Anti-glare anti-reflection films for displays
By adopting a multi-layer coating combination in the display film, utilizing the defined hierarchical structure of high refractive index and low refractive index layers, and combining the distribution of different particles, the lack of film layer hardness and wear resistance in wet coating technology is solved. problem, achieving efficient anti-glare and anti-reflection effects, improving the visibility and durability of the display.
Patent Information
- Application Number
- CN202211286869.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-20
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-10-20
AI Technical Summary
The anti-reflection film layer prepared by the existing wet coating technology has low hardness and poor wear resistance, and cannot effectively prevent glare on liquid crystal display devices, limiting the wide application of the film.
It adopts a film structure composed of a substrate, AG coating, HR coating and AR coating. The AG coating contains binder resin, inorganic wear-resistant particles and organic particles, and the HR coating contains inorganic metal oxides with high refractive index. Particles, the AR coating contains hollow silica particles, which improve anti-glare and anti-reflective properties by defining the hierarchical structure and particle size distribution.
It achieves a film layer with high definition, low flash point, good whitening suppression, high hardness and wear resistance, which improves the visibility and service life of the display.
Smart Images

Figure CN115508920B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of films, in particular to an anti-glare anti-reflection film for displays. Background Art
[0002] On display devices such as cathode ray tube display devices (CRT), plasma display devices (PDP), electroluminescent display devices (ELD) and liquid crystal display devices (LCD), anti-reflection films are usually installed on the outer surface of the display device to prevent the contrast from being reduced due to reflection of external light or to prevent external light from entering the image through reflection.
[0003] Anti-reflection film, also known as anti-reflection film, is based on the wave and interference of light. Its main function is to reduce or eliminate the reflected light on the surface of optical components, thereby increasing the transmittance of light on these components and reducing or eliminating the stray light of the system. Anti-reflection film occupies an extremely important position in the optical film industry.
[0004] Generally speaking, an anti-reflection film is an anti-reflection layer with a multilayer structure that can be formed on a transparent film substrate by chemical vapor deposition (CVD) or physical vapor deposition (PVD), as shown in the existing patent document 1. By combining a high refractive index layer and a low refractive index layer, a wide-band anti-reflection can be achieved. Although this technology has been realized in dry coating, since dry coating must be formed in a vacuum, it has the disadvantages of complex production equipment structure, high equipment investment, and low productivity. Therefore, in recent years, wet coating technology has attracted more and more attention because of its low cost, large-area coating and continuous production. However, the current existing technology is mainly a single-layer anti-reflection film coated by wet coating, as shown in patent documents 2-3.
[0005] In the field of wet coating, there is a problem that the haze of the film is too high and it cannot be used.
[0006] The light emitted by the LCD device itself and the reflected light from the ambient light source on the display screen will form glare. The long-term effect of glare on the human eye will not only cause visual discomfort, but also damage vision. For this reason, all kinds of LCD devices on the market are laminated with anti-glare film (AG film). Such hardened film must also have high wear resistance. For example, the anti-glare hardened film for electronic blackboards must also have good flash point and writing effect.
[0007] Therefore, current displays require not only an anti-reflective optical film on the surface, but also an anti-glare optical film to provide better visibility. In addition, the coating used on the display cover needs to have a higher hardness and better wear resistance, but the hardness of the low refractive index layer prepared by the current wet coating technology is low, only up to 500g / 1H, and the wear resistance is also poor, only up to 100g / 10 times. This also limits the wider application of anti-reflective films.
[0008] Existing patent technology documents:
[0009] 1. Chinese invention patent, publication number: CN104614787A.
[0010] 2. Chinese invention patent, publication number: CN1322338C.
[0011] 3. Taiwan invention patent, publication number: TWI515271B. Summary of the invention
[0012] To solve at least one of the above technical defects, the present invention provides the following technical solutions:
[0013] This application document discloses an anti-glare anti-reflection film for a display, which includes, from bottom to top, a substrate, an AG coating, an HR coating, and an AR coating;
[0014] The AG coating includes a binder resin, silica particles, organic particles, and inorganic wear-resistant particles; the silica particles are agglomerate particles of 100nm-3000nm; the organic particles are one or more of polymethyl methacrylate particles, polystyrene particles, polymethyl methacrylate-polystyrene copolymer particles, and polysilsesquioxane particles; the inorganic wear-resistant particles are formed by one or more of nano-alumina, nano-zirconia, nano-diamond, and hexagonal boron nitride nanosheets, and the inorganic wear-resistant particles are agglomerate particles of 50-200nm;
[0015] The refractive index of HR coating is 1.53-1.74;
[0016] The refractive index of AR coating is 1.2-1.48.
[0017] In this solution, the anti-glare AG coating is compounded with the high-refractive HR and low-refractive AR coatings in a defined hierarchical structure, integrating anti-glare and anti-reflection.
[0018] The composition and form of inorganic wear-resistant particles with limited form in the AG coating play the role of anti-glare and improving wear resistance by dispersing them in the binder resin. The silica form with limited particle size is preferred. The agglomerated form partially forms an undulating morphology on the surface of the coating after curing, and partially exists inside the coating, which cooperates to improve the anti-glare effect. Organic particles are preferred, which exist inside the coating and have the functions of providing internal haze, reducing the reagglomeration of silica particle agglomerates, filling resin and adjusting the refractive index difference between particles and resin, achieving internal and external haze balance. The film prepared by the coating liquid has improved properties such as hardness and wear resistance, and at the same time, the film layer has the advantages of high clarity, low flash point, and good whitening inhibition.
