Thermoplastic resin composition, method for preparing the same, and molded article comprising the same
By adding a specific proportion of polycarbonate resin and polyester resin to the thermoplastic resin, the problem of insufficient heat resistance and chemical resistance in automotive interior materials is solved, and the mechanical properties of the thermoplastic resin composition are realized and enhanced resistance, suitable for high-demand automotive interior materials.
Patent Information
- Application Number
- CN202180023852.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-10-06
- Filing Date
- 2021-08-19
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-08-19
AI Technical Summary
Existing thermoplastic resins such as ABS resin lack heat resistance and chemical resistance in automotive interior materials, resulting in prone to cracks when using chemicals, limiting their application range.
By adding polycarbonate resin and polyester resin to vinyl cyano compound-conjugated diene rubber-aromatic vinyl compound graft copolymer, α-methylstyrene-vinyl cyano compound-aromatic by specific proportions Among the base resins of vinyl compound copolymer and aromatic vinyl compound-vinyl cyanide compound copolymer, a thermoplastic resin composition is prepared to optimize its mechanical properties, moldability, heat resistance and chemical resistance.
The mechanical properties, moldability, heat resistance and chemical resistance of the thermoplastic resin composition are significantly improved, making it suitable for high-demand automotive interior materials, and can maintain stability in high temperature and chemical environments to prevent cracks from appearing.
Smart Images

Figure CN115362212B_ABST
Abstract
Description
Technical Field
[0001] [CROSS-REFERENCE TO RELATED APPLICATIONS]
[0002] This application claims the priority of Korean Patent Application No. 10-2020-0128801 filed on October 6, 2020 in the Korean Intellectual Property Office, the disclosure of which is incorporated into this specification by reference.
[0003] The present invention relates to a thermoplastic resin composition, a method for preparing the thermoplastic resin composition, and a molded article comprising the thermoplastic resin composition. More specifically, the present invention relates to a thermoplastic resin composition prepared by adding a polycarbonate resin and a polyester resin in a predetermined composition ratio to a base resin comprising a vinyl cyanide compound-conjugated diene rubber-aromatic vinyl compound graft copolymer, an α-methylstyrene-vinyl cyanide compound-aromatic vinyl compound copolymer, and an aromatic vinyl compound-vinyl cyanide compound copolymer. Due to these compositional characteristics, the mechanical properties, moldability, heat resistance, and chemical resistance of the thermoplastic resin composition can be significantly improved. Background Art
[0004] Acrylonitrile-butadiene-styrene resin (hereinafter referred to as "ABS resin") based on conjugated diene rubber has excellent processability, mechanical properties and appearance, and has therefore been used in various fields such as parts of electronic and electrical products, automobiles, small toys, furniture and building materials. However, since ABS resin lacks heat resistance compared to engineering plastics, the use of ABS resin in parts of electronic / electrical products or automotive interior materials requiring heat resistance, high strength and chemical resistance is limited.
[0005] Polycarbonate (hereinafter referred to as "PC resin") and ABS resin alloy materials are widely used in various applications such as automobiles and electronic / electrical products due to their excellent mechanical properties and low prices. For automotive applications, alloy materials are mainly used for automotive interior materials such as instrument center boxes (center fascia) and door interior panels. However, in the case of PC / ABS, since PC / ABS has weak chemical resistance due to its amorphous nature, its use is limited. Environmental stress cracking (ESC) caused by chemical products in automotive interior materials is a long-standing and serious quality problem. In particular, cracks are often caused by chemicals frequently used in automobile interiors, and the demand for chemical-resistant materials that can prevent such problems in advance is increasing.
[0006] Therefore, there is a need to develop a material that can be applied to automobile interior materials by satisfying high heat resistance, chemical resistance, rigidity, and having appropriate moldability.
[0007] [Related technical literature]
[0008] [Patent Document]
[0009] KR 10-0488857B1 Summary of the invention
[0010] Technical issues
[0011] Therefore, the present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a thermoplastic resin composition having excellent mechanical properties, moldability, heat resistance, and chemical resistance.
[0012] Another object of the present invention is to provide a method for preparing the thermoplastic resin composition and a molded product manufactured using the thermoplastic resin composition.
[0013] The above and other objects can be achieved by the present invention described below.
[0014] Technical Solution
[0015] According to one aspect of the present invention, a thermoplastic resin composition is provided, comprising: 20 wt % to 40 wt % of a vinyl cyanide compound-conjugated diene rubber-aromatic vinyl compound graft copolymer (A), 10 wt % to 35 wt % of an α-methylstyrene-vinyl cyanide compound-aromatic vinyl compound copolymer (B), 5 wt % to 30 wt % of an aromatic vinyl compound-vinyl cyanide compound copolymer (C), 23 wt % to 47 wt % of a polycarbonate resin (D) and 3 wt % to 17 wt % of a polyester resin (E), wherein the weight of the copolymer (B) is greater than or equal to the weight of the copolymer (C), and the weight ratio of the polycarbonate resin (D) to the polyester resin (E) is 2:1 to 6:1.
[0016] According to another aspect of the present invention, there is provided a method for preparing a thermoplastic resin composition, the method comprising kneading and extruding 20 wt % to 40 wt % of a vinyl cyanide compound-conjugated diene rubber-aromatic vinyl compound graft copolymer (A), 10 wt % to 35 wt % of an α-methylstyrene-vinyl cyanide compound-aromatic vinyl compound copolymer (B), 5 wt % to 30 wt % of an aromatic vinyl compound-vinyl cyanide compound copolymer (C), 23 wt % to 47 wt % of a polycarbonate resin (D) and 3 wt % to 17 wt % of a polyester resin (E) at 200° C. to 280° C., wherein the weight of the copolymer (B) is greater than or equal to the weight of the copolymer (C), and the weight ratio of the polycarbonate resin (D) to the polyester resin (E) is 2:1 to 6:1.
[0017] According to still another aspect of the present invention, provided is a molded article including the thermoplastic resin composition.
