A negative electrode material and its preparation method and use

By internal doping of ruthenium and iridium and external coating of ruthenium oxide and iridium oxide in titanium-niobium oxide, a core-shell structure is formed, which solves the problem of poor conductivity of titanium-niobium oxide and significantly increases the capacity of lithium-ion batteries. and cycle performance.

CN115458728BActive Publication Date: 2024-10-11EVE POWER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211288503.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-20
Publication Date
2024-10-11
Estimated Expiration
2042-10-20

AI Technical Summary

Technical Problem

Existing titanium-niobium oxide lithium-ion battery anode materials have poor conductivity, which limits the diffusion of lithium ions and the lithium storage performance of the battery, and cannot effectively improve capacity and cycle performance.

Method used

Through internal doping of ruthenium and iridium and external coating of ruthenium oxide and iridium oxide, a core-shell structure is formed, reducing the grain and particle size of titanium niobium oxide, changing its surface and internal structure, and improving electronic and ion conductivity.

Benefits of technology

It significantly improves the capacity performance, fast charging performance and cycle performance of the battery, and enhances the electronic conductivity and ion conductivity of titanium niobium oxide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003900355790000151
    Figure BDA0003900355790000151
Patent Text Reader

Abstract

The present invention provides a negative electrode material and a preparation method and use thereof, wherein the negative electrode material comprises a core and a shell coated on the surface of the core, wherein the core comprises titanium niobium oxide and ruthenium and iridium doped in the titanium niobium oxide, and the shell comprises ruthenium oxide and iridium oxide. The negative electrode material provided by the present invention effectively reduces the grain size of titanium niobium oxide and the particle size of the negative electrode material through internal doping of ruthenium and iridium, and external coating of ruthenium oxide and iridium oxide, and changes the surface and internal structure of titanium niobium oxide, thereby greatly improving the electronic conductivity and ion conductivity of titanium niobium oxide, and further improving the capacity performance, fast charging performance and cycle performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery production and manufacturing, and in particular relates to a negative electrode material and a preparation method and application thereof. Background Art

[0002] With the widespread application of lithium-ion batteries in energy storage systems and electric vehicles, people have higher and higher requirements for the fast charging performance and driving range of lithium-ion batteries. Commonly used negative electrode materials for lithium-ion batteries are carbon materials and lithium titanate materials (TLO). Among them, carbon materials are structurally unstable during the rapid insertion of lithium ions, and the lithium insertion potential of carbon materials is low. Rapid charging and discharging easily forms lithium dendrites, which affects the cycle and stability of the battery cell. Lithium titanate materials have a stable spinel structure and are structurally stable during the charge and discharge cycle. They are called "zero tension" materials. At the same time, lithium titanate materials have a higher lithium insertion potential, but their theoretical specific capacity is low (175mAh / g), which greatly limits the application of lithium titanate materials.

[0003] Based on lithium titanate materials, titanium niobium oxide (TNO) has attracted widespread attention as an emerging negative electrode material for lithium batteries. Titanium niobium oxide materials have high theoretical specific capacity (387mAh / g) and stable crystal structure. Their volume changes very little during the charge and discharge cycle, and they also have the "zero tension" characteristic; and their high redox potential can avoid the formation of SEI film during the charge and discharge cycle, making them an excellent negative electrode material for lithium-ion batteries; however, titanium niobium oxide materials have poor conductivity due to their wide energy band gap and the absence of unpaired electrons, which hinders the diffusion of lithium ions, thereby severely limiting the lithium storage performance and causing serious capacity loss.

[0004] CN114420901A discloses a ruthenium-doped composite material, a preparation method and an application thereof. The ruthenium-doped composite material is a titanium niobium oxide doped with ruthenium. The structural formula of the titanium niobium oxide is TiNb2O7. The mass content of ruthenium in the ruthenium-doped composite material is 2-5%. The composite material improves the conductivity of the titanium niobium oxide to a certain extent by doping with ruthenium.

[0005] CN114388772A discloses a molybdenum-vanadium-titanium-niobium composite oxide negative electrode material and a preparation method thereof, and a lithium ion battery. The preparation method comprises: (1) mixing and crushing a first solvent, a niobium source and a titanium source to form a first mixed material, and calcining the first mixed material for the first time to obtain titanium-niobium oxide; (2) mixing and crushing a second solvent, a vanadium source, a molybdenum source and titanium-niobium oxide to form a second mixed material; and calcining the second mixed material for the second time to obtain a molybdenum-vanadium-titanium-niobium composite oxide negative electrode material, wherein vanadium and molybdenum are doped into the titanium-niobium oxide to increase the degree of electron mixing, thereby improving the conductivity of the material.

[0006] CN110380054A discloses a titanium niobium oxide electrode material and a preparation method thereof, and a lithium ion button battery. The preparation method comprises: doping titanium niobium oxide with a heterogeneous metal ion M, and the molecular formula of the titanium niobium oxide is Ti x Nb y O 2x+2.5y , where x=0.1~1, y=1~2, the electronic conductivity of titanium niobium oxide is also improved by doping with heterogeneous metal ions.