[0019] Furthermore, the HR coating includes a binder resin and inorganic metal oxide particles with a refractive index of 2.0-2.8, the inorganic metal oxide particles are aggregated in the coating to form particles with a particle size of 10-80 nm, and the inorganic metal oxide particles are nano zirconium oxide or titanium oxide;
[0020] The AR coating includes a binder resin and hollow silica particles with a refractive index of 1.15-1.40.
[0021] Adding inorganic metal oxides of limited form to the HR coating can reduce haze and help improve film clarity, mechanical properties, etc. Adding hollow silica to the AR coating to adjust the refractive index, etc. The film layers under the above levels and components are stably combined and have achieved breakthroughs in hardness, wear resistance and other properties.
[0022] Further, in the AG coating, relative to 22-45 parts of the binder resin, there are 3-7 parts of silica particles, 1-3 parts of organic particles, and 1-3 parts of inorganic wear-resistant particles, by mass;
[0023] In the HR coating, the nano zirconium oxide particles are 20-75 parts by mass relative to 40-200 parts of the binder resin;
[0024] In the AR coating, the hollow silica particles are contained in an amount of 30 to 80 parts by mass relative to 9 to 25 parts by mass of the binder resin.
[0025] The binder resin and the functional particles in the appropriate amount are the basic components of the coating. Lubricants, defoamers, leveling agents and other additives as well as curing agents for curing molding can be freely added according to needs.
[0026] Furthermore, the binder resin in the coating liquid component of the curing and forming AG coating, the coating liquid component of the curing and forming HR coating, and the coating liquid component of the curing and forming AR coating all include a photocurable oligomer resin with six or more functional groups and a photocurable diluent monomer resin with three or more functional groups;
[0027] The photocurable oligomer resin is one or more of polyurethane acrylate oligomer, epoxy acrylate oligomer, polyester acrylate and polyether acrylate, polyacrylic resin oligomer, epoxy resin polymer, oxygen-containing acrylate, and uric acid acrylate;
[0028] The photocurable diluent monomer resin is one or more of ethyl (meth)acrylate, ethylhexyl (meth)acrylate, styrene, methylstyrene, N-vinyl pyrrolidone monofunctional monomer, polymethylolpropane tri(meth)acrylate, diethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, hexanediol (meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and neopentyl glycol di(meth)acrylate.
[0029] The resin component with a limited structure is preferred, which is convenient for photocuring and helps to improve the hardness and flexibility of the coating.
[0030] Furthermore, the AR coating includes 2-8 parts of fluorine-containing polymer, 5-30 parts of inorganic particles, and 5-23 parts of POSS, wherein the inorganic particles are one or more of magnesium fluoride, boron nitride, silicon dioxide, and aluminum oxide, the fluorine-containing polymer is one or more of partially fluorinated acrylic ester silicone copolymers, partially or fully fluorinated acrylic compounds, and partially or fully fluorinated vinyl ethers, and the POSS is one or more of phenyl POSS, amino POSS, vinyl POSS, and acryl POSS. The fluorine-containing polymer mainly increases the water contact angle and improves the friction resistance of the coating film, the POSS increases the hardness of the AR coating, and the inorganic particles increase the friction resistance of the AR coating.
[0031] Furthermore, the AG coating liquid comprises, by mass, 18-38% of a photocurable oligomer resin having six or more functional groups, 4-7% of a photocurable diluent monomer resin having three or more functional groups; 8-12% of silica particles, 1-3% of organic particles, 1-3% of inorganic wear-resistant particles, 1-5% of an auxiliary agent, and 1-3% of a photoinitiator; preferably, the solid content of the AG coating liquid is 42-55%;
[0032] By mass, the HR coating liquid includes 1-3% of photocurable oligomer resin with six or more functional groups, 0.3-1% of photocurable diluent monomer resin with three or more functional groups; 1-3% of nano zirconium dioxide particles, 0.05-0.2% of additives, and 0.1-0.5% of photoinitiator; preferably, the solid content of the HR coating liquid is 3-6%.
[0033] By mass, the AR coating solution includes 0.25-0.5% of a photocurable oligomer resin having six or more functional groups, 0.05-0.1% of a photocurable diluent monomer resin having three or more functional groups, 0.3-1.5% of hollow silica particles, 0.1-1% of solid silica particles, 0.1-1% of POSS, and 0.1-0.5% of a photoinitiator. Preferably, the solid content of the AR coating solution is 2.0-5.0%.
[0034] The coating liquid has a preferred component ratio and a photocuring molding mechanism. When in use, each coating liquid can be coated by known coating techniques such as slit coating, micro-concave coating, blade coating, roller coating, etc., and then cured by one or a combination of ultraviolet light curing, electron radiation curing, thermal curing, etc. Since ultraviolet light curing has the advantage of more types of raw materials to choose from, ultraviolet light curing is preferred.
[0035] As for additives, such as wet leveling agents, defoaming agents, polymerization inhibitors, surface control agents, etc., photoinitiators such as acetophenones, benzophenones, thioxanthones, benzoin, benzoin methyl ether, aromatic diazonium salts, aromatic sulfonium salts, aromatic iodonium salts, metallocene compounds, benzoin sulfonates, and active organic amines such as triethylamine, n-butylamine, etc. can also be selected as auxiliary initiators.
[0036] For solvents, such as polar solvents and non-polar solvents, specifically acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl formate, ethyl formate, propyl formate, butyl formate, methanol, ethanol, propanol, isopropanol, isobutanol, propylene glycol methyl ether, and n-butanol can be selected, preferably methyl isobutyl ketone, propylene glycol methyl ether, isobutanol, ethyl acetate, and butyl acetate. It can be a single solvent, and preferably a mixed solvent of three or more.
