in the silver electroplating composition, they are provided in an amount of 50 mg / L to 20 g / L, more preferably 100 mg / L to 10 g / L.
[0032] Preferably, in the aqueous acidic silver electroplating composition of the present invention, water included as a solvent is at least one of deionized water and distilled water to limit incidental impurities.
[0033] Optionally, one or more surfactants may be included in the silver electroplating composition of the present invention. Such surfactants include, but are not limited to, ionic surfactants, such as cationic and anionic surfactants, nonionic surfactants, and amphoteric surfactants. The surfactant may be included in conventional amounts such as 0.05 g / L to 30 g / L.
[0034] Examples of anionic surfactants are sodium di(1,3-dimethylbutyl)sulfosuccinate, sodium 2-ethylhexyl sulfate, sodium diamylsulfosuccinate, sodium lauryl sulfate, sodium lauryl ether sulfate, sodium dialkylsulfosuccinate and sodium dodecylbenzenesulfonate. Examples of cationic surfactants are quaternary ammonium salts, such as perfluorinated quaternary amines.
[0035] Other optional additives may include, but are not limited to, levelers and biocides.Such optional additives may be included in conventional amounts.
[0036] Preferably, the silver electroplating composition consists of water, one or more sources of silver ions, a counter anion, thiodiethanol, a compound selected from the group consisting of naphthalenesulfonic acid formaldehyde condensate, poly-acrylic acid-co-vinylsulfonic acid, salts thereof and mixtures thereof, optionally an acid, optionally a base, optionally a brightener, optionally a grain refiner, optionally a surfactant, optionally a leveling agent, optionally a biocide, and has a pH of less than 7.
[0037] More preferably, the silver electroplating composition consists of water, one or more silver ion sources, a counter anion, thiodiethanol, naphthalenesulfonic acid formaldehyde condensate or its salt, an acid, a grain refiner, optionally a base, optionally a brightener, optionally a surfactant, optionally a leveling agent, optionally a biocide, and has a pH of 0-6.
[0038] The silver electroplating composition of the present invention can be used to deposit a silver layer on a variety of substrates. Preferably, the substrate on which the silver layer is deposited is a nickel, copper and copper alloy substrate. Such copper alloy substrates include, but are not limited to, brass and bronze. More preferably, silver is deposited adjacent to nickel, wherein the nickel layer is adjacent to copper or copper alloy. When the substrate contains a nickel layer, a silver strike layer is first deposited adjacent to the nickel. The thickness range of the strike layer is 0.01-1 μm, preferably 0.05-0.4 μm. Then the silver layer from the plating composition of the present invention is plated adjacent to the strike layer. During plating, the electroplating composition temperature can be from room temperature to 70°C, preferably 30°C to 60°C, more preferably 40°C to 60°C. During electroplating, the silver electroplating composition is preferably under continuous stirring.
[0039] The silver electroplating method of the present invention comprises providing a substrate, providing a silver electroplating composition of the present invention, and contacting the substrate with the silver electroplating composition, such as by immersing the substrate in the composition or spraying the substrate with the composition. An electric current is applied with a conventional rectifier, wherein the substrate serves as a cathode, and a counter electrode or anode is present. The anode can be any conventional soluble or insoluble anode used for electroplating high durability silver to deposit adjacent to the surface of the substrate.
[0040] The current density for electroplating uniform high-durability silver may be 0.1 ASD or higher. Preferably, the current density ranges from 0.5 ASD to 25 ASD, and more preferably, from 1 ASD to 20 ASD.
[0041] The silver electroplating composition of the present invention enables the deposition of semi-bright to bright and uniform high durability silver layers. The silver content of the deposit is greater than or equal to 99% silver on a metal basis, excluding unavoidable impurities in the deposit.
[0042] The thickness of the silver layer of the present invention can vary depending on the function of the silver layer and the type of substrate plated thereon. Preferably, the range of the silver layer is 0.1 μm or greater. Further preferably, the silver layer has a thickness range of 0.1 μm to 100 μm, more preferably 0.5 μm to 50 μm, even more preferably 1 μm to 10 μm, most preferably 2 μm to 6 μm. The thickness can be measured by conventional methods known to those skilled in the art. For example, the thickness of the silver layer can be measured using a Bowman Series P X-ray fluorimeter (XRF) available from Bowman, Schaumburg, IL. The XRF can be calibrated using a pure silver thickness standard from Bowman.