[0018] Beneficial Effects
[0019] According to the present invention, by adding a polycarbonate resin and a polyester resin in a specific ratio to a base resin containing a vinyl cyanide compound-conjugated diene rubber-aromatic vinyl compound graft copolymer (hereinafter referred to as "ABS-based resin"), an α-methylstyrene-vinyl cyanide compound copolymer (hereinafter referred to as "heat-resistant SAN-based resin"), and a vinyl cyanide compound-aromatic vinyl compound copolymer (hereinafter referred to as "SAN-based resin") in a predetermined weight ratio, the present invention advantageously provides a thermoplastic resin composition having excellent mechanical properties, moldability, heat resistance, and chemical resistance; a method for preparing the thermoplastic resin composition; and a molded article manufactured using the thermoplastic resin composition. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The chemical resistance test results of the examples according to the present invention and the comparative examples are shown. DETAILED DESCRIPTION
[0021] Hereinafter, a thermoplastic resin composition, a method for preparing the thermoplastic resin composition, and a molded article including the thermoplastic resin composition according to the present invention will be described in detail.
[0022] The present inventors have confirmed that when an ABS-based resin is compounded with a heat-resistant SAN-based resin and a conventional SAN-based resin to improve heat resistance and moldability, and a polycarbonate resin and a polyester resin are added thereto at a predetermined weight ratio, in addition to mechanical properties and heat resistance, chemical resistance is also greatly improved. Based on these results, the present inventors have conducted further studies to complete the present invention.
[0023] The thermoplastic resin composition of the present invention comprises: 20 to 40 wt% of a vinyl cyanide compound-conjugated diene rubber-aromatic vinyl compound graft copolymer (A), 10 to 35 wt% of an α-methylstyrene-vinyl cyanide compound-aromatic vinyl compound copolymer (B), 5 to 30 wt% of an aromatic vinyl compound-vinyl cyanide compound copolymer (C), 23 to 47 wt% of a polycarbonate resin (D), and 3 to 17 wt% of a polyester resin (E), wherein the weight of the copolymer (B) is greater than or equal to the weight of the copolymer (C), and the weight ratio of the polycarbonate resin (D) to the polyester resin (E) is 2: 1 to 6: 1. In this case, mechanical properties, moldability, heat resistance, and chemical resistance may be excellent.
[0024] In the present specification, the composition ratio of a (co)polymer may refer to the content of units constituting the (co)polymer, or may refer to the content of monomers added during the polymerization of the (co)polymer.
[0025] Hereinafter, each component constituting the thermoplastic resin composition of the present invention will be described in detail.
[0026] (A) Vinyl cyanide compound-conjugated diene rubber-aromatic vinyl compound graft copolymer
[0027] Based on the total weight of the thermoplastic resin composition, the content of the vinyl cyanide compound-conjugated diene rubber-aromatic vinyl compound graft copolymer (A) (hereinafter referred to as "graft copolymer (A)") is 20 wt% to 40 wt%. In this case, mechanical properties, moldability and appearance can be excellent. As a preferred embodiment, based on a total of 100 wt% of the thermoplastic resin composition, the content of the graft copolymer (A) can be 20 wt% to 35 wt%, more preferably 20 wt% to 30 wt%. Within this range, mechanical properties, moldability, appearance and physical property balance can be excellent.
[0028] For example, the graft copolymer (A) can include 50% to 80% by weight of the conjugated diene rubber including the conjugated diene compound, 5% to 20% by weight of the vinyl cyanide compound and 10% to 40% by weight of the aromatic vinyl compound. In this case, mechanical properties, formability, appearance and physical property balance can be excellent. As a preferred embodiment, the graft copolymer (A) includes 50% to 70% by weight of the conjugated diene rubber, 5% to 15% by weight of the vinyl cyanide compound and 20% to 40% by weight of the aromatic vinyl compound, more preferably 55% to 65% by weight of the conjugated diene rubber, 10% to 15% by weight of the vinyl cyanide compound and 20% to 30% by weight of the aromatic vinyl compound. Within this range, impact resistance and physical property balance can be excellent.
[0029] For example, the average particle size of the conjugated diene rubber contained in the graft copolymer (A) may be to Best to More preferred to Within this range, impact strength may be excellent without deteriorating other physical properties.
[0030] In the present specification, the average particle size of the conjugated diene rubber may be measured by dynamic light scattering, and specifically, may be measured as an intensity value in a Gaussian mode using a Nicomp 380 particle size analyzer (manufacturer: PSS).
[0031] For example, the grafting degree of the graft copolymer (A) may be 20% to 70%, preferably 20% to 55%, more preferably 20% to 45%. Within this range, appropriate compatibility and moldability can be ensured, and the balance between compatibility, moldability and other mechanical properties can be excellent.
[0032] In this specification, in order to measure the degree of grafting, the graft (co) polymer latex is coagulated, washed and dried to obtain a powder, and then 1 g of the obtained powder is added to 30 ml of acetone, followed by stirring for 24 hours. Then, the stirred solution is centrifuged at 14,000 rpm for 4 hours using an ultracentrifuge to obtain an insoluble matter, and the insoluble matter is dried at 85° C. for 4 hours. Then, the weight of the dried insoluble matter is measured, and the degree of grafting is calculated by substituting the measured value into the following formula 1.
[0033] [Formula 1]
[0034] Grafting degree (%) = [{weight of dried insoluble matter (g) - weight of rubber added during grafting polymerization (g)} / weight of rubber added during grafting polymerization (g)] × 100
[0035] Drying can be carried out until there is no further change in weight.
[0036] For example, the weight average molecular weight of the graft copolymer (A) is 500,000 to 1,000,000 g / mol, preferably 650,000 to 900,000 g / mol. Within this range, excellent processability and impact resistance can be ensured due to appropriate fluidity.
