A dual-phase particle-reinforced additive aluminum alloy and a preparation method thereof

By introducing dual-phase particles of micro-nano-scale TiB2 and nano-scale rare earth elements into Al alloys, combined with laser additive manufacturing, the thermal cracking sensitivity and interface bonding problems of Al alloys in laser additive manufacturing are solved, significantly improving the performance of aluminum alloys. The strength and plasticity of the alloy achieve high density and uniform structure.

CN115430843BActive Publication Date: 2024-10-18SHANGHAI JIAOTONG UNIV +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202210978853.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-16
Publication Date
2024-10-18
Estimated Expiration
2042-08-16

AI Technical Summary

Technical Problem

Al alloy materials limit their application in laser additive manufacturing due to their high reflectivity, easy oxidation, and high thermal conductivity. Moreover, the increased solidification temperature range of alloy elements such as Cu, Mg, and Zn increases the sensitivity to thermal cracking, making it difficult to adopt additive manufacturing. Technical preparation, poor interfacial bonding and large particle size introduced by ceramic particles in traditional powders lead to reduced reinforcement effects.

Method used

A dual-phase particle-reinforced additive aluminum alloy preparation method is used to prepare Al-M-TiB2 alloy by melting high-purity Al, Al-M master alloy, KBF4 and K2TiF6 under mechanical stirring and ultrasonic, and then vacuum air atomization powdering and mixing with High-purity rare earth metal powder is ball milled and finally formed through laser additive manufacturing to obtain a dual-phase particle-reinforced aluminum alloy of micro-nano TiB2 particles and nano-scale rare earth elements.

Benefits of technology

It achieves good combination of ceramic particles and matrix, uniform dispersion of reinforcement phase particles, improves the strength and plasticity of aluminum alloy, reaches a density of more than 99%, improves the uniformity of the structure, and significantly improves the tensile strength and plasticity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115430843B_ABST
    Figure CN115430843B_ABST
Patent Text Reader

Abstract

The present invention designs a dual-phase particle-reinforced additively manufactured aluminum alloy and a preparation method thereof. The RE / TiB2‑Al‑M alloy powder has high sphericity, has two dispersed nano-ceramic particles in the structure at the same time, and is suitable for aluminum alloys of various systems. The present invention adopts an ultrasound-assisted in-situ autogenous method and a high-energy ball milling process to introduce reinforcing phase particles and refiner elements respectively. The in-situ autogenous method is conducive to promoting the uniform dispersion of micro-nano TiB2 particles formed in the material, and exerting its heterogeneous nucleation and reinforcement effects; the introduction of ball milling is conducive to giving full play to the heterogeneous nucleation and grain refinement effects of RE refiners such as Ti / Zr, and obtaining aluminum alloy powder with high sphericity that can be mass-produced. The alloy powder is rapidly solidified by laser additive manufacturing to obtain a high-performance component with high density, no cracks, and nearly equiaxed fine-grained structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of metal material preparation and laser additive manufacturing, and in particular to a dual-phase particle reinforced additive aluminum alloy and a preparation method thereof. Background Art

[0002] With the development of aerospace and transportation, higher requirements are put forward for material performance. Traditional manufacturing methods and single materials are gradually unable to meet service requirements. Laser additive manufacturing is a disruptive technology for rapid prototyping of complex components. It has printing flexibility that traditional manufacturing technology cannot match, and it also has the characteristics of short printing cycle and high material utilization rate. It has been widely used in aerospace, molds and medical equipment. However, Al alloy materials are limited in the field of additive manufacturing due to their high laser reflectivity, easy oxidation and high thermal conductivity. In addition, although the addition of alloying elements such as Cu, Mg and Zn to Al alloys can effectively improve the mechanical properties of the materials, it also increases the solidification temperature range of the materials, thereby increasing the thermal cracking sensitivity of such materials, and cracks are generated during the solidification process, making it difficult to prepare them using additive manufacturing technology. For this reason, it is considered to increase the laser absorption rate of Al alloy powder by adding TiB2 ceramic particles, refine the grains by mixing refiner elements, promote the formation of equiaxed crystal structure to inhibit cracks, improve the energy utilization rate of the additive manufacturing process and the density of the product, and thus improve the mechanical properties.