[0007] The above-mentioned documents all adopt the doping method to improve the conductivity of titanium niobium oxide, but they all adopt a simple immersion doping method to obtain the titanium niobium oxide composite material, and do not design and optimize the structure of the titanium niobium oxide composite material, so that the conductivity of the titanium niobium oxide composite material cannot be further improved, and further the capacity and cycle performance of the lithium-ion battery cannot be further improved. Summary of the invention

[0008] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a negative electrode material and a preparation method and use thereof, which effectively reduces the grain size of titanium niobium oxide and the particle size of the negative electrode material through internal doping with ruthenium and iridium, and external coating with ruthenium oxide and iridium oxide, and changes the surface and internal structure of titanium niobium oxide, thereby greatly improving the electronic conductivity and ion conductivity of titanium niobium oxide, and further improving the capacity performance, fast charging performance and cycle performance of the battery.

[0009] To achieve this object, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a negative electrode material, comprising a core and a shell covering the surface of the core, wherein the core comprises titanium niobium oxide and ruthenium and iridium doped in the titanium niobium oxide, and the shell comprises ruthenium oxide and iridium oxide.

[0011] In the present invention, both ruthenium oxide and iridium oxide are coated on the outer surface of titanium niobium oxide through chemical bonding force to form a core-shell structure, which can reduce the particle size of the negative electrode material, reduce the transmission path of lithium ions and electrons, and facilitate the rapid transmission of lithium ions and electrons to the inside of the negative electrode material; and there are Ru-O-Ir bonds, Ir-O-Ti bonds, Ti-O-Ru bonds and Ti-O-Nb bonds on the outer surface of titanium niobium oxide. Since Ru and Ir have greater binding energy with O, Ti-O-Ru bonds and Ir-O-Ti bonds are offset toward one end of Ru and Ir, and the position of the Ti element moves, resulting in changes in the surface structure of titanium niobium oxide, narrowing the energy band gap, and thus improving the electronic and ionic conductivity of titanium niobium oxide. In addition, ruthenium oxide and iridium oxide have good metallic conductivity, high specific surface area, high catalytic activity and excellent thermal stability.

[0012] At the same time, the present invention also dopes ruthenium and iridium inside the titanium niobium oxide. This is because during the three calcination processes, ruthenium ions and iridium ions can be embedded into the interior of the titanium niobium oxide and replace part of the titanium ions inside it. The ion radius of ruthenium and iridium is different from that of titanium ions, resulting in changes in the lattice parameters and unit cell volume of the titanium niobium oxide, and a decrease in the average grain size, thereby further improving the electronic conductivity of the titanium niobium oxide.

[0013] The negative electrode material provided by the present invention effectively reduces the grain size of titanium niobium oxide and the particle size of the negative electrode material through internal doping with ruthenium and iridium and external coating with ruthenium oxide and iridium oxide, and changes the surface and internal structure of titanium niobium oxide, thereby greatly improving the electronic conductivity and ion conductivity of titanium niobium oxide, and further improving the capacity performance, fast charging performance and cycle performance of the battery.

[0014] As a preferred technical solution of the present invention, the chemical formula of the negative electrode material is Ti x Nb y Ru a Ir b O, wherein 3<x<6, 5<y<9, 0.1<a<0.9, 0.1<b<0.9.

[0015] Wherein, x can be 3.1, 3.2, 3.4, 3.6, 3.8, 4, 4.2, 4.4, 4.6, 4.8, 5, 5.2, 5.4, 5.6, 5.8 or 5.9, y can be 5.1, 5.3, 5.5, 5.8, 6, 6.2, 6.5, 6.7, 7, 7.3, 7.5, 7.8, 8, 8.2, 8.5, 8.8 or 8.9, and a can be 0.11, 0.15, 0.2, 0.25, 0.3, 0.35 , 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85 or 0.89, b can be 0.11, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85 or 0.89, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0016] It should be noted that in the present invention, x:y:a:b represents the molar ratio of metal elements in the negative electrode material, that is, the molar ratio of titanium, niobium, ruthenium and iridium is (3-6):(5-9):(0.1-0.9):(0.1-0.9), and the numerical range in the molar ratio does not include the endpoint value. The reason why the molar ratio of titanium, niobium, ruthenium and iridium in the negative electrode material is limited to (3-6):(5-9):(0.1-0.9):(0.1-0.9) is that materials obtained with different molar ratios have different crystal structures, and the crystal structure is the fundamental reason that restricts the lithium ion deintercalation behavior; within the molar ratio range specified in the present invention, the obtained material is a spherical structure, and the spherical structure exposes more active surfaces, which is more conducive to the combination of lithium ions and materials.

[0017] Preferably, the negative electrode material has a spherical or quasi-spherical morphology.

[0018] Preferably, the particle size of the negative electrode material is 10 to 15 μm, for example, it can be 10 μm, 10.5 μm, 11 μm, 11.5 μm, 12 μm, 12.5 μm, 13 μm, 13.5 μm, 14 μm, 14.5 μm or 15 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] The present invention limits the particle size of the negative electrode material to 10-15μm. This is because small-particle negative electrode materials have better rate performance and cycle performance, while large-particle negative electrode materials have higher yield and compaction density. The present invention limits the particle size of the negative electrode material to 10-15μm, which can not only ensure that the first efficiency is higher than 89%, but also meet the needs of 3C charging, that is, meet the needs of fast-charging batteries.

[0020] In a second aspect, the present invention provides a method for preparing the negative electrode material according to the first aspect, the preparation method comprising:

[0021] A titanium-niobium mixed solution is dripped onto the surface of a substrate and calcined once to generate titanium-niobium oxide on the surface of the substrate. A ruthenium-iridium mixed solution is then dripped onto the surface of the substrate and calcined twice to generate an intermediate material on the surface of the substrate. The negative electrode material is then calcined three times to obtain the negative electrode material.

