Separator for lithium secondary battery, method for manufacturing the same, and lithium secondary battery including the same
By coating the lithium secondary battery separator with a thermosetting phenol-based resin with hydroxyl and aromatic rings to form a network structure, the problem of thermal shrinkage of the lithium secondary battery separator at high temperatures is solved, and the heat resistance and thermal safety are improved. , enhanced energy density and breathability.
Patent Information
- Application Number
- CN202180026896.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-04-03
- Filing Date
- 2021-03-31
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-03-31
AI Technical Summary
Existing lithium secondary battery separators have thermal shrinkage problems in high temperature environments, leading to the risk of short circuits, and the thickening of inorganic particles reduces energy density and increases resistance.
A thermosetting phenol-based resin with hydroxyl and aromatic rings is used to form a polymer coating, which is coated on a porous polymer substrate. It forms a network structure through a thermosetting reaction to improve heat resistance, reduce swelling in the electrolyte solution, and inhibit thermal shrinkage. .
Provides improved heat resistance and thermal safety in high temperature environments, maintains the bonding strength of the separators, increases energy density and breathability, and reduces the risk of thermal shrinkage.
Smart Images

Figure FDA0004962441660000011 
Figure FDA0004962441660000021 
Figure FDA0004962441660000031
Abstract
Description
Technical Field
[0001] The present disclosure relates to a separator for a lithium secondary battery, a method of manufacturing the same, and a lithium secondary battery including the same.
[0002] This application claims the priority of Korean Patent Application No. 10-2020-0041003 filed in Korea on April 3, 2020, the disclosure of which is incorporated herein by reference. Background Art
[0003] Recently, energy storage technology has been gaining attention. As the application of energy storage technology has expanded to mobile phones, cameras and laptops, and even electric vehicles, many efforts have been made to develop electrochemical devices. In this regard, electrochemical devices are receiving more attention, especially the development of rechargeable secondary batteries is the focus of attention, and recently, in the development of batteries, new electrode and battery designs have been developed to improve energy density and specific energy.
[0004] Among commercially available secondary batteries, lithium secondary batteries developed in the early 1990s have higher operating voltage and energy density than conventional batteries using aqueous electrolytes such as Ni-MH, Ni-Cd, and lead-acid batteries, and with these advantages, lithium secondary batteries are gaining much attention.
[0005] Electrochemical devices, including lithium secondary batteries, have been produced by multiple manufacturers, and each shows different safety characteristics. It is very important to evaluate and manage the safety of electrochemical devices. The most important consideration is that the electrochemical device should not injure the user in the event of a failure, and for this purpose, safety standards strictly prohibit combustion and fire in electrochemical devices. Among the safety characteristics of electrochemical devices, overheating and eventual thermal runaway or perforation of the separator in the electrochemical device cause a high risk of explosion.
[0006] The separator prevents short circuits between the positive and negative electrodes and provides a path for the movement of lithium ions. Therefore, the separator is an important factor affecting the safety and output characteristics of the battery. However, polyolefin-based porous polymer substrates conventionally used as separators for electrochemical devices exhibit extremely severe thermal shrinkage behavior at 130°C or higher due to material properties and procedural characteristics of the manufacturing process including stretching, resulting in a short circuit between the positive and negative electrodes.
[0007] In order to improve heat resistance, attempts have been made to form a porous coating including inorganic particles and a thermosetting binder polymer on a porous polymer substrate. When a porous coating is formed, heat resistance can be improved compared to using a porous polymer substrate alone. However, when exposed to a high temperature environment higher than the melting point of the binder polymer, there is a limitation to improving thermal safety. In addition, the porous coating including inorganic particles increases the thickness of the separator, resulting in a decrease in energy density and an increase in resistance.
[0008] Meanwhile, when the polymer coated on the porous polymer substrate is swollen or dissolved by the electrolyte solution, the adhesive strength of the coating layer to the polymer substrate is reduced, which deteriorates the function of suppressing thermal shrinkage of the separator. Summary of the invention
[0009] Technical issues
[0010] The present disclosure is directed to providing a separator that improves heat resistance without using inorganic particles and suppresses thermal shrinkage when immersed in an electrolyte solution.
[0011] The present disclosure is further directed to providing a method of manufacturing a separator for a lithium secondary battery having the above-mentioned features.
[0012] The present disclosure is further directed to providing a lithium secondary battery including the separator having the above-mentioned features.
[0013] Technical Solution
[0014] One aspect of the present disclosure provides a separator for a lithium secondary battery according to the following embodiments.
[0015] A first embodiment relates to a separator for a lithium secondary battery.
[0016] The separator for a lithium secondary battery includes a porous polymer substrate having a plurality of pores and a polymer coating formed on at least one surface of the porous polymer substrate, wherein the polymer coating includes a thermosetting phenol-based resin having at least one hydroxyl group and an aromatic ring, and the coating amount of the thermosetting phenol-based resin is based on per 1 m2 of one surface to be coated. 2 The porous polymer substrate weighs 0.01 g to 3 g.