[0043] The high durability silver deposit has a coefficient of friction (COF) of 1 or less, preferably a COF of 0.1-1, more preferably 0.15-0.5, even more preferably 0.2-0.45, most preferably a COF of 0.25-0.45. The COF can be determined by conventional tribological methods and apparatus known to those skilled in the art. For example, tribological testing can be performed in a linear mode configuration using an Anton PaarTRB3 pin-on-disc tribometer (available from Anton Paar GmbH, Graz, Austria) equipped with a linear reciprocating stage. No lubricant or chemical post-treatment is required on the electroplated silver deposit. A vertical force of 1-5N is applied to each tribological measurement, and the coefficient of friction is determined using conventional tribometer software and apparatus. The tribometer software can mathematically determine the COF (μ) based on the ratio between the applied vertical or normal force (1-5N) and the measured friction force required to move the load-bearing object (cap) at a set speed. The mathematical expression is COF=F摩擦 / F 垂直 .
[0044] The high durability silver deposit has minimal wear, as determined by using a wear scar depth profile measured using laser profilometry to determine the extent of wear. Conventional laser profilometry known to those skilled in the art can be used. For example, profilometry measurements can be made using a Keyence VK-X laser scanning confocal microscope (available from Keyence Corporation of America, Elmwood Park, NJ). Wear scars can be measured using laser profilometry at a magnification of 50 to 100X.
[0045] The carbon content of the high durability silver of the present invention is greater than or equal to 0.1 mass basis % of the silver deposit, but not greater than 5 mass basis % of the silver deposit, excluding particles having a crystal domain size greater than 100 nm in diameter. Crystal domain refers to coherent crystals or grains, which are interchangeable terms. Preferably, the carbon content of the high durability silver of the present invention is 0.5-3.5 mass % carbon, more preferably 1-3 mass % carbon. Carbon particles, such as graphite or other carbon allotropes and their oxidized forms, are not used in the silver electroplating composition, eliminating any hazards associated with the use of small particles. The carbon content in the wear-resistant silver deposit can be determined by conventional methods known in the art. The determination of the carbon content can be achieved by burning a sample of the plated silver deposit on a platinum wire at about 1200° C. in an oxygen stream. The resulting carbon dioxide is determined by infrared spectroscopy according to DIN EN ISO 15350:2010 (conventional methods known in the art).
[0046] The following examples are included to further illustrate the invention but are not intended to limit the scope thereof.
[0047] Silver plating examples 1-20:
[0048] Unless otherwise stated, the electroplated substrates were flat phosphor bronze (alloy C51100) coupons with dimensions of 1.25 cm x 2.5 cm or C26000 brass coupons (70% copper, 30% zinc) with dimensions of 2.5 cm x 3.5 cm. The choice of substrate between C51100 and C2600 did not significantly affect the tribological results and were used interchangeably in the following examples. The tribological moving wear partner was a hemispherical phosphor bronze substrate (C51100) with a diameter of 0.7 cm and the diameter of the flat substrate was 0.9 cm. Prior to electroplating, the coupons were placed in a RONACLEAN TMElectrocleaning was performed in DLF electrolytic alkaline degreaser (available from DuPont deNemours) with cathodic DC at a current density of 4 ASD at 50°C for 30 seconds. In this configuration, stainless steel was used as the anode. After electrocleaning, the coupons were rinsed with DI water, activated in a 40 g / L sodium persulfate and 1% sulfuric acid solution for 30 seconds, rinsed with DI water, then further activated in 10% sulfuric acid for 20 seconds, rinsed again with DI water, and then placed in the electroplating bath. For plating on brass substrates, no persulfate activation was performed. Unless otherwise noted, prior to silver plating, NIKAL TM SC electrolytic nickel (obtainable