Chromium-free hydrogenation catalyst with improved water and acid stability

By preparing Cu-Al catalyst profiles, especially copper in the form of copper spinel CuAl2O4, the mechanical stability problem of the catalyst in acidic and aqueous media was solved, achieving higher catalytic activity and stability.

CN115279488BActive Publication Date: 2024-11-05CLARIANT INT LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180020294.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-13
Filing Date
2021-03-09
Publication Date
2024-11-05
Estimated Expiration
2041-03-09

AI Technical Summary

Technical Problem

Existing catalysts exhibit poor mechanical stability during the hydrogenation of organic compounds and are susceptible to corrosion by acidic compounds and water, leading to the loss of catalytically active metals and affecting catalytic activity.

Method used

The Cu-Al catalyst is used to form a molded body, in which copper exists in the form of copper spinel CuAl2O4. It is prepared into sheets, extrusions or granules through a specific process, and lubricants and binders are added. After calcination and reduction treatment, the mechanical stability is improved.

Benefits of technology

It improves the stability of the catalyst in acidic and aqueous media, reduces copper ion loss, maintains catalytic activity, and is suitable for carbonyl conversion in hydrogenated organic compounds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003839745240000091
    Figure BDA0003839745240000091
  • Figure BDA0003839745240000121
    Figure BDA0003839745240000121
  • Figure BDA0003839745240000131
    Figure BDA0003839745240000131
Patent Text Reader

Abstract

The invention relates to an improved catalyst based on a shaped catalyst body for hydrogenating carbonyl groups in organic compounds under the action of acid and water, characterized in that the shaped catalyst body has a copper content of 17.5 to 34.5 wt.%, relative to the shaped catalyst body, at least 70% of the copper being present in the shaped catalyst body in the form of copper spinel CuAl2O4. The invention also relates to the preparation of the catalyst and its use in the hydrogenation of carbonyl groups in organic compounds in the presence of acid and / or water.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to an improved catalyst based on a shaped catalyst body for the hydrogenation of carbonyl groups in organic compounds, characterised in that the shaped catalyst body comprises 17.5% to 34.5% by weight of copper, wherein at least 70% of the copper is present in the form of copper spinel CuAl2O4. The invention further relates to the preparation of the shaped catalyst body and its use in the hydrogenation of carbonyl groups in organic compounds.

[0002] Catalytic processes for hydrogenating carbonyl groups in organic compounds such as esters, diesters, aldehydes or ketones are of great industrial importance. Their purpose includes converting carboxylic acids or their esters, in particular fatty acid esters, into the corresponding alcohols.

[0003] Suitable catalysts here are systems based on copper in combination with other transition metal elements. The catalysts are usually in the form of tablets, extrudates or granules.

[0004] WO 2004 / 085356 describes the preparation of a catalyst for the hydrogenation of carbonyl compounds which, in addition to copper and aluminum, comprises at least one oxide of lanthanum, tungsten, molybdenum, titanium or zirconium and additionally has copper powder or flakes, cement powder or graphite added.

[0005] DE 40 21 230 A1 describes a process for preparing alcohols by hydrogenating organic carboxylic acid ester compounds in the presence of a copper-zirconium catalyst composed of copper, zirconium and oxygen to give the corresponding alcohols, such as higher alcohols or diols.

[0006] EP 0 434 062 A1 provides a process for the hydrogenation of substance mixtures to the corresponding alcohols, using a catalyst which is prepared by coprecipitation of a metal selected from the group consisting of Mg, Zn, Ti, Zr, Sn, Ni, Co and mixtures thereof.

[0007] The catalyst disclosed in EP 0 552 463 A1 for the hydrogenation of carbonyl groups in organic compounds has in its oxide form the composition Cu a Al b Zr c Mn d O d , where a>0; b>0; c>0; d>0; a>b / 2; b>a / 4; a>c; a>d; and x is the number of oxygen ions per unit formula required to maintain electrical neutrality.

[0008] US 2018 / 0280940 A1 provides the use of powdered catalysts based on NiAl2O4 or CuAl2O4 for hydrogenating ketones to alcohols. The copper content of the analyzed sample is at least 42.7% by weight.

[0009] The catalyst described in US Pat. No. 6,455,464 B1 consists essentially of copper and aluminum and has a spinel content of less than 60% by weight. The catalyst is used for hydrogenolysis.

[0010] The starting compounds in the hydrogenation process often include traces of acidic compounds. These are, for example, carboxylic acids which are present as by-products in esterification reactions. Under the reaction conditions of the hydrogenation reaction, these compounds attack the catalyst and lead to a reduction in mechanical stability, and sometimes leaching of catalytically active metals is observed, which are discharged from the reactor together with the product stream and have to be separated therefrom. In addition, the catalytic activity of the catalyst also decreases with the gradual discharge of catalytically active metals.