[0037] Further, in the AG coating liquid group: the silicon dioxide particles are added in the form of a dispersion liquid, and mixed with a solvent with a primary particle size of 10nm-50nm to obtain a silicon dioxide particle dispersion liquid with a secondary particle size of 100nm-2000nm;
[0038] The inorganic wear-resistant particles are added in the form of a dispersion, and mixed with a solvent with a primary particle size of 10-50 nm to obtain a dispersion with a secondary particle size of 50-200 nm;
[0039] The particle size of the organic particles is 1 μm-10 μm.
[0040] The limited shape and addition form have been tested to help further improve the performance of the film.
[0041] Furthermore, the average particle size of nano zirconium oxide particles is 5%-80% of the thickness of the HR coating; the hollow silica particle size is 50-80nm, and the average particle size of solid silica is 30%-100% of the thickness of the AR film layer, which helps to improve the performance of the film layer.
[0042] Furthermore, the inorganic wear-resistant particles are formed of hexagonal boron nitride nanosheets, and the pretreatment step is: mixing the hexagonal boron nitride nanosheets of the original particle size with the solvent and performing ultrasonic dispersion treatment to obtain a glue solution, and centrifuging the glue solution to obtain a bottom solid;
[0043] Repeat the above pretreatment steps on the primary bottom solid to obtain a secondary bottom solid;
[0044] Repeat the above pretreatment steps for the secondary bottom solid and collect the resulting centrifuge liquid, which is the dispersion liquid of the inorganic wear-resistant particles. Targeted design of the dispersion liquid preparation process helps to evenly distribute and thus improve the performance of the membrane layer.
[0045] Hexagonal boron nitride nanosheets can be prepared by known preparation methods, such as arc discharge method, solvent thermal method, vapor deposition method, and liquid phase method. Because nanoparticles have high surface energy and are easy to agglomerate, their surfaces need to be treated, such as polymer dispersant and coupling agent treatment, preferably a silane coupling agent that can react with resin to obtain reactive functional groups is used as the surface treatment agent.
[0046] Furthermore, the nano zirconium oxide particles are in tetragonal phase, cubic phase or a mixture of the two. The limited phase helps to improve the performance of the film layer.
[0047] Further, the nano zirconium oxide particles are added to the coating solution of the cured HR coating in the form of a dispersion. The dispersion of the nano zirconium oxide particles is prepared as follows:
[0048] First, a zirconium-containing compound is mixed with a mixture of a solvent and an organic acid in proportion, the temperature is raised to 250-320° C., and the reaction is carried out at a constant temperature for 3-18 hours;
[0049] Second, the filtered product obtained by the reaction is washed several times to obtain tetragonal or cubic nano zirconium oxide particles;
[0050] Third, the obtained nano-zirconia particles and dispersing aid are added into a solvent to obtain a transparent nano-zirconia dispersion, in which the nano-zirconia particles form an agglomerated state with a secondary dispersion particle size of 10-50 nm.
[0051] Crystalline nano zirconium oxide is prepared by a one-step solvent thermal synthesis method. The raw materials are a zirconium-containing compound and an organic solvent, or a mixture of an organic solvent and an organic acid. The zirconium-containing compound can be an organic zirconium compound, including n-propanol, zirconium n-butoxide, zirconium tetra-tert-butoxide, etc., or an inorganic zirconium compound, including zirconium nitrate, zirconium chloride, basic zirconium carbonate, etc., preferably an organic zirconium compound, more preferably zirconium n-propanol. The organic solvent includes methanol, ethanol, butyl ether, benzyl alcohol, etc., preferably methanol, ethanol, benzyl alcohol, and the organic acid includes formic acid, hemp acid, stearic acid, oleic acid, etc., preferably formic acid and oleic acid.
[0052] The solvent used for the nano zirconium oxide dispersion can be a polar solvent or a non-polar solvent, such as n-hexane, toluene, ethanol, butyl acetate, ethyl acetate, isopropanol, isobutanol, acetone, butanone, methyl isobutyl ketone, propylene glycol methyl ether, etc., preferably toluene, butyl acetate, isopropanol, isobutanol, methyl isobutyl ketone, propylene glycol methyl ether, etc.
[0053] When preparing the nano zirconium oxide dispersion, it is necessary to add an appropriate amount of dispersing aid, which can be a silane coupling agent, a titanate coupling agent, a high molecular polymer with surface affinity, an acrylate monomer and an acrylate oligomer, preferably a high molecular polymer with surface affinity and an acrylate monomer, to disperse the zirconium oxide powder.
[0054] The process flow and reaction temperature are limited under this technology, which helps to obtain the desired form of nano zirconium oxide.
[0055] Furthermore, the thickness of the AG coating is 2-50 μm and the surface water contact angle of the AG coating is less than 80°, and the optical thickness of the HR coating is 1 / 2λ 0 , the optical thickness of the AR coating is 1 / 4λ 0 .
[0056] By limiting the optical thickness relationship of the coating, a wide-band anti-reflection film with a W-shaped reflectivity curve can be obtained.
[0057] As for the substrate, it can be one of the substrates such as triacetylcellulose film (TAC), polyethylene terephthalate film (PET), polynorbornene film (COP), polymethyl methacrylate film (PMMA), polycarbonate film (PC), transparent polyimide film (CPI), etc. In terms of transparency and optical retardation, triacetylcellulose film (TAC) is preferred. The thickness of the transparent substrate is preferably 25μm-300μm. When used as a polarizer surface protective film, it is preferably 25μm-80μm for thinning considerations.