[0022] The present invention drips a titanium-niobium mixed solution evenly onto the surface of a substrate, and the spherical or quasi-spherical titanium-niobium oxide generated after a primary calcination adheres to the surface of the substrate; then drips a ruthenium-iridium mixed solution for secondary calcination to coat the titanium-niobium oxide on the surface of the substrate, that is, the intermediate material in the present invention also presents a core-shell structure, wherein the core includes titanium-niobium oxide, and the shell includes ruthenium oxide and iridium oxide; finally, by calcining three times, ruthenium ions and iridium ions are prompted to enter the core of the titanium-niobium oxide to replace part of the titanium ions, thereby forming a core-shell structured negative electrode material in which the core includes titanium-niobium oxide and ruthenium and iridium doped in the titanium-niobium oxide, and the shell includes ruthenium oxide and iridium oxide. In addition, the substrate in the present invention can be an inorganic glass plate.

[0023] As a preferred technical solution of the present invention, the process of generating titanium niobium oxide on the surface of the substrate includes:

[0024] The titanium-niobium mixed solution is dripped onto the surface of the substrate and calcined once, and after cooling, the process of dripping the titanium-niobium mixed solution and calcining once is repeated to generate the titanium-niobium oxide on the surface of the substrate.

[0025] The present invention adopts a method of repeated coating and calcination to prepare titanium niobium oxide, thereby loading multiple layers of titanium niobium oxide on the surface of a substrate. The repeated coating method is simple to operate, the product is controllable, and can ensure that each layer of titanium niobium mixed solution can be fully calcined to generate a complete crystal structure.

[0026] Preferably, the preparation process of the titanium-niobium mixed solution comprises: mixing a titanium source, a niobium source and a first solvent to obtain the titanium-niobium mixed solution.

[0027] In the present invention, the amount of titanium source and niobium source added can be determined according to the molar ratio in the chemical formula of the negative electrode material to be obtained and the mass of the negative electrode material to be prepared in the actual production process.

[0028] Preferably, the titanium source includes any one of titanium dioxide, metatitanic acid, titanium ethoxide, tetrabutyl titanate, tetraethyl titanate or tetraisopropyl titanate, or a combination of at least two thereof, and titanium dioxide is more preferably used.

[0029] Preferably, the niobium source includes any one of niobium pentoxide, niobium ethoxide, niobium pentachloride or niobium hydroxide, or a combination of at least two thereof, and more preferably niobium pentoxide.

[0030] Preferably, the solvent comprises deionized water.

[0031] Preferably, the titanium source, the niobium source and the solvent are mixed under stirring.

[0032] The present invention does not impose any specific requirements or restrictions on the rotation speed and time of stirring, as long as it can ensure that the titanium source and the niobium source are fully dissolved in the first solvent.

[0033] As a preferred technical solution of the present invention, the temperature of the primary calcination is 1000-1400°C, for example, it can be 1000°C, 1200°C, 1400°C, 1600°C, 1800°C, 2000°C, 2200°C, 2400°C, 2600°C, 2800°C, 3000°C, 3200°C, 3400°C, 3600°C, 3800°C or 4000°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the primary calcination time is 15 min to 1 h, for example, 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min or 60 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] When the present invention adopts the method of repeated coating and calcination to prepare titanium niobium oxide, it is preferred that the temperature and time of each calcination should be the same.

[0036] Preferably, the primary calcination is performed under an air atmosphere.

[0037] As a preferred technical solution of the present invention, the preparation process of the intermediate material includes:

[0038] The ruthenium-iridium mixed solution is dripped onto the titanium-niobium oxide and subjected to secondary calcination. After cooling, the process of dripping the ruthenium-iridium mixed solution and conducting the secondary calcination is repeated to generate the intermediate material on the surface of the substrate.

[0039] The present invention also adopts a method of repeated coating and calcination to prepare the intermediate material. The repeated coating method is simple to operate, further promotes the uniform and sufficient coating of titanium niobium oxide by ruthenium oxide and iridium oxide, and is more conducive to controlling the structure of the intermediate material.

[0040] Preferably, the preparation process of the ruthenium-iridium mixed solution comprises: mixing a ruthenium source, an iridium source and a second solvent to obtain the ruthenium-iridium mixed solution.

[0041] In the present invention, the amount of the titanium source and the niobium source added can be determined according to the molar ratio in the chemical formula of the negative electrode material to be obtained and the amount of the titanium source and the niobium source added.

[0042] Preferably, the ruthenium source includes any one of ruthenium trichloride, metallic ruthenium, ruthenium sulfate or hexachlororuthenate ammonium, or a combination of at least two thereof, and more preferably ruthenium trichloride.

[0043] Preferably, the iridium source comprises iridium chlorate.

[0044] Preferably, the second solvent comprises anhydrous ethanol.

[0045] Preferably, the ruthenium source, the iridium source and the second solvent are mixed under stirring.

[0046] The present invention does not impose any specific requirements or restrictions on the rotation speed and time of stirring, as long as it can ensure that the ruthenium source and the iridium source are fully dissolved in the second solvent.