by Dupont Nemours) nickel plating bath is coated with a nickel layer of at least 2 μm thick. Nickel anode is used to electroplate nickel in a square glass beaker with a current density of 4ASD with DC for 4 minutes. Stirring is provided by a 5 cm long, TEFLON coated stirring rod with a rotation rate of 400 rpm and a solution volume of about 400 mL. Electroplating is carried out at a temperature of 50 ° C. After nickel deposition, the substrate is washed with DI water. If a nickel layer is deposited, a silver primer is subsequently plated. In the absence of nickel, silver is plated without plating a silver primer. A primer bath consisting of 1 g / L silver metal, 9.3 g / L 2,2'-thiodiethanol and 18 g / L methanesulfonic acid solution from silver methanesulfonate is used to deposit a silver primer. A DC current density of 2ASD is applied in a glass beaker with a platinized titanium anode for 15 seconds. A charged or hot entry technique is used, in which the substrate is introduced into the bath under polarization, wherein the limiting voltage is set to about 0.05-01 volts higher than the cell potential required to plate the substrate at the desired current density. The bath is stirred with a 5 cm long, TEFLON coated stirring rod at a rotation rate of 400 rpm. The primer bath is operated at 22°C-27°C. After a primer deposition of 0.05-0.4 μm, silver is electrodeposited using the charged entry technique as described above without a rinse step. Silver is deposited in a square glass beaker using the same stirring and solution volume conditions as above. The silver bath is operated with a DC of 2-4 ASD using a silver anode. Electroplating is carried out at a temperature of 40°C-60°C. The plating time is adjusted to obtain a 2-6 μm thick silver deposit. After plating, the specimen is then rinsed with DI water and dried using compressed air. All silver electroplating baths are water-based. Thus, water is added to each bath to bring it to the desired volume. The pH of the silver electroplating bath is adjusted with potassium hydroxide or methanesulfonic acid.
[0049] The thickness of the electroplated silver was measured using a Bowman Series P X-ray fluorimeter (XRF) available from Bowman Corporation, Schaumburg, Ill. The XRF was calibrated using a pure silver thickness standard from Bowman Corporation.
[0050] For example, tribological tests were performed using an Anton Paar TRB3 pin-on-disc tribometer (available from Anton Paar, Graz, Austria) equipped with a linear reciprocating stage in a linear mode configuration. No lubricant or chemical post-treatment was applied to the electroplated silver deposit. A flat specimen was used as a static partner for the tribological measurements. The moving wear partner plated with silver had a hemispherical cap geometry with a spherical diameter of 0.7 cm. All tests were performed "like-on-like," meaning that the flat specimen and the cap were each plated with the same silver metal deposit under identical conditions. A vertical force of 1-5 N was applied to each tribological measurement, and the coefficient of friction was recorded. The tribometer software Anton Paar Instrum X version 8.1.5 was used to mathematically determine the COF (μ) based on the ratio between the applied vertical or normal force (1-5 N) and the measured friction force required to move the load-bearing object (cap) at a set speed. The mathematical expression is COF=F 摩擦 / F 垂直 The mobile partner was programmed to oscillate linearly on a static flat substrate with an amplitude of 1 cm at a maximum linear velocity of 1 cm / s. Linear cycles were repeated between 500 and 10,000 to simulate accelerated contact wear on plated parts.
[0051] After the tribological measurements, the resulting wear scar depth profiles were measured using laser profilometry to determine the extent of wear. Profilometry measurements were performed using a Keyence VK-X laser scanning confocal microscope (available from Keyence Corporation, Elmwood Park, NJ, USA). Wear scars were measured using laser profilometry at a magnification of 50 to 100X.
[0052] The carbon content of some of the following examples was determined using the DIN EN ISO 15350:2000 standard method which is well known in the art.