[0003] Ball milling is a common method for reinforcing phase mixing in powders. However, the introduction of hard ceramic particles by this method can easily cause poor interface bonding and agglomeration problems due to the large difference in performance between the ceramic particles and the aluminum alloy matrix. At the same time, the particle size introduced by this method is large, which greatly reduces the reinforcing effect and the refinement effect on the aluminum alloy. In addition, the addition of a single alloying element in this way has limited contribution to strength. Summary of the invention

[0004] In order to overcome the above defects, the present invention adopts the following technical solutions:

[0005] A first aspect of the present invention provides a method for preparing a dual-phase particle reinforced additive aluminum alloy, comprising the following steps:

[0006] S1 Preparation of Al-M-TiB2 alloy: 60-92wt% high-purity Al, 1-10wt% Al-M master alloy, 3.62-36.2wt% KBF4 and 3.45-34.5wt% K2TiF6 are added to a mixed melt according to a ratio for smelting, while mechanical stirring and ultrasound are used, and then casting is performed to prepare an Al-M-TiB2 alloy ingot with uniform particles;

[0007] S2 vacuum air atomization powder making: under the action of protective gas, at a superheat of 400-4600°C, the alloy ingot obtained in step S1 is melted to obtain an alloy ingot melt, and then vacuum air atomization powder making is performed at an atomization pressure of 2-6 MPa to obtain alloy powder;

[0008] S3 ball milling: the alloy powder obtained in S2 is ball milled with high-purity rare earth (abbreviated as RE) metal powder to obtain RE-TiB2-Al-M alloy powder, and then dried to obtain dried RE-TiB2-Al-M alloy powder, wherein the mass ratio of the high-purity rare earth metal powder to the alloy powder is 0.1:99.941:99, and the mass ratio of the sum of the mass of the high-purity rare earth metal powder and the alloy powder to the mass of the ball milling ball is 1:10420;

[0009] S4 laser additive manufacturing: performing laser additive manufacturing on the RE-TiB2-Al-M alloy powder obtained in S3 to obtain the dual-phase particle reinforced additive aluminum alloy;

[0010] Furthermore, in S1, the purity of the high-purity Al is ≥ 99.999%;

[0011] Further, in S1, the Al-M master alloy is selected from any one or more of Al-50Si, Al-50Cu, Al-10Mn, and Al-10Zn;

[0012] Further, in S1, the mass ratio of Al:M:TiB2 in the Al-M-TiB2 alloy is 0.840.98:0.0140.1:0.0140.1;

[0013] Further, in S1, the average size of the Al-M-TiB2 alloy particles is 10041000nm; further, in S1, the average size of the Al-M-TiB2 alloy particles is 500nm;

[0014] Further, in S1, the primary aluminum phase grain size in the Al-M-TiB2 alloy is 2-10 μm;

[0015] Further, the specific steps of preparing Al-M-TiB2 alloy in S1 include:

[0016] S11: placing 1-10wt% Al-M master alloy and 60-92wt% high-purity Al in a crucible in sequence according to the mass ratio, then heating the alloy in the crucible to 6504800° C., and after melting, mechanically stirring the mixed melt for 5410 min;

[0017] S12: The reaction system is heated to 8104900°C, 3.62436.2wt% KBF4 and 3.45-34.5wt.% K2TiF6 are added according to the ratio, and ultrasonic treatment is performed for 10420min;

[0018] Furthermore, in S11, the speed of the graphite rotor for mechanical stirring is 150-250 r / min;

[0019] Furthermore, in S12, the ultrasonic frequency is 10430kHz and the power is 30041500W;

[0020] Further, in S2, the mass flow rate of the alloy ingot melt is 245 kg / min;

[0021] Further, in S2, the protective gas is selected from any one or two of Ar and He;

[0022] Further, in S2, the mass flow rate of the protective gas is 10430 kg / min;

[0023] Further, in S2, the nozzle diameter of the atomizing device is 0.545 mm;

[0024] Furthermore, the alloy powder obtained in step S2 is spherical and has a particle size of 20470 μm;