[0058] Compared with the prior art, the present invention has the following beneficial effects:
[0059] 1. The film layer of the present invention integrates anti-glare and anti-reflection, and has the advantages of high clarity, low flash point, good whitening inhibition, high hardness, wear resistance, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0061] Figure 1 The film structure of AG-HR-AR film is described;
[0062] Figure 2 The transmittance and reflectance spectra of the AG1-HR1-AR1 film of Example 1;
[0063] Figure 3 The transmittance and reflectance spectra of the AG2-HR1-AR1 film of Example 2;
[0064] Figure 4 The transmittance and reflectance spectra of the AG1-HR1-AR2 film of Comparative Example 1;
[0065] Figure 5 The transmittance and reflectance spectra of the AG1-AR1 film of Comparative Example 2;
[0066] Figure 6 This is a scanning electron microscope cross-sectional view of the AG layer of the AG1-HR1-AR1 film of Example 1;
[0067] Figure 7 This is a magnified cross-sectional view of the AG layer of the AG1-HR1-AR1 film of Example 1 taken by scanning electron microscopy;
[0068] Figure 8 This is a scanning electron microscope cross-sectional view of the AR layer of the AG1-HR1-AR1 film of Example 1;
[0069] Fig. 9 This is an electron microscope photo of the crystalline nano-zirconia of Example 7;
[0070] Fig.10 This is the XRD spectrum of the crystalline nano zirconium oxide of Example 7;
[0071] Fig.11 This is the particle size distribution diagram of the zirconium oxide dispersion of Example 7.
[0072] Wherein, the accompanying drawings are marked as follows:
[0073] 10. substrate; 20. AG coating; 21. organic microparticles; 22. silica particle agglomerates; 23. inorganic wear-resistant particle agglomerates; 30. HR coating; 31. nano zirconium oxide particle agglomerates; 40. AR coating; 41. hollow silica particles; 42. solid silica particles. DETAILED DESCRIPTION
[0074] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.
[0075] First, preparation of crystalline nano-zirconia dispersion
[0076] Case 1, Preparation method of crystalline nano zirconium oxide dispersion: add zirconium propoxide and benzyl alcohol in a mass ratio of 0.6:1 into the kettle (the total volume of the reactants does not exceed 60% of the kettle volume), set the speed to 450 rpm, and the maximum temperature of the kettle is 225°C. After the reaction is completed, the obtained powder is washed with ethanol and propylene glycol methyl ether for multiple times, and then propylene glycol methyl ether is used as a solvent and a high molecular polymer is used as a dispersing aid to ultrasonically disperse the zirconium oxide powder to obtain a nano zirconium oxide dispersion, and the solid content of the dispersion is 20%. The dispersed particle size of nano zirconium oxide is 52nm, and the primary particle size of nano zirconium oxide is 5-10nm. According to XRD test, the crystal form of nano zirconium oxide is a mixed type of tetragonal and cubic zirconium oxide.
[0077] Case 2, preparation method of crystalline nano zirconium oxide dispersion: n-butoxide zirconium and diacetone alcohol are added to the kettle at a mass ratio of 0.56:1 (the total volume of the reactants does not exceed 60% of the kettle volume), the speed is set to 450 rpm, and the maximum temperature of the kettle is 225°C. After the reaction is completed, the obtained powder is washed with ethanol and MIBK for multiple times, and then MIBK is used as a solvent and a high molecular polymer is used as a dispersing aid to ultrasonically disperse the zirconium oxide powder to obtain a nano zirconium oxide dispersion, and the solid content of the dispersion is 20%. The dispersed particle size of nano zirconium oxide is 42nm, and the primary particle size of nano zirconium oxide is 8-12nm. According to XRD testing, the crystal form of nano zirconium oxide is a mixed type of tetragonal and cubic zirconium oxide.
[0078] Case 3, Preparation method of crystalline nano zirconium oxide dispersion: add basic zirconium carbonate and n-hexanol into the kettle at a mass ratio of 0.62:1 (the total volume of the reactants does not exceed 60% of the kettle volume), set the speed to 450 rpm, and the maximum temperature of the kettle is 225°C. After the reaction is completed, the obtained powder is washed with ethanol and MIBK for multiple times, and then MIBK is used as a solvent and a high molecular polymer is used as a dispersing aid to ultrasonically disperse the zirconium oxide powder to obtain a zirconium oxide dispersion, and the solid content of the dispersion is 20%. The dispersed particle size of nano zirconium oxide is 45nm, and the primary particle size of nano zirconium oxide is 8-12nm. According to XRD test, the crystal form of nano zirconium oxide is a mixed type of tetragonal and cubic zirconium oxide.
[0079] Case 4, preparation method of crystalline nano zirconium oxide dispersion: add zirconium n-butoxide and benzyl alcohol into the kettle at a mass ratio of 0.48:1 (the total volume of the reactants does not exceed 60% of the kettle volume), set the speed to 450 rpm, and the maximum temperature of the kettle is 225°C. After the reaction is completed, the obtained powder is washed with ethanol and MIBK for multiple times, and then MIBK is used as a solvent and a high molecular polymer is used as a dispersing aid to ultrasonically disperse the zirconium oxide powder to obtain a zirconium oxide dispersion, and the solid content of the dispersion is 20%. The dispersed particle size of nano zirconium oxide is 45nm, and the primary particle size of nano zirconium oxide is 8-12nm. According to XRD test, the crystal form of nano zirconium oxide is a mixed type of tetragonal and cubic zirconium oxide.