[0053] Example 1 (the present invention)
[0054] A mercury-containing electroplating bath having the following composition was prepared and tested under the following tribological conditions:
[0055] Silver methanesulfonate that supplies 20g / L of silver ions
[0056] 2,2'-Thiodiethanol (TDE): 40g / L
[0057] Naphthalenesulfonic acid formaldehyde condensate (NSFC): 20g / L
[0058] Adjust pH to 1
[0059] Friction force measurement: 1N, 500 cycles
[0060] After electroplating at 45°C, the electrodeposited coating looked metallic and semi-bright. The coefficient of friction of the silver deposit was measured to be about 0.45. The silver deposit did not wear through to the substrate on the wear mark and was essentially flat relative to the background baseline.
[0061] Example 2 (the present invention)
[0062] A mercury-containing electroplating bath having the following composition was prepared and tested under the following tribological conditions:
[0063] Silver methanesulfonate supplying 40g / L of silver ions
[0064] 2,2'-Thiodiethanol: 180g / L
[0065] Naphthalenesulfonic acid formaldehyde condensate: 8g / L
[0066] Methanesulfonic acid: 47.3g / L
[0067] pH about 3
[0068] Friction force measurement: 2N, 10,000 cycles
[0069] After electroplating at 55°C, the electrodeposited coating looked metallic and semi-bright. The coefficient of friction of the silver deposit was measured to be about 0.45. The silver deposit did not wear through to the substrate on the wear mark and was essentially flat against the background baseline.
[0070] Example 3 (the present invention)
[0071] A mercury-containing electroplating bath having the following composition was prepared and tested under the following tribological conditions:
[0072] Silver methanesulfonate supplying 60g / L of silver ions
[0073] 2,2'-Thiodiethanol: 272g / L
[0074] Naphthalenesulfonic acid formaldehyde condensate: 8g / L
[0075] Methanesulfonic acid: 94.5g / L
[0076] pH about 0
[0077] Friction force measurement: 4N, 500 cycles
[0078] Wt% Carbon: Approx. 1.5
[0079] After electroplating at 55°C, the electrodeposited coating looked metallic and semi-bright. The coefficient of friction of the silver deposit was measured to be about 0.45. The silver deposit did not wear through to the substrate on the wear mark and was essentially flat against the background baseline.
[0080] Example 4 (the present invention)
[0081] A mercury-containing electroplating bath having the following composition was prepared and tested under the following tribological conditions:
[0082] Silver methanesulfonate supplying 40g / L of silver ions
[0083] 2,2'-Thiodiethanol: 136g / L
[0084] Naphthalenesulfonic acid formaldehyde condensate: 8g / L
[0085] Methanesulfonic acid: 94.5g / L
[0086] pH about 0
[0087] Friction force measurement: 4N, 500 cycles
[0088] Wt% Carbon: Approx. 1.8
[0089] After electroplating at 55°C, the electrodeposited coating looked metallic and semi-bright. The coefficient of friction of the silver deposit was measured to be about 0.35. The silver deposit did not wear through to the substrate on the wear mark and was essentially flat against the background baseline.
[0090] Example 5 (the present invention)
[0091] A mercury-containing electroplating bath having the following composition was prepared and tested under the following tribological conditions:
[0092] Silver methanesulfonate supplying 40g / L of silver ions
[0093] 2,2'-Thiodiethanol: 272g / L
[0094] Naphthalenesulfonic acid formaldehyde condensate: 8g / L
[0095] Methanesulfonic acid: 94.5g / L
[0096] pH about 0
[0097] Friction force measurement: 4N, 500 cycles
[0098] After electroplating at 55°C, the electrodeposited coating looked metallic and semi-bright. The coefficient of friction of the silver deposit was measured to be about 0.25. The silver deposit did not wear through to the substrate on the wear mark and was essentially flat against the background baseline.
[0099] Example 6 (present invention)
[0100] A mercury-containing electroplating bath having the following composition was prepared and tested under the following tribological conditions:
[0101] Silver methanesulfonate that supplies 20g / L of silver ions
[0102] 2,2'-Thiodiethanol: 68g / L
[0103] Naphthalenesulfonic acid formaldehyde condensate: 2.5g / L
[0104] Adjust pH to 2.3
[0105] Friction force measurement: 2N, 1000 cycles
[0106] Wt% Carbon: Approx. 2.5
[0107] After electroplating at 45°C, the electrodeposited coating looked metallic and bright. The measured coefficient of friction of the silver deposit was about 0.4. The silver deposit did not wear through to the substrate on the wear mark and was essentially flat against the background baseline.