[0047] As a preferred technical solution of the present invention, the temperature of the secondary calcination is 300-700°C, for example, it can be 300, 320, 350, 380, 400, 430, 450, 480, 500, 520, 550, 580, 600, 620, 650, 680 or 700, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0048] Preferably, the secondary calcination time is 5 to 20 min, for example, 5 min, 7 min, 9 min, 10 min, 12 min, 14 min, 16 min, 18 min or 20 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0049] Preferably, the secondary calcination is performed in an air atmosphere.

[0050] As a preferred technical solution of the present invention, the temperature of the three calcinations is 400-600°C, for example, it can be 400°C, 420°C, 440°C, 460°C, 480°C, 500°C, 520°C, 540°C, 560°C, 580°C or 600°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0051] The present invention limits the temperature of the three calcinations to 400-600°C. This is because the sintering temperature is crucial to the integrity of the crystal form. When the temperature of the three calcinations is lower than 400°C, the generated crystal form has incomplete growth and defects, and the structural stability is poor; when the temperature of the three calcinations is higher than 600°C, although the crystal form is complete, the grains are too large and the amount of active matter per unit volume is less.

[0052] Preferably, the three calcinations are performed for 0.5 to 2 h, for example, 0.5 h, 0.7 h, 0.9 h, 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h or 2 h, but are not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0053] Preferably, the three calcinations are performed under an inert atmosphere.

[0054] Preferably, the inert atmosphere comprises an argon atmosphere.

[0055] Preferably, after the three calcinations, the negative electrode material is generated on the surface of the substrate, and then separation treatment and grinding treatment are performed in sequence to obtain the negative electrode material.

[0056] The separation process in the present invention refers to separating the negative electrode material attached to the surface of the substrate, thereby obtaining the negative electrode material with a particle size of 10 to 15 μm through grinding.

[0057] Preferably, the separation process includes ultrasonic cleaning and drying.

[0058] Preferably, the grinding process comprises ball milling.

[0059] The grinding process in the present invention may be performed by ball milling in a ball mill.

[0060] As a preferred technical solution of the present invention, the preparation method comprises:

[0061] S1: a titanium source, a niobium source and a first solvent are mixed to obtain a titanium-niobium mixed solution, the titanium-niobium mixed solution is dripped onto the surface of a substrate, and a primary calcination is performed in an air atmosphere at a temperature of 1000 to 1400° C. for 15 min to 1 h, and after cooling, the process of dripping the titanium-niobium mixed solution and performing the primary calcination is repeated to generate titanium-niobium oxide on the surface of the substrate;

[0062] S2: a ruthenium source, an iridium source and a second solvent are mixed to obtain a ruthenium-iridium mixed solution, the ruthenium-iridium mixed solution is dripped onto the titanium niobium oxide, and secondary calcined at 300 to 700° C. for 5 to 20 minutes in an air atmosphere, and after cooling, the process of dripping the ruthenium-iridium mixed solution and secondary calcining is repeated to generate an intermediate material on the surface of the substrate;

[0063] S3: After the intermediate material is generated on the surface of the substrate, calcination is performed three times at a temperature of 400 to 600° C. for 0.5 to 2 h in an inert atmosphere to generate a negative electrode material on the surface of the substrate, followed by separation treatment and grinding treatment in sequence to obtain the negative electrode material.

[0064] In a third aspect, the present invention provides a lithium-ion battery, wherein the lithium-ion battery comprises the negative electrode material described in the first aspect.

[0065] Compared with the prior art, the present invention has the following beneficial effects:

[0066] The negative electrode material provided by the present invention effectively reduces the grain size of titanium niobium oxide and the particle size of the negative electrode material through internal doping with ruthenium and iridium and external coating with ruthenium oxide and iridium oxide, and changes the surface and internal structure of titanium niobium oxide, thereby greatly improving the electronic conductivity and ion conductivity of titanium niobium oxide, and further improving the capacity performance, fast charging performance and cycle performance of the battery. DETAILED DESCRIPTION

[0067] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only used to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0068] In a specific embodiment, the present invention provides a negative electrode material, which includes a core and a shell covering the surface of the core, the core includes titanium niobium oxide and ruthenium and iridium doped in the titanium niobium oxide, and the shell includes ruthenium oxide and iridium oxide; the morphology of the negative electrode material is spherical or quasi-spherical.

[0069] Example 1

[0070] This embodiment provides a method for preparing a negative electrode material, the preparation method comprising:

[0071] S1: titanium dioxide, niobium pentoxide and deionized water are mixed to obtain a titanium-niobium mixed solution, the titanium-niobium mixed solution is dripped onto the surface of the inorganic glass plate, and a primary calcination is performed at a temperature of 1200° C. for 30 minutes in an air atmosphere, and after cooling, the process of dripping the titanium-niobium mixed solution and performing the primary calcination is repeated to generate titanium-niobium oxide on the surface of the inorganic glass plate;

[0072] S2: mixing ruthenium trichloride, chloroiridic acid and anhydrous ethanol to obtain a ruthenium-iridium mixed solution, dropping the ruthenium-iridium mixed solution onto the titanium niobium oxide, and performing secondary calcination at 500° C. for 10 minutes in an air atmosphere, and repeating the process of dropping the ruthenium-iridium mixed solution and performing the secondary calcination after cooling to generate an intermediate material on the surface of the inorganic glass plate;

[0073] S3: After the intermediate material is generated on the surface of the inorganic glass plate, calcination is performed three times at a temperature of 500° C. for 1 hour in an argon atmosphere to generate a negative electrode material on the surface of the inorganic glass plate, followed by separation treatment and grinding treatment in sequence to obtain the negative electrode material; the chemical formula of the negative electrode material is Ti5Nb7Ru 0.5 Ir 0.5 O, the average particle size is 12 μm.