[0017] A second embodiment relates to a separator for a lithium secondary battery according to the first embodiment,
[0018] The phenol-based binder polymer includes at least one of a novolac-type phenol resin represented by the following Formula 1 and a resole-type phenol resin represented by the following Formula 2:
[0019] [Formula 1]
[0020]
[0021] (In Formula 1, n is an integer of 1 or greater, and R is any one of H, an optionally substituted alkyl group having 1 to 100 carbon atoms, an optionally substituted alkoxy group having 1 to 100 carbon atoms, and an optionally substituted alkenyl group having 1 to 100 carbon atoms).
[0022] [Formula 2]
[0023]
[0024] (In Formula 2, n and m are each an integer of 1 or greater, and R is any one of H, an optionally substituted alkyl group having 1 to 100 carbon atoms, an optionally substituted alkoxy group having 1 to 100 carbon atoms, and an optionally substituted alkenyl group having 1 to 100 carbon atoms).
[0025] A third embodiment relates to a separator for a lithium secondary battery according to the first or second embodiment,
[0026] The thermosetting phenol-based resin is thermoset at 120°C to 200°C.
[0027] A fourth embodiment relates to the separator for a lithium secondary battery according to any one of the first to third embodiments,
[0028] The thermosetting phenol-based resin is a phenol-formaldehyde resin.
[0029] A fifth embodiment relates to the separator for a lithium secondary battery according to any one of the first to fourth embodiments,
[0030] The coating amount of the thermosetting phenolic resin is based on the coating surface per 1m 2 The porous polymer substrate is 0.05 g to 2.5 g, and more specifically, the coating amount of the thermosetting phenol-based resin is based on per 1 m 2 The porous polymer substrate weighs 0.35 g to 2.1 g.
[0031] A sixth embodiment relates to the separator for a lithium secondary battery according to any one of the first to fifth embodiments,
[0032] The porous polymer substrate comprises a porous polymer film made of at least one of polyethylene or polypropylene.
[0033] Another aspect of the present disclosure provides a method of manufacturing a separator according to the following embodiments.
[0034] A seventh embodiment relates to a method of manufacturing a separator for a lithium secondary battery,
[0035] The method comprises: (S1) preparing a polymer solution in which a thermosetting phenol-based resin having at least one hydroxyl group and an aromatic ring is dissolved in a solvent; and (S2) coating the polymer solution on at least one surface of a porous polymer substrate so that the coating amount of the thermosetting phenol-based resin is 100% based on per 1 m2 of the coated surface. 2 The porous polymer substrate weighs 0.01 g to 3 g and is dried to form a polymer coating.
[0036] An eighth embodiment relates to the method for manufacturing the separator for a lithium secondary battery according to the seventh embodiment,
[0037] The phenol-based binder polymer includes at least one of a novolac-type phenol resin represented by the following Formula 1 and a resole-type phenol resin represented by the following Formula 2:
[0038] [Formula 1]
[0039]
[0040] (In Formula 1, n is an integer of 1 or greater, and R is any one of H, an optionally substituted alkyl group having 1 to 100 carbon atoms, an optionally substituted alkoxy group having 1 to 100 carbon atoms, and an optionally substituted alkenyl group having 1 to 100 carbon atoms).
[0041] [Formula 2]
[0042]
[0043] (In Formula 2, n and m are each an integer of 1 or greater, and R is any one of H, an optionally substituted alkyl group having 1 to 100 carbon atoms, an optionally substituted alkoxy group having 1 to 100 carbon atoms, and an optionally substituted alkenyl group having 1 to 100 carbon atoms).
[0044] A ninth embodiment relates to the method for manufacturing a lithium secondary battery according to the seventh or eighth embodiment,
[0045] The thermosetting phenol-based resin is thermoset at 120°C to 200°C.
[0046] A tenth embodiment relates to a method for manufacturing a lithium secondary battery according to any one of the seventh to ninth embodiments,
[0047] The coating amount of the thermosetting phenolic resin is based on the coating surface per 1m2 The porous polymer substrate is 0.05 g to 2.5 g, and more specifically, the coating amount of the thermosetting phenol-based resin is based on per 1 m 2 The porous polymer substrate weighs 0.35 g to 2.1 g.
[0048] Yet another embodiment of the present disclosure provides a lithium secondary battery including a positive electrode, a negative electrode, and a separator interposed between the cathode and the anode, wherein the separator is the separator defined in any one of the aforementioned embodiments.
[0049] Beneficial Effects
[0050] According to an embodiment of the present disclosure, a polymer coating layer including a thermosetting phenol-based resin having at least one hydroxyl group and an aromatic ring is formed on at least one surface of a porous polymer substrate, and the coating amount of the thermosetting phenol-based resin is controlled to be 0.1% based on per 1 m2 of the coated one surface. 2 The porous polymer substrate weighs 0.01 g to 3 g.
[0051] When an electrochemical device including the separator is exposed to high temperature due to combustion or the like, the thermosetting phenol-based resin is thermoset to form a network structure. Thus, a separator having enhanced heat resistance and improved thermal safety can be provided without using inorganic particles.