[0108] Example 7 (present invention)
[0109] A mercury-containing electroplating bath having the following composition was prepared and tested under the following tribological conditions:
[0110] Silver methanesulfonate supplying 40g / L of silver ions
[0111] 2,2'-Thiodiethanol: 180g / L
[0112] Naphthalenesulfonic acid formaldehyde condensate: 32g / L
[0113] Methanesulfonic acid: 47.3g / L
[0114] pH about 0.3
[0115] Friction force measurement: 4N, 500 cycles
[0116] After electroplating at 55°C, the electrodeposited coating looked metallic and semi-bright. The coefficient of friction of the silver deposit was measured to be about 0.45. The silver deposit did not wear through to the substrate on the wear mark and was essentially flat against the background baseline.
[0117] Example 8 (present invention)
[0118] A mercury-containing electroplating bath having the following composition was prepared and tested under the following tribological conditions:
[0119] Silver methanesulfonate that supplies 20g / L of silver ions
[0120] 2,2'-Thiodiethanol: 68g / L
[0121] Naphthalenesulfonic acid formaldehyde condensate: 2.5g / L
[0122] Aminosulfonic acid: 5g / L
[0123] Potassium methanesulfonate: 30g / L
[0124] Adjust pH to 2
[0125] Friction force measurement: 2N, 1000 cycles
[0126] After electroplating at 45°C, the electrodeposited coating looked metallic and bright. The measured coefficient of friction of the silver deposit was about 0.3. The silver deposit did not wear through to the substrate on the wear mark and was essentially flat relative to the background baseline.
[0127] Example 9 (present invention)
[0128] A mercury-containing electroplating bath having the following composition was prepared and tested under the following tribological conditions:
[0129] Silver methanesulfonate that supplies 20g / L of silver ions
[0130] 2,2'-Thiodiethanol: 68g / L
[0131] Naphthalenesulfonic acid formaldehyde condensate: 2.5g / L
[0132] Nickel methanesulfonate that supplies 5g / L of nickel ions
[0133] Aminosulfonic acid: 1g / L
[0134] Potassium methanesulfonate: 30g / L
[0135] Adjust pH to 2.5
[0136] Friction force measurement: 2N, 1000 cycles
[0137] After electroplating at 45°C, the electrodeposited coating looked metallic and bright. The measured coefficient of friction of the silver deposit was about 0.3. The silver deposit did not wear through to the substrate on the wear mark and was essentially flat relative to the background baseline.
[0138] Example 10 (present invention)
[0139] A mercury-containing electroplating bath having the following composition was prepared and tested under the following tribological conditions:
[0140] Silver methanesulfonate that supplies 20g / L of silver ions
[0141] 2,2'-Thiodiethanol: 50g / L
[0142] Naphthalenesulfonic acid formaldehyde condensate: 20g / L
[0143] 5-Sulfosalicylic acid: 10g / L
[0144] Adjust pH to 1
[0145] Friction force measurement: 2N, 1000 cycles
[0146] After electroplating at 40°C, the electrodeposited coating looked metallic and semi-bright. The measured coefficient of friction of the silver deposit was about 0.3. The silver deposit did not wear through to the substrate on the wear mark and was slightly elevated relative to the background baseline.
[0147] Example 11 (present invention)
[0148] A mercury-containing electroplating bath having the following composition was prepared and tested under the following tribological conditions:
[0149] Silver methanesulfonate that supplies 20g / L of silver ions
[0150] 2,2'-Thiodiethanol: 68g / L
[0151] Naphthalenesulfonic acid formaldehyde condensate: 2.5g / L
[0152] Nickel methanesulfonate that supplies 5g / L of nickel ions
[0153] 5-Sulfosalicylic acid: 1g / L
[0154] Adjust pH to 2
[0155] Friction force measurement: 5N, 10,000 cycles
[0156] After electroplating at 45°C, the electrodeposited coating looked metallic and bright. The coefficient of friction of the silver deposit was measured to be about 0.35. The silver deposit did not wear through to the substrate on the wear mark and was essentially flat relative to the background baseline.