[0074] Example 2

[0075] This embodiment provides a method for preparing a negative electrode material, the preparation method comprising:

[0076] S1: titanium dioxide, niobium pentoxide and deionized water are mixed to obtain a titanium-niobium mixed solution, the titanium-niobium mixed solution is dripped onto the surface of an inorganic glass plate, and a primary calcination is performed at a temperature of 1000° C. for 1 hour in an air atmosphere, and after cooling, the process of dripping the titanium-niobium mixed solution and performing the primary calcination is repeated to generate titanium-niobium oxide on the surface of the inorganic glass plate;

[0077] S2: mixing ruthenium trichloride, chloroiridic acid and anhydrous ethanol to obtain a ruthenium-iridium mixed solution, dropping the ruthenium-iridium mixed solution onto the titanium niobium oxide, and performing secondary calcination at 700° C. for 5 minutes in an air atmosphere, and repeating the process of dropping the ruthenium-iridium mixed solution and performing the secondary calcination after cooling to generate an intermediate material on the surface of the inorganic glass plate;

[0078] S3: After the intermediate material is generated on the surface of the inorganic glass plate, calcination is performed three times at a temperature of 400° C. for 2 hours in an argon atmosphere to generate a negative electrode material on the surface of the inorganic glass plate, followed by separation treatment and grinding treatment in sequence to obtain the negative electrode material; the chemical formula of the negative electrode material is Ti 3.2 Nb 5.1 Ru 0.15 Ir 0.13 O, the average particle size is 10 μm.

[0079] Example 3

[0080] This embodiment provides a method for preparing a negative electrode material, the preparation method comprising:

[0081] S1: titanium dioxide, niobium pentoxide and deionized water are mixed to obtain a titanium-niobium mixed solution, the titanium-niobium mixed solution is dripped onto the surface of the inorganic glass plate, and a primary calcination is performed at a temperature of 1400° C. for 15 minutes in an air atmosphere, and after cooling, the process of dripping the titanium-niobium mixed solution and performing the primary calcination is repeated to generate titanium-niobium oxide on the surface of the inorganic glass plate;

[0082] S2: mixing ruthenium trichloride, chloroiridic acid and anhydrous ethanol to obtain a ruthenium-iridium mixed solution, dropping the ruthenium-iridium mixed solution onto the titanium niobium oxide, and performing secondary calcination at 300° C. for 20 minutes in an air atmosphere, and repeating the process of dropping the ruthenium-iridium mixed solution and performing the secondary calcination after cooling to generate an intermediate material on the surface of the inorganic glass plate;

[0083] S3: After the intermediate material is generated on the surface of the inorganic glass plate, calcination is performed three times for 0.5 h at 600° C. in an argon atmosphere to generate a negative electrode material on the surface of the inorganic glass plate, followed by separation treatment and grinding treatment in sequence to obtain the negative electrode material; the chemical formula of the negative electrode material is Ti 5.8 Nb 8.6 Ru 0.86 Ir 0.88 O, the average particle size is 15 μm.

[0084] Example 4

[0085] The difference between this embodiment and embodiment 1 is that the amount of ruthenium trichloride added in step S2 is increased, and the chemical formula Ti5Nb7Ru is obtained in step S3 1.2 Ir 0.5 O, the remaining process parameters and operating conditions are the same as those in Example 1.

[0086] Example 5

[0087] The difference between this embodiment and embodiment 1 is that the amount of ruthenium trichloride added in step S2 is reduced, and the chemical formula of Ti5Nb7Ru is obtained in step S3 0.05 Ir 0.5 O, the remaining process parameters and operating conditions are the same as those in Example 1.

[0088] Example 6

[0089] The difference between this embodiment and embodiment 1 is that the amount of chloroiridic acid added in step S2 is increased, and the chemical formula of Ti5Nb7Ru is obtained in step S3 0.5 Ir 1.2 O, the remaining process parameters and operating conditions are the same as those in Example 1.

[0090] Example 7

[0091] The difference between this embodiment and embodiment 1 is that the amount of chloroiridic acid added in step S2 is reduced, and the chemical formula Ti5Nb7Ru is obtained in step S3 0.5 Ir 0.05 O, the remaining process parameters and operating conditions are the same as those in Example 1.

[0092] Example 8

[0093] The difference between this embodiment and embodiment 1 is that the temperature of the three calcinations in step S3 is 350° C., and the other process parameters and operating conditions are the same as those in embodiment 1.

[0094] Example 9

[0095] The difference between this embodiment and embodiment 1 is that the temperature of the three calcinations in step S3 is 650° C., and the other process parameters and operating conditions are the same as those in embodiment 1.

[0096] Example 10

[0097] The difference between this embodiment and embodiment 1 is that in step S1 , the required titanium-niobium mixed solution is dripped onto the surface of the inorganic glass plate at one time, and the other process parameters and operating conditions are the same as those in embodiment 1.

[0098] Embodiment 11

[0099] The difference between this embodiment and embodiment 1 is that in step S2, the required ruthenium-iridium mixed solution is added dropwise onto the titanium-niobium oxide at one time, and the other process parameters and operating conditions are the same as those in embodiment 1.