[0011] Catalysts containing copper and chromium are used for such reactions. These generally have an enhanced stability to the action of acids. Due to stricter environmental regulations, the use of chromium catalysts involves higher requirements, so there is a need to replace the existing CuCr systems with alternatives that are environmentally compatible but still have comparable catalytic and physical properties.

[0012] Therefore, an object of the present invention is to provide a catalyst for the hydrogenation of carbonyl groups in organic compounds, characterized by improved mechanical stability and being less affected by acidic compounds or water. In addition, it should be possible to use such a catalyst, in particular in hydrogenations occurring in acidic and / or aqueous media.

[0013] This object is achieved by the catalyst according to the invention.

[0014] The invention relates to a Cu-Al shaped catalyst body, characterized in that it contains 17.5% to 34.5% by weight of copper, based on the total weight of the shaped catalyst body after burnout, wherein at least 70% of the copper is present in the form of copper spinel CuAl2O4.

[0015] The shaped catalyst bodies can be present in various forms, for example in the form of extrudates, spheres, granules or tablets. In a preferred embodiment, the shaped catalyst bodies are present in the form of tablets.

[0016] The catalyst shaped bodies may be present in different sizes. The diameter of the tablets may be between 2 and 6 mm, preferably between 3 and 5 mm. The diameter is particularly preferably between 4.4 and 4.6 mm. The height of the tablets may be between 2 and 6 mm, preferably between 2 and 4 mm. The height is particularly preferably between 2.5 and 3.5 mm.

[0017] The side crushing strength of the catalyst shaped body of the present invention is 80 to 300 N, preferably 150 to 250 N, more preferably 170 to 230 N. Preferably, the catalyst shaped body of the present invention has a diameter in the range of 3 to 5 mm, a height in the range of 2 to 4 mm, and a side crushing strength in the range of 170 to 230 N.

[0018] The pore volume of the catalyst shaped body according to the present invention measured by mercury porosimetry is 100 to 500 mm 3 / g, preferably 150 to 400 mm 3 / g, more preferably 200 to 400 mm 3 / g.

[0019] The catalyst shaped body of the present invention has a diameter of 20 to 150 m 2 / g, preferably 70 to 120m 2 / g BET specific surface area.

[0020] The amounts of copper and aluminium in the shaped catalyst bodies according to the invention stated below relate to the oxidised, non-reduced form of the shaped catalyst bodies in which the elements are present in oxidised form, such as Cu(II) and Al(III).

[0021] In one embodiment, the oxidic form of the catalyst body comprises Cu in an amount of from 22.1 wt.%, preferably 24.5 wt.%, further preferably 25.0 wt.%, more preferably 24.5 wt.%, more preferably 25.0 wt.%, even more preferably 27.0 wt.%, most preferably 27.5 wt.%, to 33.8 wt.%, preferably 31.0 wt.%, more preferably 30.4 wt.%, based on the total weight of the catalyst body after burnout.

[0022] In another embodiment, the oxidic shaped catalyst body comprises Al in an amount of 21.2 wt.-%, preferably 21.8 wt.-%, more preferably 24.9 wt.-%, more preferably 29.0 wt.-%, even more preferably 29.5 wt.-%, most preferably 30.1 wt.-%, and 38.3 wt.-%, preferably 36.9 wt.-%, more preferably 36.7 wt.-%, more preferably 36.4 wt.-%, particularly preferably 35.1 wt.-%, most preferably 34.7 wt.-%, based on the total weight of the shaped catalyst body after burnout.

[0023] At least 70% of the copper present in the shaped catalyst body is in the form of copper spinel CuAl2O4. In a preferred embodiment, this proportion is in the range of 70 to 98%, more preferably in the range of 70 to 95%, even more preferably in the range of 75 to 90%, most preferably in the range of 80 to 90%.

[0024] In one embodiment, the Cu / Al2 atomic ratio is less than 1, preferably less than 0.97, and more preferably less than 0.94. In another embodiment, the Cu / Al2 atomic ratio is greater than 0.49 and less than 1, preferably greater than 0.57 and less than 0.97, more preferably greater than 0.58 and less than 0.94, and particularly preferably greater than 0.79 and less than 0.94.

[0025] In one embodiment, the catalyst does not contain manganese and zirconium in oxidic or metallic form. In another embodiment, the catalyst does not contain any other transition metals in oxidic or metallic form other than copper.