[0025] Furthermore, in S2, powder with a particle size of ≤50 μm accounts for more than 65 wt % of the total powder;

[0026] Furthermore, in S3, the high-purity rare earth element is Ti or Zr;

[0027] Furthermore, in S3, the purity of the high-purity rare earth metal is ≥ 99.999%;

[0028] Furthermore, in S3, the particle size of the high-purity rare earth metal powder is 40460 nm;

[0029] Further, in S3, the ball milling method is intermittent forward and reverse alternating ball milling; the ball-to-material ratio is 10:1-20:1, the ball mill speed is 200-350rpm, the ball milling time is 5-15h, and the machine is stopped for 10420min every 0.5-1h of operation;

[0030] Further, in S3, the RE-TiB2-Al-M alloy powder has a particle size of 10450 μm;

[0031] Further, in S3, the drying temperature is 70490°C and the drying time is 6410h;

[0032] Further, in S4, the parameter settings of laser additive manufacturing include: laser spot diameter is 754130μm; scanning power is 200-350W; scanning speed is 1004350mm / s; scanning spacing is 704130μm; powder thickness is 30450μm; protective gas is Ar, its flow rate is 10430kg / min, and the oxygen content of the manufacturing system is less than 20ppm; scanning strategy is strip, chessboard or honeycomb;

[0033] A second aspect of the present invention provides a dual-phase particle reinforced additive aluminum alloy prepared by any of the above methods;

[0034] Furthermore, the dual-phase particle-reinforced additive aluminum alloy contains: 1410wt% of micro-nano-scale TiB2 particles and 0.341.0wt% of nano-scale rare earth elements.

[0035] Beneficial Effects

[0036] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0037] (1) The ceramic particle introduction method provided by the present invention is an ultrasonic-assisted in-situ autogenous smelting method. The obtained particles have good interface bonding with the matrix, less agglomeration, uniform dispersion, and an average grain size of the reinforcing phase particles of 500nm, which is conducive to the full play of its reinforcing effect. At the same time, ultrasonic assistance can well promote the refining process and improve the reliability and efficiency of smelting.

[0038] (2) The refiner provided by the present invention is introduced in a manner of high-energy ball milling. The resulting metal powder has good sphericity and fluidity, which can meet the powder spreading requirements in the additive manufacturing process and facilitate the smooth progress of the laser additive manufacturing process.

[0039] (3) Compared with the existing preparation technology, the strength and plasticity of the components obtained by laser additive manufacturing are effectively improved by introducing reinforcing particles TiB2 and refiners (Ti / Zr) into the dual-phase particle reinforced aluminum alloy by in-situ ultrasonic assisted melting coupled with ball milling.

[0040] (4) The density of components formed by laser additive manufacturing of dual-phase particle reinforced aluminum alloy can reach more than 99%, and the structure is nearly equiaxed grains, which improves the uniformity of the aluminum alloy structure. The tensile strength is increased by more than 100 MPa compared with the base alloy, and the plasticity is improved by more than 100%.

[0041] (5) The method of the present invention is simple and easy to operate, has low cost and high efficiency, and has high material utilization rate, which is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1A flow chart of a dual-phase particle reinforced aluminum alloy and an additive manufacturing method thereof provided by the present invention; Specific implementation plan

[0043] The present invention is described in detail below with reference to the accompanying drawings and embodiments.

[0044] Embodiment 1:

[0045] Take the high-strength and hot-cracking Al-Cu-Mg alloy system as an example.