[0080] Case 5, Preparation method of crystalline nano zirconium oxide dispersion: Add zirconium nitrate, urea and water in a mass ratio of 0.48: 1 to the kettle (the total volume of the reactants does not exceed 60% of the kettle volume), set the speed to 450 rpm, and the maximum temperature of the kettle to 220°C. After the reaction is completed, the obtained powder is washed with ethanol and MIBK for multiple times, and then MIBK is used as a solvent and a high molecular polymer is used as a dispersing aid to ultrasonically disperse the zirconium oxide powder to obtain a zirconium oxide dispersion, and the solid content of the dispersion is 20%. The primary particle size of nano zirconium oxide is 20-25nm. According to XRD testing, the crystal form of nano zirconium oxide is a mixture of monoclinic phase and tetragonal phase. Since the reaction is carried out in an aqueous solution, it is difficult to completely remove the water in subsequent treatment, so the secondary particle size of the obtained dispersion is larger, greater than 100nm, and the dispersion is slightly turbid, not transparent.
[0081] Case 6, Preparation method of crystalline nano zirconium oxide dispersion: add zirconium tetratert-butoxide and benzyl alcohol into the kettle at a mass ratio of 0.6:1 (the total volume of the reactants does not exceed 60% of the kettle volume), set the speed to 450 rpm, and the maximum temperature of the kettle is 300°C. After the reaction is completed, the obtained powder is washed with ethanol and propylene glycol methyl ether for multiple times, and then propylene glycol methyl ether is used as a solvent, and a high molecular polymer is used as a dispersing aid to ultrasonically disperse the zirconium oxide powder to obtain a zirconium oxide dispersion, and the solid content of the dispersion is 20%. The primary particle size of nano zirconium oxide is 15-25nm. According to XRD testing, the crystal form of nano zirconium oxide is mainly cubic phase. The primary particle size of nano zirconium oxide prepared at too high a reaction temperature is larger and more difficult to disperse. The secondary particle size of the nano zirconium oxide dispersion prepared under this condition is greater than 100nm, and the dispersion is slightly turbid and not transparent.
[0082] The above examples and comparative examples show that the selection of different raw materials and solvents will affect the primary particle size and crystal form of nano-zirconia, and the obtained nano-zirconia dispersed particle size is larger. When this nano-zirconia dispersion is added to the HR coating, the transmittance of the coating will be low, the haze will be high, and the refractive index of the coating will be affected, see the following comparative example 3.
[0083] Second, the preparation of dispersion
[0084] Silica particle dispersion: The dispersion is obtained by grinding commercially available solid silica particles (without surface treatment) with an original particle size of 10-50 nm in an ethanol solvent by ball milling to obtain a silica particle dispersion with a secondary dispersion particle size within a predetermined range. The secondary dispersion particle size can be adjusted by adjusting the solvent ratio, grinding parameters, etc., which will not be described in detail.
[0085] Inorganic wear-resistant particle dispersion: First, pretreatment step: deionized water and ethanol are mixed in a volume ratio of 1:1, and commercially available hexagonal boron nitride nanosheets (without surface treatment) with a primary particle size of 10-50nm are added under stirring, stirred for 6-24 hours, and ultrasonically dispersed for about 10 minutes. The dispersion is then centrifuged at a centrifuge speed of 6000-10000rpm for 5-10 minutes, the upper clear liquid is discarded, and a precipitate (primary bottom solid) is left.
[0086] Then, the above pretreatment steps (mixing with solvent, stirring, ultrasonication, centrifugation) are repeated with the primary bottom solid to obtain a secondary bottom solid for standby use.
[0087] Finally, the solvent and the secondary bottom solid are subjected to the above-mentioned pretreatment step to obtain a centrifugal colloidal solution, which is a nano hexagonal boron nitride dispersion.
[0088] The bottom precipitate continues to undergo the above pretreatment step, collects the centrifugal colloidal solution, and then performs the above pretreatment step on the bottom solid precipitate centrifuged until there is no precipitate at the bottom. The collected centrifugal colloidal solution is the nano hexagonal boron nitride dispersion.
[0089] The particle size can be obtained by adjusting parameters such as stirring, ultrasound, and centrifugation, which will not be elaborated here.
[0090] Third, the preparation of coating solution
[0091] Preparation of coating liquid AG1: 10 kg of coating liquid is prepared according to mass percentage, of which 28% is a decafunctional polyurethane acrylate oligomer, 3% is a hexafunctional polyurethane acrylate oligomer, 3% is a trifunctional acrylate monomer, 3% is a hexafunctional acrylate monomer, 2% is a thiol inhibitor, 8% is silica with a dispersed particle size of 240 nm, 0.5% is polysilsesquioxane microparticles, 2% is hexagonal boron nitride nanosheets with a dispersed particle size of 80 nm, and 2% is a photoinitiator. The above raw materials are added to a mixed solvent of butyl acetate and isobutyl alcohol, and stirred until the above components are completely dissolved to obtain a coating liquid AG1 with a solid content of 51.5%.
[0092] Preparation of coating liquid AG2: 10 kg of coating liquid is prepared according to mass percentage, of which nine-functional polyurethane acrylate oligomer accounts for 21.5%, thirty-functional hyperbranched acrylate oligomer accounts for 2.8%, three-functional acrylate monomer accounts for 1.0%, six-functional acrylate monomer accounts for 2.4%, thiol inhibitor accounts for 2%, polyethylene glycol 600DA accounts for 1.9%, silicon dioxide with a dispersed particle size of 350 nm accounts for 8%, cross-linked polystyrene particles account for 1%, nano-diamond particles with a dispersed particle size of 100 nm account for 2%, and photoinitiator accounts for 2.1%. Add the above raw materials into a mixed solvent of butyl acetate and propylene glycol methyl ether, stir until the above components are completely dissolved, and obtain a coating liquid AG2 with a solid content of 44.7%.