[0026] The catalyst shaped body of the present invention is prepared by the following steps according to the present invention:

[0027] a) combining (i) an aqueous solution A of a copper compound and optionally a transition metal compound with (ii) an alkaline aqueous solution B to form a precipitate, wherein solution A and / or solution B also comprises a dissolved aluminum compound,

[0028] b) isolating the precipitate and optionally washing the precipitate,

[0029] c) drying the precipitate to obtain a dried precipitate,

[0030] d) calcining the dried precipitate from step c) at a temperature of 200 to 800° C. for a period of 30 minutes to 4 hours.

[0031] e) shaping the calcined precipitate from step d) to obtain a shaped body.

[0032] Suitable starting compounds for the compounds of copper, aluminum and any transition metals used in step a) are in principle all compounds which are soluble in water or alkaline or acidic aqueous solutions. Preference is given to using carbonates, nitrates, halides, oxides, sulfates, acetates or formates.

[0033] The aluminum compound here may already be present in the copper-containing solution A, or may be added together with the precipitant in the form of an alkaline aqueous solution B.

[0034] The proportion of the copper compound in solution A in step a) is selected such that the proportion of copper in the finished catalyst is in the range from 17.5% to 34.5% by weight, based on the total weight of the shaped catalyst bodies after burnout.

[0035] In one embodiment, the precipitate in step a) is formed by passing an alkaline aqueous solution B comprising the precipitant into a solution A comprising dissolved copper and any transition metal compounds, preferably under continuous stirring of the metal-containing solution.

[0036] In another embodiment, the precipitate in step a) is formed by passing an alkaline aqueous solution B comprising the precipitant and the aluminum compound into a solution A comprising dissolved copper and any transition metal compounds, preferably under continuous stirring of the metal-containing solution.

[0037] In a further embodiment, the alkaline aqueous solution B comprising the precipitant is passed together with the metal-containing solution A into a common precipitation vessel.

[0038] The temperature of the mixed solution in step a) is generally in the range of 10 to 90°C, preferably in the range of 30 to 90°C, more preferably in the range of 50 to 85°C.

[0039] The pH during the precipitation of the metal-containing compound in step a) is in the range of 6.0 to 8.0, preferably in the range of 6.5 to 7.5, more preferably in the range of 6.5 to 7.0.

[0040] After precipitation, the resulting precipitate is separated. This is usually done by filtration. Alternatively, the precipitate can be separated by decantation or centrifugation.

[0041] The separated precipitate can then optionally be subjected to one or more washing steps to remove any adhering impurities, such as excess hydroxide ions or alkali metal ions. The precipitate here can be retained directly in the filter chamber in the form of a filter cake and passed through a washing medium, preferably deionized water, or it can be pulped in a washing medium and separated out again by means of filter pressing, decantation or centrifugation. This process is usually repeated until the conductivity of the washing medium drops below a certain value. This is usually 0.5 mS / cm, in particular 0.3 mS / cm. The conductivity is determined according to DIN 38404 Part 8.

[0042] After the precipitate has been separated and optionally washed, it is dried at a temperature in the range of 50 to 150° C., preferably in the range of 70 to 130° C., more preferably in the range of 80 to 120° C. Drying can be carried out in a spray dryer. Alternatively, drying can also be carried out in a static oven, in which case the drying time is generally in the range of 30 minutes to 6 hours.

[0043] The dried powder is then calcined. This takes place at a temperature of 200 to 800° C., preferably 400 to 800° C., more preferably 600 to 750° C. The calcination duration is 30 minutes to 4 hours, preferably 1 to 3 hours, more preferably 1.5 to 2.5 hours.

[0044] The dried and calcined precipitate is then subjected to a shaping process.

[0045] Conventional shaping processes are tableting, extrusion and granulation. In a preferred embodiment, the calcined precipitate is tableted.

[0046] Tabletting is usually carried out using a tablet press, such as a Kilian Pressima tablet press. Tabletting is preferably carried out with the addition of a lubricant, such as graphite, oil or stearate, preferably graphite. For this purpose, the calcined precipitate obtained in step d) is mixed with at least one lubricant, optionally compacted and / or granulated, and then tabletted. The proportion of lubricant in the mixture is usually 0.5% to 5.0% by weight, preferably 1% to 4% by weight, based on the total weight of the composition to be tableted.

[0047] In one embodiment, a binder is added to the precipitate to be shaped. In principle, all compounds which increase the mechanical stability of the shaped body are suitable as binders. Suitable binders are aluminum oxides, such as pseudoboehmite, boehmite or corundum, silicon dioxide, calcium aluminates, calcium silicates or clay minerals such as bentonite.

[0048] The binder is usually added to the mixture in an amount such that the binder content in the molded body is in the range of 2% to 30% by weight, preferably in the range of 2% to 10% by weight, more preferably in the range of 2% to 5% by weight, based on the total weight of the molded body after burnout.