[0052] Furthermore, in the separator of the present disclosure having the above-mentioned features, the polymer coating layer is less swollen or dissolved by the electrolyte solution when immersed in the electrolyte solution, thereby suppressing thermal shrinkage of the separator. DETAILED DESCRIPTION
[0053] Hereinafter, embodiments of the present disclosure will be described. Prior to the description, it should be understood that the terms used in the specification and the appended claims should not be interpreted as being limited to the common meaning and dictionary meaning, but should be interpreted based on the meaning and concept of the technical aspects of the corresponding present disclosure on the basis of the principle that the inventor is allowed to appropriately define the terms for the best interpretation. Therefore, the configuration described in the embodiments disclosed in this specification is only the most preferred embodiment of the present disclosure, and does not fully describe the technical aspects of the present disclosure, so it should be understood that various other equivalents or improvements may be made to it when submitting this application.
[0054] The term “comprising”, when used in the present specification, specifies the presence of claimed elements, but does not exclude the presence or addition of one or more other elements, unless the context clearly indicates otherwise.
[0055] In general, lithium secondary batteries use porous polymer substrates as separators. The porous polymer substrate may include a nonwoven fabric substrate made of polymer fibers and a film substrate formed by melting and extruding the polymer, and among the polymer substrates, the film substrate especially shows thermal shrinkage behavior. Therefore, in order to improve the heat resistance of the separator, a porous coating including inorganic particles and a binder polymer on at least one surface of the porous polymer substrate is introduced. When the porous coating is formed, the heat resistance of the separator can be improved compared to using the porous polymer substrate alone.
[0056] Thermosetting fluorine-based binder resins are mainly used for the binder polymer, and there is a limit to improving thermal safety when exposed to a high temperature environment higher than the melting point of the binder polymer. In addition, when a porous coating including inorganic particles is introduced as described above, the thickness of the separator increases, resulting in a decrease in energy density and an increase in resistance. At the same time, when the polymer coated on the porous polymer substrate is swollen or dissolved by the electrolyte solution, the bonding strength of the coating to the polymer substrate is reduced, which significantly deteriorates the function of suppressing thermal shrinkage of the separator.
[0057] In order to solve this problem, the present inventors aim to provide a separator having improved heat resistance of a porous coating when an electrochemical device including the separator is exposed to high temperature due to combustion or the like, and which is less swollen or dissolved by an electrolyte solution when immersed in an electrolyte solution, thereby suppressing thermal shrinkage of the separator.
[0058] In order to solve the above problems, a separator for a lithium secondary battery according to one aspect of the present disclosure includes:
[0059] a porous polymer substrate having a plurality of pores and a polymer coating formed on at least one surface of the porous polymer substrate,
[0060] wherein the polymer coating comprises a thermosetting phenolic resin having at least one hydroxyl group and an aromatic ring, and
[0061] The coating amount of the thermosetting phenolic resin is based on the coating surface per 1m 2 The porous polymer substrate weighs 0.01 g to 3 g.
[0062] In a separator according to one aspect of the present disclosure, when the separator is exposed to an abnormal environment such as high temperature, the thermosetting phenol-based resin of the polymer coating is thermoset to form a network structure. In this case, the network structure refers to a structure formed by a thermosetting reaction of the thermosetting phenol-based resin, and the network structure may be a three-dimensional network structure.
[0063] When the thermosetting phenol-based resin of the polymer coating forms a network structure through a thermosetting reaction in an abnormal environment such as high temperature, the heat resistance is better than when a thermoplastic polymer is used, and safety can be improved. That is, when a network structure is formed through a thermosetting reaction, the polymer coating can be made strong at very high temperatures.
[0064] That is, according to the present disclosure, a separator with improved heat resistance can be provided without a porous coating including inorganic particles. In addition, since it is not a porous coating including inorganic particles, it can be formed into a small thickness, thereby providing a battery with a high energy density for the same capacity. In addition, the thermosetting phenol-based resin is less swollen or dissolved by the electrolyte solution used in the lithium secondary battery, and there is no significant decrease in the bonding strength of the polymer coating to the porous polymer substrate after being immersed in the electrolyte solution, thereby preventing the functional degradation of suppressing the thermal shrinkage of the separator after being immersed in the electrolyte solution.
[0065] [Polymer coating comprising a thermosetting phenolic resin]
[0066] The polymer coating includes a thermosetting phenolic-based resin.
[0067] In this specification, the polymer coating refers to a coating including a polymer as a main component and having no inorganic particles. Of course, the polymer coating may include other components besides the inorganic particles without departing from the present disclosure.
[0068] Thermosetting phenol-based resins have at least one hydroxyl group and an aromatic ring.
[0069] Thermosetting phenol-based resins form a network structure through a curing reaction caused by heat at high temperatures. Specifically, the thermosetting phenol-based resins may be thermoset through a thermosetting reaction at high temperatures, for example, 120°C or higher, or more specifically 120°C to 200°C.
[0070] The thermosetting phenol-based resin may include at least one of a novolac-type phenol resin represented by the following Formula 1 or a resole-type phenol resin represented by the following Formula 2, and may further include a modified phenol resin. Specifically, any thermosetting phenol-based resin obtained by an aldehyde condensation reaction of phenol and its derivatives may be used.
[0071] In this case, the above formula 1 can be expressed as follows:
[0072] [Formula 1]
[0073]
[0074] In the above Formula 1, n is an integer of 1 or more, and R may be any one of H, an optionally substituted alkyl group having 1 to 100 carbon atoms, an optionally substituted alkoxy group having 1 to 100 carbon atoms, and an optionally substituted alkenyl group having 1 to 100 carbon atoms. In this case, the number of carbon atoms may be 1 to 100, 1 to 50, 1 to 30, or 1 to 10.