[0157] Example 12 (present invention)
[0158] A mercury-containing electroplating bath having the following composition was prepared and tested under the following tribological conditions:
[0159] Silver methanesulfonate that supplies 20g / L of silver ions
[0160] 2,2'-Thiodiethanol: 74g / L
[0161] Poly-acrylic acid-co-vinyl sulfonic acid: 10g / L
[0162] Adjust pH to 2.7
[0163] Friction force measurement: 1N, 500 cycles
[0164] After electroplating at 55°C, the electrodeposited coating looked metallic and semi-bright. No nickel layer was plated. The measured coefficient of friction of the silver deposit was about 0.5. The silver deposit did not wear through to the substrate on the wear mark and was essentially flat relative to the background baseline.
[0165] Example 13 (Comparison)
[0166] A mercury-containing electroplating bath having the following composition was prepared and tested under the following tribological conditions:
[0167] Silver methanesulfonate that supplies 20g / L of silver ions
[0168] 2,2'-Thiodiethanol: 113g / L
[0169] Polyvinyl sulfonic acid: 10g / L
[0170] Methanesulfonic acid: 47.3g / L
[0171] pH about 0.3
[0172] Friction force measurement: 1N, 500 cycles
[0173] After electroplating at 55°C, the electrodeposited coating appeared matte white. No nickel layer was plated. The coefficient of friction of the silver deposit was measured to be about 1.6. The silver deposit showed partial wear of the silver at the wear track, with the worn area showing a depth of 2-4 μm relative to the background baseline.
[0174] Example 14 (Comparison)
[0175] A mercury-containing electroplating bath having the following composition was prepared:
[0176] Silver methanesulfonate that supplies 20g / L of silver ions
[0177] 2,2'-Thiodiethanol: 50g / L
[0178] Naphthalenetrisulfonic acid sodium salt: 10g / L
[0179] Adjust pH to 1.5
[0180] After electroplating at 40°C, the electrodeposited coating appeared very rough, dark brown and brittle. The deposit was not suitable for wear testing.
[0181] Example 15 (Comparison)
[0182] A mercury-containing electroplating bath having the following composition was prepared:
[0183] Silver methanesulfonate that supplies 20g / L of silver ions
[0184] 2,2'-Thiodiethanol: 68g / L
[0185] Sodium polystyrene sulfonate (M n About 70k): 8g / L
[0186] Methanesulfonic acid: 47.5g / L
[0187] pH about 0.3
[0188] After electroplating at 55°C, the electrodeposited coating appeared very rough, grey and brittle. No nickel layer was plated. The deposit was not suitable for wear testing.
[0189] Example 16 (Comparison)
[0190] A mercury-containing electroplating bath having the following composition was prepared and tested under the following tribological conditions:
[0191] Silver methanesulfonate that supplies 20g / L of silver ions
[0192] 2,2'-Thiodiethanol: 27g / L
[0193] 5-Sulfosalicylic acid: 15g / L
[0194] Adjust pH to 1
[0195] Friction force measurement: 1N, 500 cycles
[0196] After electroplating at 40°C, the electrodeposited coating appeared matte brown and white. No nickel layer was plated. The deposit wore through to the substrate within a few cycles, demonstrating poor wear resistance.
[0197] Example 17 (Comparison)
[0198] A mercury-containing electroplating bath having the following composition was prepared:
[0199] Silver methanesulfonate that supplies 20g / L of silver ions
[0200] 2,2'-Thiodiethanol: 45g / L
[0201] Ethylenediaminetetra(propoxylate-block-ethoxylate)tetraol (M n About 3600): 10g / L
[0202] Adjust pH to 1
[0203] After electroplating at 40°C, the electrodeposited coating appeared very rough, brown and brittle. No nickel layer was plated. The deposit was not suitable for wear testing.