[0049] The shaped body obtained in step e) can then be subjected to a heat treatment in step f). This is carried out at a temperature of 200 to 800° C., preferably 400 to 700° C., more preferably 400 to 600° C. The duration of the heat treatment is 30 minutes to 4 hours, preferably 1 to 3 hours, more preferably 1.5 to 2.5 hours.

[0050] The shaped catalyst bodies obtainable by the process according to the invention can be reduced in a further step before they are used in catalytic reactions.

[0051] The reduction is preferably carried out by heating the shaped catalyst body in a reducing atmosphere. The reducing atmosphere is in particular hydrogen. The reduction is carried out, for example, at a temperature in the range of 150° C. to 450° C., preferably in the range of 160° C. to 250° C., more preferably in the range of 170° C. to 200° C. The reduction is carried out, for example, in a period of 1 hour to 20 days, preferably in a period of 2 hours to 120 hours, more preferably in a period of 24 to 48 hours. In a preferred embodiment, the reduction is carried out at a temperature in the range of 190° C. to 210° C. for 24 to 48 hours.

[0052] In a preferred embodiment, the catalyst shaped body is stabilized in wet or dry form after reduction. In the case of wet stabilization, the catalyst shaped body is covered with a liquid to minimize contact with oxygen. Suitable liquids include organic liquids and water, preferably organic liquids. Preferred organic liquids are those with a vapor pressure of 0.5 hPa or less at 20°C. Examples of such suitable organic liquids are isodecyl alcohol, Nafol, fatty alcohols, hexadecane, 2-ethylhexanol, propylene glycol and mixtures thereof, particularly isodecyl alcohol. In the case of dry stabilization, oxygen or an oxygen-containing gas, preferably a mixture of air and an inert gas such as argon or nitrogen, is metered into the reduction space. The oxygen concentration in the mixture is preferably increased from about 0.04% by volume to about 21% by volume. For example, a mixture of air and an inert gas can be metered in, wherein the ratio of air to inert gas is initially about 0.2% by volume of air to 99.8% by volume of inert gas. The ratio of air to inert gas is then gradually increased (e.g., continuously or stepwise) until, for example, 100% by volume of air (corresponding to an oxygen concentration of about 21% by volume) is finally metered in. Without being bound by any particular theory, it is assumed that the metered addition of air or oxygen produces a thin oxide layer with a thickness of, for example, 0.5 to 50 nm, preferably 1 to 20 nm, more preferably 1 to 10 nm, on the catalyst surface, which protects the shaped catalyst body from further oxidation. In the case of dry stabilization, the reactor temperature is preferably 100° C. or less, more preferably 20° C. to 70° C., most preferably 30° C. to 50° C. The reduction can be carried out ex situ or in situ in the reaction system into which the shaped catalyst body is introduced as a catalyst.

[0053] In one embodiment, the crystallite size of copper in the reduced shaped body is in the range of 7 to 12 nm, preferably in the range of 8 to 11 nm, more preferably in the range of 9 to 11 nm.

[0054] The side crushing strength of the reduced plate-like shaped catalyst body is 50 to 250N, preferably 60 to 200N, more preferably 70 to 150N.

[0055] After reduction, the shaped catalyst body according to the invention or the shaped catalyst body obtainable by the process according to the invention comprises Cu(0), i.e. copper in oxidation state 0, in particular in a proportion of 5 to 36% by weight, preferably in a proportion of 10 to 34% by weight, more preferably in a proportion of 20 to 32% by weight, based on the total weight of the reduced catalyst after burn-off.

[0056] The catalysts according to the invention have an improved stability towards acidic or aqueous media, for example organic solutions or organic gas mixtures containing acids and / or water as impurities. In addition to the improved lateral crushing strength of the shaped catalyst bodies, this is also reflected in the reduction of copper ion losses in the material that is essential for the catalytic activity. In addition, the shaped catalyst bodies according to the invention also have a lower total metal ion loss, which is a sign of an increased stability of the solid structure with respect to leaching of individual metal ions.

[0057] In order to determine the stability of the catalyst shaped bodies according to the invention to the action of acids, the shaped bodies are treated in an acidic and aqueous medium, after which the lateral crushing strength of the shaped bodies treated in this way and the proportion of metal ions in the acidic and aqueous medium are determined.

[0058] The invention further provides the use of the catalysts according to the invention in the catalytic hydrogenation of carbonyl groups in organic compounds in an acidic and / or aqueous medium. Possible reactions include the hydrogenation of aldehydes to alcohols, in particular the hydrogenation of carbonyl aldehydes to carbonyl alcohols, the hydrogenation of fatty acids, for example by esterification, in particular the esterification to fatty acid methyl esters, and subsequent hydrogenolysis, or the hydrogenation of ketones to the corresponding alcohols.