[0075] In the present disclosure, "novolak-type phenol resin" may be obtained by a reaction between a phenol compound and an aldehyde compound in the presence of an acidic catalyst. The novolac-type phenol resin has a phenolic hydroxyl group and is soluble in an alkali, but the solubility decreases as the molecular weight increases.
[0076] Since novolac resins have almost no hydroxymethyl groups that contribute to the curing reaction, novolac resins are easily 2 ) 6 N 4 ) and heated to form a cured product with a 3D structure.
[0077] The novolac-type resin may exist in an ortho-linkage or a para-linkage. In a specific embodiment of the present disclosure, the ratio of ortho-to-para in the novolac-type phenol resin may be less than 0.2, and more specifically less than 0.1.
[0078] In a specific embodiment of the present disclosure, the novolac phenol resin may include at least two types of novolac phenol resins having different ratios of ortho to para. In this case, when a high-para novolac phenol resin having more para connections than ortho connections is used, curing occurs more rapidly at high temperatures, thereby improving the safety of the separator.
[0079] The novolac type phenol resin preferably has a weight average molecular weight (Mw) of 1000 to 4000 and a polydispersity index (Mw / Mn, Mn is a number average molecular weight) of 2.0 or less. When the weight average molecular weight of the novolac type phenol resin has the above range, it is more advantageous for heat resistance and flowability when the slurry of the thin porous coating is prepared and formed. The novolac type phenol resin may have a hydroxyl equivalent of 100 g / eq to 200 g / eq.
[0080] The above formula 2 may have the following structure:
[0081] [Formula 2]
[0082]
[0083] In Formula 2 above, n and m are each an integer of 1 or greater, and R may be any one of H, an optionally substituted alkyl group having 1 to 100 carbon atoms, an optionally substituted alkoxy group having 1 to 100 carbon atoms, and an optionally substituted alkenyl group having 1 to 100 carbon atoms.
[0084] In the present disclosure, "resole type phenol resin" may be obtained by a reaction between a phenol compound and an aldehyde compound in the presence of a metal catalyst. The resole type phenol resin has a hydroxyl group and may form a crosslinked structure by a reaction with a novolac type phenol resin.
[0085] In this case, the metal catalyst may include manganese, magnesium, and zinc. Specifically, the metal catalyst may be a metal acetate. For example, the metal catalyst may include manganese acetate, magnesium acetate, and zinc acetate. These may be used alone or in combination.
[0086] The resol type phenol resin preferably has a weight average molecular weight (Mw) of 420 to 1,500 and a polydispersity index (Mw / Mn, Mn is a number average molecular weight) of 2.0 or less. When the weight average molecular weight of the resol type phenol resin has the above range, it is more advantageous for heat resistance and flowability when the slurry of the thin porous coating is prepared and formed. The resol type phenol resin may have a hydroxyl equivalent of 100 g / eq to 200 g / eq.
[0087] In this case, the weight average molecular weight may be measured using gel permeation chromatography (GPC) (PL GPC220, Agilent Technologies).
[0088] Specifically, the weight average molecular weight can be measured under the following analysis conditions:
[0089] - Column: PL MiniMixed B x 2
[0090] -Solvent: THF or DMF
[0091] -Flow rate: 0.3ml / min
[0092] - Sample concentration: 2.0mg / ml
[0093] -Injection volume: 10μl
[0094] - Column temperature: 40℃
[0095] -Detector: Agilent RI detector
[0096] -Standard: Polystyrene (fit to a third order polynomial)
[0097] -Data processing: ChemStation
[0098] In a specific embodiment of the present disclosure, the thermosetting phenol-based resin may be 2,3,4-trihydroxybenzophenone, 2,4,6-trihydroxybenzophenone, 2,2'-tetrahydroxybenzophenone, 4,4'-tetrahydroxybenzophenone, 2,3,4,3'-tetrahydroxybenzophenone, 2,3,4,4'-tetrahydroxybenzophenone, 2,3,4,2'-tetrahydroxy 4'-methylbenzophenone, 2,3,4,4'-tetrahydroxy 3'-methoxybenzophenone, 2,3,4,2'-pentahydroxybenzophenone, 2,3,4,6'-pentahydroxybenzophenone, 2,4,6,3'-hexahydroxybenzophenone, 2,4,6,4'-hexahydroxybenzophenone, 2,4,6,5'-hexahydroxybenzophenone, 3,4,5,3'-hexahydroxybenzophenone. The thermosetting phenol-based resin may be prepared from 1,2-dihydroxyphenyl-2-ol, 1,4-dihydroxyphenyl-3-ol, 1,1-tri(2,5-dimethyl-4-hydroxyphenyl)-3-phenylpropane, 4,4'-[1-[4-[1-[4-hydroxyphenyl]-1-methylethyl]phenyl]ethylidene]bisphenol, or bis(2,5-dimethyl-4-hydroxyphenyl)-2-hydroxyphenylmethane, and the above compounds may be used alone or in combination for manufacture. For example, the thermosetting phenol-based resin may be a phenolic resin.