[0037] In this specification, the weight average molecular weight can be measured using a gel permeation chromatograph (GPC) filled with porous silica as a column filler and tetrahydrofuran (THF) as a solvent at 40° C. In this case, the weight average molecular weight is obtained as a relative value relative to a polystyrene (PS) standard sample.
[0038] For example, the graft copolymer (A) can be prepared by a known polymerization method including emulsion polymerization, suspension polymerization, bulk polymerization, etc., preferably emulsion polymerization.
[0039] For example, the graft copolymer (A) can be prepared by continuously or intermittently adding a monomer mixture comprising 5 to 20 parts by weight of the vinyl cyanide compound and 10 to 40 parts by weight of the aromatic vinyl compound to a mixed solution comprising 50 to 80 parts by weight (solid basis) of the conjugated diene rubber, 0.1 to 5 parts by weight of an emulsifier, 0.1 to 3 parts by weight of a molecular weight regulator and 0.05 to 1 part by weight of an initiator, based on 100 parts by weight in total of the conjugated diene rubber, the aromatic vinyl compound and the vinyl cyanide compound contained in the graft copolymer, and then performing polymerization.
[0040] As another example, based on a total of 100 parts by weight of the conjugated diene rubber, the aromatic vinyl compound and the vinyl cyanide compound, the graft copolymer (A) can be prepared by: adding a mixed solution containing 5 to 20 parts by weight of the vinyl cyanide compound, 10 to 40 parts by weight of the aromatic vinyl compound, 10 to 50 parts by weight of deionized water, 0.09 to 1.5 parts by weight of an initiator, 0.1 to 2 parts by weight of an emulsifier and 0.05 to 1.5 parts by weight of a molecular weight regulator mixed in a separate mixing device to 50 to 80 parts by weight (based on solids) of conjugated diene rubber latex and 60 to 150 parts by weight of deionized water at 65 to 75° C. for 2 to 4 hours; adding 0.01 to 0.5 parts by weight of an initiator thereto; raising the temperature to 75 to 80° C. for 30 to 90 minutes; and terminating the graft polymerization when the polymerization conversion rate is 93 to 99% by weight. In this case, impact resistance, mechanical strength and moldability can be excellent.
[0041] In this specification, based on the total weight of monomers added until the completion of polymerization as 100%, the polymerization conversion rate can be defined as the weight percentage of monomers converted into polymers until the measurement time. There is no particular limitation on the method for measuring the polymerization conversion rate as long as the method follows this definition. As a specific example, after 1.5g of the prepared (co)polymer latex is dried in a hot air dryer at 150°C for 15 minutes, the weight of the dried latex is measured, and the total solid content (TSC) is calculated by the following formula 2. Then, the polymerization conversion rate is calculated by substituting the total solid content value into the following formula 3. In formula 3, the total weight of the added monomers is set to 100 parts by weight.
[0042] [Formula 2]
[0043] Total solid content (TSC; %) = (weight after drying / weight before drying) × 100
[0044] [Equation 3]
[0045] Polymerization conversion (%) = [total solid content (TSC) × (total weight of added monomers, deionized water and auxiliary raw materials) / 100] - (weight of auxiliary raw materials added except monomers and deionized water)
[0046] In Formula 3, the auxiliary raw materials include an initiator, an emulsifier, and a molecular weight regulator, and include an electrolyte when an electrolyte is used.
[0047] For example, the conjugated diene compound may include one or more selected from the group consisting of 1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-ethyl-1,3-butadiene, 1,3-pentadiene, isoprene, and chloroprene.
[0048] For example, the vinyl cyanide compound may include one or more selected from acrylonitrile, methacrylonitrile, ethacrylonitrile and isopropylacrylonitrile, preferably acrylonitrile.
[0049] For example, the aromatic vinyl compound may include one or more selected from styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, m-methylstyrene, ethylstyrene, isobutylstyrene, tert-butylstyrene, o-bromostyrene, p-bromostyrene, m-bromostyrene, o-chlorostyrene, p-chlorostyrene, m-chlorostyrene, vinyltoluene, vinylxylene, fluorostyrene and vinylnaphthalene, preferably one or more selected from styrene and α-methylstyrene, more preferably styrene. In this case, due to appropriate fluidity, processability and mechanical properties such as impact resistance can be excellent.
[0050] In the present specification, a derivative is a compound produced by substituting a hydrogen atom or an atomic group of an initial compound with another atom or an atomic group, for example, refers to a compound produced by substitution with a halogen or an alkyl group.
[0051] For example, the emulsifier may include one or more selected from allyl aryl sulfonate, methyl alkyl sulfonic acid alkali metal salt, sulfonated alkyl ester, fatty acid soap and rosin acid alkali metal salt. In this case, polymerization stability may be excellent.
[0052] For example, the molecular weight regulator may include one or more selected from tert-dodecyl mercaptan, n-dodecyl mercaptan, n-octyl mercaptan and carbon tetrachloride, preferably tert-dodecyl mercaptan.
[0053] For example, the initiator can be a water-soluble persulfate polymerization initiator, a fat-soluble polymerization initiator or an oxidation-reduction catalyst system. For example, the water-soluble persulfate polymerization initiator can include one or more selected from potassium persulfate, sodium persulfate and ammonium persulfate, and the fat-soluble polymerization initiator can include one or more selected from cumene hydroperoxide, diisopropylbenzene hydroperoxide, azobisisobutyronitrile, tert-butyl hydroperoxide, p-menthane hydroperoxide and benzoyl peroxide.
[0054] For example, latex prepared by emulsion polymerization may be coagulated using a coagulant such as sulfuric acid, MgSO4, CaCl2 or Al2(SO4)3, and then the coagulated latex may be aged, dehydrated and dried to obtain a powdered latex.
[0055] For example, when preparing the graft copolymer (A), an oxidation-reduction catalyst may be further included. For example, the oxidation-reduction catalyst may include one or more selected from sodium formaldehyde sulfoxylate, sodium ethylenediaminetetraacetate, ferrous sulfate, glucose, sodium pyrophosphate and sodium sulfite, but is not limited thereto. The oxidation-reduction catalyst commonly used when preparing the ABS graft copolymer may be used in the present invention without particular limitation.