[0046] 430g Al-50Cu, 300g Al-10Mn master alloy and 3320g high-purity Al material are placed in a melting crucible in turn for melting, the temperature is raised to 780℃ for melting, mechanical stirring is performed for 5min, the temperature is raised to 850℃, 576g KBF4 and 550g K2TiF6 mixed salt are added, the external ultrasonic auxiliary system is turned on, the ultrasonic application time is 10min, the power is 1.5kW, and then the temperature is lowered to 700℃, 800g Al-10Mg master alloy is added, and after stirring with a stone mill rod, ultrasound is continuously applied for 5min at a power of 1kW. Subsequently, the melt is cast at 730℃ to obtain an Al-Cu-Mg-TiB2 alloy ingot, wherein the mass fraction of Cu element is 4wt.%, the mass fraction of Mg element is 1.5wt.%, the mass fraction of Mn element is 0.6wt.%, and the TiB2 content is 2wt.%. After the vacuum gas atomization process, the alloy powder containing the particle reinforcement phase was obtained. The gas atomization operation process was an atomization pressure of 5.5MPa, a mass flow rate of 4.28Kg / min, a nozzle diameter of 3.5mm, a superheat of 500℃, and Ar was used as the process protective gas. The powder obtained by gas atomization was sieved with a 200-mesh screen to obtain TiB2-Al-Cu-Mg powder with a particle size of less than 75μm.

[0047] Take high-purity Ti powder with a particle size of 40-60nm, and place 997g TiB2-Al-Cu-Mg alloy powder and 3g high-purity Ti powder in a planetary high-energy ball mill according to the mass fraction ratio (Ti:TiB2-Al-Cu-Mg=0.3:99.7). During the ball milling process, Ar is used as a protective gas, and stainless steel with a diameter of Φ4mm is added. The ball-to-material ratio is 10:1, the ball mill speed is 200rpm, the ball milling time is 8h, and the machine is stopped for 10min after each operation for 1h, and then reversed. The entire ball milling process is carried out alternately in forward and reverse directions; the ball-milled alloy powder is sieved with a 270-mesh sieve to obtain Ti / TiB2-Al-Cu-Mg powder with a particle size between 10-50μm, and placed in a vacuum drying oven at 75℃ for drying for 8h.

[0048] The Prox DMP200 laser powder bed equipment from 3D System was used for additive manufacturing. The forming parameters were: laser spot diameter: 75μm, scanning power: 250W, scanning speed maintained at 100mm / s, scanning spacing 110μm, powder thickness 40μm, scanning strategy was strip-shaped; the protective gas was Ar, and the oxygen content was less than 20ppm.

[0049] Embodiment 2:

[0050] Take the high-strength and hot-cracking Al-Cu-Mg alloy system as an example.

[0051] 430g Al-50Cu, 300g Al-10Mn master alloy and 3320g high-purity Al material are placed in a melting crucible in sequence for melting, the temperature is raised to 780℃ for melting, mechanical stirring is carried out for 5min, the graphite rotor speed is 150r / min, the temperature is raised to 850℃, 1728g KBF4 and 1650g K2TiF6 mixed salt are added, the external ultrasonic auxiliary system is turned on, the ultrasonic application time is 15min, the power is 1.5kW, and then the temperature is lowered to 700℃, 800g Al-10Mg master alloy is added, and after stirring with a stone mill rod, ultrasound is continuously applied for 8min with a power of 1kW. Subsequently, the melt is cast at 725℃ to obtain a TiB2-Al-Cu-Mg alloy ingot, wherein the mass fraction of Cu element is 4.5wt.%, the mass fraction of Mg element is 1.5wt.%, the mass fraction of Mn element is 0.6wt.%, and the TiB2 content is 6wt.%. After the vacuum gas atomization process, the alloy powder containing the particle reinforcement phase was obtained. The gas atomization operation process was an atomization pressure of 5.5MPa, a mass flow rate of 3.1Kg / min, a nozzle diameter of 3.5mm, a superheat of 450℃, and Ar was used as the process protective gas. The powder obtained by gas atomization was sieved with a 200-mesh screen to obtain TiB2-Al-Cu-Mg powder with a particle size of less than 75μm.

[0052] Take high-purity Zr powder with a particle size of 40-60nm, and place 995g TiB2-Al-Cu-Mg alloy powder and 5g high-purity Zr powder in a planetary high-energy ball mill according to the mass fraction ratio (Zr:TiB2-Al-Cu-Mg=0.5:99.5). During the ball milling process, Ar is used as a protective gas, and stainless steel with a diameter of Φ4mm is added. The ball-to-material ratio is 15:1, the ball mill speed is 300rpm, the ball milling time is 10h, and the machine is stopped for 10min after each operation for 1h, and then reversed. The entire ball milling process is carried out alternately in forward and reverse directions; the ball-milled alloy powder is sieved with a 270-mesh sieve to obtain Zr / TiB2-Al-Cu-Mg powder with a particle size between 10-50μm, and placed in a vacuum drying oven at 80℃ for drying for 5h.