[0059] The typical acid value of the reaction medium used here is between 0.1 and 3.4 mg KOH / g 溶液 In the range of 0.2 to 1.0 mg KOH / g 溶液 The acid number is a measure of the presence of acidic OH groups, for example in carboxylic acids, in a solution and can be determined, for example, by titrating the corresponding solution with KOH solution to the neutralization point. The amount of KOH consumed here corresponds to the acid number, in mg, based on the weight of the solution. KOH / g 溶液 express.

[0060] The water content in this reaction medium is generally in the range of 0.1 to 5.0% by weight, more preferably in the range of 0.2 to 5.0% by weight, particularly preferably in the range of 0.5 to 3.0% by weight.

[0061] Fatty acids to be hydrogenated in the context of the present invention are saturated or unsaturated fatty acids, which are divided into short-chain (up to 6-8 carbon atoms), medium-chain (6-8 to 12 carbon atoms) and long-chain (13 to 21 carbon atoms) fatty acids according to the chain length. In addition, fatty acids with more than 22 carbon atoms can also be used. Example

[0062] The loss on ignition in the context of the present invention is determined according to DIN 51081 by measuring the weight of a sample of about 1-2 g of the material to be analyzed, which is then heated to 900° C. in an ambient atmosphere and stored at this temperature for 3 hours. The sample is then cooled in an inert atmosphere and the residual weight is measured. The difference in weight before and after the heat treatment corresponds to the loss on ignition.

[0063] The side crush strength (SCS) is determined according to ASTM 04179-01 without pre-drying the sheets. This is done by measuring a statistically sufficient number of sheets (at least 20 sheets) and calculating the arithmetic mean of the individual measurements. This mean corresponds to the side crush strength of the particular sample.

[0064] The chemical elements were determined by ICP (Inductively Coupled Plasma) measurement in accordance with DIN EN ISO 11885.

[0065] The acid value is determined by mixing about 4 g of sample solution with 25 mL of propanol and adding phenolphthalein as an indicator. The solution is titrated with tetrabutylammonium hydroxide solution (0.1 mol / L in 2-propanol / methanol) at room temperature until a color change occurs. The acid value in mg is calculated according to the following formula KOH / g 溶液 Acid value AV:

[0066]

[0067] Where AV = acid value, consumed volume = volume of tetrabutylammonium hydroxide solution consumed, in mL, c = concentration of tetrabutylammonium hydroxide solution, M = molar mass of KOH, sample weight = amount of sample solution used, in g.

[0068] The BET specific surface area is determined in accordance with DIN 66131 by nitrogen adsorption.

[0069] The pore volume of the shaped catalyst bodies is measured by mercury porosimetry in accordance with DIN 66133 in a pressure range of 1 to 2000 bar.

[0070] The weight proportion of copper spinel CuAl2O4 and the crystallite size of copper in the catalyst shaped bodies were determined by X-ray diffraction and Rietveld refinement. This was done by analyzing the samples in a Bruker D4 Endeavor in the range of 5 to 90° 2θ (step sequence 0.020° 2θ, measuring time per step 1.5 seconds). The radiation used was CuKα1 radiation (wavelength 40kV, 35mA). During the measurement, the sample stage rotates around its axis at a speed of 30 rpm. The reflection intensity diffraction pattern obtained by quantitative calculation is refined by Rietveld, and the proportion of copper spinel CuAl2O4 in the sample is determined. The proportion of each crystalline phase is determined using TOPAS software version 6 from Bruker. The crystallite size of copper is calculated by the software using the Scherrer formula based on the reflection of 43.3°2θ.

[0071] Example 1: Preparation of reference powder

[0072] Aqueous solution 1 was prepared by adding 4482 g of Cu(NO3)2.2.5H2O to 3000 mL of demineralized water. The mixture was then mixed with 3000 mL of nitric acid (65% by weight HNO3). The acidic solution was made up to a total volume of 23330 mL with demineralized water. The pH of the solution was -0.20. The solution was then heated to 80°C.

[0073] In addition, 1600 g of Na2CO3 and 4625 g of NaAlO2 were dissolved in 26670 mL of demineralized water; the pH value of the solution was 12.43.

[0074] A precipitation vessel containing 8000 mL of demineralized water was provided for precipitation. The copper-containing solution and the carbonate-containing solution were simultaneously introduced therein. The feed rate was adjusted so that the pH value of the precipitation solution was about 6.5.