[0056] Other additives not specifically mentioned in this specification such as electrolytes may be appropriately selected as needed. The additives may be used within the range commonly used in the preparation of vinyl cyanide compound-conjugated diene compound-aromatic vinyl compound graft copolymer latex without particular limitation.
[0057] In the method for preparing the graft copolymer, in addition to the above conditions, other reaction conditions such as reaction time, reaction temperature, pressure and addition time of reactants may be appropriately selected and used without particular limitation, as long as the other reaction conditions are commonly used in the field to which the present invention belongs.
[0058] (B) α-Methylstyrene-vinyl cyanide compound-aromatic vinyl compound copolymer
[0059] The content of the α-methylstyrene-vinyl cyanide compound-aromatic vinyl compound copolymer (B) (hereinafter referred to as "copolymer (B)") is 15 wt% to 35 wt% based on the total weight of the thermoplastic resin composition. In this case, heat resistance and mechanical properties can be excellent. As a preferred example, the content of the copolymer (B) can be 10 wt% to 30 wt%, more preferably 15 wt% to 35 wt%, based on 100 wt% of the thermoplastic resin composition. Within this range, heat resistance can be excellent without deteriorating the appearance.
[0060] For example, copolymer (B) may contain 50 to 80% by weight of α-methylstyrene, 10 to 30% by weight of vinyl cyanide compounds, and 5 to 25% by weight of aromatic vinyl compounds (excluding α-methylstyrene), preferably 50 to 75% by weight of α-methylstyrene, 15 to 30% by weight of vinyl cyanide compounds, and 5 to 25% by weight of aromatic vinyl compounds (excluding α-methylstyrene), more preferably 55 to 75% by weight of α-methylstyrene, 15 to 25% by weight of vinyl cyanide compounds, and 5 to 20% by weight of aromatic vinyl compounds (excluding α-methylstyrene). Within this range, heat resistance may be excellent without deteriorating other physical properties.
[0061] For example, the weight average molecular weight of the copolymer (B) may be 50,000 to 200,000 g / mol, preferably 60,000 to 180,000 g / mol, and more preferably 70,000 to 160,000 g / mol. Within this range, heat resistance may be excellent.
[0062] For example, the glass transition temperature (Tg) of the copolymer (B) may be 100° C. to 140° C., preferably 110° C. to 130° C. Within this range, heat resistance may be excellent without deteriorating other physical properties.
[0063] In the present specification, the glass transition temperature (Tg) can be measured using Pyris 6DSC (Perkin Elmer Co.) at a heating rate of 10° C. / min.
[0064] The preparation method commonly used in the field of the present invention can be used as the method for preparing copolymer (B), without particular limitation. As a specific example, the method for preparing copolymer (B) can include adding 0.05 to 0.5 weight portion of a multifunctional initiator to 100 weight portions of a monomer mixture comprising 50 weight % to 80 weight % of alpha-methylstyrene, 10 weight % to 30 weight % of a vinyl cyanide compound and 5 weight % to 25 weight % of an aromatic vinyl compound (except alpha-methylstyrene) and performing polymerization. In this case, the polymerization can be suspension polymerization, emulsion polymerization, solution polymerization or bulk polymerization, preferably bulk polymerization. In this case, heat resistance and fluidity can be excellent.
[0065] As the polymer (B), a commercially available product may be used as long as the commercially available product complies with the definition of the present invention.
[0066] (C) Aromatic vinyl compound-vinyl cyanide compound copolymer
[0067] Based on the total weight of the thermoplastic resin composition, the content of the aromatic vinyl compound-vinyl cyanide compound copolymer (C) (hereinafter referred to as "copolymer (C)") is 5 wt% to 30 wt%. In this case, mechanical properties, moldability and appearance can be excellent. As a preferred example, based on 100 wt% of the thermoplastic resin composition, the content of the copolymer (C) can be 10 wt% to 30 wt%, more preferably 15 wt% to 30 wt%. Within this range, chemical resistance, mechanical properties, moldability, appearance and physical property balance can be excellent.
[0068] For example, the copolymer (C) may contain 20 to 40% by weight of a vinyl cyanide compound and 60 to 80% by weight of an aromatic vinyl compound (excluding α-methylstyrene), preferably 20 to 35% by weight of a vinyl cyanide compound and 65 to 80% by weight of an aromatic vinyl compound (excluding α-methylstyrene), and more preferably 23 to 33% by weight of a vinyl cyanide compound and 67 to 77% by weight of an aromatic vinyl compound (excluding α-methylstyrene). Within this range, moldability may be excellent due to appropriate fluidity.
[0069] For example, the weight average molecular weight of the copolymer (C) may be 70,000 to 200,000 g / mol, preferably 80,000 to 180,000 g / mol, and more preferably 90,000 to 160,000 g / mol. Within this range, chemical resistance, processability, and physical property balance may be excellent.
[0070] For example, the aromatic vinyl compound contained in the copolymer (C) may include one or more selected from styrene, ethylstyrene, o-bromostyrene, p-bromostyrene, m-bromostyrene, o-chlorostyrene, p-chlorostyrene, m-chlorostyrene, vinyltoluene, vinylxylene, fluorostyrene and vinylnaphthalene, preferably styrene.
[0071] For example, the vinyl cyanide compound may include one or more selected from acrylonitrile, methacrylonitrile, ethacrylonitrile and isopropylacrylonitrile, preferably acrylonitrile.
[0072] For example, copolymer (C) may further comprise 0 to 30 wt %, preferably 1 to 20 wt %, more preferably 5 to 10 wt % of one or more monomers selected from unsaturated carboxylic acids, anhydrides of unsaturated carboxylic acids and maleimide-based monomers. Therefore, when the copolymer comprises a comonomer during polymerization, heat resistance and processability may be excellent.