[0053] The Prox DMP200 laser powder bed equipment from 3D System was used for additive manufacturing. The forming parameters were: laser spot diameter: 75μm, scanning power: 250W, scanning speed maintained at 100mm / s, scanning spacing 110μm, powder thickness 40μm, scanning strategy was strip-shaped; the protective gas was Ar, and the oxygen content was less than 20ppm.

[0054] Embodiment 3:

[0055] Take the high-strength and hot-cracking Al-Cu-Mg alloy system as an example.

[0056] 430g Al-50Cu, 300g Al-10Mn master alloy and 3320g high-purity Al material are placed in a melting crucible in sequence for melting, the temperature is raised to 780℃ for melting, mechanical stirring is carried out for 5min, the graphite rotor speed is 150r / min, the temperature is raised to 850℃, 2880g KBF4 and 2750g K2TiF6 mixed salt are added, the external ultrasonic auxiliary system is turned on, the ultrasonic application time is 15min, the power is 2kW, and then the temperature is lowered to 700℃, 800g Al-10Mg master alloy is added, and after stirring with a stone mill rod, ultrasound is continuously applied for 6min with a power of 1kW. Subsequently, the melt is cast at 725℃ to obtain a TiB2-Al-Cu-Mg alloy ingot, wherein the mass fraction of Cu element is 4.3wt.%, the mass fraction of Mg element is 1.5wt.%, the mass fraction of Mn element is 0.6wt.%, and the TiB2 content is 10wt.%. After the vacuum gas atomization process, the alloy powder containing the particle reinforcement phase is obtained. The gas atomization operation process is an atomization pressure of 6MPa, a nozzle diameter of 3.5mm, a mass flow rate of 5Kg / min, a superheat of 550℃, and Ar is used as the process protective gas. The powder obtained by gas atomization is sieved with a 200-mesh screen to obtain TiB2-Al-Cu-Mg powder with a particle size of less than 75μm.

[0057] Take high-purity Zr powder with a particle size of 40-60nm, and place 990g TiB2-Al-Cu-Mg alloy powder and 10g high-purity Zr powder in a planetary high-energy ball mill according to the mass fraction ratio (Zr:TiB2-Al-Cu-Mg=1:99) for ball milling. Ar is used as the protective gas during the ball milling process, and stainless steel with a diameter of Φ4mm is added. The ball-to-material ratio is 10:1, the ball mill speed is 300rpm, the ball milling time is 15h, and the machine is stopped for 10min after each operation for 1h, and then reversed. The entire ball milling process is carried out alternately in forward and reverse directions; the ball-milled alloy powder is sieved with a 270-mesh sieve to obtain Zr / TiB2-Al-Cu-Mg powder with a particle size between 10-50μm, and placed in a vacuum drying oven at 80℃ for drying for 10h.

[0058] The Prox DMP200 laser powder bed equipment from 3D System was used for additive manufacturing. The forming parameters were: laser spot diameter: 75μm, scanning power: 200W, scanning speed maintained at 100mm / s, scanning spacing 90μm, powder thickness 40μm, scanning strategy was strip-shaped; the protective gas was Ar, and the oxygen content was less than 20ppm.

[0059] Experimental example

[0060] Taking Al4.3Cu1.6Mg0.6Mn alloy as a comparative example, the microstructure and tensile mechanical properties of Examples 1-3 and the comparative example are shown in the following table:

[0061]

[0062] The present invention is described above by way of example in conjunction with the accompanying drawings. The specific implementation of the present invention is not limited to the above-mentioned manner. As long as various non-substantial improvements are made by using the method concept and technical solution of the present invention, or the above-mentioned concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.