[0093] Preparation of coating liquid AG3: 10 kg of coating liquid is prepared according to mass percentage, of which nine-functional polyurethane acrylate oligomer accounts for 21.7%, thirty-functional hyperbranched acrylate oligomer accounts for 3.1%, three-functional acrylate monomer accounts for 1.2%, six-functional acrylate monomer accounts for 2.4%, thiol inhibitor accounts for 1.9%, polyethylene glycol 600DA accounts for 2%, the secondary particle size of the dispersion is 600 nm, silicon dioxide accounts for 10%, polymethyl methacrylate particles account for 1.5%, nano-alumina particles with a dispersed particle size of 80 nm account for 2%, and photoinitiator accounts for 2.1%. The above raw materials are added to a mixed solvent of butyl acetate and propylene glycol methyl ether, and stirred until the above components are completely dissolved to obtain a coating liquid AG3 with a solid content of 47.9%.
[0094] Preparation of coating liquid AG4: The preparation method of coating liquid 3 is followed, except that no polymethyl methacrylate particles are added.
[0095] Preparation of coating liquid AG5: The preparation method of coating liquid 3 is followed, except that no nano-alumina particles are added.
[0096] Preparation of coating liquid HR1: 10 kg of coating liquid is prepared according to mass percentage, wherein aliphatic hexaacrylate accounts for 1.24%, pentafunctional polyurethane acrylate prepolymer accounts for 0.165%, tetrafunctional acrylate monomer accounts for 0.245%, trifunctional acrylate monomer accounts for 0.31%, nano zirconium oxide with a dispersed particle size of 20 nm (Case 1) accounts for 1.4%, leveling agent accounts for 0.11%, and photoinitiator accounts for 0.27%. The above raw materials are added to propylene glycol methyl ether solvent. Stir until the above components are completely dissolved to obtain coating liquid HR1 with a solid content of 3.7%.
[0097] Preparation of coating liquid HR2: According to the preparation method of coating liquid HR1, the zirconium oxide dispersion with a dispersed particle size greater than 100 nm prepared in Case 5 was selected.
[0098] Preparation of coating liquid AR1: 10 kg of coating liquid is prepared according to mass percentage, of which nine-functional aliphatic polyurethane acrylate accounts for 0.314%, trifunctional epoxy acrylate accounts for 0.078%, 70 nm hollow silica accounts for 1.26%, solid silica accounts for 0.27%, POSS accounts for 0.5%, and photoinitiator accounts for 0.24%. The above raw materials are added to methyl isobutyl ketone and a mixed solvent of methyl isobutyl ketone, propylene glycol methyl ether, isobutyl alcohol, ethyl acetate, and butyl acetate, and stirred until the above components are completely dissolved to obtain a coating liquid AR1 with a solid content of 2.7%.
[0099] Preparation of coating liquid AR2: The same preparation method as coating liquid AR1 was used, except that 20 nm hollow silica was used.
[0100] Preparation of coating liquid AR3: The same preparation method as coating liquid AR1 was used, except that solid silica was not added.
[0101] Preparation of coating liquid AR4: Use the preparation method of coating liquid AR1 without adding POSS.
[0102] Fourth, coating preparation
[0103] The film structure in the following embodiments is shown in Table 1.
[0104] Example 1
[0105] First, the coating liquid AG1 was coated on a triacetylcellulose film with a thickness of 80 μm using a micro-concave roll coater and dried at 80° C. Thereafter, the coating was cured with a high-pressure mercury lamp at a curing energy of 600 mJ / cm2 in a nitrogen atmosphere, and the coating thickness was 4 μm to obtain a film AG1. The surface water contact angle of the AG coating was less than 80°.
[0106] Then, the coating liquid HR1 was coated on the AG1 film using a slit coater and dried at 80°C. After that, the coating was cured using a high-pressure mercury lamp at a curing energy of 600 mJ / cm2 in a nitrogen atmosphere. The coating thickness of HR was (1 / 2)λ 0 , and obtained membrane AG1-HR1.
[0107] Finally, the coating liquid AR1 was coated on the above AG1-HR1 film using a slit coater and dried at 80°C. After that, the coating was cured with a high-pressure mercury lamp at a curing energy of 600mJ / cm2 in a nitrogen atmosphere. The coating thickness of AR was (1 / 4) λ 0 , and obtained membrane AG1-HR1-AR1.
[0108] Example 2
[0109] According to the method of Example 1, the coating thickness of HR is halved to 1 / 4λ 0 , and the film AG1-HR1(1 / 4λ 0 )-AR1.
[0110] Example 3
[0111] According to the method of Example 1, the coating liquid AG1 was replaced by AG2 (the surface water contact angle was lower than 80°) to obtain the film AG2-HR1-AR1.
[0112] Example 4
[0113] According to the method of Example 1, the coating liquid AG1 was replaced by AG3 (the surface water contact angle was lower than 80°) to obtain the film AG3-HR1-AR1.
[0114] Example 5
[0115] According to the method of Example 1, the coating liquid AG1 was replaced by AG4 (the surface water contact angle was lower than 80°) to obtain the film AG4-HR1-AR1.
[0116] Example 6
[0117] According to the method of Example 1, the coating liquid AG1 was replaced by AG5 (the surface water contact angle was lower than 80°) to obtain the film AG5-HR1-AR1.
[0118] Comparative Example 1
[0119] According to the method of Example 1, the coating liquid AR1 is replaced by AR2 to obtain the film AG1-HR1-AR2.
[0120] Comparative Example 2
[0121] Films AG1-AR1 were obtained by following the method of Example 1 without coating the HR layer.
[0122] Comparative Example 3
[0123] According to the method of Example 1, the coating liquid HR1 is replaced by HR2 to obtain the film AG1-HR2-AR1.
[0124] Comparative Example 4
[0125] According to the method of Example 1, the coating liquid AG1 is replaced by AG2, and the coating liquid AR1 is replaced by AR3 to obtain the film AG2-HR1-AR3.