[0099] In a specific embodiment of the present disclosure, the thermosetting phenol-based resin may form a network structure of the following structure when thermosetting in an abnormally high temperature environment.
[0100] For example, the network structure can be expressed by the following equation 3:
[0101] [Formula 3]
[0102]
[0103] In this case, the coating amount of the thermosetting phenol-based resin is based on the coating amount per 1m 2 The porous polymer substrate is 0.01 g to 3 g. Specifically, the loading amount of the thermosetting phenol-based resin can be 1 g per 1 m 2 The porous polymer substrate is 0.05 g to 2.5 g, and more specifically, the loading amount of the thermosetting phenol-based resin may be 1 m 2 Porous polymer substrate 0.35 g to 2.1 g.
[0104] Within the above range, the thermosetting phenol-based resin is coated on the pore walls of the porous polymer substrate, thereby improving the heat resistance of the separator. When the amount of the thermosetting phenol-based resin is less than 0.01 g, the desired thermal shrinkage may not be achieved. When the amount of the thermosetting phenol-based resin is greater than 3 g, the porosity decreases and the air permeation time increases too much.
[0105] The polymer coating of the present disclosure may include the above-mentioned thermosetting phenol-based resin alone or any other thermosetting resin or thermoplastic resin as the polymer without departing from the scope of the present disclosure.
[0106] [Porous polymer substrate]
[0107] In the separator according to one aspect of the present disclosure, the porous polymer substrate may specifically be a porous polymer film substrate or a porous polymer nonwoven substrate.
[0108] In the separator according to one aspect of the present disclosure, the porous polymer substrate may specifically be a porous polymer film substrate or a porous polymer nonwoven substrate.
[0109] The porous polymer film substrate may be a porous polymer film of polyolefin such as polyethylene and polypropylene, and the polyolefin porous polymer film substrate exhibits a shutdown function at a temperature of 80°C to 150°C, for example.
[0110] In this case, the polyolefin porous polymer film may be formed of polyolefin-based polymers including polyethylene such as high density polyethylene, linear low density polyethylene, low density polyethylene, and ultra high molecular weight polyethylene, polypropylene, polybutene, and polypentene alone or in combination.
[0111] In addition, in addition to polyolefins, the porous polymer film substrate can be manufactured by molding various types of polymers, such as polyesters, into a film shape. In addition, the porous polymer film substrate can be formed into a stacked structure with two or more film layers, and each film layer can be formed by polymers such as the above-mentioned polyolefins and polyesters alone or in combination.
[0112] Preferably, the porous polymer substrate may include a porous polymer film made of at least one of polyethylene or polypropylene.
[0113] In addition, in addition to the above-mentioned polyolefins, the porous polymer film substrate and the porous non-woven substrate can be made of polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenyleneoxide, polyphenylenesulfide, and polyethylenenaphthalene, alone or in combination.
[0114] There is no particular limitation on the thickness of the porous polymer substrate, but the thickness of the porous polymer substrate is preferably 1 μm to 20 μm, and more specifically 5 μm to 15 μm, and there is no particular limitation on the pore size and porosity of the porous polymer substrate, but the pore size is preferably 0.01 μm to 50 μm and the porosity is preferably 20% to 75%.
[0115] A method of manufacturing a separator according to one aspect of the present disclosure is as follows. However, the method is not limited thereto.
[0116] First, a polymer solution (S1) in which a thermosetting phenol-based resin having at least one hydroxyl group and an aromatic ring is dissolved in a solvent is prepared. In this case, the solvent preferably has a solubility index and a low boiling point similar to the thermosetting phenol-based resin. This is for ease of homogeneous mixing and subsequent solvent removal. Non-limiting examples of usable solvents may include at least one selected from ethanol, acetone, tetrahydrofuran, dichloromethane, chloroform, dimethylformamide, N-methyl-2-pyrrolidone, methyl ethyl ketone, and cyclohexane having 2 to 5 carbon atoms.
[0117] In this case, the solid in the binder polymer solution is preferably present in an amount of 7% or less.
[0118] Subsequently, the polymer solution is coated on at least one surface of the porous polymer substrate so that the coating amount of the thermosetting phenol-based resin is 100% based on per 1 m2 of the coated one surface. 2 The porous polymer substrate weighs 0.01 g to 3 g and is dried to form a polymer coating (S2).
[0119] There is no particular limitation on the method of coating the polymer solution on the porous polymer substrate, but a slit coating method or a dip coating method is preferably used. Slit coating can adjust the coating amount of the polymer coating by coating the composition supplied via a slit die on the surface of the substrate according to the flow rate supplied from a constant volume pump. In addition, dip coating is a coating method including dipping the substrate in a tank containing a slurry, and the coating amount of the polymer coating can be controlled according to the concentration of the composition and the speed at which the substrate is taken out of the composition tank, and in order to more accurately control the coating amount, after dipping, the measurement can be performed by a Meyer rod.
[0120] The porous polymer substrate coated with the polymer solution is dried using a dryer such as an oven to form a polymer coating layer on at least one surface of the porous polymer substrate.