[0204] Example 18 (Comparison)
[0205] A mercury-containing electroplating bath having the following composition was prepared:
[0206] Silver methanesulfonate that supplies 20g / L of silver ions
[0207] 2,2'-Thiodiethanol: 27g / L
[0208] Polymethacrylic acid: 5g / L
[0209] Adjust pH to 1
[0210] After electroplating at 40°C, the electrodeposited coating appeared very rough, black and brittle. No nickel layer was plated. The deposit was not suitable for wear testing.
[0211] Example 19 (Comparison)
[0212] A mercury-containing electroplating bath having the following composition was prepared:
[0213] Silver methanesulfonate that supplies 20g / L of silver ions
[0214] 2,2'-Thiodiethanol: 27g / L
[0215] Polyvinyl pyrrolidone: 15g / L
[0216] Adjust pH to 1.5
[0217] The contents of the bath were not completely soluble. After electroplating at 40°C, the electrodeposited coating appeared grey. No nickel layer was plated. The deposit was not suitable for wear testing.
[0218] Example 20 (Comparison)
[0219] A mercury-containing electroplating bath having the following composition was prepared and tested under the following tribological conditions:
[0220] Silver methanesulfonate that supplies 20g / L of silver ions
[0221] 3,6-dithia-1,8-octanediol: 101.4 g / L
[0222] Naphthalenesulfonic acid formaldehyde condensate: 10g / L
[0223] Adjust pH to 2.1
[0224] Friction force measurement: 1N, 500 cycles
[0225] After electroplating at 50°C, the electrodeposited coating appeared matte grey and white. No nickel layer was plated. The deposit wore through to the substrate within a few cycles, demonstrating poor wear resistance.
[0226] Example 21 (Comparison)
[0227] Wear resistance of standard silver
[0228] Standard silver wear performance uses as a benchmark the deposit produced by an alkaline silver cyanide bath comprising 33 g / L silver ions from silver cyanide, 113 g / L potassium cyanide, conventional plating additives for alkaline silver cyanide plating baths at pH=12. The silver plating bath does not include TDE or NSFC. Instead of using a hemispherical cap, the mobile wear partner is a ball made of C26000 brass (70% copper, 30% zinc) with a diameter of 5.55 mm. According to the above procedure, after electrolytic cleaning and sulfuric acid activation, the ball is electroplated directly on the substrate with about 5 μm of silver. The flat coupon is also made of C26000 brass and is electroplated with about 5 μm of silver.
[0229] Silver was deposited on the substrate in a glass square beaker. A 400 mL bath was stirred at a rotation rate of 400 rpm with a 5 cm long, TEFLON coated stirring rod. The silver bath was operated with cathode DC at the current density specified above using a platinized titanium anode. The electroplating was carried out at a temperature of 40° C. The plating time was adjusted to obtain a silver deposit of approximately 5 μm thick. After plating, the specimen was then rinsed with DI water and dried using compressed air.
[0230] The tribological tests were performed using the same instrument and similar procedures as previously described. Likewise, no lubricant or chemical post-treatment was applied to the silver deposit after plating. The tests were performed using a 1 N load, a stroke length of 1 cm, and a sliding speed of 0.5 cm / s. The tests were performed in a "like-for-like" manner, which means that the flat specimen and the spherical ball were each plated with the same silver metal deposit produced by the same electroplating bath. During the test, the friction coefficient was monitored using a tribometer, and the wear scar depth was measured using a laser profilometry method afterwards. 100 linear cycles under a 1 N force were all required to break through the silver plated deposit onto the substrate, while showing a friction coefficient of approximately 1.6.
[0231] Example 22 (Comparison)
[0232] Standard Silver Carbon Content
[0233] The substrate was a flat stainless steel coupon with dimensions of 1.25 cm x 2.5 cm. Prior to electroplating, the coupon was TM Electrocleaning was performed in DLF electrolytic alkaline degreaser (available from Dupont Nemours) with cathodic DC at a current density of 4 ASD at 50°C for 30 seconds. In this configuration, stainless steel was used as the anode. After electrocleaning, the coupons were rinsed with DI water, activated in a 40 g / L sodium persulfate and 1% sulfuric acid solution for 30 seconds, rinsed with DI water, then further activated in 10% sulfuric acid for 20 seconds, rinsed again with DI water, and then silver plated in a square glass beaker containing a conventional alkaline silver cyanide bath.