[0075] At the end of the addition and when precipitation is complete, the precipitate is filtered off and washed with demineralized water to remove adhering impurities. The filter cake is then resuspended in 8000 mL of demineralized water and dried.

[0076] The spray dried powder was then calcined at 750°C for 2 hours.

[0077] The relative weight proportions, based on the total mass after burn-off, are Cu=30 wt % and Al=30 wt %.

[0078] Example 2: Preparation of Catalyst 1 of the Present Invention

[0079] 1529 g of the calcined powder obtained in Example 1 were combined with 36 g of Pural SCF binder, 5 g of demineralized water and 31 g of graphite and mixed for 10 minutes to provide a homogeneous mixture. The mixture was first compacted and granulated and then pressed into tablets 4.5 mm wide and 3 mm high in a Kilian Pressima tablet press. The tablets were finally calcined at 450°C for 2 hours. The bulk density of the tablets thus obtained was 1111 g / l and the side crushing strength of the tablets was 198 N. 84% of the copper present in the catalyst molded body was in the form of copper spinel CuAl2O4. The crystallite size of copper in the molded body after reduction was 9.5 nm. The pore volume was 314 mm3 / g, BET specific surface area is 103m 2 / g.

[0080] Example 3: Preparation of Catalyst 2 of the Present Invention

[0081] To prepare the catalyst 2 according to the invention, 360 g of the calcined powder obtained in Example 1 was combined with 7.2 g of graphite and mixed for 10 minutes to obtain a homogeneous mixture. The mixture was first compacted and granulated and then pressed into tablets with a width of 4.5 mm and a height of 3 mm in a Kilian Pressima tablet press. The tablets were finally calcined at 450° C. for 2 hours. The side crushing strength of the tablets was 155 N.

[0082] Comparative Example 1 (Catalyst A)

[0083] Catalyst A was prepared by precipitating a copper- and chromium-containing precipitate, converting it into oxide form by heat treatment, and then pressing it into tablets 4.5 mm wide and 3 mm high. The relative weight proportions, based on the total mass after burnout, were Cu=37.5% by weight and Cr=23.0% by weight.

[0084] Comparative Example 2 (Catalyst B)

[0085] To prepare catalyst B, aqueous solution 1 was prepared by dissolving 1250 g of Cu(NO3)2.3H2O, 220 g of Mn(NO3)2.4H2O and 1800 g of Al(NO3)3.9H2O in 9000 g of distilled water. Solution 2 was prepared by dissolving 1720 g of Na2CO3 in 7500 g of distilled water. The two solutions were heated to 80° C. respectively while stirring. The two solutions were then metered into a precipitation vessel with continuous stirring. The resulting precipitate was filtered off and washed with distilled water to remove adhering impurities until the conductivity of the washing water was less than 0.25 mS. The filter cake was then dried. The dried powder was then heat treated at 750° C. for 3 hours; the relative weight proportions in the tablets, based on the total mass after ignition loss, were Cu=44.8% by weight, Mn=7.0% by weight and Al=17.92% by weight.

[0086] 1706 g of this powder was combined with 51 g of Secar 71 binder, 5 g of demineralized water and 34 g of graphite and mixed for 10 minutes to provide a homogeneous mixture. The mixture was first compacted and granulated and then pressed into tablets with a width of 4.5 mm and a height of 3 mm in a Kilian Pressima tablet press. The tablets were finally calcined at 600° C. for 2 hours. The relative weight proportions in the tablets, based on the total mass after burnout, were Cu=43.5 wt. %, Mn=6.8 wt. %, Al=18.5 wt. % and Ca=0.6 wt. %.

[0087] Comparative Example 3 (Catalyst C)

[0088] The powder of catalyst C was prepared according to the method for preparing the powder of catalyst B, except that the proportion of Mn(NO3)2·4H2O was selected so that the relative weight proportion of manganese in the powder thus obtained, based on the mass lost after burning, was 0.1% by weight. The relative weight proportions, based on the total mass lost after burning, were Cu=49.7% by weight, Mn=0.1% by weight and Al=20.0% by weight. 1706 g of the powder thus obtained were combined with 5 g of demineralized water and 34 g of graphite and mixed for 10 minutes to provide a homogeneous mixture. The mixture was first compacted and granulated and then pressed into tablets with a width of 4.5 mm and a height of 3 mm in a Kilian Pressima tablet press. The relative weight proportions in the tablets, based on the total mass lost after burning, were Cu=49.7% by weight, Mn=0.1% by weight and Al=20.0% by weight. The bulk density of the tablets thus obtained was 1152 g / L.