[0126] Comparative Example 5
[0127] According to the method of Example 1, the coating liquid AG1 was replaced by AG3, and the coating liquid AR1 was replaced by AR4 to obtain the film AG3-HR1-AR4.
[0128] Fifth, testing
[0129] The structure of the film layer of the present invention Figure 1 As shown, the bottom is a transparent substrate 10, on which are arranged in sequence an AG coating 20, an HR coating 30, and an AR coating 40; the AG coating 20 contains organic microparticles 21, silica particle agglomerates 22, inorganic wear-resistant particle agglomerates 23, and silica particle agglomerates 22 located on the surface; the HR coating 30 contains nano-zirconia particle agglomerates 31; and the AR coating 40 contains hollow silica particles 41 and solid silica particles 42.
[0130] Description of test evaluation method:
[0131] 1. Optical properties of anti-reflection film
[0132] Testing instrument: UV spectrophotometer
[0133] Testing method: The coated flexible film is subjected to an optical performance test to test the transmittance and reflectivity of the film in the range of 300-1100nm.
[0134] 2. Hydrophobic function of anti-reflection film
[0135] Testing instrument: contact angle tester
[0136] Detection method: The coated flexible film is subjected to a water contact angle test with a water drop volume of 2 μl.
[0137] 3. Wear resistance of anti-reflection film
[0138] Testing equipment: Friction tester
[0139] Testing method: The coated flexible film is subjected to a friction resistance test, weights are placed according to different requirements, and the number of sliding times and speed are changed.
[0140] 4. Hardness of anti-reflection film
[0141] Testing instrument: Electric pencil hardness tester
[0142] Testing method: The coated flexible film is subjected to a hardness test, the test requirements are: 500g, speed 40.
[0143] 5. Determination of coating refractive index:
[0144] Inspection instrument: Ellipsometer Semilab SE-2000
[0145] Test method: The coating liquid is plated on the silicon wafer by the pull-up coating method, and the silicon wafer is placed in an ellipsometer for testing.
[0146] 6. Coating thickness:
[0147] Inspection instrument: Thickness gauge
[0148] Test method: Place the coated flexible film on a thickness gauge for testing.
[0149] 7. Coating haze:
[0150] Inspection instrument: Photoelectric haze meter WGW
[0151] Test method: Place the coated flexible film in a haze meter for testing.
[0152] 8. Clarity and whitening suppression test of anti-glare film
[0153] Clarity: Observe the outline of the fluorescent lamp tube through the anti-glare film and evaluate the film's transmittance and diffusion properties.
[0154] The lamp is clearly visible, with clear outlines and no diffusion effect
[0155] ○: The lamp can be seen, but its outline is slightly blurred
[0156] ×: The lamp cannot be seen clearly, and the diffusion effect is obvious
[0157] Whitening inhibition: stick the anti-glare film on a black acrylic plate and observe the whitening of the coating:
[0158] Excellent whitening inhibition
[0159] ○: Good whitening suppression
[0160] ×: Poor whitening suppression property.
[0161] The test results are shown in Table 1. Figure 2-Figure 11 As shown:
[0162]
[0163] It can be seen from the results of Example 1 and Comparative Example 1 that when 20 nm hollow silica particles are selected for the AR coating, the wear resistance will be improved, but the optical properties will be affected, so it is necessary to select hollow silica particles with a suitable particle size.
[0164] It can be seen from the results of Example 1 and Comparative Example 2 that when the HR layer is added, the hardness and wear resistance of the coating film are improved, the transmittance is increased, and the reflectivity is reduced, so it is necessary to select hollow silica particles with a suitable particle size.
[0165] From the results of Example 1 and Comparative Example 3, it can be seen that when nano zirconium oxide particles with a dispersed particle size greater than 100 nm are added to the HR coating, the optical transmittance of the coating will be affected, so HR is preferred.
[0166] It can be seen from the results of Example 3 and Comparative Example 4 that when solid silica particles are not added to the AR coating, the wear resistance of the coating decreases.
[0167] It can be seen from the results of Example 4 and Comparative Example 5 that when POSS is not added to the AR coating, the hardness and wear resistance of the coating film decrease.
[0168] It can be seen from the results of Example 5 that when no organic particles are added to the AG layer, the total haze of the coating film is significantly reduced because the internal haze cannot be obtained by increasing the internal scattering.
[0169] It can be seen from the results of Example 6 that when no inorganic wear-resistant particles are added to the AG layer, the steel wool wear resistance of the coating film is significantly reduced.
[0170] The above are only preferred embodiments of the present invention. The protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. An anti-glare anti-reflection film for a display, characterized in that: From bottom to top, it includes substrate, AG coating, HR coating, and AR coating; The AG coating includes a binder resin, silica particles, organic particles, and inorganic wear-resistant particles; the silica particles are 600nm agglomerate particles; the organic particles are one or more of polymethyl methacrylate particles, polystyrene particles, polymethyl methacrylate-polystyrene copolymer particles, and polysilsesquioxane particles; the inorganic wear-resistant particles are one or more of nano-alumina, nano-zirconia, nano-diamond, and hexagonal boron nitride nanosheets, and the inorganic wear-resistant particles are 50-200nm agglomerate particles; The refractive index of HR coating is 1.53-1.74; The refractive index of AR coating is 1.2-1.48; The HR coating includes a binder resin and inorganic metal oxide particles with a refractive index of 2.0-2.