Claims

1. A method for preparing an Al-Cu-Mg alloy, It is characterized in that The following steps are involved: 430 g Al-50Cu, 300 g Al-10Mn master alloy and 3320 g high purity Al were placed in a melting crucible and melted in turn. The temperature was raised to 780 °C and mechanically stirred for 5 min. The temperature was raised to 850 °C and 576 g KBF was added. 4 and 550 gK 2 TiF 6 The salt was mixed, and the external ultrasonic auxiliary system was turned on. The ultrasonic application time was 10 min at a power of 1.5 kW. The temperature was then lowered to 700 °C, 800 g of Al-10Mg master alloy was added, and the mixture was stirred with a stone mill rod and then the ultrasonic was applied for 5 min at a power of 1 kW. The melt was then cast at 730 °C to obtain Al-Cu-Mg-TiB 2 Alloy ingot, in which the mass fraction of Cu element is 4 wt.%, the mass fraction of Mg element is 1.5 wt.%, the mass fraction of Mn element is 0.6 wt.%, and the mass fraction of TiB 2 The content is 2 wt.%, and the alloy powder containing particle reinforcement phase is obtained after vacuum gas atomization process. The gas atomization operation process is atomization pressure of 5.5 MPa, mass flow rate of 4.28 Kg / min, nozzle diameter of 3.5 mm, superheat of 500 °C, and Ar is used as the process protection gas. The powder obtained by gas atomization is sieved with a 200-mesh screen to obtain TiB with a particle size of less than 75 μm. 2 - Al-Cu-Mg powder; Take high-purity Ti powder with a particle size of 40-60 nm and mix it according to the mass fraction ratio of Ti:TiB 2 -Al-Cu-Mg is 0.3:99.7, 997g TiB 2 -Al-Cu-Mg alloy powder and 3 g high-purity Ti powder were placed in a planetary high-energy ball mill for ball milling. Ar was used as the protective gas during the ball milling process, and stainless steel balls with a diameter of Φ4 mm were added. The ball-to-material ratio was 10:1, the ball mill speed was 200 rpm, the ball milling time was 8 h, and the machine was stopped for 10 min after each operation for 1 h, and then reversed. The whole ball milling process was carried out alternately in forward and reverse directions. The alloy powder after ball milling was sieved with a 270-mesh screen to obtain a particle size of 10-50 μ m between Ti / TiB 2 -Al-Cu-Mg powder was placed in a vacuum drying oven at 75 °C for 8 h; Laser powder bed equipment is used for additive manufacturing, and the forming parameters are: the laser spot diameter is 75 μ m, the scanning power was 250 W, the scanning speed was maintained at 100 mm / s, and the scanning interval was 110 μ m, powder thickness 40 μ m, the scanning strategy is stripe, the shielding gas is Ar, and the oxygen content is less than 20 ppm.

2. A method for preparing an Al-Cu-Mg alloy, It is characterized in that The following steps are involved: 430 g Al-50Cu, 300 g Al-10Mn master alloy and 3320 g high-purity Al were melted in a crucible, heated to 780 °C, stirred mechanically for 5 min, with the graphite rotor rotating at 150 r / min, heated to 850 °C, and 1728 g KBF was added. 4 and 1650 g K 2 TiF 6 The salt was mixed, and the external ultrasonic auxiliary system was turned on. The ultrasonic application time was 15 min at a power of 1.5 kW. The temperature was then lowered to 700 °C, 800 g of Al-10Mg master alloy was added, and after stirring with a stone mill rod, the ultrasonic was continued for 8 min at a power of 1 kW. The melt was then cast at 725 °C to obtain TiB 2 -Al-Cu-Mg alloy ingot, wherein the mass fraction of Cu element is 4.5 wt.%, the mass fraction of Mg element is 1.5 wt.%, the mass fraction of Mn element is 0.6 wt.%, and the mass fraction of TiB 2 The content is 6wt.%; the alloy powder containing particle reinforcement phase is obtained after vacuum gas atomization process. The gas atomization operation process is as follows: atomization pressure 5.5 MPa, mass flow rate 3.1 Kg / min, nozzle diameter 3.5 mm, superheat 450℃, Ar is used as process protection gas, and the powder obtained by gas atomization is sieved with a 200-mesh screen to obtain a particle size of 75 μ m or less TiB 2 - Al-Cu-Mg powder; Take high-purity Zr powder with a particle size of 40-60 nm and mix 995 g TiB 2 -Al-Cu-Mg alloy powder and 5 g high purity Zr powder according to the mass fraction ratio of Zr:TiB 2 -Al-Cu-Mg with a ratio of 0.5:99.5 were placed in a planetary high-energy ball mill for ball milling. Ar was used as the protective gas during the ball milling process, and stainless steel balls with a diameter of Φ4 mm were added. The ball-to-material ratio was 15:1, the ball mill speed was 300 rpm, the ball milling time was 10 h, and the machine was stopped for 10 min after each operation for 1 h, and then reversed. The whole ball milling process was carried out alternately in forward and reverse directions; the alloy powder after ball milling was sieved with a 270-mesh screen to obtain a particle size of 10-50 μ m between Zr / TiB 2 -Al-Cu-Mg powder, placed in a vacuum drying oven at 80 °C for 5 h; Laser powder bed equipment is used for additive manufacturing, and the forming parameters are: the laser spot diameter is 75 μ m, scanning power: 250 W, scanning speed maintained at 100 mm / s, scanning spacing 110 μ m, powder thickness 40 μ m, the scanning strategy is stripe; the protective gas is Ar, and the oxygen content is less than 20 ppm.