[0073] For example, the unsaturated carboxylic acid may include one or more selected from maleic acid, acrylic acid and methacrylic acid, the anhydride of the unsaturated carboxylic acid may be the anhydride of the unsaturated carboxylic acid, and the maleimide monomer may be a maleimide N-substituted by an alkyl group having 1 to 5 carbon atoms or an aryl group having 6 to 10 carbon atoms, as a specific example, it may be N-phenylmaleimide, maleimide or a mixture thereof.
[0074] The aromatic vinyl compound-vinyl cyanide compound copolymer (C) can be prepared by emulsion polymerization, suspension polymerization, bulk polymerization or continuous bulk polymerization, preferably emulsion polymerization or suspension polymerization.
[0075] A commercially available product can be used as the copolymer (C) as long as the commercially available product complies with the definition of the present invention.
[0076] (D) Polycarbonate resin
[0077] Based on the total weight of the thermoplastic resin composition, the content of the polycarbonate resin (D) is 23% to 47% by weight. In this case, without deteriorating other physical properties, mechanical properties and heat resistance can be excellent. As a preferred example, based on a total of 100% by weight of the thermoplastic resin composition, the content of the copolymer (D) can be 25% to 47% by weight, more preferably 25% to 45% by weight, and even more preferably 30% to 40% by weight. Within this range, heat resistance and mechanical properties can be excellent.
[0078] There is no particular limitation on the type of the polycarbonate resin (D). For example, the polycarbonate resin (D) may be a resin obtained by polymerizing a bisphenol-based monomer and a carbonate precursor.
[0079] For example, the bisphenol monomers may include bis(4-hydroxyphenyl)methane, bis(4-hydroxyphenyl)ether, bis(4-hydroxyphenyl)sulfone, bis(4-hydroxyphenyl)sulfoxide, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxyphenyl)ketone, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)propane (bisphenol A; BPA), 2,2-bis(4-hydroxyphenyl)butane, 1,1-bis(4-hydroxyphenyl)cyclohexane (bisphenol Z; BPZ), 2,2-bis(4-hydroxy-3,5-dibromophenyl)-1,4-bis(4-hydroxyphenyl)-2,4-bis(4-hydroxyphenyl) ... One or more of bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dichlorophenyl)propane, 2,2-bis(4-hydroxy-3-bromophenyl)propane, 2,2-bis(4-hydroxy-3-chlorophenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, bis(4-hydroxyphenyl)diphenylmethane and α,ω-bis[3-(o-hydroxyphenyl)propyl]polydimethylsiloxane.
[0080] For example, the carbonate precursor may include one or more selected from dimethyl carbonate, diethyl carbonate, dibutyl carbonate, dicyclohexyl carbonate, diphenyl carbonate, ditolyl carbonate, bis(chlorophenyl) carbonate, m-tolyl carbonate, dinaphthyl carbonate, bis(diphenyl) carbonate, phosgene, triphosgene, diphosgene, phosgene bromide and dihaloformates.
[0081] For example, the polycarbonate resin (D) may include one or more selected from a linear polycarbonate resin, a branched polycarbonate resin, and a polyester carbonate copolymer resin, preferably a linear polycarbonate resin. In this case, fluidity may be improved, and thus the appearance may be excellent.
[0082] As a specific example, the linear polycarbonate resin may be a bisphenol A-based polycarbonate resin, without being limited thereto.
[0083] For example, the weight average molecular weight of the polycarbonate resin (D) may be 15,000 to 40,000 g / mol, preferably 20,000 to 35,000 g / mol. Within this range, mechanical properties such as impact strength and appearance may be excellent.
[0084] For example, the polycarbonate resin (D) may have a melt index of 10 g / 10 min or more, preferably 10 to 30 g / 10 min, and more preferably 15 to 25 g / 10 min, as measured at 300° C. under a load of 1.2 kg according to ASTM D1238. Within this range, compatibility, moldability, and physical property balance may be excellent.
[0085] For example, the polycarbonate resin (D) may have an Izod impact strength of 60 kg·cm / cm or more, preferably 60 to 80 kg·cm / cm, measured at a thickness of 1 / 8" according to ASTM D256. Within this range, mechanical properties may be excellent without deteriorating other physical properties.
[0086] A preparation method commonly used in the art can be used to prepare the polycarbonate resin (D), and a commercially available product can be used as the polycarbonate resin (D), as long as the commercially available product complies with the definition of the present invention.
[0087] (E) Polyester resin
[0088] Based on the total weight of the thermoplastic resin composition, the content of the polyester resin (E) is 3% to 17% by weight. In this case, without deteriorating other physical properties, mechanical properties and chemical resistance can be excellent. As a preferred example, based on 100% by weight of the thermoplastic resin composition, the content of the polyester resin (E) can be 3% to 15% by weight, more preferably 5% to 15% by weight, and even more preferably 5% to 10% by weight. Within this range, chemical resistance and mechanical properties can be excellent.
[0089] For example, the polyester resin (E) may have an intrinsic viscosity of 0.5 to 2 dl / g, preferably 0.5 to 1.5 dl / g, more preferably 0.5 to 1.0 dl / g, measured using dichloromethane as a solvent at 20° C. Within this range, mechanical properties and processability may be excellent.
[0090] In this specification, when measuring the intrinsic viscosity, unless otherwise noted, the sample to be measured is completely dissolved in dichloromethane and then filtered using a filter to obtain a filtrate. Then, using the obtained filtrate, the intrinsic viscosity is measured at 20°C using an Ubbelohde viscometer.
[0091] For example, the polyester resin (E) may include one or more selected from polyethylene adipate (PEA), polybutylene succinate (PBS), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT) and polyethylene naphthalate (PEN), preferably, one or more selected from polyethylene terephthalate and polybutylene terephthalate. In this case, the mechanical properties and formability of the composition can be good, so the physical property balance and chemical resistance can be excellent.