[0100] Example 12

[0101] The difference between this embodiment and embodiment 1 is that in step S3, calcination is performed three times in an air atmosphere, and the other process parameters and operating conditions are the same as those in embodiment 1.

[0102] Comparative Example 1

[0103] The difference between this comparative example and Example 1 is that the three calcination steps are omitted in step S3, that is, the intermediate material obtained in step S2 is used as the negative electrode material, and the other process parameters and operating conditions are the same as those in Example 1.

[0104] Comparative Example 2

[0105] This comparative example provides a method for preparing a non-core-shell structured negative electrode material, the preparation method comprising:

[0106] S1: titanium dioxide, niobium pentoxide and deionized water are mixed to obtain a titanium-niobium mixed solution, ruthenium trichloride, chloroiridic acid and anhydrous ethanol are mixed to obtain a ruthenium-iridium mixed solution, and then the titanium-niobium mixed solution, the ruthenium-iridium mixed solution and the SBA-15 template are mixed to obtain a raw material mixed solution;

[0107] S2: dropping the raw material mixture in step S1 onto the surface of the inorganic glass plate, and calcining it at 1000°C for 40 minutes in an air atmosphere to generate a negative electrode material on the surface of the inorganic glass plate; then performing separation treatment and grinding treatment in sequence to obtain the negative electrode material; the chemical formula of the negative electrode material is Ti5Nb7Ru 0.5 Ir 0.5 O, the average particle size is 12 μm.

[0108] Comparative Example 3

[0109] The difference between this comparative example and Example 1 is that step S2 and the three calcination processes in S3 are omitted, that is, the titanium niobium oxide obtained in step S1 is directly used as the negative electrode material, and the other process parameters and operating conditions are the same as those in Example 1.

[0110] Comparative Example 4

[0111] In this comparative example, graphite material (material source: Shanghai Shanshan QC8 Graphite) is used as the negative electrode material.

[0112] The negative electrode materials in Examples 1-12 and Comparative Examples 1-4 were prepared into negative electrode sheets, and the negative electrode sheets were assembled into batteries. The specific process and test parameters are as follows:

[0113] (1) Preparation process of negative electrode sheet: CMC is used as a binder and mixed with water in advance to obtain a CMC solution with a solid content of 1.5%. Then, the negative electrode material, SP and CMC are added to a stirring tank in a mass ratio of 96.7:0.8:1.5 for mixing (CMC is added according to the powder mass / CMC glue solid content) to obtain a uniformly dispersed negative electrode slurry. The negative electrode slurry is evenly coated on the surface of the copper foil, and the slurry is baked to remove the moisture in the slurry to obtain a negative electrode sheet. A certain pressure is applied to the sheet for rolling to reduce the distance between particles. The rolled sheet can be cut into the required shape.

[0114] (2) Preparation process of positive electrode sheet: LFP, SP, CNT and PVDF are mixed evenly in a stirring tank at a ratio of 97.4%: 0.5%: 0.4%: 1.7%, and NMP solution is added (the required amount of NMP is calculated based on the final slurry solid content of 62%) to obtain positive electrode slurry; the evenly dispersed positive electrode slurry is coated on the surface of aluminum foil, dried, and rolled. The rolled positive electrode sheet is cut into the required size.

[0115] (3) Battery assembly process: The battery is assembled in the order of a positive electrode sheet, a separator, and a negative electrode sheet, followed by liquid injection, formation, and capacity separation. The separator is a conventional double-sided adhesive-coated separator with a base film thickness of 12 μm, a double-sided coating thickness of 4 μm, and an overall separator thickness of 16 μm.

[0116] (4) 3C charge-discharge specific capacity test parameters: The negative electrode sheet and the lithium sheet after rolling are assembled into a button battery in the glove box. The button battery is clamped on the test channel and the Land battery test program is started. Test steps: ① 3C constant current discharge to 5mv, ② stand for 10min, ③ 0.5C constant current discharge to 5mv, ④ stand for 10min, ⑤ 0.05C constant current discharge to 5mv, ⑥ stand for 10min, ⑦ 0.1C constant current charge to 2V, ⑧ cycle for 3 weeks. The average value of ①+③+⑤ for 3 times is taken as the 3C discharge gram capacity (C = 350mAh / g*negative electrode sheet weight / g*96.7%).

[0117] The results of electrochemical performance tests on batteries prepared using the negative electrode materials in Examples 1-12 and Comparative Examples 1-4 are shown in Table 1.

[0118] Table 1

[0119]

[0120] From the data in Table 1, we can get:

[0121] (1) The battery assembled from the negative electrode materials of Examples 1-3 exhibits excellent fast charging performance and cycle performance, which shows that the negative electrode material provided by the present invention effectively reduces the grain size of titanium niobium oxide and the particle size of the negative electrode material through internal doping with ruthenium and iridium, and external coating with ruthenium oxide and iridium oxide, and changes the surface and internal structure of titanium niobium oxide, thereby greatly improving the electronic conductivity and ion conductivity of titanium niobium oxide, and further improving the capacity performance, fast charging performance and cycle performance of the battery.