[0121] A lithium secondary battery according to one aspect of the present disclosure includes a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, and the separator is the above-mentioned separator according to an embodiment of the present disclosure.
[0122] The lithium secondary battery may include a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, or a lithium ion polymer secondary battery.
[0123] There are no particular restrictions on the positive and negative electrodes to be used with the separator of the present disclosure, and the two electrodes can be manufactured by combining the electrode active material with the electrode current collector used in the lithium secondary battery by the method commonly used in the art. In the electrode active material, non-limiting examples of positive electrode active materials include positive electrode active materials commonly used in the positive electrode of the lithium secondary battery, in particular, lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide, lithium iron oxide, or their lithium composite oxides are preferably used. Non-limiting examples of negative electrode active materials may include negative electrode active materials commonly used in the negative electrode of the lithium secondary battery, and particularly preferably include lithium adsorption materials such as lithium metal or lithium alloys, carbon, petroleum coke, activated carbon, graphite or other carbon. Non-limiting examples of positive electrode current collectors include foils made of aluminum, nickel, or a combination thereof, and non-limiting examples of negative electrode current collectors include foils made of copper, gold, nickel, or copper alloys, or a combination thereof.
[0124] The electrolyte solution that can be used in the lithium secondary battery of the present disclosure includes a salt dissolved or dissociated in an organic solvent, wherein the salt has a + B - A salt of the structure + Such as Li + 、Na + , K+ , or a combination thereof such as an alkali metal cation, B - Is such as PF 6 - , BF 4 - , Cl - Br - ,I - , ClO 4 - , AsF 6 - , CH 3 CO 2 - CF 3 SO 3 - 、N(CF 3 SO 2 ) 2 - , C(CF 2 SO 2 ) 3 - , or a combination thereof, the organic solvent comprising at least one of propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), or γ-butyrolactone.
[0125] The injection of the electrolyte solution can be performed at any appropriate step of the battery manufacturing process according to the manufacturing process and the desired properties of the final product. That is, the injection of the electrolyte solution can be applied before the battery assembly or in the final step of the battery assembly.
[0126] Hereinafter, the present disclosure will be described in detail by embodiments / examples. However, embodiments / examples according to the present disclosure may be improved in a variety of other forms, and the scope of the present disclosure should not be interpreted as being limited to the following embodiments / examples. Embodiments / examples of the present disclosure are provided to fully explain the present disclosure to those with ordinary knowledge in the field to which the present disclosure belongs.
[0127] Examples 1-3
[0128] A thermosetting phenol-based resin (Gangnam Hwasung, resol type phenol resin, thermosetting temperature: about 150° C., acetone soluble, solid 50%, viscosity 250 mPas at 25° C.) was added to an acetone solvent in the amount shown in Table 1 and stirred at 23° C. for 30 minutes to prepare a polymer solution.
[0129] The prepared binder polymer solution was coated on both surfaces of a porous polymer substrate (polypropylene, thickness 16 μm, porosity 46%) by dip coating at 23° C. and 30% relative humidity, and then dried. Accordingly, a separator coated with a phenol-based binder polymer on both surfaces of a porous polymer substrate was manufactured.
[0130] Comparative Example 1
[0131] A porous polymer substrate (polypropylene, thickness 16 μm, porosity 46%) was used as a separator.
[0132] Comparative Example 2
[0133] Instead of the thermosetting phenol-based resin, polyvinylidene fluoride-co-hexafluoropropylene (HFP substitution rate: 8 wt %, weight average molecular weight 500,000) was added to an acetone solvent in the amount shown in Table 1 and stirred at 50° C. for 4 hours to prepare a 5 wt % polymer solution.
[0134] The prepared binder polymer solution was coated on both surfaces of a porous polymer substrate (polypropylene, thickness 16 μm, porosity 46%) by dip coating at 23° C. and 40% relative humidity, and then dried. Accordingly, a separator coated with a PVDF-HFP binder polymer on both surfaces of a porous polymer substrate was manufactured.
[0135] Embodiment 4-7
[0136] A separator was manufactured by the same method as in Example 1, except that polyethylene (9 μm, porosity 45%) was used as the porous polymer substrate and the amount of the polymer solution was controlled as shown in Table 1.
[0137] Comparative Example 3
[0138] A separator was manufactured by the same method as in Example 1, except that the amount of the thermosetting phenol-based resin in the coating solution was changed as shown in Table 1.
[0139] Comparative Example 4
[0140] Polyethylene (9 μm, porosity 45%) itself was used as a separator.
[0141] Comparative Example 5
[0142] The slurry for forming the porous coating layer is prepared by the following method. Specifically, aluminum hydroxide (Al(OH) 3) (particle size: 500nm) was added to the solvent acetone so that the percentage of solids was 30%. In this case, the percentage of solids refers to the amount of powder remaining after drying and removing the solvent in the sum of the solvent and the raw material composition. Here, isopropyl trioleyl titanate was added as a dispersant and stirred for 2 hours to prepare an inorganic particle dispersion.
[0143] Subsequently, polyvinylidene fluoride-co-hexafluoropropylene (PVDF-HFP) was added to an acetone solvent and dissolved at 50° C. for 4 hours to prepare a polymer solution.