[0092] For example, the polyester resin (E) may be a copolymer prepared by polymerizing one or more selected from polytetramethylene glycol (PTMG), polyethylene glycol (PEG), polypropylene glycol (PPG), and low molecular weight aliphatic polyamide. In this case, mechanical properties may be excellent, but the present invention is not limited thereto.
[0093] A preparation method commonly used in the art can be used to prepare the polyester resin (E), and a commercially available product can be used as the polyester resin (E), as long as the commercially available product complies with the definition of the present invention.
[0094] Thermoplastic resin composition
[0095] The thermoplastic resin composition of the present invention comprises 20 to 40 wt% of a vinyl cyanide compound-conjugated diene rubber-aromatic vinyl compound graft copolymer (A), 10 to 35 wt% of an α-methylstyrene-vinyl cyanide compound-aromatic vinyl compound copolymer (B), 5 to 30 wt% of an aromatic vinyl compound-vinyl cyanide compound copolymer (C), 23 to 47 wt% of a polycarbonate resin (D), and 3 to 17 wt% of a polyester resin (E), wherein the weight of the copolymer (B) is greater than or equal to the weight of the copolymer (C), and the weight ratio of the polycarbonate resin (D) to the polyester resin (E) is 2:1 to 6:1. In this case, mechanical properties, moldability, heat resistance, and chemical resistance can be greatly improved.
[0096] For example, when a thermoplastic resin composition is prepared according to the specific composition ratio, when a sample having a size of 200 mm × 12.7 mm × 3.2 mm is fixed to a bending fixture having a strain of 1.1%, 1 cc of a diluent is applied thereto, and then the time for cracks to be generated on the surface of the sample is measured, the chemical resistance of the thermoplastic resin composition is 600 seconds or more, showing excellent chemical resistance (environmental stress cracking resistance, ESCR). For example, when the chemical resistance satisfies this range, cracks can be prevented from being generated due to organic solvents and detergents used in post-treatment processes such as painting and deposition. As another example, when the thermoplastic resin composition is used as a vent component of a vehicle, cracks can be prevented from occurring due to a vehicle air freshener. Therefore, the thermoplastic resin composition can be applied to various fields, and product degradation caused during use can be prevented.
[0097] The weight ratio of the polycarbonate resin (D) to the polyester resin (E) may be 2: 1 to 6: 1, preferably 2: 1 to 5: 1, more preferably 2: 1 to 4.5: 1, as a preferred example, may be 2.5: 1 to 6: 1, more preferably 3: 1 to 5.5: 1, as another preferred example, may be 2.2: 1 to 4.8: 1, more preferably 2.7: 1 to 4.6: 1, still more preferably 3: 1 to 4.5: 1, still more preferably 3: 1 to 4: 1. Within this range, mechanical properties and chemical resistance may be excellent without deteriorating other physical properties.
[0098] Preferably, the weight of the copolymer (B) is greater than or equal to the weight of the copolymer (C). In this case, moldability may be excellent without deteriorating other physical properties, thereby further improving the appearance.
[0099] For example, the thermoplastic resin composition may have a melt index of 55 g / 10 min or more, preferably 55 to 80 g / 10 min, more preferably 58 to 80 g / 10 min, and more preferably 58 to 75 g / 10 min, measured at 250° C. under a load of 10 kg according to ASTM D1238. Within this range, moldability and appearance may be excellent without deteriorating other physical properties.
[0100] For example, the heat deformation temperature (HDT) of the thermoplastic resin composition may be 100° C. or more, preferably 100° C. to 120° C., and more preferably 100° C. to 110° C., as measured according to ASTM D648-7. Within this range, heat resistance may be excellent without deteriorating other physical properties. In addition, for example, when the thermoplastic resin composition is used as an interior material for a vehicle, even if the temperature inside the vehicle rises to more than 50° C. in summer, product degradation may be prevented.
[0101] For example, the thermoplastic resin composition may have an Izod impact strength of 40 kgf·cm / cm or more, preferably 40 to 70 kgf·cm / cm, and more preferably 45 to 65 kgf·cm / cm, as measured using a test specimen having a thickness of 1 / 8" according to ASTM D256. Within this range, mechanical strength may be excellent without deteriorating other physical properties.
[0102] Method for preparing thermoplastic resin composition
[0103] The thermoplastic resin composition of the present invention can be prepared by a method comprising kneading and extruding 20 to 40 wt % of a vinyl cyanide compound-conjugated diene rubber-aromatic vinyl compound graft copolymer (A), 10 to 35 wt % of an α-methylstyrene-vinyl cyanide compound-aromatic vinyl compound copolymer (B), 5 to 30 wt % of an aromatic vinyl compound-vinyl cyanide compound copolymer (C), 23 to 47 wt % of a polycarbonate resin (D), and 3 to 17 wt % of a polyester resin (E) at 200 to 280° C., wherein the weight of the copolymer (B) is greater than or equal to the weight of the copolymer (C), and the weight ratio of the polycarbonate resin (D) to the polyester resin (E) is 2:1 to 6:1. In this case, mechanical properties, moldability, heat resistance, and chemical resistance may be excellent.
[0104] When a specimen having a size of 200 mm×12.7 mm×3.2 mm was fixed to a bending jig having a strain of 1.1%, 1 cc of a diluent was applied thereto, and then the time for cracks to occur on the surface of the specimen was measured, the chemical resistance of the thermoplastic resin composition prepared by the method was 600 seconds or more, showing excellent chemical resistance.
[0105] For example, the kneading and extruding steps may be performed at a temperature of 200° C. to 280° C. and a screw speed of 500 to 700 rpm, preferably at a temperature of 220° C. to 260° C. and a screw speed of 550 to 650 rpm. In this case, mechanical properties, chemical resistance, heat resistance, and appearance may be excellent.