3. A method for preparing an Al-Cu-Mg alloy, It is characterized in that The following steps are involved: 430 g Al-50Cu, 300 g Al-10Mn master alloy and 3320 g high purity Al were placed in a melting crucible and melted in turn. The temperature was raised to 780 °C and mechanically stirred for 5 min. The graphite rotor speed was 150 r / min. The temperature was raised to 850 °C and 2880 g KBF was added. 4 and 2750g K 2 TiF 6 The salt was mixed, and the external ultrasonic auxiliary system was turned on. The ultrasonic application time was 15 min at a power of 2 kW. The temperature was then lowered to 700 °C, 800 g of Al-10Mg master alloy was added, and after stirring with a stone mill rod, the ultrasonic was continued for 6 min at a power of 1 kW. The melt was then cast at 725 °C to obtain TiB 2 -Al-Cu-Mg alloy ingot, wherein the mass fraction of Cu element is 4.3 wt.%, the mass fraction of Mg element is 1.5 wt.%, the mass fraction of Mn element is 0.6 wt.%, and the mass fraction of TiB 2 The content is 10wt.%, and the alloy powder containing particle reinforcement phase is obtained after vacuum gas atomization process. The gas atomization operation process is as follows: atomization pressure 6 MPa, nozzle diameter 3.5 mm, mass flow rate 5 Kg / min, superheat 550℃, Ar is used as process protection gas, and the powder obtained by gas atomization is sieved with a 200-mesh screen to obtain a particle size of 75 μ TiB2-Al-Cu-Mg powder below m; High-purity Zr powder with a particle size of 40-60 nm was taken, and 990 g of TiB2-Al-Cu-Mg alloy powder and 10 g of high-purity Zr powder were placed in a planetary high-energy ball mill with a mass fraction ratio of Zr:TiB2-Al-Cu-Mg of 1:

99. Ar was used as a protective gas during the ball milling process, and stainless steel balls with a diameter of Φ4 mm were added. The ball-to-material ratio was 10:1, the ball mill speed was 300 rpm, the ball milling time was 15 h, and the machine was stopped for 10 min after each operation for 1 h, and then reversed. The whole ball milling process was carried out alternately in forward and reverse directions; the alloy powder after ball milling was sieved with a 270-mesh sieve to obtain a particle size of 10-50 μ The Zr / TiB2-Al-Cu-Mg powder with a diameter of 100 μm was placed in a vacuum drying oven at 80 °C for 10 h; Laser powder bed equipment is used for additive manufacturing, and the forming parameters are: laser spot diameter: 75 μ m, scanning power: 200 W, scanning speed maintained at 100 mm / s, scanning spacing 90 μ m, powder thickness 40 μ m, the scanning strategy is stripe; the protective gas is Ar, and the oxygen content is less than 20 ppm.

Citation Information

Patent Citations

  • Aluminum-based composite material powder for laser reinforcement manufacturing and preparation method thereof

    CN108372292A