[0144] The prepared inorganic particle dispersion and the polymer solution were mixed so that the weight ratio of the inorganic particles to the binder polymer was 75:25, and the inorganic particles were ground and dispersed using a ball milling method for 3 hours to prepare a porous coating layer forming slurry having a solid percentage of 15%.
[0145] Subsequently, the slurry forming the porous coating layer was coated on both surfaces of polypropylene (9 μm, porosity 45%) produced by a wet process at 23° C. and 40% relative humidity so that the total loading amount of the solid in the slurry was 6.9 g / m 2 , and dried to produce a separator having a porous coating layer.
[0146] Comparative Example 6
[0147] Instead of the phenol-based binder resin, polyvinylidene fluoride-co-hexafluoropropylene (HFP substitution rate: 8 wt %, weight average molecular weight 500,000) was added to an acetone solvent in an amount shown in Table 1 and stirred at 50° C. for 4 hours to prepare a 5 wt % polymer solution.
[0148] The prepared binder polymer solution was coated on both surfaces of a porous polymer substrate (polyethylene (9 μm, porosity 45%)) by dip coating at 23° C. and 40% relative humidity, and then dried. Accordingly, a separator coated with a PVDF-HFP binder polymer on both surfaces of a porous polymer substrate was manufactured.
[0149] Comparative Example 7
[0150] A separator was manufactured by the same method as in Example 4, except that the amount of the thermosetting phenol-based resin in the coating solution was changed as shown in Table 1.
[0151] [Table 1]
[0152]
[0153]
[0154] (1) Method for measuring the thermosetting temperature of thermosetting phenolic resin
[0155] For the thermosetting phenol-based resin, the exothermic peak temperature measured using a differential scanning calorimeter (DSC) is measured as the thermosetting temperature.
[0156] (2) Method for measuring air permeability
[0157] The air permeability was measured using a Gurley air permeability tester according to JIS P-8117. In this case, 100 ml of air was measured through a 28.6 mm diameter and 645 mm area. 2 The time required.
[0158] (3) Method for measuring thermal shrinkage of the separator itself before immersion in an electrolyte solution
[0159] For the separators of Comparative Examples 1 to 3 and Examples 1 to 3, the thermal shrinkage of the separator itself before being immersed in the electrolyte solution was measured. The separators of Comparative Examples 1 to 3 and Examples 1 to 3 used a polypropylene film as a porous polymer substrate, and the melting point of the polypropylene porous polymer substrate was above 150° C. Accordingly, the thermal shrinkage was calculated as (initial length-length after thermal shrinkage treatment at 150° C. / 30 min) / (initial length)×100.
[0160] Meanwhile, for the separators of Comparative Examples 4 to 7 and Examples 4 to 7, the thermal shrinkage of the separator itself before being immersed in the electrolyte solution was measured. The separators of Comparative Examples 4 to 7 and Examples 4 to 7 used a polyethylene film as a porous polymer substrate, and the thermal shrinkage was measured at 130°C, which is lower than the melting point of the polyethylene porous polymer substrate. Accordingly, the thermal shrinkage was calculated as (initial length - length after thermal shrinkage treatment at 130°C / 30min) / (initial length)×100.
[0161] (4) Method of measuring thermal shrinkage of separator after immersion in electrolyte solution
[0162] For the separators of Comparative Examples 4 to 7 and Examples 4 to 7 using a polyethylene porous polymer substrate having lower heat resistance than polypropylene, the thermal shrinkage of the separator immersed in the electrolyte solution was measured. In this case, the thermal shrinkage was calculated as (initial length - length after thermal shrinkage treatment at 150°C / 30min) / (initial length)×100.
[0163] Referring to the results of Table 1 above, Examples 1 to 3 are separators coated with a thermosetting phenol-based resin on a polypropylene porous polymer substrate, and can provide equal or similar air permeability and low thermal shrinkage when compared to Comparative Example 1 having no coating.
[0164] Comparative Example 2 is a separator having a PVDF-based polymer coating formed on a polypropylene porous polymer substrate. Comparative Example 2 and Example 2 use different resins and have the same solid content in the coating solution. It can be seen that the separator of Example 2 has improved air permeability compared with Comparative Example 2, and although every 1m 2 The porous substrates had lower polymer coating amounts but still exhibited suppressed thermal shrinkage.
[0165] The separators of Examples 4 to 7 are separators using polyethylene as the porous polymer substrate. Comparative Example 6 and Example 6 use different resins and have the same solid content in the coating solution. It can be seen that the separator of Example 6 has improved air permeability compared with Comparative Example 6, and the effect is that although the permeability is improved every 1m 2 The porous substrate has a lower polymer coating amount but still shows good thermal shrinkage suppression effect.
[0166] Meanwhile, it can be seen that in the case of Examples 1 to 3 using polypropylene as the porous polymer substrate, the increase in air permeability is small even if a coating layer is formed on the basis of Comparative Example 1. For example, it can be seen that in the case of Comparative Example 1, the air permeability is 119 sec / 100 ml, while in the case of Example 3, the air permeability value is 276 sec / 100 ml, which is increased by about 56%. It seems that since polypropylene is manufactured by a dry process, the pores in the porous polymer substrate are formed in a straight line, resulting in low tortuosity.