8. The inorganic metal oxide particles are aggregated in the coating to form particles with a particle size of 10-80 nm. The inorganic metal oxide particles are nano zirconium oxide or titanium oxide. The AR coating includes a binder resin, hollow silica particles with a refractive index of 1.15-1.40; In the AG coating, the content of silica particles is 3-7 parts, organic particles is 1-3 parts, and inorganic wear-resistant particles is 1-3 parts, relative to 22-45 parts of the binder resin, by mass; In the HR coating, the nano zirconium oxide particles are 20-75 parts by mass relative to 40-200 parts of the binder resin; In the AR coating, the hollow silica particles are 30-80 parts by mass relative to 9-25 parts by mass of the binder resin; In the AG coating liquid group: the silicon dioxide particles are added in the form of a dispersion liquid, and are mixed with a solvent with a primary particle size of 10nm-50nm to obtain a silicon dioxide particle dispersion liquid with a secondary particle size of 600nm; The inorganic wear-resistant particles are added in the form of a dispersion, and mixed with a solvent with a primary particle size of 10-50 nm to obtain a dispersion with a secondary particle size of 50-200 nm; The particle size of the organic particles is 1 μm-10 μm; The binder resin of the AG coating includes a photocurable oligomer resin having six or more functional groups and a photocurable diluent monomer resin having three or more functional groups.
2. The anti-glare anti-reflection film for display according to claim 1, characterized in that: The binder resins in the AG coating, HR coating and AR coating all include photocurable oligomer resins with six or more functional groups and photocurable diluent monomer resins with three or more functional groups; The photocurable oligomer resin is one or more of polyurethane acrylate oligomer, epoxy acrylate oligomer, polyester acrylate and polyether acrylate, polyacrylic resin oligomer, epoxy resin polymer, oxygen-containing acrylate, and uric acid acrylate; The photocurable diluent monomer resin is one or more of ethyl (meth)acrylate, ethylhexyl (meth)acrylate, styrene, methylstyrene, N-vinyl pyrrolidone monofunctional monomer, polymethylolpropane tri(meth)acrylate, diethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, hexanediol (meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and neopentyl glycol di(meth)acrylate.
3. The anti-glare anti-reflection film for display according to claim 2, characterized in that: The AR coating includes 2-8 parts of fluorine-containing polymer, 5-30 parts of inorganic particles, and 5-23 parts of POSS. The inorganic particles are one or more of magnesium fluoride, boron nitride, silicon dioxide, and aluminum oxide. The fluorine-containing polymer is one or more of partially fluorinated acrylate silicone copolymers, partially or fully fluorinated acrylic compounds, and partially or fully fluorinated vinyl ethers. The POSS is one or more of phenyl POSS, amino POSS, vinyl POSS, and acryl POSS.
4. The anti-glare anti-reflection film for display according to claim 3, characterized in that: By mass, the AG coating liquid includes 18-38% of photocurable oligomer resin with six functional groups or more, 4-7% of photocurable diluent monomer resin with three functional groups or more; 8-12% of silica particles, 1-3% of organic particles, 1-3% of inorganic wear-resistant particles, 1-5% of additives, and 1-3% of photoinitiator; By mass, the HR coating liquid includes 1-3% of photocurable oligomer resin with six functional groups or more, 0.3-1% of photocurable diluent monomer resin with three functional groups or more; 1-3% of nano zirconium dioxide particles, 0.05-0.2% of additives, and 0.1-0.5% of photoinitiator; By mass, the AR coating solution includes 0.25-0.5% of photocurable oligomer resin with six or more functional groups, 0.05-0.1% of photocurable diluent monomer resin with three or more functional groups, 0.3-1.5% of hollow silica particles, 0.1-1% of solid silica particles, 0.1-1% of POSS, and 0.1-0.5% of photoinitiator.
5. The anti-glare anti-reflection film for display according to claim 3, characterized in that: The average particle size of the nano zirconium oxide particles is 5%-80% of the thickness of the HR coating; the particle size of the hollow silica is 50-80nm, and the average particle size of the solid silica is 30%-100% of the thickness of the AR film.
6. The anti-glare anti-reflection film for display according to claim 4, characterized in that: The inorganic wear-resistant particles are formed of hexagonal boron nitride nanosheets, and the pretreatment step is: mixing the hexagonal boron nitride nanosheets of the original particle size with the solvent and performing ultrasonic dispersion treatment to obtain a glue solution, and centrifuging the glue solution to obtain a bottom solid; Repeat the above pretreatment steps on the primary bottom solid to obtain a secondary bottom solid; Repeat the above pretreatment steps for the secondary bottom solid and collect the resulting centrifuge liquid, which is the dispersion of inorganic wear-resistant particles.
7. The anti-glare anti-reflection film for display according to claim 1, characterized in that: The nano zirconium oxide particles are of tetragonal phase, cubic phase or a mixture of the two.
8. The anti-glare anti-reflection film for display according to claim 7, characterized in that: Nano-zirconia particles are added to the coating solution of the cured HR coating in the form of a dispersion. The dispersion of nano-zirconia particles is prepared as follows: First, a zirconium-containing compound is mixed with a mixture of a solvent and an organic acid in proportion, the temperature is raised to 250-320° C., and the reaction is carried out at a constant temperature for 3-18 hours; Second, the filtered product obtained by the reaction is washed several times to obtain tetragonal or cubic nano zirconium oxide particles; Third, the obtained nano-zirconia particles and dispersing aid are added into a solvent to obtain a transparent nano-zirconia dispersion, in which the nano-zirconia particles form an agglomerated state with a secondary dispersion particle size of 10-50 nm.
9. The anti-glare anti-reflection film for display according to claim 1, characterized in that: The thickness of the AG coating is 2-50 μm and the surface water contact angle of the AG coating is lower than 80°, the optical thickness of the HR coating is 1 / 2λ0, and the optical thickness of the AR coating is 1 / 4λ0.