[0106] For example, the kneading and extruding steps can be performed using one or more selected from a single screw extruder, a twin screw extruder and a Banbury mixer. The kneading and extruding steps can be performed by uniformly mixing the components using a single screw extruder, a twin screw extruder or a Banbury mixer and extruding to obtain a thermoplastic resin composition in the form of a pellet. In this case, the deterioration of mechanical properties and heat resistance can be prevented, and the appearance can be excellent.
[0107] As required, in the kneading and extrusion steps, the thermoplastic resin composition may further include one or more additives selected from lubricants, heat stabilizers, light stabilizers, antioxidants, UV stabilizers, dyes, pigments, colorants, mold release agents, antistatic agents, antibacterial agents, processing aids, compatibilizers, metal passivators, flame retardants, smoke suppressants, anti-drip agents, foaming agents, plasticizers, reinforcing agents, fillers, matte agents, friction reducers and anti-wear agents. For example, based on the sum of 100 parts by weight of graft copolymer (A), copolymer (B), copolymer (C), polycarbonate resin (D) and polyester resin (E), additives may be further included in an amount of 0.01 to 5 parts by weight, preferably 0.05 to 3 parts by weight, 0.05 to 2 parts by weight or 0.05 to 1 part by weight. Within this range, the desired physical properties can be effectively exhibited without deteriorating the inherent physical properties of the thermoplastic resin composition.
[0108] For example, the lubricant may include one or more selected from ethylene bisstearamide, oxidized polyethylene wax, magnesium stearate, calcium stearate, stearic acid, and silicone oil, without being limited thereto.
[0109] For example, the silicone oil may include one or more selected from dimethyl silicone oil, methyl hydrogen silicone oil, ester-modified silicone oil, hydroxy silicone oil, carbinol-modified silicone oil, vinyl silicone oil, and silicone acrylate.
[0110] For example, as the antioxidant, a phenol antioxidant, a phosphorus antioxidant, etc. can be used, but it is not limited thereto.
[0111] For example, as the antistatic agent, one or more selected from anionic surfactants and nonionic surfactants may be used without being limited thereto.
[0112] For example, as the release agent, one or more selected from glyceryl stearate and polyethylene glycol tetrastearate may be used without being limited thereto.
[0113] Molding
[0114] The molded article of the present invention comprises the thermoplastic resin composition of the present invention. In this case, mechanical properties, moldability, appearance, heat resistance and chemical resistance may be excellent.
[0115] The molded product has excellent mechanical strength, heat resistance and chemical resistance. Therefore, the molded product is suitable for automotive interior materials. As a specific example, the molded product can be an automotive vent, an instrument center box, a door interior panel or a spray paint product.
[0116] In describing the thermoplastic resin composition, the method for preparing the thermoplastic resin composition, and the molded article including the thermoplastic resin composition of the present invention, it should be noted that other conditions or equipment not explicitly described herein may be appropriately selected within the range generally practiced in the art without particular limitation.
[0117] Hereinafter, the present invention will be described in more detail with reference to the following preferred embodiments. However, these embodiments are provided for illustrative purposes only and should not be construed as limiting the scope and spirit of the present invention. In addition, it will be apparent to those skilled in the art that various changes and modifications may be made without departing from the spirit and scope of the present invention, and these changes and modifications are also within the scope of the appended claims.
[0118] [Example]
[0119] Materials used in the following Examples and Comparative Examples are as follows.
[0120] (A) Vinyl cyanide compound-conjugated diene rubber-aromatic vinyl compound graft copolymer: containing 60% by weight of an average particle size of ABS graft copolymer of 10 wt% butadiene rubber, 10 wt% acrylonitrile and 30 wt% styrene (DP270, LG Chemical Co.)
[0121] (B) α-methylstyrene-vinyl cyanide compound-aromatic vinyl compound copolymer: a heat-resistant AMS-SAN resin prepared by copolymerizing 66 wt% of α-methylstyrene, 28 wt% of acrylonitrile and 6 wt% of styrene (weight average molecular weight: 95,000 g / mol, 99 UH, LG Chemical Co.)
[0122] (C) Aromatic vinyl compound-vinyl cyanide compound copolymer: SAN resin prepared by copolymerizing 28 wt% acrylonitrile and 72 wt% styrene (weight average molecular weight: 130,000 g / mol, 92RF, LG Chemical Co.)
[0123] (D) Polycarbonate resin: bisphenol A type polycarbonate resin (PC30, LG Chemical Co.) having a weight average molecular weight of 27,000 g / mol, an intrinsic viscosity of 1.0 dl / g, and a melt index of 30 g / min at 300° C. under a load of 1.2 kg according to ASTM D1238
[0124] (E) Polyester resin: polyethylene terephthalate with an intrinsic viscosity of 0.65 dl / g (JSB599, Huvis Co.)
[0125] (F) Antioxidant: Primary antioxidant (Wingstay-L, ELIOKEM Co.)
[0126] (G) Lubricant: Oxidized polyethylene wax lubricant (PETS-AHS, FACI Co.)
[0127] Examples 1 to 4 and Comparative Examples 1 to 9
[0128] The graft copolymer (A), copolymer (B), copolymer (C), polycarbonate resin (D), polyester resin (E), antioxidant (F) and lubricant (G) were mixed using a super mixer according to the contents shown in Table 1 below, and then the mixture was extruded using a twin-screw extruder (screw diameter: 26 mm, L / D=40) at an extrusion temperature of 240° C. and a screw speed of 600 rpm to obtain pellets.
[0129] The prepared thermoplastic resin composition in the form of pellets was dried at 80° C. for more than 4 hours, and then injection molded using an injection molding machine at an injection temperature of 240° C., a mold temperature of 60° C., and an injection rate of 30 mm / sec to obtain a specimen. The specimen was left to stand at room temperature (20° C. to 26° C.) for more than 48 hours, and then its physical properties were measured.
[0130] [Test example]
[0131] The physical properties of the samples prepared in Examples and Comparative Examples were measured according to the following methods, and the results are shown in Table 2 below.