[0167] In contrast, in the case of Examples 4 to 7 using polyethylene as a porous polymer substrate, the increase in air permeability is higher than that of polypropylene. For example, in the case of Comparative Example 4, the air permeability is 81sec / 100ml, in the case of Example 4, the air permeability is 86sec / 100ml, and in the case of Example 7, the air permeability is 439sec / 100ml, an increase of about 81%. It seems that this is because polyethylene is manufactured by a wet method. Specifically, since the filaments in the wet separator form a pore structure under a complex entangled state, the air permeability increases very high when the adhesive polymer is wetted. However, when compared with Comparative Examples 2 and 5 with a conventional porous coating, the embodiment shows a very small increase in air permeability. In addition, compared with Comparative Examples 5 and 6 using PVDF-HFP polymers, the separators of Examples 4 to 7 using thermosetting phenol-based resins as components of the polymer coating do not have a significant reduction in the thermal shrinkage of the separator after being immersed in an electrolyte solution.
[0168] At the same time, it can be seen that including more than every 1m 2 The separators of Comparative Examples 3 and 7 of the thermosetting phenol-based resin of the porous polymer substrate 3g showed a significant decrease in air permeability.
Claims
1. A lithium secondary battery, comprising: a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, The separator comprises: a porous polymer substrate having a plurality of pores and a polymer coating formed on at least one surface of the porous polymer substrate, wherein the polymer coating comprises a thermosetting phenolic resin having at least one hydroxyl group and an aromatic ring and is free of inorganic particles, and The coating amount of the thermosetting phenolic resin is based on the coating surface per 1m 2 The porous polymer substrate is 0.01 g to 3 g; When the lithium secondary battery including the separator is exposed to a high temperature of 120° C. or higher due to combustion, the thermosetting phenol-based resin in the polymer coating layer is thermoset to form a network structure. The thermosetting phenol-based resin includes at least one of a novolac-type phenol resin represented by the following Formula 1 and a resol-type phenol resin represented by the following Formula 2: [Formula 1] In Formula 1, n is an integer of 1 or more, and R is any one of H, an optionally substituted alkyl group having 1 to 100 carbon atoms, an optionally substituted alkoxy group having 1 to 100 carbon atoms, and an optionally substituted alkenyl group having 1 to 100 carbon atoms, [Formula 2] In Formula 2, n and m are each an integer of 1 or greater, and R is any one of H, an optionally substituted alkyl group having 1 to 100 carbon atoms, an optionally substituted alkoxy group having 1 to 100 carbon atoms, and an optionally substituted alkenyl group having 1 to 100 carbon atoms. 2 . The lithium secondary battery according to claim 1 , wherein the thermosetting phenol-based resin is thermoset at 120° C. to 200° C. 3 . The lithium secondary battery according to claim 1 , wherein the thermosetting phenol-based resin is a phenolic resin.
4. The lithium secondary battery according to claim 1, wherein the coating amount of the thermosetting phenol-based resin is based on per 1 m 2 The porous polymer substrate weighs 0.05 g to 2.5 g.
5. The lithium secondary battery according to claim 1, wherein the coating amount of the thermosetting phenol-based resin is based on per 1 m 2 The porous polymer substrate weighs 0.35 g to 2.1 g. 6 . The lithium secondary battery according to claim 1 , wherein the porous polymer substrate comprises a porous polymer film made of at least one of polyethylene or polypropylene.
7. A method for manufacturing a separator for a lithium secondary battery, comprising: (S1) preparing a polymer solution in which a thermosetting phenol-based resin having at least one hydroxyl group and an aromatic ring is dissolved in a solvent; and (S2) coating the polymer solution on at least one surface of the porous polymer substrate, such that the coating amount of the thermosetting phenol-based resin is based on per 1 m2 of the coated surface. 2 0.01 g to 3 g of the porous polymer substrate, and drying to form a polymer coating, wherein the polymer coating does not contain inorganic particles; When a lithium secondary battery including the separator is exposed to a high temperature of 120° C. or higher due to combustion, the thermosetting phenol-based resin in the polymer coating layer is thermoset to form a network structure. The thermosetting phenol-based resin includes at least one of a novolac-type phenol resin represented by the following Formula 1 and a resol-type phenol resin represented by the following Formula 2: [Formula 1] In Formula 1, n is an integer of 1 or more, and R is any one of H, an optionally substituted alkyl group having 1 to 100 carbon atoms, an optionally substituted alkoxy group having 1 to 100 carbon atoms, and an optionally substituted alkenyl group having 1 to 100 carbon atoms, [Formula 2] In Formula 2, n and m are each an integer of 1 or greater, and R is any one of H, an optionally substituted alkyl group having 1 to 100 carbon atoms, an optionally substituted alkoxy group having 1 to 100 carbon atoms, and an optionally substituted alkenyl group having 1 to 100 carbon atoms. 8 . The method of manufacturing a separator for a lithium secondary battery according to claim 7 , wherein the thermosetting phenol-based resin is thermoset at 120° C. to 200° C.
9. The method for manufacturing a separator for a lithium secondary battery according to claim 7, wherein the coating amount of the thermosetting phenol-based resin is based on per 1 m 2 The porous polymer substrate weighs 0.05 g to 2.5 g.