[0089] A portion of the material obtained after tableting of the comparative catalysts A, B and C and the catalyst 1 according to the invention was reduced. This was achieved by subjecting the sample to a heat treatment at a temperature of 200° C. in a gas mixture of 2% by volume H2 and 98% by volume N2, in order to reduce the Cu present in an oxidized state. The sample was then cooled to room temperature under nitrogen and stored under liquid isodecyl alcohol. The side crushing strength of this sample was then measured and used in Use Examples 1 to 3.

[0090] Use Example 1: Stability Test

[0091] For the inventive catalyst 1 and the comparative catalysts A, B and C, the acid stability was determined in each case by combining a total of 25 g of the tableted, reduced and stabilized sample with a liquid mixture consisting of 75 g of oxoaldehyde solution, with a water content of 1% by weight and an acid number of 0.2 mg KOH / g 溶液 The mixture was heated at 120°C for 4 days under a nitrogen atmosphere. At the end of the test the tablet sample was separated from the liquid mixture. Its side crushing strength was then immediately measured.

[0092] After the test was performed, the carbonyl aldehyde solution was analyzed for the presence of Cu, Al, Cr and Mn.

[0093] Table 1

[0094] Example Side crushing strength after reduction [N] Side crushing strength after acid / water treatment [N] Catalyst 1 137 119 Comparative Catalyst A 97 86 Comparative Catalyst B 93 74 Comparative Catalyst C 47 Not measurable because the sample material has broken

[0095] Table 1 clearly shows that the side crush strength of the catalyst according to the invention after reduction is already higher than that of the catalysts known from the prior art. The side crush strength values ​​at the end of the test demonstrate even more clearly the increased stability to acid and water. Here again, the catalyst according to the invention has the highest side crush strength values, whereas, in contrast, the tablets of the chromium-free CuAlMn catalyst broke during the test and no meaningful measurement of the side crush strength was possible.

[0096] Table 2

[0097]

[0098] The data from Table 2 show that the catalyst of the present invention is very stable to the loss of copper species under the severe test conditions, while the comparative catalyst is significantly higher in this regard. In summary, the catalyst of the present invention has a low total metal loss compared to the comparative catalyst.

[0099] Use Example 2: Hydrogenation of carbonyl aldehydes to carbonyl alcohols

[0100] A bed of the catalyst 1 according to the invention in reduced and moisture-stabilized form with a volume of 100 mL was introduced into the reactor and heated to a temperature in the range of 120 to 180° C. under a nitrogen stream, the reaction time at each temperature being selected to be 2 days. A liquid phase containing 45% by weight of aldehydes, 25% by weight of the corresponding alcohols and 30% by weight of by-products (paraffins, olefins, etc.), a water content of 0.7% by weight and an acid number of 0.2 was then passed through the reactor.

[0101] The composition of the product stream downstream of the reactor was analyzed by gas chromatography. The conversion and alcohol content in the product stream calculated over the entire operating time at each temperature are shown in Table 3.

[0102] For comparison, a sample of Comparative Catalyst A and a sample of Comparative Catalyst B were subjected to the same conditions, and the results obtained are also shown in Table 3.

[0103] Table 3

[0104]

[0105] As is clear from Table 3, the inventive catalyst 1 achieves aldehyde conversion under comparable test conditions which correspond approximately to the commercial chromium-containing catalyst A. A similar behavior is also demonstrated for the formation of the corresponding alcohol. The inventive catalyst is therefore an environmentally friendly alternative to the chromium-containing catalysts used to date.

[0106] The data also show that although Comparative Catalyst B achieves comparable conversions and even significantly improves alcohol formation, its low physical stability makes it unsuitable for prolonged use under harsh reaction conditions.

Claims

1. A Cu-Al catalyst shaped body for hydrogenating carbonyl groups in organic compounds, characterized in that The catalyst body contains copper in a proportion of 17.5% by weight to 34.5% by weight, based on the total weight of the catalyst body after burnout, and wherein at least 70% of the copper is present in the form of copper spinel CuAl2O4, and wherein the Cu / Al2 atomic ratio is greater than 0.49 and less than 1. 2 . The shaped catalyst body according to claim 1 , wherein 70% to 98% of the copper is present in the form of copper spinel CuAl 2 O 4 .

3. The shaped catalyst body according to claim 1, wherein 70% to 95% of the copper is present in the form of copper spinel CuAl2O4.

4. The shaped catalyst body according to claim 1, wherein 75% to 90% of the copper is present in the form of copper spinel CuAl2O4.

5. The shaped catalyst body according to claim 1, wherein 80% to 90% of the copper is present in the form of copper spinel CuAl2O4.

6. The shaped catalyst body according to claim 1, wherein copper is present in a proportion of 25.0% by weight to 34.5% by weight, based on the total weight of the shaped catalyst body after burnout.