[0132] *Izod impact strength (kgf·cm / cm): The Izod impact strength was measured according to ASTM D256 using a test specimen having a thickness of 1 / 8″.
[0133] * Melt flow index (g / 10 min): The melt flow index was measured at 250° C. for 10 minutes under a load of 10 kg according to ASTM D1238.
[0134] *Heat Deflection Temperature (℃): According to ASTM D648-7, using a 1 / 4″ thick specimen at 18.6kgf / cm 2 The heat deformation temperature is measured under a load of .
[0135] *Chemical resistance: By injection molding, a specimen with a size of 200 mm × 12.7 mm × 3.2 mm was prepared. The specimen was fixed to a bending fixture with a strain of 1.1%, and 1 cc of a diluent (T803, NOROOBEE Chemical Co.) was applied thereto. Then, cracks appearing on the surface of the specimen were observed with the naked eye and the time for the crack to appear was measured. On a 600 second basis, when the time for the crack to appear was 600 seconds or more, it was recorded as "O", and when the time for the crack to appear was less than 600 seconds, it was recorded as "X".
[0136] [Table 1]
[0137]
[0138] [Table 2]
[0139]
[0140] As shown in Tables 1 and 2, in the case of Examples 1 to 4 according to the present invention, impact strength, melt index, heat deformation temperature, and chemical resistance are excellent compared to Comparative Examples 1 to 9 outside the scope of the present invention.
[0141] Figure 1 The chemical resistance test results of the embodiments and comparative examples according to the present invention are shown. Figure 1 In the case of Examples 1 and 3 according to the present invention, no cracks occurred even after 600 seconds after the diluent was applied. On the other hand, in the case of Comparative Examples 1, 2, and 4, the specimens were broken. These results show that the examples according to the present invention exhibit significantly improved chemical resistance.
Claims
1. A thermoplastic resin composition comprising: 20 to 30 wt% of a vinyl cyanide compound-conjugated diene rubber-aromatic vinyl compound graft copolymer (A), 15 to 30% by weight of an α-methylstyrene-vinyl cyanide compound-aromatic vinyl compound copolymer (B), 15 to 30 wt% of an aromatic vinyl compound-vinyl cyanide compound copolymer (C), 30 to 40 wt% of a polycarbonate resin (D); and 5 to 10 wt% of a polyester resin (E), in, The weight of the copolymer (B) is greater than or equal to the weight of the copolymer (C), and the weight ratio of the polycarbonate resin (D) to the polyester resin (E) is 2:1 to 4.5:
1.
2. The thermoplastic resin composition according to claim 1, in, The thermoplastic resin composition has chemical resistance of 600 seconds or more when a specimen having a size of 200 mm×12.7 mm×3.2 mm is fixed to a bending jig having a strain of 1.1%, 1 cc of a diluent is applied thereto, and then the time for cracks to be generated on the surface of the specimen is measured.
3. The thermoplastic resin composition according to claim 1, in, The graft copolymer (A) includes 50 to 80 wt % of a conjugated diene rubber, 5 to 20 wt % of a vinyl cyanide compound, and 10 to 40 wt % of an aromatic vinyl compound.
4. The thermoplastic resin composition according to claim 1, in, The average particle size of the conjugated diene rubber is to 5. The thermoplastic resin composition according to claim 1, in, The copolymer (B) contains 50 to 80% by weight of α-methylstyrene, 10 to 30% by weight of a vinyl cyanide compound, and 5 to 25% by weight of an aromatic vinyl compound other than α-methylstyrene.
6. The thermoplastic resin composition according to claim 1, in, The copolymer (C) contains 20 to 40 wt % of a vinyl cyanide compound and 60 to 80 wt % of an aromatic vinyl compound.
7. The thermoplastic resin composition according to claim 1, in, The polycarbonate resin (D) includes one or more selected from the group consisting of a linear polycarbonate resin, a branched polycarbonate resin, and a polyester carbonate copolymer resin.
8. The thermoplastic resin composition according to claim 1, in, The polycarbonate resin (D) has a melt index of 10 g / 10 min or more as measured at 300° C. under a load of 1.2 kg according to ASTM D1238.
9. The thermoplastic resin composition according to claim 1, in, The polycarbonate resin (D) has a weight average molecular weight of 15,000 g / mol to 40,000 g / mol.
10. The thermoplastic resin composition according to claim 1, in, The polyester resin (E) includes one or more selected from polyethylene adipate (PEA), polybutylene succinate (PBS), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT) and polyethylene naphthalate (PEN).
11. The thermoplastic resin composition according to claim 1, in, The polyester resin (E) has an intrinsic viscosity of 0.5 to 2 dl / g as measured at 20°C using dichloromethane as a solvent.
12. The thermoplastic resin composition according to claim 1, in, The thermoplastic resin composition has a melt index of 55.0 g / 10 min or more as measured at 250° C. under a load of 10 kg according to ASTM D1238.
13. The thermoplastic resin composition according to claim 1, in, According to ASTM D648, use a 1 / 4″ thick specimen at 18.6 kgf / cm 2 The heat deformation temperature of the thermoplastic resin composition is 100° C. to 120° C. when measured under a load of .
14. A method for preparing a thermoplastic resin composition, comprising the steps of kneading and extruding 20 wt % to 30 wt % of a vinyl cyanide compound-conjugated diene rubber-aromatic vinyl compound graft copolymer (A), 15 wt % to 30 wt % of an α-methylstyrene-vinyl cyanide compound-aromatic vinyl compound copolymer (B), 15 wt % to 30 wt % of an aromatic vinyl compound-vinyl cyanide compound copolymer (C), 30 wt % to 40 wt % of a polycarbonate resin (D) and 5 wt % to 10 wt % of a polyester resin (E) at 200° C. to 280° C., in, The weight of the copolymer (B) is greater than or equal to the weight of the copolymer (C), and the weight ratio of the polycarbonate resin (D) to the polyester resin (E) is 2:1 to 4.5:
1.