[0234] The alkaline silver cyanide bath contained 33 g / L silver ions from silver cyanide, 113 g / L potassium cyanide, and conventional plating additives for alkaline silver cyanide plating baths at pH = 12. The silver cyanide electroplating bath did not include TDE or NSFC.
[0235] The bath was stirred with a 5 cm long, TEFLON coated stirring rod at a rotation rate of 400 rpm. The silver bath was operated with cathode DC at a current density of 2-4 ASD using a silver anode. The electroplating was carried out at a temperature of 40°C. The plating time was adjusted to obtain a 2-6 μm thick silver deposit. After plating, the specimen was then rinsed with DI water and dried using compressed air.
[0236] The carbon content in standard silver deposits was determined according to DIN EN ISO 15350:2000. The silver deposits were plated on stainless steel coupons with poor adhesion to the silver layer. The silver deposits were removed from the stainless steel substrate, weighed and burned on a platinum wire in a chamber using an oxygen flow at about 1200°C. The resulting carbon dioxide from the combustion of the organic carbon in the silver deposits was determined by infrared spectroscopy and used to determine the carbon mass in the silver deposits. This value was divided by the total mass of each silver deposit to obtain the carbon weight percentage in each deposit. The resulting carbon dioxide was determined by infrared spectroscopy. The average amount of carbon deposited in the silver deposits was only less than 0.005%.
Claims
1. A silver electroplating composition comprising the following substances: water, Silver ion source, Sulfide compounds having the formula: HO(CH2)2-S-(CH2)2OH(I), a sulfonated anionic polymer, a salt thereof, or a mixture thereof capable of being co-deposited with silver to provide a silver deposit comprising a coefficient of friction of 1 or less without the use of a lubricant, the sulfonated anionic polymer being selected from the group consisting of naphthalenesulfonic acid formaldehyde condensate or a salt thereof, poly-acrylic acid-co-vinylsulfonic acid or a salt thereof, and a mixture thereof, The silver electroplating composition does not contain cyanide, The silver electroplating composition does not contain carbon in particulate form, the carbon in particulate form comprising graphitic carbon, other carbon allotropes, or mixtures thereof, And the pH is less than 7.
2. The silver electroplating composition of claim 1, further comprising an acid.
3. The silver electroplating composition according to claim 2, wherein: The acid is an alkanesulfonic acid.
4. The silver electroplating composition of claim 1, further comprising a grain refiner.
5. The silver electroplating composition according to claim 4, wherein The grain refiner is a thiol compound.
6. The silver electroplating composition of claim 1, further comprising a brightener.
7. A method for electroplating silver metal on a substrate, the method comprising: a) providing the substrate; b) contacting the substrate with the silver electroplating composition according to claim 1; as well as c) applying an electric current to the silver electroplating composition and the substrate to electroplate a silver deposit on the substrate.
8. An article comprising a silver layer on a substrate, wherein the silver layer is prepared from the silver electroplating composition according to any one of claims 1 to 6, and the silver layer has a coefficient of friction of 1 or less without using a lubricant.
9. The article of claim 8, wherein: The silver layer is 99 metal basis % or greater silver metal.
10. The article of claim 8, wherein: The silver layer further has a friction coefficient of 0.6 or less without using a lubricant.
11. The article of claim 8, wherein: The silver layer has a carbon content of 0.1 to 5 mass % and does not include particles having a crystal domain size having a diameter greater than 100 nm.
12. The article of claim 11, wherein: The silver layer has a carbon content of 0.5 to 3.5 mass % and does not include particles having a crystal domain size greater than 100 nm in diameter.
13. The article of claim 12, wherein: The silver layer has a carbon content of 1 to 3 mass % and does not include particles having a crystal domain size having a diameter greater than 100 nm.
Citation Information
Cited By
Cyanide-free silver plating solution with long service life as well as electroplating method, application and product thereof
CN122303979A
A long-life cyanide-free silver plating solution, its electroplating method, application and product
CN122303979B