[0122] (2) The fast charging performance and cycle performance of the battery assembled from the negative electrode material of Example 4 are not much different from those of Example 1, which shows that even if the amount of ruthenium trichloride added is increased, the electrochemical performance of the battery will not be further improved, but the cost will increase; the fast charging performance and cycle performance of the battery assembled from the negative electrode material of Example 5 are lower than those of Example 1. This is because the amount of ruthenium trichloride added in Example 5 is too low, which shows that adjusting the amount of ruthenium added to an appropriate range is conducive to further improving the fast charging performance and cycle performance of the battery.

[0123] (3) The fast charging performance and cycle performance of the battery assembled from the negative electrode material of Example 6 are not much different from those of Example 1, which shows that even if the amount of chloroiridic acid added is increased, the electrochemical performance of the battery will not be further improved, but will lead to increased costs; the fast charging performance and cycle performance of the battery assembled from the negative electrode material of Example 7 are lower than those of Example 1. This is because the amount of chloroiridic acid added in Example 7 is too low, which shows that regulating the amount of iridium added to an appropriate range is conducive to further improving the fast charging performance and cycle performance of the battery.

[0124] (4) The fast charging performance and cycle performance of the battery assembled with the negative electrode material in Example 8 are lower than those in Example 1, and the cycle performance of the battery assembled with the negative electrode material in Example 9 is lower than that in Example 1. This is because the temperature of the three calcinations in Example 8 is too low, and the temperature of the three calcinations in Example 9 is too high. When the temperature of the three calcinations is too low, the generated crystal growth is incomplete and has defects, and the structural stability is poor; when the temperature of the three calcinations is too high, although the crystal is complete, the grains are too large and the amount of active substance per unit volume is less.

[0125] (5) The fast charging performance and cycle performance of the battery assembled from the negative electrode materials of Examples 10-12 are lower than those of Example 1. This is because in Example 10, the titanium-niobium mixed solution is added dropwise to the surface of the inorganic glass plate at one time, which cannot ensure that the titanium-niobium mixed solution is fully calcined, and the controllability of the titanium-niobium oxide is low, and the crystal integrity is poor; in Example 11, the ruthenium-iridium mixed solution is added dropwise to the titanium-niobium oxide at one time, and the coating uniformity of the titanium-niobium oxide by ruthenium oxide and iridium oxide is poor, which is not conducive to controlling the structure of the intermediate material; in Example 12, the three calcinations are carried out in an air atmosphere, which is not conducive to the ruthenium ions and iridium ions entering the inner core of the titanium-niobium oxide and replacing part of the titanium ions.

[0126] (6) The fast charging performance and cycle performance of the battery assembled from the negative electrode materials of Comparative Examples 1-3 are lower than those of Example 1. This is because Comparative Example 1 omits the three calcination processes, and thus cannot dope ruthenium and iridium inside the titanium niobium oxide. Comparative Example 2 mixes and calcines the titanium niobium mixed solution, the ruthenium iridium mixed solution and the template agent to obtain irregular Ti5Nb7Ru 0.5 Ir 0.5 O negative electrode material, rather than forming a core-shell structure; in Comparative Example 3, titanium niobium oxide is directly used as the negative electrode material; it is illustrated that the present application forms a core-shell structured negative electrode material through internal doping of ruthenium and iridium, and external coating of ruthenium oxide and iridium oxide, which can effectively reduce the grain size of titanium niobium oxide and the particle size of the negative electrode material, and change the surface and internal structure of titanium niobium oxide, thereby greatly improving the electronic conductivity and ion conductivity of titanium niobium oxide, and further improving the capacity performance, fast charging performance and cycle performance of the battery.

[0127] (7) In Comparative Example 4, the battery is directly assembled with graphite material as the negative electrode material. Although the battery has a high 3C first-cycle discharge capacity, it undergoes lithium deposition at 80% SOC during 3C constant current charging, and its cycle stability is much lower than that of Example 1. x Nb y Ru a Ir bThe 3C kinetic performance of the battery assembled with O negative electrode materials is 10% higher than that of graphite, and the capacity retention rate at room temperature and high temperature is about 5% higher. The kinetic performance is significantly better than that of graphite, which shows that the TiO2 battery provided by this application x Nb y Ru a Ir b O negative electrode material is more suitable for fast charging system than graphite.

[0128] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A negative electrode material, characterized in that: The negative electrode material comprises a core and a shell covering the surface of the core, wherein the core comprises titanium niobium oxide and ruthenium and iridium doped in the titanium niobium oxide, and the shell comprises ruthenium oxide and iridium oxide; The negative electrode material is prepared by the following method, which comprises: A titanium-niobium mixed solution is dripped onto the surface of a substrate and calcined once to generate titanium-niobium oxide on the surface of the substrate, and then a ruthenium-iridium mixed solution is dripped and calcined twice to generate an intermediate material on the surface of the substrate, and then calcined three times to obtain the negative electrode material; The secondary calcination temperature is 300-700°C and the time is 5-20min; The secondary calcination is carried out in an air atmosphere; The temperature of the three calcinations is 400-600°C and the time is 0.5-2h; The three calcinations were performed under an inert atmosphere.

2. The negative electrode material according to claim 1, characterized in that The chemical formula of the negative electrode material is Ti x Nb y Ru a Ir b Oh, Among them, 3<x<6, 5<y<9, 0.1<a<0.9, 0.1<b<0.

9.

3. The negative electrode material according to claim 1, characterized in that The negative electrode material has a spherical or quasi-spherical shape.

4. The negative electrode material according to claim 1, characterized in that The particle size of the negative electrode material is 10 to 15 μm.