7. The shaped catalyst body according to claim 6, wherein copper is present in a proportion of 27.5% by weight to 31% by weight, based on the total weight of the shaped catalyst body after burnout. 8 . The shaped catalyst body according to claim 1 , wherein the shaped catalyst body is in the form of a tablet. 9 . The shaped catalyst body according to claim 1 , wherein the lateral crushing strength is 80 to 300 N.

10. The catalyst shaped body according to claim 9, wherein the side crushing strength is 150 to 250N.

11. The catalyst shaped body according to claim 9, wherein the side crushing strength is 170 to 230N.

12. The shaped catalyst body according to any one of claims 1 to 7, wherein it comprises Al in an amount ranging from 21.2% to 38.3% by weight, based on the total weight of the shaped catalyst body after burnout.

13. The shaped catalyst body according to claim 12, wherein it comprises Al in an amount ranging from 21.8 wt% to 36.9 wt%, based on the total weight of the shaped catalyst body after burnout.

14. The shaped catalyst body according to claim 12, wherein it comprises Al in an amount ranging from 24.9 wt% to 36.7 wt%, based on the total weight of the shaped catalyst body after burnout.

15. The shaped catalyst body according to claim 12, wherein it comprises Al in an amount ranging from 29.0 wt% to 36.4 wt%, based on the total weight of the shaped catalyst body after burnout.

16. The shaped catalyst body according to claim 12, wherein it comprises Al in an amount ranging from 29.5 wt% to 35.1 wt%, based on the total weight of the shaped catalyst body after burnout.

17. The shaped catalyst body according to claim 12, wherein it comprises Al in an amount ranging from 30.1 wt% to 34.7 wt%, based on the total weight of the shaped catalyst body after burnout.

18. The shaped catalyst body according to any one of claims 1 to 7, wherein the Cu / Al2 atomic ratio in the shaped catalyst body is less than 0.

97.

19. The catalyst shaped body according to claim 18, wherein the Cu / Al2 atomic ratio in the catalyst shaped body is less than 0.

94.

20. The shaped catalyst body according to claim 18, wherein the Cu / Al2 atomic ratio is greater than 0.57 and less than 0.

97.

21. The shaped catalyst body according to claim 20, wherein the Cu / Al2 atomic ratio is greater than 0.58 and less than 0.

94.

22. The catalyst shaped body according to claim 20, wherein the Cu / Al2 atomic ratio is greater than 0.79 and less than 0.

94.

23. The shaped catalyst body according to any one of claims 1 to 7, wherein the BET specific surface area is in the range of 20 to 150 m 2 / g range.

24. The catalyst shaped body according to claim 23, wherein the BET specific surface area is in the range of 70 to 120 m 2 / g range.

25. A process for producing a shaped catalyst body according to any one of claims 1 to 24, wherein the shaped catalyst body contains copper in a proportion of 17.5% by weight to 34.5% by weight, based on the shaped catalyst body after burnout, comprising the following steps: a) combining (i) at least one aqueous solution A formed from a copper compound and an aluminum compound with (ii) at least one alkaline aqueous solution B to form a precipitate, wherein solution A and / or solution B additionally comprises a dissolved aluminum compound, b) isolating the precipitate, optionally washing the precipitate, c) drying the precipitate to obtain a dried precipitate, d) calcining the dried precipitate from step c) at a temperature of 200 to 800° C. for a duration of 30 minutes to 4 hours, e) shaping the calcined precipitate from step d) to obtain a shaped body. 26 . The process according to claim 25 , wherein the shaped catalyst body comprises, based on the shaped catalyst body after burnout, copper in a proportion of 25.0% by weight to 34.5% by weight. 27 . The process according to claim 25 , wherein the shaped catalyst body comprises, based on the shaped catalyst body after burnout, copper in a proportion of 27.5% by weight to 31% by weight.

28. The method according to any one of claims 25 to 27, wherein the shaped body obtained from step (e) is subjected to a heat treatment in step f) at a temperature of 200 to 800°C for a duration of 30 minutes to 4 hours.

29. The method according to claim 28, wherein the shaped body obtained from step (e) is subjected in step f) to a temperature of 400 to 700°C for a duration of 1 hour to 3 hours.

30. The method according to any one of claims 25 to 27, wherein the shaping in step e) is performed with a binder.

31. The method according to claim 28, wherein the shaped body is reduced after step f).

32. A process for hydrogenating carbonyl groups in organic compounds using a shaped catalyst body according to any one of claims 1 to 24 or a shaped catalyst body prepared by a process according to any one of claims 25 to 31.

33. A process according to claim 32 for the hydrogenation of oxo aldehydes to oxo alcohols.