5. A method for preparing a negative electrode material according to any one of claims 1 to 4, characterized in that: The preparation method comprises: A titanium-niobium mixed solution is dripped onto the surface of a substrate and calcined once to generate titanium-niobium oxide on the surface of the substrate, and then a ruthenium-iridium mixed solution is dripped and calcined twice to generate an intermediate material on the surface of the substrate, and then calcined three times to obtain the negative electrode material; The secondary calcination temperature is 300-700°C and the time is 5-20min; The secondary calcination is carried out in an air atmosphere; The temperature of the three calcinations is 400-600°C and the time is 0.5-2h; The three calcinations were performed under an inert atmosphere.

6. The preparation method according to claim 5, characterized in that: The process of generating titanium niobium oxide on the surface of the substrate comprises: The titanium-niobium mixed solution is dripped onto the surface of the substrate and calcined once, and after cooling, the process of dripping the titanium-niobium mixed solution and calcining once is repeated to generate the titanium-niobium oxide on the surface of the substrate.

7. The preparation method according to claim 5, characterized in that: The preparation process of the titanium-niobium mixed solution includes: mixing a titanium source, a niobium source and a first solvent to obtain the titanium-niobium mixed solution.

8. The preparation method according to claim 7, characterized in that: The titanium source includes any one of titanium dioxide, metatitanic acid, titanium ethoxide, tetrabutyl titanate, tetraethyl titanate or tetraisopropyl titanate, or a combination of at least two thereof.

9. The preparation method according to claim 8, characterized in that: The titanium source is titanium dioxide.

10. The preparation method according to claim 7, characterized in that: The niobium source includes any one of niobium pentoxide, niobium ethoxide, niobium pentachloride or niobium hydroxide, or a combination of at least two thereof.

11. The preparation method according to claim 10, characterized in that: The niobium source is niobium pentoxide.

12. The preparation method according to claim 7, characterized in that: The solvent includes deionized water.

13. The preparation method according to claim 7, characterized in that: The titanium source, the niobium source and the solvent are mixed under stirring.

14. The preparation method according to claim 5, characterized in that: The primary calcination temperature is 1000-1400°C.

15. The preparation method according to claim 5, characterized in that: The time of the first calcination is 15min to 1h.

16. The preparation method according to claim 5, characterized in that: The primary calcination is performed in an air atmosphere.

17. The preparation method according to claim 5, characterized in that: The preparation process of the intermediate material comprises: The ruthenium-iridium mixed solution is dripped onto the titanium-niobium oxide and subjected to secondary calcination. After cooling, the process of dripping the ruthenium-iridium mixed solution and conducting the secondary calcination is repeated to generate the intermediate material on the surface of the substrate.

18. The preparation method according to claim 5, characterized in that: The preparation process of the ruthenium-iridium mixed solution includes: mixing a ruthenium source, an iridium source and a second solvent to obtain the ruthenium-iridium mixed solution.

19. The preparation method according to claim 18, characterized in that: The ruthenium source includes any one of ruthenium trichloride, metallic ruthenium, ruthenium sulfate or hexachlororuthenate ammonium, or a combination of at least two thereof.

20. The preparation method according to claim 19, characterized in that: The ruthenium source is ruthenium trichloride.

21. The preparation method according to claim 18, characterized in that: The iridium source includes iridium chlorate.

22. The preparation method according to claim 18, characterized in that: The second solvent includes anhydrous ethanol.

23. The preparation method according to claim 18, characterized in that: The ruthenium source, the iridium source and the second solvent are mixed under stirring.

24. The preparation method according to claim 5, characterized in that: The inert atmosphere includes an argon atmosphere.

25. The preparation method according to claim 5, characterized in that: After the three calcinations, the negative electrode material is generated on the surface of the substrate, and then separation treatment and grinding treatment are performed in sequence to obtain the negative electrode material.

26. The preparation method according to claim 25, characterized in that: The separation process includes ultrasonic cleaning and drying.

27. The preparation method according to claim 25, characterized in that: The grinding process includes ball milling.

28. The preparation method according to claim 5, characterized in that: The preparation method comprises: S1: a titanium source, a niobium source and a first solvent are mixed to obtain a titanium-niobium mixed solution, the titanium-niobium mixed solution is dripped onto the surface of a substrate, and a primary calcination is performed in an air atmosphere at a temperature of 1000 to 1400° C. for 15 min to 1 h, and after cooling, the process of dripping the titanium-niobium mixed solution and performing the primary calcination is repeated to generate titanium-niobium oxide on the surface of the substrate; S2: a ruthenium source, an iridium source and a second solvent are mixed to obtain a ruthenium-iridium mixed solution, the ruthenium-iridium mixed solution is dripped onto the titanium niobium oxide, and secondary calcined at 300 to 700° C. for 5 to 20 minutes in an air atmosphere, and after cooling, the process of dripping the ruthenium-iridium mixed solution and secondary calcining is repeated to generate an intermediate material on the surface of the substrate; S3: After the intermediate material is generated on the surface of the substrate, calcination is performed three times at a temperature of 400 to 600° C. for 0.5 to 2 h in an inert atmosphere to generate a negative electrode material on the surface of the substrate, followed by separation treatment and grinding treatment in sequence to obtain the negative electrode material.

29. A lithium ion battery, characterized in that: The lithium-ion battery comprises the negative electrode material according to any one of claims 1 to 4.